A method for improving the bonding strength of tire inner liner by using functionalized dull powder
By functionalizing the desulfurization tailings of molten iron and combining the gradient inner lining structure with a four-stage composite bonding process, the problem of insufficient interface bonding strength between the tire inner lining and the reinforcing layer is solved, achieving high-strength interface bonding and excellent airtightness. It is suitable for the differentiated performance optimization of tubeless, inner tube and mining tires.
Patent Information
- Application Number
- CN202611254929.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-18
- Publication Date
- 2026-11-24
Smart Images

Figure CN123152174A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of tire manufacturing technology, and in particular relates to a method for improving the bonding strength of tire inner liner using functionalized passivation powder. Background Technology
[0002] The tire inner liner (also known as the airtight layer) is a core component that ensures tire inflation pressure. Its main function is to prevent gas penetration and slow tire leakage. The lamination of the inner liner with the reinforcing layer (ply) is one of the key processes in tire forming. Currently, there are several main technical routes for the lamination of the inner liner and reinforcing layer: First, calendering lamination, which involves pressing the airtight layer and transition layer rubber into sheets of a fixed width using a four-roll calender and then thermally bonding them to the fiber ply; second, extrusion thermal bonding, which involves extruding the airtight layer and transition layer separately using an extruder and then thermally bonding them using a lamination roller machine; third, cutting the inner liner to a fixed length on a forming machine and bonding it to the surface of a bonding drum, followed by the sequential bonding of the ply layers. In addition, there are derivative processes such as cold lamination and dual-head lamination. These processes are widely used in the tire industry, with mature equipment and high production efficiency, meeting the production needs of conventional tire products.
[0003] However, the existing technologies still have the following shortcomings: First, in existing bonding processes, the interfacial bonding between the liner and the reinforcing layer mainly relies on the adhesiveness of the rubber material itself and the chemical cross-linking during vulcanization, lacking active means to strengthen the bonding interface, resulting in limited interfacial bonding strength and easy interlayer delamination. Second, the liner usually adopts a homogeneous structure design, with fillers (such as carbon black) uniformly distributed in the thickness direction, making it impossible to achieve functional differentiation in different parts of the liner—high density is required near the airtight layer to ensure airtight performance, while high activity is required near the reinforcing layer to improve interfacial bonding strength; a homogeneous structure cannot meet both of these dual requirements. Third, existing bonding processes usually use a one-time pressing method with constant temperature and pressure, lacking precise control over the penetration depth of the rubber compound and the quality of interfacial bonding during the bonding process, making it difficult for the rubber compound to fully penetrate into the fabric gaps, resulting in insufficient interfacial bonding strength. Fourth, research on the application of industrial solid waste (such as desulfurization tailings from molten iron) in tire inner linings is still in its early stages. When unfunctionalized passivated powder is used directly as a filler, its interfacial bonding with the rubber matrix is weak, and its porous structure may become a gas permeation channel, further deteriorating airtightness. These shortcomings restrict further improvement in the composite bonding quality of tire inner linings and reinforcing layers. Summary of the Invention
[0004] To overcome the aforementioned deficiencies of the prior art, this invention provides a method for improving the bonding strength of tire inner liner using functionalized passivation powder. This method solves the problems in the prior art where homogeneous inner liners cannot simultaneously meet the dual requirements of airtightness and interfacial bonding; constant temperature and pressure bonding lacks active reinforcement methods, resulting in insufficient rubber penetration and limited interlayer bonding strength; and the problem that unfunctionalized passivation powder has weak bonding force with rubber when used directly.
[0005] To achieve the above objectives, the present invention provides the following technical solution: A method for improving the bonding strength of tire inner liner using functionalized passivation powder includes the following steps: S1. Passivation powder pretreatment: After crushing the desulfurization tailings of molten iron, the powder is acid-washed, washed, dried and roasted to obtain activated passivation powder. S2. Passive powder pore filling: The activated passive powder obtained in S1 is placed in an impregnation tank. After vacuuming, the filler containing thermoplastic polymer and microcapsules coated with cross-linking active ingredients is heated to melt and injected to impregnate and fill the pores of the passive powder. The vacuum is then released to obtain filled passive powder. S3. Surface sealing: The passivating powder obtained in S2 is mixed with a sealing agent, so that the sealing agent coats the surface of the passivating powder to obtain a sealed passivating powder; the sealing agent seals the pore openings on the surface of the passivating powder in the early stage of mixing (when the temperature is below its melting point) to prevent the filler from escaping prematurely under the mechanical shearing action of mixing; when the mixing temperature rises above the melting point of the sealing agent, the sealing agent melts and integrates into the rubber matrix. At this time, the filler is still bound by the capillary force of the pores of the passivating powder and will not be released spontaneously until sufficient pressure difference is applied in the subsequent negative pressure stage before it is extracted; S4. Surface chemical grafting modification: The sealing passivation powder obtained in S3 is grafted with silane coupling agent and titanate coupling agent in sequence to obtain modified functionalized passivation powder. S5. Mixing and gradient compounding: The modified functionalized passivation powder obtained in S4 is mixed with the rubber matrix to prepare the first compound, the second compound, and the third compound with a gradient change in passivation powder content. S6. Multilayer co-extrusion: The first rubber compound, the second rubber compound, and the third rubber compound are co-extruded to form an inner liner layer consisting of a surface layer, an intermediate transition layer, and a bottom layer along the thickness direction. The content of modified functionalized passivation powder in the bottom layer is higher than that in the surface layer, and the content of the intermediate transition layer is between the two. S7. Four-stage composite bonding: A bonding drum with through holes distributed on the surface and a vacuum channel connected to a vacuum source is provided inside. The inner liner and the reinforcing layer with fiber bundle gaps are positioned on the bonding drum so that the bottom layer of the inner liner is opposite to the reinforcing layer. Phase 1: Start the vacuum source to create a first negative pressure on the surface of the bonding drum, and pre-press the bonding with a first temperature and a first pressure; Phase Two: Adjusting the vacuum source creates a second negative pressure with a larger absolute value on the surface of the bonding drum. This second pressure continues the pressing process, causing the filler material within the pores of the passivated powder to be released under the pressure difference. The perforated structure on the surface of the bonding drum allows the negative pressure to act on microscopic local areas of the liner layer, forming low-pressure zones at the perforations. Driven by the pressure difference, the high-pressure filler material within the pores is released outwards and migrates to the interface between the liner layer and the reinforcing layer. Simultaneously, the liner layer is adsorbed onto the drum surface, ensuring close contact between the bottom layer and the reinforcing layer, providing favorable conditions for the directional migration of the released filler material into the gaps between the fiber bundles of the reinforcing layer. Phase 3: Adjust the vacuum source to generate a third negative pressure on the surface of the bonding drum, raise the temperature to the second temperature and the pressure to the third pressure, so that the released filler can penetrate into the gaps between the fiber bundles of the reinforcing layer under the combined action of positive pressure and negative pressure. Stage 4: Heat to the third temperature and maintain the third pressure to allow the filler to solidify in the gaps between the fiber bundles of the reinforcing layer to form a micro-bonded structure.
[0006] Preferably, in S1, the pulverized powder is pulverized to D50≤18μm; the acid washing is to soak in 5%, 10%, and 15% phosphoric acid aqueous solutions for 10~30min each; the drying is to dry at 105~110℃ to constant weight; and the calcination is to calcinate at 300~350℃ for 2h.
