A modified flame retardant resistant to precipitation, and a preparation method and application thereof
By forming a core-shell structure with an organosilicon hydrophobic shell on the surface of the flame retardant, the problem of precipitation of halogen-free flame retardant PA66 under high temperature and high humidity environments is solved, achieving high efficiency flame retardancy and long-term material stability, which is suitable for new energy vehicles and other fields.
Patent Information
- Application Number
- CN202510672571.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-05-23
- Publication Date
- 2026-11-24
AI Technical Summary
Existing halogen-free flame-retardant PA66 is prone to precipitation in high temperature and high humidity environments, affecting the appearance of products and the safety of electronic components. In addition, its flame-retardant efficiency is insufficient, which limits its application in fields such as new energy vehicles.
Modified flame retardants with a core-shell structure form a phosphorus, silicon, and nitrogen synergistic flame retardant effect by depositing an organosilicon hydrophobic shell on the flame retardant surface, preventing moisture-induced core precipitation, and improving flame retardant efficiency by depositing an organosilicon shell on the flame retardant surface.
The flame retardant does not leach out under high temperature and high humidity conditions, and achieves UL-94 V-0 rating with a small amount of addition, thus improving flame retardant efficiency and the practicality of the material.
Smart Images

Figure CN123152175A_ABST
Abstract
Description
Technical Field
[0001] This invention specifically relates to a modified flame retardant resistant to precipitation, its preparation method, and its application, belonging to the field of flame retardant technology. Background Technology
[0002] Polyamide 66, also known as PA66, is an engineering plastic with excellent overall performance. It possesses good mechanical strength, heat resistance, and processing properties, and is widely used in electronics, automotive manufacturing, and rail transportation. However, its inherent flame retardancy is poor, and it produces a large amount of molten droplets during combustion, which can easily lead to the spread of fire. Therefore, flame retardant modification is crucial to expand its applications in fields requiring flame retardancy.
[0003] Currently, flame-retardant PA66 is mainly halogen-free, and is mostly prepared using additive methods. Mainstream halogen-free flame retardants include aluminum diethylphosphite (ADP), melamine polyphosphate (MPP), and melamine cyanurate (MCA). However, due to the poor compatibility of most halogen-free flame retardants with PA66, and the fact that the flame retardants themselves are hydrophilic, under high temperature and humidity environments or long-term storage, the flame retardants will precipitate onto the surface of PA66 products under the induction of moisture. This not only affects the appearance of the products but also causes corrosion and short circuits in electronic components. With the rapid development of new energy vehicles, this problem has become increasingly prominent, severely limiting the application of halogen-free flame-retardant PA66 in the new energy field.
[0004] In response to the problem of flame retardant precipitation, the industry has made some improvements: (1) Modifying the flame retardant to resist precipitation, such as the prior art CN114231025A which discloses a high heat resistance and precipitation resistance environmentally friendly flame retardant polyamide composition, which uses aniline to modify MPP, improving the water resistance of MPP, and at the same time purifying ADP to improve its heat resistance and flame retardant efficiency; (2) Adding a precipitation resistant agent, such as the prior art CN118222086A which discloses a flame retardant precipitation resistant agent (1-hydroxyethyl-3-methylimidazolium p-toluenesulfonate), which can form hydrogen bonds with polyamide, greatly reducing the precipitation rate of halogen-free flame retardant; (3) Modifying the resin body to resist precipitation, such as the prior art CN109679338A which discloses a low precipitation halogen-free flame retardant polyamide alloy material, which uses two polyamides with different solubility parameters to extend the precipitation path of the flame retardant, thereby achieving the purpose of delaying precipitation.