[0007] Preferably, in S2, the vacuum condition is an absolute pressure of 2-5 kPa inside the container, maintained for 30 min; the filling material impregnation temperature is 60-70℃, and the impregnation time is 60-90 min; the thermoplastic polymer is at least one of low molecular weight butyl rubber and polyisobutylene, with a Mooney viscosity ML(1+8) at 125℃ of 25-35 or a number-average molecular weight of 1000-3000; the microcapsule shell material is melamine resin or urea-formaldehyde resin, and the core material is at least one of accelerator CZ, accelerator DM, sulfur, and insoluble sulfur, with a particle size of 1-10 μm, a shell thickness of 0.2-0.5 μm, and a thermal decomposition temperature of 80-100℃; based on 100 parts of the total mass of the filling material, the thermoplastic polymer accounts for 70-85 parts, and the microcapsules account for 15-30 parts.
[0008] Preferably, in step S3, the sealing agent is stearic acid or a low softening point wax with a melting point of 50-60°C; the mass ratio of filler powder to sealing agent is 100:1-3; the mixing temperature is 70-80°C, the rotation speed is 500-1000 rpm, and the time is 10-15 min.
[0009] Preferably, in step S4, the silane coupling agent is KH-550 or Si-69, the mass ratio of sealing passivation powder to silane coupling agent is 100:1.5~3.0, the grafting reaction temperature is 80~90℃, and the time is 30~60min; the titanate coupling agent is CS-105, the mass ratio of primary modified passivation powder to titanate coupling agent is 100:0.5~1.5, the grafting reaction temperature is 80~90℃, and the time is 30~60min.
[0010] Preferably, in S5, based on 100 parts by weight of the rubber matrix, the first rubber compound has a passive powder content of 5-10 phr, the second rubber compound has a content of 15-20 phr, and the third rubber compound has a content of 25-30 phr; the rubber matrix is at least one of natural rubber, butyl rubber, chlorinated butyl rubber, and brominated butyl rubber; the mixing and discharge temperature is 140-150℃.
[0011] Preferably, in S5, based on 100 parts by weight of the rubber matrix, the raw materials of the first rubber compound, the second rubber compound, and the third rubber compound each further include 20-40 parts of carbon black N660, 3-5 parts of zinc oxide, 1-3 parts of stearic acid, 1-2 parts of accelerator, 1.5-2.5 parts of sulfur, and 1-2 parts of antioxidant.
[0012] Preferably, in S6, the surface layer thickness accounts for 15-25% of the total thickness of the inner liner layer, the intermediate transition layer accounts for 45-55%, and the bottom layer accounts for 25-35%; the co-extrusion temperature is 90-100℃.
[0013] Preferably, in S7, the reinforcing layer is a fiber fabric layer; the aperture of the through hole on the surface of the bonding drum is 0.2~0.5mm; the negative pressure is gauge pressure, with the first negative pressure being -30~-50kPa, the second negative pressure being -60~-80kPa, and the third negative pressure being -40~-50kPa; the first pressure being 0.2~0.3MPa, the second pressure being 0.3~0.5MPa, and the third pressure being 0.5~1.2MPa; the first temperature being 80~90℃, the second temperature being 90~100℃, and the third temperature being 100~110℃; the duration of stage one being 0~0.5s, stage two being 0.5~1.0s, stage three being 1.0~2.0s, and stage four being 1.0~2.0s.
[0014] Preferably, in S7, for tubeless tires, the second negative pressure is -70~-80 kPa, the third pressure is 0.5~0.8 MPa, and the third temperature is 100~105℃; for tubed tires, the second negative pressure is -60~-70 kPa, the third pressure is 0.6~1.0 MPa, and the third temperature is 105~110℃; for mining tires, the second negative pressure is -65~-75 kPa, the third pressure is 1.0~1.2 MPa, and the third temperature is 105~110℃.
[0015] The technical effects and advantages of the method for improving the bonding strength of tire inner liner using functionalized passivation powder according to the present invention are as follows: 1. This invention transforms the passivation powder from an inert filler into a functionalized active filler with temperature and pressure response release capability by sequentially performing S1 phosphoric acid gradient treatment to create pores, S2 vacuum impregnation filling with thermoplastic polymers and microcapsules, S3 surface sealing, and S4 double coupling agent grafting modification on the passivation powder. The multi-level porous structure formed by the phosphoric acid gradient treatment in S1 provides physical loading space for the filler; the vacuum negative pressure impregnation in S2 allows the filler to fully penetrate into the pores of the passivation powder at each level; the surface sealing in S3 ensures that the filler is stably sealed and does not release prematurely during mixing and extrusion; the stepwise grafting of silane coupling agent and titanate coupling agent in S4 forms a chemical bond layer on the surface of the passivation powder, improving the interfacial compatibility between the passivation powder and the rubber matrix. At the same time, the alkaline surface of the unmodified area promotes rubber vulcanization, forming a synergistic effect of "the modified area providing chemical bonding force and the unmodified area promoting vulcanization". The synergistic effect of the above-mentioned technical features enables the passive powder and the rubber matrix to form a dual bonding mechanism of chemical bonding and physical anchoring, which significantly improves the interfacial bonding strength between the filler and the rubber matrix.
[0016] 2. This invention involves preparing three sets of adhesives with passivation powder contents of 5-10 phr, 15-20 phr, and 25-30 phr respectively via S5. These are then co-extruded in three layers via S6 to form an inner liner layer consisting of a surface layer, an intermediate transition layer, and a bottom layer along the thickness direction. The bottom layer has a higher passivation powder content than the surface layer, while the intermediate transition layer falls between the two. This gradient structure enables functional division of the inner liner layer along the thickness direction: the low passivation powder content of the surface layer forms a dense, airtight layer, effectively blocking gas permeation; the high passivation powder content of the bottom layer provides a sufficient source of filler release for the bonding interface, facilitating interlayer penetration and bonding; and the intermediate transition layer provides a buffer transition in modulus and performance between the surface and bottom layers, eliminating interlayer stress concentration. The synergistic effect of the three-layer gradient structure gives the inner liner layer both excellent airtightness and interfacial bonding performance.
[0017] 3. This invention divides the bonding process into four stages via S7, each stage employing different combinations of vacuum negative pressure, bonding temperature, and bonding pressure parameters. Stage 1 achieves precise positioning and pre-bonding of the liner layer and reinforcing layer through a first negative pressure, first temperature, and first pressure. Stage 2 triggers the controlled release of the filler within the pores of the passivation powder under pressure differential driven by a second negative pressure with a larger absolute value, causing the filler to migrate from the passivation powder interior to the interface region. Stage 3 drives the released filler to penetrate into the fiber bundle gaps of the reinforcing layer through the synergistic effect of a third negative pressure and positive pressure, achieving full penetration at the microscale. Stage 4 heats up to the third temperature, causing the filler to solidify in the fiber bundle gaps to form a micro-bonded structure. A sequential logical chain of "positioning—release—penetration—solidification" is formed between the four stages. The temperature and pressure parameters of each stage are interconnected and coordinated, achieving on-demand release, directional migration, and in-situ solidification of the filler, forming a micro-anchoring structure in the fiber bundle gaps of the reinforcing layer, significantly enhancing the interfacial bonding strength between the liner layer and the reinforcing layer.
[0018] 4. In this invention, the three-layer gradient inner liner structure of S6 and the four-stage composite bonding process of S7 form a synergistic effect: the high passivation powder content in the bottom layer of the gradient structure provides a sufficient material basis for the release of fillers in the four-stage bonding, ensuring a sufficient source of fillers for the negative pressure-triggered release in stage two; the low passivation powder content in the surface layer ensures that even if some fillers migrate towards the surface during bonding, the airtightness of the airtight layer can still be guaranteed; the buffering effect of the intermediate transition layer ensures that the stress generated by the alternating positive and negative pressure during bonding is uniformly transmitted in the thickness direction, avoiding interface damage caused by interlayer stress concentration. The material gradient distribution provided by the three-layer gradient structure and the time-sequential temperature and pressure control provided by the four-stage bonding work together to achieve a high-strength interfacial bond between the inner liner and the reinforcing layer, while maintaining the excellent overall airtightness of the inner liner.
[0019] 5. This invention achieves differentiated performance optimization for tubeless tires, tubed tires, and mining tires by adjusting the composition of the passivation powder filler, the type of coupling agent, and the bonding process parameters. For tubeless tires, a high proportion of butyl rubber filler is used to significantly improve air tightness and fatigue resistance. For tubed tires, antioxidants are added to the filler, and a natural rubber matrix and Si-69 coupling agent are used to significantly improve bead flexural durability and resistance to thermo-oxidative aging. For mining tires, a blended NR / BR rubber matrix is used, and reinforcing resin is added to the filler to significantly improve abrasion resistance and tear resistance. These differentiated solutions enable this invention to meet the diverse needs of different markets for the composite bonding performance of tire inner liner and reinforcing layer.
[0020] 6. This invention organically combines the passivation powder functionalization treatment (S1-S4), the three-layer gradient inner liner structure (S5-S6), and the four-stage composite bonding process (S7). This transforms the passivation powder from a "passive filler" into an "active functional element" with temperature and pressure response release function; transforms the inner liner from a "homogeneous material" into a "structured material" with gradient functional distribution; and transforms the bonding process from "constant temperature and pressure single-stage pressing" to "time-sequential temperature and pressure precisely controlled staged composite bonding." The technical features at these three levels are interdependent and synergistic, jointly achieving a comprehensive improvement in the interfacial bonding strength, airtightness, and fatigue life between the inner liner and the reinforcing layer. Attached Figure Description
[0021] Figure 1 This is a flowchart of a method for improving the bonding strength of tire inner liner using functionalized passivation powder, as proposed in this invention. Detailed Implementation
[0022] The technical solutions of the present invention will be clearly and completely described below with reference to the accompanying drawings of the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. All other embodiments obtained by those skilled in the art based on the embodiments of the present invention without creative effort are within the scope of protection of the present invention.
[0023] It should be noted that, in this document, relational terms such as "first" and "second" are used only to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include," "contain," or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, article, or apparatus that includes a list of elements includes not only those elements but also other elements not expressly listed, or elements inherent to such a process, method, article, or apparatus. Without further limitation, an element defined by the phrase "includes..." does not exclude the presence of other identical elements in the process, method, article, or apparatus that includes the element.
[0024] refer to Figure 1 The scope of protection of this invention is not limited to the following embodiments. All raw materials used in the embodiments are commercially available industrial products. The desulfurization tailings of molten iron are taken from the desulfurization process of steel enterprises, and their main chemical composition, by mass percentage, is: CaO 35~50%. 10~20% 15~30% The content of free calcium oxide is 3-8%, zinc oxide 3-10%, and carbon black N660, zinc oxide, stearic acid, accelerator CZ, accelerator DM, sulfur, and antioxidant 4010NA are all commercially available products commonly used in the rubber industry. Silane coupling agents KH-550 (γ-aminopropyltriethoxysilane), Si-69 (bis-[γ-(triethoxysilyl)propyl]tetrasulfide), and CS-105 (isopropyltris(dioctylpyrophosphate)titanate) are all commercially available industrial products. The Mooney viscosity (ML(1+8)) of low molecular weight butyl rubber at 125℃ is 25-35, and the number average molecular weight of polyisobutylene is 1000-3000. The microcapsules are prepared in the laboratory. The shell material is melamine resin or urea-formaldehyde resin, and the core material is selected from at least one of accelerator CZ, accelerator DM, sulfur and insoluble sulfur. In this embodiment, a mixture of accelerator CZ and sulfur (mass ratio 1:1) is used as an example. The microcapsule particle size is 1~10μm, the shell thickness is 0.2~0.5μm, and the thermal decomposition temperature is 80~100℃.
[0025] The bonding drum is a laboratory-simulated bonding device. The drum surface has through-holes with a diameter of 0.2~0.5mm, and an internal vacuum channel connected to a vacuum pump. The reinforcing layer is a polyester fiber cord layer (1100 dtex / 2, warp and weft density 100×100 threads / 10cm) with fiber bundle gaps. The bonding pressure roller is a heat-controlled rubber roller equipped with a pressure sensor and temperature control device.
[0026] Performance testing methods: Tensile strength is tested according to GB / T528-2009; tear strength is tested according to GB / T529-2008; Shore A hardness is tested according to GB / T531.1-2008; abrasion loss is tested according to GB / T1689-2014; flexural fatigue is tested according to GB / T13934-2006; air tightness (permeability) is tested according to GB / T7755-2003; dynamic heat generation is tested according to GB / T1687-2010; and peel strength is tested according to GB / T532-2008. Fatigue life is tested using an MTS fatigue testing machine in strain control mode. Test conditions: frequency 10Hz, strain amplitude ±50%, temperature 25℃. The fatigue life is defined as the number of cycles at which the specimen fractures.
[0027] The microcapsules and modified functionalized passivation powder used in this application are not novel chemical entities, but are prepared from known materials using known methods. The shell material (melamine resin or urea-formaldehyde resin), core material (accelerator CZ, DM, sulfur, insoluble sulfur), particle size (1~10 μm), shell thickness (0.2~0.5 μm), and thermal decomposition temperature (80~100℃) of the microcapsules are all clearly defined. The preparation method (S1~S4) of the modified functionalized passivation powder fully describes all steps and process conditions of acid washing activation, vacuum impregnation filling, surface sealing, and double coupling agent grafting modification. Those skilled in the art can confirm its structure based on the description in the specification, combined with conventional analytical methods (such as thermogravimetric analysis to verify the filler content, contact angle testing to verify the modification effect, etc.), without excessive labor.
[0028] General methods for passivation powder pretreatment and functionalized filling: In the following embodiments, the passivation powder pretreatment and functionalization filling are carried out according to the following general method. The type of coupling agent and the amount of passivation powder in each embodiment are adjusted according to the specific formula.
[0029] S1. Passivation Powder Pretreatment: The desulfurization tailings of molten iron are coarsely crushed by a jaw crusher, medium-crushed by a roller mill, and then pulverized to D50≤18μm using an air jet mill. The pulverized passivation powder is then soaked sequentially in a 5% (w / w) phosphoric acid aqueous solution for 30 min, a 10% (w / w) phosphoric acid aqueous solution for 20 min, and a 15% (w / w) phosphoric acid aqueous solution for 10 min. The phosphoric acid-treated passivation powder is repeatedly washed with deionized water until the pH reaches 6.5~7.5, dried to constant weight in a forced-air drying oven at 105~110℃, and then calcined in a muffle furnace at 300~350℃ for 2 h to obtain activated passivation powder.