[0005] However, while the above methods offer some resistance to exudation, the flame retardant will still precipitate after prolonged use, albeit in reduced amounts, which still fails to meet practical application requirements. Therefore, developing a long-lasting, exudation-resistant flame retardant is an urgent technical problem to be solved. Summary of the Invention
[0006] To address the problem that existing flame retardants are prone to precipitation in high-temperature and high-humidity environments, thus hindering their application in the production of halogen-free flame-retardant PA66, this paper provides a precipitation-resistant modified flame retardant, its preparation method, and its application. This technical solution proposes a precipitation-resistant modified flame retardant with a core-shell structure. A hydrophobic organosilicon shell is deposited on the surface of the flame retardant using a deposition method. Under the action of this shell, moisture is unlikely to induce the core flame retardant to precipitate to the surface. The halogen-free flame-retardant PA66 prepared using this modified flame retardant did not precipitate after 600 hours of testing with 85% alpha. Simultaneously, the introduction of silicon into this modified flame retardant plays a synergistic role of phosphorus, silicon, and nitrogen in flame retardancy, improving the flame retardant efficiency. With an addition of 15-18 wt.%, this modified flame retardant enables 10-30 wt.% glass fiber reinforced PA66 to achieve the UL-94 V-0 rating at a thickness of 0.8 mm.
[0007] To achieve the above technical objectives, the following technical solution is proposed: The primary objective of this technical solution is to propose a modified flame retardant resistant to exudation, with the flame retardant as the core and organosilicon as the shell. In this process, organosilicon is deposited on the surface of a flame retardant, and then the organosilicon deposited on the flame retardant surface is subjected to free radical polymerization through vulcanization to form an organosilicon shell. The flame retardant involved is a flame retardant containing both phosphorus and nitrogen elements. After the organosilicon is coated, the synergistic flame retardancy of phosphorus, nitrogen and silicon elements is achieved, thereby improving the flame retardant efficiency.
[0008] The flame retardant is specifically one or a combination of two or more of aluminum diethyl phosphite (ADP), melamine polyphosphate (MPP), and melamine cyanurate (MCA). Preferably, the flame retardant is a combination of aluminum diethyl phosphite (ADP) and melamine polyphosphate (MPP), with a mass ratio of ADP to MPP of 2-5:1; or the flame retardant is a combination of aluminum diethyl phosphite (ADP) and melamine cyanurate (MCA), with a mass ratio of ADP to MCA of 2-5:1. Since organosilicon is the shell structure of flame retardants, it is required that organosilicon has a high crosslinking density. Therefore, organosilicon intermediates before crosslinking need to have more double bond structures as crosslinking sites to ensure that the shell of organosilicon is formed after crosslinking. That is, organosilicon intermediates refer to organosilicon raw materials containing double bond structures but not crosslinked. The structural formula of the organosilicon intermediate is as follows: ; or ; or ; R1 is methyl or ethyl, R2 is methyl or ethyl; x, y, and z are all integers greater than 0; The structural formula of the silicone shell is as follows: ; or ; or R1 is methyl or ethyl, R2 is methyl or ethyl; x, y, and z are all integers greater than 0; The second objective of this technical solution is to propose a method for preparing a modified flame retardant resistant to exudation, comprising the following steps: S1: Mix the solvent, organosilicon intermediate and vulcanizing agent evenly, then add it to the flame retardant and mechanically mix for 10 to 30 minutes at a speed of 500 to 800 r / min to obtain a slurry containing organosilicon intermediate and flame retardant; Among them, the rotation speed of "500~800 r / min" ensures uniform mixing of materials. If the speed is lower than this, it will lead to uneven mixing of materials; if the speed is higher than this, it will increase the load on the equipment, increase energy consumption, and reduce the service life of the equipment. The mixing time is "10-30 min". It is also important to ensure that the materials are mixed evenly. If the time is less than this, the materials will not mix evenly. If the time is greater than this, the production efficiency will be low even if the materials are mixed evenly. S2: The slurry obtained in step S1 is dried in a vacuum oven at 90-120 ℃ to remove excess solvent, and then cured for 1-2 h; then, the product is crushed using a pulverizer to obtain a modified flame retardant resistant to precipitation. The specified vacuum temperature of 90–120 °C effectively ensures both curing quality and efficiency. Temperatures below this range will prevent the silicone intermediate from curing; temperatures above this range will result in excessively rapid curing and agglomeration of the flame retardant. Curing, also known as vulcanization, takes 1-2 hours to ensure complete curing. For example, if the curing time is less than this, the silicone may not be fully cured and will remain liquid; if the curing time is greater than this, even if it is fully cured, the efficiency will be low. The above operations are all aimed at uniformly dispersing the organosilicon intermediate on the flame retardant surface, and then curing / curing the organosilicon intermediate into a film at high temperature, forming an organosilicon shell on the flame retardant surface. Under the action of this shell, moisture is less likely to induce the core flame retardant to precipitate to the surface, thereby improving the usability of the corresponding product.