[0030] S2. Passivation Powder Pore Filling: Activated passivation powder is placed in a vacuum impregnation tank, and a vacuum is drawn to an absolute pressure of 2-5 kPa, maintained for 30 minutes. The filler (composed of thermoplastic polymer and microcapsules in a specific ratio) is heated to 60-70°C until it reaches a molten state, and then injected into the impregnation tank under vacuum for 60-90 minutes. After impregnation, the vacuum is released to atmospheric pressure to obtain the filled passivation powder. In the filler, the thermoplastic polymer is at least one of low molecular weight butyl rubber and polyisobutylene; the microcapsule shell material is melamine resin or urea-formaldehyde resin; and the core material is at least one of accelerator CZ, accelerator DM, sulfur, and insoluble sulfur. Based on 100 parts by weight of the filler, the thermoplastic polymer accounts for 70-85 parts, and the microcapsules account for 15-30 parts.
[0031] S3. Surface sealing: Add the filler passivation powder and stearic acid to a high-speed mixer at a mass ratio of 100:1~3, and mix at 70~80℃ and 500~1000rpm for 10~15min to obtain the sealing passivation powder.
[0032] S4. Surface chemical grafting modification: The sealing passivation powder is mixed with silane coupling agent KH-550 or Si-69 at a mass ratio of 100:1.5~3.0, and stirred at 80~90℃ for 30~60 min to obtain primary modified passivation powder. The primary modified passivation powder is then mixed with titanate coupling agent CS-105 at a mass ratio of 100:0.5~1.5, and stirred at 80~90℃ for 30~60 min to obtain modified functionalized passivation powder.
[0033] S5. Mixing and Gradient Compounding: The modified functionalized passivation powder is mixed with the rubber matrix in an internal mixer at a discharge temperature of 140-150℃. Based on 100 parts by weight of the rubber matrix, three compounds are prepared: a first compound with a passivation powder content of 5-10 phr, a second compound with a passivation powder content of 15-20 phr, and a third compound with a passivation powder content of 25-30 phr. Each compound also contains 20-40 phr of carbon black N660, 3-5 phr of zinc oxide, 1-3 phr of stearic acid, 1-2 phr of accelerator, 1.5-2.5 phr of sulfur, and 1-2 phr of antioxidant.
[0034] S6. Multilayer Co-extrusion: The first, second, and third rubber compounds are fed into the three channels of a three-layer co-extrusion die and co-extruded at 90-100°C to form an inner liner layer consisting of a surface layer, an intermediate transition layer, and a bottom layer along the thickness direction. The surface layer accounts for 15-25% of the total thickness of the inner liner layer, the intermediate transition layer accounts for 45-55%, and the bottom layer accounts for 25-35%. The content of modified functionalized passivation powder in the bottom layer is higher than that in the surface layer, and the content in the intermediate transition layer is between the two.
[0035] S7. Four-stage composite bonding: The aforementioned inner liner layer and the reinforcing layer with fiber bundle gaps are positioned on the bonding drum, with the bottom layer of the inner liner layer facing the reinforcing layer. The bonding drum surface has through holes and an internal vacuum channel communicating with a vacuum source. Bonding is performed in the following four stages: Phase 1: Start the vacuum source to create a first negative pressure on the surface of the bonding drum, and pre-press the bonding with a first temperature and a first pressure; Phase Two: Adjust the vacuum source to generate a second negative pressure with a larger absolute value on the surface of the bonding drum, and continue to press with the second pressure to release the filler in the pores of the passivation powder under the action of pressure difference; Phase 3: Adjust the vacuum source to generate a third negative pressure on the surface of the bonding drum, raise the temperature to the second temperature and the pressure to the third pressure, so that the released filler can penetrate into the gaps between the fiber bundles of the reinforcing layer under the combined action of positive pressure and negative pressure. Stage 4: Heat to the third temperature and maintain the third pressure to allow the filler to solidify in the gaps between the fiber bundles of the reinforcing layer to form a micro-bonded structure.
[0036] Example 1 Purpose of implementation: This embodiment focuses on the inner liner of tubeless tires, aiming to improve the airtightness and fatigue life of the inner liner and verify the applicability and effectiveness of the process of the present invention in the field of tubeless tires.
[0037] Implementation steps: S1. Passivation powder pretreatment: The desulfurization tailings of molten iron are crushed to D50≤18μm, and then soaked in 5% phosphoric acid aqueous solution for 30min, 10% phosphoric acid aqueous solution for 20min, and 15% phosphoric acid aqueous solution for 10min in sequence. After washing with deionized water to pH 7.0, it is dried at 108℃ to constant weight and then calcined at 320℃ for 2h to obtain activated passivation powder.
[0038] S2. Passivation Powder Pore Filling: Activated passivation powder is placed in a vacuum impregnation tank, and a vacuum is drawn to an absolute pressure of 3 kPa, maintained for 30 min. The filler consists of low molecular weight butyl rubber (Mounney viscosity ML(1+8) 125℃ = 30), microcapsule core material is accelerator CZ and sulfur (mass ratio 1:1), and shell material is melamine resin. Based on a total filler mass of 100 parts, low molecular weight butyl rubber accounts for 80 parts, and microcapsules account for 20 parts. The filler is heated to 65℃ to a molten state and injected into the impregnation tank under vacuum for 75 min. The vacuum is released to atmospheric pressure to obtain the filled passivation powder.
[0039] S3. Surface sealing: Add the filler passivation powder and stearic acid to a high-speed mixer at a mass ratio of 100:2 and mix at 800 rpm for 12 minutes at 75°C to obtain the sealing passivation powder.
[0040] S4. Surface chemical grafting modification: The sealing passivation powder and silane coupling agent KH-550 were mixed at a mass ratio of 100:2.0 and stirred at 85℃ for 45 min to obtain primary modified passivation powder. The primary modified passivation powder was then mixed with titanate coupling agent CS-105 at a mass ratio of 100:1.0 and stirred at 85℃ for 45 min to obtain modified functionalized passivation powder.
[0041] S5. Mixing and Gradient Compounding: The modified functionalized passivation powder and brominated butyl rubber (BIIR) are mixed in an internal mixer at a discharge temperature of 145°C. Based on 100 parts by weight of the rubber matrix, the modified functionalized passivation powder in the first compound is 8 phr, in the second compound 18 phr, and in the third compound 28 phr. Each compound also contains carbon black N660, zinc oxide, stearic acid, accelerator CZ, sulfur, and antioxidant 4010NA. See Table 1 below for specific formulations: Table 1: Formulation Parameters for Example 1 ; S6. Multilayer Co-extrusion: The first, second, and third rubber compounds are fed into the three channels of a three-layer co-extrusion die and co-extruded at 95°C to form an inner liner layer consisting of a surface layer, an intermediate transition layer, and a bottom layer along the thickness direction. The total thickness of the inner liner layer is 2.0 mm, with the surface layer accounting for 20% (0.4 mm), the intermediate transition layer accounting for 50% (1.0 mm), and the bottom layer accounting for 30% (0.6 mm). The content of modified functionalized passivation powder in the bottom layer (28 phr) is higher than that in the surface layer (8 phr), while the content in the intermediate transition layer (18 phr) is between the two.
[0042] S7. Four-stage composite bonding: The inner liner layer and the polyester fiber cord layer are positioned on the bonding drum, with the bottom layer of the inner liner layer facing the reinforcing layer. The bonding drum surface has through holes and an internal vacuum channel connected to a vacuum source.
[0043] Phase 1: Start the vacuum source to make the vacuum gauge pressure on the surface of the bonding drum -40kPa, preheat the bonding roller to 85℃, and pre-press the bonding with a pressure of 0.25MPa for 0.3s. Phase 2: Adjust the vacuum source to raise the vacuum gauge pressure on the bonding drum surface to -75kPa, maintain the bonding roller at 85°C, and continue pressing with a pressure of 0.4MPa for 0.8s. Phase 3: Adjust the vacuum source to reduce the vacuum gauge pressure on the bonding drum surface to -45 kPa, heat the bonding roller to 95°C, and increase the pressure to 0.6 MPa for 1.5 seconds. Phase 4: The bonding roller is heated to 103°C and maintained at a pressure of 0.6 MPa for 1.5 seconds.
[0044] Implementation results: The properties of the tire inner liner / reinforcing layer composite sample prepared by the above method are: peel strength 6.8 kN / m, air permeability (30℃, 0.2 MPa) is... Fatigue life (50% strain, 10Hz) is Tensile strength 12.5 MPa, tear strength The Shore A hardness is 58. Compared with Comparative Example 1, the peel strength is increased by 94%, the air permeability is reduced by 57%, the fatigue life is increased by 166%, the tensile strength is increased by 28%, and the tear strength is increased by 25%. This embodiment verifies that the application of the process of the present invention in the inner liner of tubeless tires can significantly improve air tightness and fatigue life.
[0045] Example 2 Purpose of implementation: This embodiment is for bead rubber for tubed tires, and aims to improve the flexural durability and resistance to heat and oxygen aging of the bead, and reduce the shoulder clearance rate.
[0046] Implementation steps: S1. Passivation powder pretreatment: The desulfurization tailings of molten iron are crushed to D50≤18μm, and then soaked in 5% phosphoric acid aqueous solution for 25min, 10% phosphoric acid aqueous solution for 25min, and 15% phosphoric acid aqueous solution for 15min in sequence. After washing with deionized water to pH 6.8, it is dried at 108℃ to constant weight and then calcined at 320℃ for 2h to obtain activated passivation powder.
[0047] S2. Passivation Powder Pore Filling: Activated passivation powder is placed in a vacuum impregnation tank, and a vacuum is drawn to an absolute pressure of 4 kPa, maintained for 30 min. The thermoplastic polymer in the filler is polyisobutylene (number average molecular weight 2000), the microcapsule core material is accelerator DM and sulfur (mass ratio 1:1), and the shell material is urea-formaldehyde resin. Based on a total filler mass of 100 parts, polyisobutylene accounts for 75 parts, and microcapsules account for 25 parts. Antioxidant 1010 (accounting for 2% of the total filler mass) is also added to the filler. The filler is heated to 65℃ to a molten state and injected into the impregnation tank under vacuum conditions for impregnation for 80 min. The vacuum is released to atmospheric pressure to obtain the filled passivation powder.
[0048] S3. Surface sealing: Add the filler passivation powder and low softening point wax (melting point 55℃) into a high-speed mixer at a mass ratio of 100:2.5, and mix at 700 rpm for 12 minutes at 75℃ to obtain the sealing passivation powder.
[0049] S4. Surface chemical grafting modification: The sealing passivation powder and silane coupling agent Si-69 were mixed at a mass ratio of 100:2.5 and stirred at 85℃ for 50 min to obtain primary modified passivation powder. The primary modified passivation powder was then mixed with titanate coupling agent CS-105 at a mass ratio of 100:1.2 and stirred at 85℃ for 50 min to obtain modified functionalized passivation powder.
[0050] S5. Mixing and Gradient Compounding: The modified functionalized passivation powder is mixed with natural rubber (NR) in an internal mixer at a discharge temperature of 145°C. Based on 100 parts by weight of the rubber matrix, the modified functionalized passivation powder in the first compound is 6 phr, in the second compound 16 phr, and in the third compound 26 phr. Each compound also contains carbon black N660, zinc oxide, stearic acid, accelerator CZ, sulfur, and antioxidant 4010NA. See Table 2 below for specific formulations. Table 2: Formulation Parameters for Example 2 ; S6. Multilayer Co-extrusion: The first, second, and third rubber compounds are fed into the three channels of a three-layer co-extrusion die and co-extruded at 95°C to form an inner liner layer consisting of a surface layer, an intermediate transition layer, and a bottom layer along the thickness direction. The total thickness of the inner liner layer is 2.5 mm, with the surface layer accounting for 20% (0.5 mm), the intermediate transition layer accounting for 50% (1.25 mm), and the bottom layer accounting for 30% (0.75 mm). The content of modified functionalized passivation powder in the bottom layer (26 phr) is higher than that in the surface layer (6 phr), while the content in the intermediate transition layer (16 phr) is between the two.
[0051] S7. Four-stage composite bonding: The inner liner layer and the polyester fiber cord layer are positioned on the bonding drum, with the bottom layer of the inner liner layer facing the reinforcing layer. The bonding drum surface has through holes and an internal vacuum channel connected to a vacuum source.
[0052] Phase 1: Start the vacuum source to make the vacuum gauge pressure on the surface of the bonding drum -35kPa, preheat the bonding roller to 85℃, and pre-press the bonding with a pressure of 0.25MPa for 0.3s. Phase 2: Adjust the vacuum source to raise the vacuum gauge pressure on the bonding drum surface to -65kPa, maintain the bonding roller at 85°C, and continue pressing with a pressure of 0.4MPa for 0.8s. Phase 3: Adjust the vacuum source to reduce the vacuum gauge pressure on the bonding drum surface to -42 kPa, heat the bonding roller to 95°C, and increase the pressure to 0.8 MPa for 1.5 seconds. Phase 4: The bonding roller is heated to 108°C and maintained at a pressure of 0.8MPa for 1.5 seconds.
[0053] Implementation results: The properties of the bead rubber sample prepared by the above method are: tensile strength 18.6 MPa, tear strength... The tire has a Shore A hardness of 62, a flexural fatigue (after 100,000 cycles) crack grade of 1, a tensile strength retention rate of 82% after 72 hours of hot air aging at 100℃, and a dynamic heat generation (temperature rise) of 28℃. Compared with Comparative Example 1, the tensile strength is increased by 90%, the tear strength by 39%, the flexural fatigue performance is improved by 2 grades, the tensile strength retention rate after aging is increased by 15 percentage points, and the dynamic heat generation is reduced by approximately 22%. This embodiment verifies that the application of the process of the present invention in the bead rubber of inner tube tires can significantly improve flexural durability and resistance to thermo-oxidative aging, and is expected to reduce the shoulder breakage rate by more than 10%.
[0054] Example 3 Purpose of implementation: This embodiment focuses on tread rubber for mining tires, aiming to improve wear resistance and tear resistance, and to verify the applicability and effectiveness of the process of the present invention in the field of mining tires.
[0055] Implementation steps: S1. Passivation powder pretreatment: The desulfurization tailings of molten iron are crushed to D50≤18μm, and then soaked in 5% phosphoric acid aqueous solution for 30min, 10% phosphoric acid aqueous solution for 20min, and 15% phosphoric acid aqueous solution for 10min in sequence. After washing with deionized water to pH 7.0, it is dried at 108℃ to constant weight and then calcined at 320℃ for 2h to obtain activated passivation powder.