[0009] Furthermore, the solvent is one or any combination of two or more of anhydrous ethanol, tetrahydrofuran, and ethyl acetate. The solvent is used to disperse or dissolve the organosilicon intermediate, reduce the viscosity of the system, and enable the organosilicon intermediate to be uniformly deposited on the surface of the core flame retardant during the mixing process.
[0010] Furthermore, the vulcanizing agent is one or a combination of any two or more of benzoyl peroxide, 2,5-dimethyl-2,5-di-tert-butylperoxide, and di-tert-butyl peroxide. The vulcanizing agent is used to initiate the free radical polymerization of the organosilicon intermediate at high temperature, thereby curing it into a film and forming a uniform shell on the surface of the flame retardant.
[0011] Furthermore, the mass ratio of solvent to flame retardant is 20–100:100, the mass ratio of organosilicon intermediate to flame retardant is 1–20:100, and the mass ratio of vulcanizing agent to organosilicon intermediate is 0.5–5:100. The 20–100:100 mass ratio of solvent to flame retardant ensures that the flame retardant can form a slurry while conserving solvent, thus guaranteeing subsequent coating. For example, if the mass ratio is less than this, the flame retardant will not be able to form a slurry, thus failing to achieve coating; if the mass ratio is greater than this, solvent will be wasted, and post-processing will be more cumbersome. The mass ratio of organosilicon intermediates to flame retardants is 1–20:100, which effectively ensures hydrophobic and flame-retardant effects. For example, if the mass ratio is less than this, the shell material is too small and cannot be uniformly dispersed, thus failing to guarantee the hydrophobic effect; if the mass ratio is greater than this, the content of organosilicon intermediates is too high, and since organosilicon intermediates are flammable materials, this will lead to a deterioration in the flame-retardant performance of the material. The mass ratio of the vulcanizing agent to the organosilicon intermediate is 0.5–5:100 to ensure effective curing (vulcanization) and facilitate post-processing. For example, if the mass ratio is less than this, the amount of initiator-vulcanizing agent will be insufficient, resulting in incomplete curing of the organosilicon shell; if the mass ratio is greater than this, the amount of initiator-vulcanizing agent will be excessive, and the post-processing process may not be able to completely remove the substance, potentially causing PA66 cross-linking and affecting material processing.
[0012] The third objective of this technical solution is to propose using the modified flame retardant to prepare halogen-free flame retardant PA66.
[0013] Furthermore, in the process of preparing halogen-free flame retardant PA66, 15-18 wt.% of modified flame retardant is added to 10-30 wt.% of glass fiber reinforced PA66 by weight percentage. Specifically, "10-30 wt.% glass fiber reinforced PA66" refers to PA66 with 10-30 wt.% glass fiber added, resulting in 10-30 wt.% glass fiber reinforced PA66. The halogen-free flame retardant PA66 achieves UL-94 V-0 at a thickness of 0.8 mm and does not exhibit precipitation during 600 h of 85% damp heat aging test.
[0014] The beneficial technical effects of adopting this technical solution are as follows: 1. In this invention, organosilicon is uniformly dispersed on the surface of the flame retardant by deposition to form a hydrophobic shell, which isolates the flame retardant from direct contact with water, thereby preventing the flame retardant from precipitating under high temperature and high humidity conditions. Second, in this invention, silicon is introduced into the original flame retardant to prepare a core-shell structured modified flame retardant, which achieves synergistic flame retardancy of phosphorus, silicon and nitrogen, and with a small amount of addition, 10-30 wt.% glass fiber reinforced PA66 can achieve UL-94V-0 rating with a thickness of 0.8 mm. III. The present invention provides a method for preparing a modified flame retardant resistant to precipitation. This preparation method has the advantages of simple process, readily available raw materials, mild reaction conditions, stable reaction process, high safety and low energy consumption. Attached Figure Description
[0015] Figure 1 This is a structural model diagram of the organosilicon shell and flame retardant involved in this invention; Figure 2 Here is a SEM image of the modified flame retardant in Example 1; Figure 3 The image shows the SEM image of the unmodified flame retardant in Comparative Example 1. Figure 4 This is a comparison chart of the hydrophilic and hydrophobic property evaluation results of the modified flame retardant in Example 1 and the unmodified flame retardant in Control Example 1 (the left side is the hydrophilic and hydrophobic property evaluation result chart of Example 1, and the right side is the hydrophilic and hydrophobic property evaluation result chart of Control Example). Figure 5 This is an image showing the appearance morphology of unaged flame-retardant glass fiber reinforced PA66 corresponding to Example 1; Figure 6 This is a diagram showing the appearance morphology of unaged flame-retardant glass fiber reinforced PA66 corresponding to Example 1. Figure 7 The appearance morphology of flame-retardant glass fiber reinforced PA66 corresponding to column 1 after 600 h of humid heat aging; Figure 8 The image shows the appearance morphology of flame-retardant glass fiber reinforced PA66 corresponding to Comparative Example 1 after 600 h of humid heat aging. Detailed Implementation
[0016] The technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only a part of the embodiments of the present invention, and not all of them. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.