[0056] S2. Passivation Powder Pore Filling: Activated passivation powder is placed in a vacuum impregnation tank, and the tank is evacuated to an absolute pressure of 3 kPa, maintained for 30 min. The filler consists of a mixture of low molecular weight butyl rubber (Mounney viscosity ML(1+8) 125℃ = 28) and polyisobutylene (number average molecular weight 1500) (mass ratio 1:1), a microcapsule core material of accelerator CZ and sulfur (mass ratio 1:1), and a melamine resin shell material. Based on a total filler mass of 100 parts, the thermoplastic polymer accounts for 78 parts, and the microcapsules account for 22 parts. A phenolic resin reinforcing agent (3% of the total filler mass) is also added to the filler. The filler is heated to 65℃ and molten, then injected into the impregnation tank under vacuum for 85 min. The vacuum is released to atmospheric pressure to obtain the filled passivation powder.
[0057] S3. Surface sealing: Add the filler passivation powder and stearic acid to a high-speed mixer at a mass ratio of 100:2 and mix at 900 rpm for 12 minutes at 75°C to obtain the sealing passivation powder.
[0058] S4. Surface chemical grafting modification: The sealing passivation powder and silane coupling agent KH-550 were mixed at a mass ratio of 100:2.5 and stirred at 85℃ for 50 min to obtain primary modified passivation powder. The primary modified passivation powder was then mixed with titanate coupling agent CS-105 at a mass ratio of 100:0.8 and stirred at 85℃ for 50 min to obtain modified functionalized passivation powder.
[0059] S5. Mixing and Gradient Blending: The modified functionalized passivation powder is mixed with a blend of natural rubber (NR) and butadiene rubber (BR) (mass ratio 70:30) in an internal mixer at a discharge temperature of 148℃. Based on 100 parts by mass of the rubber matrix, the modified functionalized passivation powder in the first compound is 10 phr, in the second compound 20 phr, and in the third compound 30 phr. Each compound also contains carbon black N660, zinc oxide, stearic acid, accelerator CZ, sulfur, and antioxidant 4010NA. See Table 3 below for specific formulations. Table 3: Formulation Parameters of Example 3 ; S6. Multilayer Co-extrusion: The first, second, and third rubber compounds are fed into the three channels of a three-layer co-extrusion die and co-extruded at 95°C to form an inner liner layer consisting of a surface layer, an intermediate transition layer, and a bottom layer along the thickness direction. The total thickness of the inner liner layer is 3.0 mm, with the surface layer accounting for 20% (0.6 mm), the intermediate transition layer accounting for 50% (1.5 mm), and the bottom layer accounting for 30% (0.9 mm). The content of modified functionalized passivation powder in the bottom layer (30 phr) is higher than that in the surface layer (10 phr), while the content in the intermediate transition layer (20 phr) is between the two.
[0060] S7. Four-stage composite bonding: The inner liner layer and the polyester fiber cord layer are positioned on the bonding drum, with the bottom layer of the inner liner layer facing the reinforcing layer. The bonding drum surface has through holes and an internal vacuum channel connected to a vacuum source.
[0061] Phase 1: Start the vacuum source to make the vacuum gauge pressure on the surface of the bonding drum -40kPa, preheat the bonding roller to 85℃, and pre-press the bonding with a pressure of 0.3MPa for 0.3s. Phase 2: Adjust the vacuum source to raise the vacuum gauge pressure on the bonding drum surface to -70kPa, maintain the bonding roller at 85°C, and continue pressing with a pressure of 0.5MPa for 0.8s. Phase 3: Adjust the vacuum source to reduce the vacuum gauge pressure on the bonding drum surface to -45 kPa, heat the bonding roller to 95°C, and increase the pressure to 1.1 MPa for 1.5 seconds. Phase 4: The bonding roller is heated to 108°C and maintained at a pressure of 1.1 MPa for 1.5 seconds.
[0062] Implementation results: The properties of the mining tread rubber sample prepared by the above method are: tensile strength 19.2 MPa, tear strength... The Shore A hardness is 68, and the Akron abrasion loss is 0.12 cm³ / 1.61 km. Compared with Comparative Example 1, the tensile strength is increased by 96%, the tear strength is increased by 53%, and the abrasion loss is reduced by 33%. This embodiment verifies that the application of the process of the present invention in mining tire tread can significantly improve abrasion resistance and tear resistance.
[0063] Example 4 Purpose of implementation: This embodiment is a comprehensive preferred solution, and its purpose is to verify the optimization effect of the synergistic effect of each component on the overall performance by adjusting the composition of the thermoplastic polymer (a compound of low molecular weight butyl rubber and polyisobutylene) and the coupling agent system (a compound of KH-550 and Si-69) in the passivation powder filler.
[0064] Implementation steps: S1. Passivation powder pretreatment: Same as in Example 1.
[0065] S2. Passivation Powder Pore Filling: Activated passivation powder is placed in a vacuum impregnation tank, and a vacuum is drawn to an absolute pressure of 2 kPa, maintained for 30 min. The filler consists of a mixture of low molecular weight butyl rubber (Mounney viscosity ML(1+8) 125℃ = 30) and polyisobutylene (number average molecular weight 2000) (mass ratio 3:1), a microcapsule core material of a mixture of accelerator CZ, accelerator DM, and sulfur (mass ratio 1:1:2), and a shell material of melamine resin. Based on a total filler mass of 100 parts, the thermoplastic polymer accounts for 80 parts, and the microcapsules account for 20 parts. The filler is heated to 68℃ and molten, then injected into the impregnation tank under vacuum for 90 min. The vacuum is released to atmospheric pressure to obtain the filled passivation powder.
[0066] S3. Surface sealing: Add the filler passivation powder and stearic acid to a high-speed mixer at a mass ratio of 100:1.5 and mix at 800 rpm for 12 minutes at 75°C to obtain the sealing passivation powder.
[0067] S4. Surface chemical grafting modification: The sealing passivation powder was mixed with a mixture of silane coupling agents KH-550 and Si-69 (mass ratio 1:1) at a mass ratio of 100:2.5, and stirred at 85℃ for 50 min to obtain primary modified passivation powder. The primary modified passivation powder was then mixed with titanate coupling agent CS-105 at a mass ratio of 100:1.0, and stirred at 85℃ for 50 min to obtain modified functionalized passivation powder.
[0068] S5. Mixing and graded compounding: The formulation system is the same as in Example 1, with the first compound having a passive ash content of 8 phr, the second compound having 18 phr, and the third compound having 28 phr.
[0069] S6. Multilayer co-extrusion: Same as Example 1.
[0070] S7. Four-stage composite bonding: Same as Example 1.
[0071] Implementation results: The composite sample prepared by the above method has the following properties: peel strength 7.2 kN / m, air permeability... Fatigue life The tensile strength was 13.1 MPa, and the tear strength was... The Shore A hardness is 60. Compared with Example 1, the peel strength is increased by 5.9%, the air permeability is reduced by 8.3%, and the fatigue life is increased by 8.2%. The overall performance is better than that of each individual example, indicating that the compounding of low molecular weight butyl rubber and polyisobutylene, as well as the synergistic use of silane coupling agents KH-550 and Si-69, produced a significant synergistic enhancement effect.
[0072] Example 5 Purpose of implementation: This embodiment sets three different combinations of bonding parameters (stage two vacuum negative pressure and stage four temperature) to investigate the influence of key parameters on the bonding effect in the four-stage composite bonding process and to determine the optimal process parameter range.
[0073] Implementation steps: The raw materials, formulas, and operating conditions for S1 to S6 are the same as those in Example 1.
[0074] S7. Four-stage composite bonding: Set the following three sets of bonding parameter combinations: see Table 4 for details.
[0075] Table 4: Three sets of bonding parameters ; Implementation results: The performance test results of the three schemes are as follows: see Table 5 for details.
[0076] Table 5: Performance test results of the three schemes ; The results show that the optimal overall performance (Scheme B) is achieved when the vacuum pressure in Stage 2 is -75 kPa and the temperature in Stage 4 is 105 °C. When the vacuum pressure is too low (-65 kPa), the filler release is insufficient, the interfacial bonding is weak, and both peel strength and fatigue life are low. When the vacuum pressure is too high (-85 kPa), excessive filler absorption and loss may occur, leading to increased air permeability and decreased fatigue life. When the temperature in Stage 4 is too low (100 °C), cross-linking and curing are incomplete; when the temperature is too high (110 °C), premature vulcanization of the compound may occur, both of which adversely affect the overall performance. This embodiment verifies the rationality of the parameter ranges of -60 to -80 kPa for the vacuum gauge pressure in Stage 2 and 100 to 110 °C for the temperature in Stage 4, with -70 to -75 kPa and 103 to 108 °C being the preferred ranges.
[0077] Comparative Example 1 Purpose of implementation: This comparative example uses a traditional bonding process (without passivation powder functionalization treatment, without three-layer gradient co-extrusion, and without four-stage composite bonding) to form a comparison with the embodiments of the present invention and to verify the overall superiority of the technical solution of the present invention.
[0078] Implementation steps: (1) Passivation treatment: The desulfurization tailings of molten iron are crushed to D50≤18μm and used directly as filler without phosphoric acid treatment, pore filling, sealing and coupling agent modification.
[0079] (2) Mixing: The rubber matrix is brominated butyl rubber (BIIR). Based on 100 parts by weight of the rubber matrix, the formula is as follows: 100 parts brominated butyl rubber, 20 parts unmodified passivating powder, 30 parts carbon black N660, 4 parts zinc oxide, 2 parts stearic acid, 1.5 parts accelerator CZ, 2.0 parts sulfur, and 1.5 parts antioxidant 4010NA. The mixing discharge temperature is 145℃.
[0080] (3) Inner liner preparation: Single-layer extrusion is used, without three-layer gradient co-extrusion, and the thickness of the inner liner after extrusion is 2.0 mm.
[0081] (4) Lamination process: The traditional constant temperature and pressure one-time lamination process is adopted. No vacuum negative pressure is applied to the lamination drum, the lamination roller temperature is 100℃, the pressure is 0.6MPa, the duration of one lamination is 3.0s, and the four stages described in S7 are not divided.
[0082] Implementation results:
[0083] The composite sample prepared by the above method has the following properties: peel strength 3.5 kN / m, air permeability... Fatigue life Tensile strength 9.8 MPa, tear strength Shore A hardness 55, flexural fatigue (after 100,000 cycles) crack grade 3, Akron wear 0.18 cm³ / 1.61 km, tensile strength retention rate after 100℃×72h hot air aging 37%, dynamic heat generation (temperature rise) 36℃.
[0084] Overall performance comparison between the examples and comparative examples: The performance comparison of each embodiment with Comparative Example 1 is as follows: see Table 6 for details.
[0085] Table 6: Comparison of performance parameters between the examples and Comparative Example 1 ; The above results show that, compared with Comparative Example 1, Examples 1-4 using the technical solution of the present invention have significantly improved peel strength, air tightness, fatigue life, tensile strength, tear strength, flexural fatigue, and wear resistance. Specifically, the fatigue life of the inner liner for tubeless tires (Example 1) is increased by 166%, and the air tightness is improved by 57%; the flexural fatigue performance of the bead compound for tubed tires (Example 2) is improved by two levels, and the resistance to thermo-oxidative aging is significantly improved; the wear resistance of the tread compound for mining tires (Example 3) is improved by 33%, and the tear resistance is improved by 53%; the optimal comprehensive solution (Example 4) has the best overall performance, with peel strength increased by 106% and fatigue life increased by 188% compared to Comparative Example 1. This indicates that the passivation powder functionalization treatment, the three-layer gradient inner liner structure, and the four-stage composite bonding process of the present invention produce a significant synergistic enhancement effect.
[0086] The thermoplastic polymer and microcapsules used in the S2 stage of this invention, which fill the pores of the passivated powder, are released from the pores under vacuum negative pressure (-60~-80 kPa) in the S7 stage. In the S7 stage, the combined effect of positive pressure (0.5~1.2 MPa) and negative pressure (-40~-50 kPa) in the S7 stage allows the released filler to fully penetrate the fiber bundle gaps in the reinforcing layer. In the S7 stage, the temperature is raised to 100~110°C, causing the microcapsule shell to rupture and release the core material (accelerator and sulfur). This triggers a cross-linking and curing reaction between the thermoplastic polymer in the filler and the surrounding rubber matrix, forming a micro-bonded structure in the fiber bundle gaps. This micro-bonded structure macroscopically manifests as a significant increase in peel strength and a substantial extension of fatigue life.
[0087] The hierarchical porous structure formed by the phosphoric acid gradient treatment of the passivation powder in S1 provides physical space for the loading of fillers in S2. The surface sealing treatment in S3 ensures that the fillers are not prematurely released during the mixing in S5 and the extrusion in S6. The dual coupling agent grafting modification in S4 (silane coupling agent + titanate coupling agent) improves the interfacial compatibility between the passivation powder and the rubber matrix, enabling the passivation powder to be uniformly dispersed in the rubber matrix. At the same time, the alkaline sites (unmodified areas) on the surface of the passivation powder promote rubber vulcanization. In the three-layer gradient structure of S6, the high passivation powder content in the bottom layer (25~30 phr) provides a sufficient source for filler release, serving the interlayer penetration and bonding; the low passivation powder content in the surface layer (5~10 phr) ensures the airtightness of the airtight layer. The synergistic effect of the three-layer structure enables the inner liner to achieve a functional gradient design in the thickness direction of "dense air barrier in the surface layer - buffer transition in the middle layer - anchoring and reinforcement in the bottom layer".
[0088] The above are merely specific embodiments of this application, but the scope of protection of this application is not limited thereto. Any variations or substitutions that can be easily conceived by those skilled in the art within the scope of the technology disclosed in this application should be included within the scope of protection of this application. Therefore, the scope of protection of this application should be determined by the scope of protection of the claims.
[0089] In conclusion, the above are merely preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.