[0017] Example 1 At room temperature, 5 g of methylphenyl vinyl polysiloxane (organosilicon intermediate), 0.025 g of benzoyl peroxide (vulcanizing agent) and 100 g of anhydrous ethanol (solvent) were uniformly mixed; then, the mixture was mixed with 500 g of flame retardant (ADP to MPP mass ratio of 3:1) in a high-speed stirrer for 30 min at a speed of 500 r / min to obtain a slurry containing organosilicon intermediate and flame retardant. Finally, the slurry was placed in a vacuum oven at 90 °C for 2 h to remove solvents and solidify. After crushing, a modified flame retardant with a methylphenyl silicone rubber shell (e.g., [missing information]) was obtained to resist exudation. Figure 1 (As shown). The obtained modified flame retardant was subjected to electron microscopy, and the results are shown in the figure. Figure 2 As shown; The hydrophilicity and hydrophobicity properties of the obtained modified flame retardant were evaluated, specifically by mixing 2 g of unmodified flame retardant with 20 mL of water and stirring for 5 min. The results are as follows. Figure 4 As shown; The structural formula of methylphenylvinyl polysiloxane (phenyl silicone rubber) is as follows: ; Where R1 is methyl or ethyl, and R2 is methyl or ethyl; x, y, and z are all integers greater than 0; The reaction formulas involved are as follows: .
[0018] Example 2 At room temperature, 100 g of methyl vinyl polysiloxane (organosilicon intermediate), 2 g of 2,5-dimethyl-2,5-di-tert-butylperoxyhexane (vulcanizing agent) and 500 g of ethyl acetate (solvent) were uniformly mixed; then, the mixture was mixed with 500 g of flame retardant (ADP to MPP mass ratio of 3:1) in a high-speed stirrer for 30 min at a speed of 500 r / min to obtain a slurry containing organosilicon intermediate and flame retardant. Finally, the slurry was placed in a vacuum oven at 90 °C for 2 h to remove solvent and cure. After crushing, a modified flame retardant with a shell of methyl vinyl silicone rubber was obtained to resist exudation.
[0019] The structural formula of methyl vinyl polysiloxane (methyl silicone rubber) is as follows: ; Where R1 is methyl or ethyl, and R2 is methyl or ethyl; x, y, and z are all integers greater than 0; The reaction formulas involved are as follows: .
[0020] Example 3 At room temperature, 50 g of trifluoropropyl vinyl polysiloxane (organosilicon intermediate), 0.5 g of di-tert-butyl peroxide (vulcanizing agent), and 250 g of tetrahydrofuran (solvent) were uniformly mixed. Then, the mixture was mixed with 500 g of flame retardant (ADP to MPP mass ratio of 3:1) in a high-speed stirrer for 30 min at a speed of 500 r / min to obtain a slurry containing organosilicon intermediate and flame retardant. Finally, the slurry was placed in a vacuum oven at 90 °C for 2 h to remove solvent and solidify. After crushing, a modified flame retardant with a fluorosilicone rubber shell was obtained to resist exudation.
[0021] The structural formula of trifluoropropyl vinyl polysiloxane (fluorosilicone rubber) is as follows: ; Where R1 is methyl or ethyl, and R2 is methyl or ethyl; x, y, and z are all integers greater than 0; The reaction formulas involved are as follows: .
[0022] Example 4 At room temperature, 100 g of methyl vinyl polysiloxane (organosilicon intermediate), 1 g of 2,5-dimethyl-2,5-di-tert-butylperoxyhexane (vulcanizing agent) and 500 g of ethyl acetate (solvent) were uniformly mixed; then, the mixture was mixed with 500 g of flame retardant (ADP to MCA mass ratio of 3:1) in a high-speed stirrer for 30 min at a speed of 500 r / min to obtain a slurry containing organosilicon intermediate and flame retardant. Finally, the slurry was placed in a vacuum oven at 90 °C for 2 h to remove solvent and cure, and then crushed to obtain a modified flame retardant with a shell of methyl silicone rubber that is resistant to exudation.
[0023] The structural formula of methyl vinyl polysiloxane (methyl silicone rubber) is as follows: ; Where R1 is methyl or ethyl, and R2 is methyl or ethyl; x, y, and z are all integers greater than 0; The reaction formulas involved are as follows: .
[0024] Compare with Example 1 ADP and MPP were mixed at a mass ratio of 3:1 to serve as a flame retardant (i.e., an unmodified flame retardant).
[0025] Then, the obtained unmodified flame retardant was subjected to electron microscopy, and the results are as follows: Figure 3 As shown; The hydrophilicity and hydrophobicity properties of the obtained unmodified flame retardant were evaluated, specifically by mixing 2 g of the unmodified flame retardant with 20 mL of water and stirring for 5 min. The results are as follows. Figure 4 As shown; It can be seen that, compared with the unmodified flame retardant, the modified flame retardant obtained in Example 1 has a surface covered by a layer of silicone rubber shell, and there is partial aggregation between MPP (particle size < 5 μm) and ADP (15 μm < particle size < 30 μm).
[0026] Compare with Example 2 ADP and MCA were mixed at a mass ratio of 3:1 to serve as a flame retardant (i.e., an unmodified flame retardant).
[0027] Compare with Example 3 Based on Example 2, this comparative example reduces the amount of organosilicon intermediate to discuss the effect of the ratio between the organosilicon intermediate and the flame retardant on the flame retardant properties of flame-retardant glass fiber reinforced PA66. Specifically: At room temperature, 1 g of methyl vinyl polysiloxane (organosilicon intermediate), 0.01 g of 2,5-dimethyl-2,5-di-tert-butylperoxyhexane (vulcanizing agent), and 500 g of ethyl acetate (solvent) were uniformly mixed. Then, the mixture was mixed with 500 g of flame retardant (ADP to MPP mass ratio of 3:1) in a high-speed stirrer for 30 min at a speed of 500 r / min to obtain a slurry containing organosilicon intermediate and flame retardant. Finally, the slurry was placed in a vacuum oven at 90 °C for 2 h to remove solvent and cure, and then crushed to obtain a modified flame retardant with a shell of methyl silicone rubber that is resistant to exudation.
[0028] The structural formula of methyl silicone rubber is as follows: ; Where R1 is methyl or ethyl, and R2 is methyl or ethyl; x, y, and z are all integers greater than 0; The reaction formulas involved are as follows: .
[0029] Application examples Based on Examples 1-4 and Comparative Examples 1-3, the obtained modified flame retardants and unmodified flame retardants were formulated according to the formulas in Table 1 below and prepared into flame retardant glass fiber reinforced PA66 by a twin-screw extruder.
[0030] Table 1 The prepared flame-retardant PA66 was injection molded into flame-retardant strips with a thickness of 0.8 mm and circular pieces with a diameter of 10 cm and a thickness of 3 mm. Under the conditions of temperature of 85 ℃ and relative humidity of 85%, flame retardancy tests were conducted according to UL-94 standard at 0 h, 200 h, 400 h and 600 h respectively. The results are shown in Table 2 below.
[0031] Table 2 The morphology of the discs before and after 600 hours of double 85 testing are as follows: Figures 5-8 As shown, PA66 with the modified flame retardant has no white bloom on its surface, while PA66 with the unmodified flame retardant has a large amount of white bloom on its surface. This is caused by the large-area bloom of the flame retardant on the material surface. As can be seen from the above test results, the modified flame retardant with anti-exudation provided by the present invention can not only enable PA66 to achieve UL-94 V-0 rating with a thickness of 0.8 mm with a small amount of addition, but also maintain its anti-exudation status for a long time under high temperature and high humidity environment; As can be seen from Comparative Example 3, when the amount of organosilicon intermediate is reduced, the flame retardant properties and exudation resistance of the corresponding flame-retardant glass fiber reinforced PA66 product decrease.