Claims
1. A method for improving the adhesion strength of tire inner liner by using functionalized dull powder, characterized by, Includes the following steps: S1. Passivation powder pretreatment: After crushing the desulfurization tailings of molten iron, the powder is acid-washed, washed, dried and roasted to obtain activated passivation powder. S2. Passive powder pore filling: The activated passive powder obtained in S1 is placed in an impregnation tank. After vacuuming, the filler containing thermoplastic polymer and microcapsules coated with cross-linking active ingredients is heated to melt and injected to impregnate and fill the pores of the passive powder. The vacuum is then released to obtain filled passive powder. S3. Surface sealing: The filler powder obtained in S2 is mixed with a sealing agent, so that the sealing agent coats the surface of the filler powder to obtain a sealed filler powder; the sealing agent seals the pore openings on the surface of the filler powder in the early stage of mixing to prevent the filler from escaping prematurely under the mechanical shearing action of mixing; when the mixing temperature rises above the melting point of the sealing agent, the sealing agent melts and integrates into the rubber matrix. At this time, the filler is still bound by the capillary force of the pores of the filler powder and will not be released spontaneously until sufficient pressure difference is applied in the subsequent negative pressure stage before it is extracted; S4. Surface chemical grafting modification: The sealing passivation powder obtained in S3 is grafted with silane coupling agent and titanate coupling agent in sequence to obtain modified functionalized passivation powder. S5. Mixing and gradient compounding: The modified functionalized passivation powder obtained in S4 is mixed with the rubber matrix to prepare the first compound, the second compound, and the third compound with a gradient change in passivation powder content. S6. Multilayer co-extrusion: The first rubber compound, the second rubber compound, and the third rubber compound are co-extruded to form an inner liner layer consisting of a surface layer, an intermediate transition layer, and a bottom layer along the thickness direction. The content of modified functionalized passivation powder in the bottom layer is higher than that in the surface layer, and the content of the intermediate transition layer is between the two. S7. Four-stage composite bonding: A bonding drum with through holes distributed on the surface and a vacuum channel connected to a vacuum source is provided inside. The inner liner and the reinforcing layer with fiber bundle gaps are positioned on the bonding drum so that the bottom layer of the inner liner is opposite to the reinforcing layer. Phase 1: Start the vacuum source to create a first negative pressure on the surface of the bonding drum, and pre-press the bonding with a first temperature and a first pressure; Phase Two: Adjusting the vacuum source creates a second negative pressure with a larger absolute value on the surface of the bonding drum. This second pressure continues the pressing process, causing the filler material within the pores of the passivated powder to be released under the pressure difference. The perforated structure on the surface of the bonding drum allows the negative pressure to act on microscopic local areas of the liner layer, forming low-pressure zones at the perforations. Driven by the pressure difference, the high-pressure filler material within the pores is released outwards and migrates to the interface between the liner layer and the reinforcing layer. Simultaneously, the liner layer is adsorbed onto the drum surface, ensuring close contact between the bottom layer and the reinforcing layer, providing favorable conditions for the directional migration of the released filler material into the gaps between the fiber bundles of the reinforcing layer. Phase 3: Adjust the vacuum source to generate a third negative pressure on the surface of the bonding drum, raise the temperature to the second temperature and the pressure to the third pressure, so that the released filler can penetrate into the gaps between the fiber bundles of the reinforcing layer under the combined action of positive pressure and negative pressure. Stage 4: Heat to the third temperature and maintain the third pressure to allow the filler to solidify in the gaps between the fiber bundles of the reinforcing layer to form a micro-bonded structure.
2. A method for improving the adhesion strength of the inner liner of a tire by using functionalized mill base according to claim 1, characterized in that, In S1, the blunt powder is pulverized to D50≤18μm; the acid washing is to soak in 5%, 10%, and 15% phosphoric acid aqueous solutions for 10~30min each; the drying is to dry at 105~110℃ to constant weight; and the calcination is to calcinate at 300~350℃ for 2h.
3. A method for improving the adhesion strength of the inner liner of a tire by using functionalized mill base according to claim 1, characterized in that, In S2, the vacuum condition is an absolute pressure of 2-5 kPa inside the container, maintained for 30 minutes; the filling material impregnation temperature is 60-70℃, and the impregnation time is 60-90 minutes; the thermoplastic polymer is at least one of low molecular weight butyl rubber and polyisobutylene, with a Mooney viscosity ML(1+8) at 125℃ of 25-35 or a number-average molecular weight of 1000-3000; the microcapsule shell material is melamine resin or urea-formaldehyde resin, and the core material is at least one of accelerator CZ, accelerator DM, sulfur, and insoluble sulfur, with a particle size of 1-10 μm, a shell thickness of 0.2-0.5 μm, and a thermal decomposition temperature of 80-100℃; based on 100 parts of the total mass of the filling material, the thermoplastic polymer accounts for 70-85 parts, and the microcapsules account for 15-30 parts.
4. A method for improving the adhesion strength of the inner liner of a tire by using functionalized mill base according to claim 1, characterized in that, In S3, the sealing agent is stearic acid or a low softening point wax with a melting point of 50-60℃; the mass ratio of filler powder to sealing agent is 100:1-3; the mixing temperature is 70-80℃, the rotation speed is 500-1000rpm, and the time is 10-15min.
5. A method for improving the adhesion strength of the inner liner of a tire by using functionalized mill base according to claim 1, characterized in that, In S4, the silane coupling agent is KH-550 or Si-69, the mass ratio of sealing passivation powder to silane coupling agent is 100:1.5~3.0, the grafting reaction temperature is 80~90℃, and the time is 30~60min; the titanate coupling agent is CS-105, the mass ratio of primary modified passivation powder to titanate coupling agent is 100:0.5~1.5, the grafting reaction temperature is 80~90℃, and the time is 30~60min.
6. A method for improving the adhesion strength of the inner liner of a tire by using functionalized mill base according to claim 1, characterized in that, In S5, based on 100 parts by weight of the rubber matrix, the first rubber compound has a passive powder content of 5-10 phr, the second rubber compound has a content of 15-20 phr, and the third rubber compound has a content of 25-30 phr; the rubber matrix is at least one of natural rubber, butyl rubber, chlorinated butyl rubber, and brominated butyl rubber; the mixing and discharge temperature is 140-150℃.
7. A method for improving the adhesion strength of the inner liner of a tire by using functionalized mill base as claimed in claim 6, characterized in that, In S5, based on 100 parts by weight of the rubber matrix, the raw materials of the first rubber compound, the second rubber compound, and the third rubber compound each further include 20-40 parts of carbon black N660, 3-5 parts of zinc oxide, 1-3 parts of stearic acid, 1-2 parts of accelerator, 1.5-2.5 parts of sulfur, and 1-2 parts of antioxidant.
8. A method for improving the bonding strength of tire inner liner using functionalized passivation powder as described in claim 1, characterized in that, In S6, the surface layer thickness accounts for 15-25% of the total thickness of the inner liner layer, the intermediate transition layer accounts for 45-55%, and the bottom layer accounts for 25-35%; the co-extrusion temperature is 90-100℃.
9. A method for improving the bonding strength of tire inner liner using functionalized passivation powder as described in claim 1, characterized in that, In S7, the reinforcing layer is a fiber fabric layer; the aperture of the through hole on the surface of the bonding drum is 0.2~0.5mm; the negative pressure is gauge pressure, with the first negative pressure being -30~-50kPa, the second negative pressure being -60~-80kPa, and the third negative pressure being -40~-50kPa; the first pressure being 0.2~0.3MPa, the second pressure being 0.3~0.5MPa, and the third pressure being 0.5~1.2MPa; the first temperature being 80~90℃, the second temperature being 90~100℃, and the third temperature being 100~110℃; the duration of stage one being 0~0.5s, stage two being 0.5~1.0s, stage three being 1.0~2.0s, and stage four being 1.0~2.0s.
10. A method for improving the bonding strength of tire inner liner using functionalized passivation powder as claimed in claim 9, characterized in that, In S7, for tubeless tires, the second negative pressure is -70~-80 kPa, the third pressure is 0.5~0.8 MPa, and the third temperature is 100~105℃; for tubed tires, the second negative pressure is -60~-70 kPa, the third pressure is 0.6~1.0 MPa, and the third temperature is 105~110℃; for mining tires, the second negative pressure is -65~-75 kPa, the third pressure is 1.0~1.2 MPa, and the third temperature is 105~110℃.