[0032] The above description is merely a preferred embodiment of the present invention and is not intended to limit the present invention in any way. Any simple modifications or equivalent changes made to the above embodiments based on the technical essence of the present invention shall fall within the protection scope of the present invention.
Claims
1. A modified flame retardant resistant to precipitation, characterized in that, The flame retardant is used as the core and the organosilicon is used as the shell. The organosilicon intermediate is deposited on the surface of the flame retardant, and then the organosilicon deposited on the surface of the flame retardant is subjected to free radical polymerization by vulcanization to form an organosilicon shell. The flame retardant is a flame retardant containing both phosphorus and nitrogen elements; The organosilicon intermediate is an organosilicon containing a double bond structure and not cross-linked; The modified flame retardant product with anti-exudation properties, at an addition amount of 15-18 wt.%, enables 10-30 wt.% glass fiber reinforced PA66 to achieve UL-94 V-0 rating at a thickness of 0.8 mm.
2. The modified flame retardant resistant to exudation according to claim 1, characterized in that, The flame retardant is one or any combination of two or more of diethylaluminum hypophosphite, melamine polyphosphate, and melamine cyanurate.
3. The modified flame retardant resistant to exudation according to claim 2, characterized in that, The flame retardant is a combination of diethyl aluminum hypophosphite and melamine polyphosphate, with a mass ratio of 2-5:1 between the two.
4. The modified flame retardant resistant to exudation according to claim 2, characterized in that, The flame retardant is a combination of diethyl aluminum hypophosphite and melamine cyanurate, with a mass ratio of 2-5:1 between the two.
5. The modified flame retardant resistant to exudation according to any one of claims 1-4, characterized in that, The structural formula of the organosilicon intermediate is as follows: ; or ; or ; R1 and R2 independently represent methyl or ethyl; x, y, and z are all integers greater than 0.
6. The modified flame retardant resistant to exudation according to claim 5, characterized in that, The structural formula of the silicone shell is as follows: ; or ; or R1 and R2 are independent representations; x, y, and z are all integers greater than 0.
7. A method for preparing a modified flame retardant resistant to precipitation, characterized in that, The preparation method of the modified flame retardant resistant to exudation according to any one of claims 1-6, the preparation method comprising the following steps: S1: Mix the solvent, organosilicon intermediate and vulcanizing agent evenly, then add it to the flame retardant and mix to obtain a slurry containing organosilicon intermediate and flame retardant; S2: The slurry obtained in step S1 is dried in a vacuum oven at 90-120 ℃ and cured for 1-2 h. Then, the product is crushed using a pulverizer to obtain a modified flame retardant resistant to precipitation.
8. The method for preparing the modified flame retardant resistant to precipitation according to claim 8, characterized in that, The solvent is one or any combination of two or more of anhydrous ethanol, tetrahydrofuran, and ethyl acetate; The vulcanizing agent is one or any combination of two or more of benzoyl peroxide, 2,5-dimethyl-2,5-di-tert-butylperoxide and di-tert-butyl peroxide.
9. The method for preparing the modified flame retardant resistant to precipitation according to claim 7, characterized in that, The mass ratio of the solvent to the flame retardant is 20–100:100, the mass ratio of the organosilicon intermediate to the flame retardant is 1–20:100, and the mass ratio of the vulcanizing agent to the organosilicon intermediate is 0.5–5:
100.
10. Using the efflorescence-resistant modified flame retardant according to any one of claims 1-6, or the efflorescence-resistant modified flame retardant produced by the preparation method according to any one of claims 7-9, to prepare halogen-free flame retardant PA66.
Citation Information
Patent Citations
Halogen-free and flame-retardant polyamide alloy material with low precipitation and preparation method of polyamide alloy material
CN109679338A
High-heat-resistant precipitation-resistant environment-friendly flame-retardant polyamide composition and preparation method thereof
CN114231025A
Precipitation-resistant halogen-free flame-retardant polyamide composition and preparation method thereof