Preparation method of graphite-phase carbon nitride-based composite flame retardant, flame retardant, application of flame retardant to PBAT flame-retardant composite material and preparation method
Thin-layer g-C₃N₄ was prepared by gradient thermal polymerization and metal ion coordination composite modification, which solved the problems of dispersion and interfacial compatibility of graphitic carbon nitride in PBAT matrix, formed a dense carbon layer, realized efficient flame retardancy and industrial production, and improved the fire resistance performance of PBAT.
Patent Information
- Application Number
- CN202611310737.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-27
- Publication Date
- 2026-11-24
AI Technical Summary
Existing graphitic carbon nitride (g-C₃N₄) exhibits poor dispersibility and interfacial compatibility in PBAT matrix, resulting in weak char formation performance. Traditional modification schemes are insufficient in synergistic flame retardant effects, making industrial production difficult. Furthermore, it suffers from poor high-temperature thermal stability, failing to meet high fire protection requirements.
Thin-layer g-C₃N₄ was prepared by gradient thermal polymerization. An integrated composite flame retardant system was constructed by in-situ coating of polydopamine (PDA) and coordination composite with metal ions. This improved the dispersibility and interfacial bonding of fillers, formed a dense char layer, and enhanced the flame retardant performance.
It achieves highly efficient flame retardancy of PBAT composite materials, reaching the UL-94 V-0 rating, while maintaining the material's mechanical properties and processability, making it suitable for industrial production at a low cost.
Smart Images

Figure CN123152176A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of flame retardant preparation technology, and in particular to a method for preparing a graphite-phase carbon nitride-based composite flame retardant, the flame retardant, its application in PBAT flame retardant composite materials, and the preparation method thereof. Background Technology
[0002] Graphite-phase carbon nitride (g-C3N4) is a two-dimensional conjugated planar carbonitridium material composed solely of C and N elements. It possesses advantages such as excellent thermal stability, readily available and inexpensive raw materials, simple preparation processes, and the potential for large-scale production, making it widely studied in the field of polymer flame retardancy. Its two-dimensional layered structure can form a physical barrier layer during combustion, blocking the transfer of heat and combustible gases, thus exhibiting basic flame retardant potential. PBAT (polybutylene terephthalate) is a mainstream fully biodegradable thermoplastic widely used in packaging, films, and disposable products. However, the material itself is flammable and has a low fire safety rating, necessitating modification with halogen-free, high-efficiency flame retardants.
[0003] Currently, flame-retardant modification technologies for g-C3N4 mainly include heteroatom doping modification (such as high-temperature doping with heteroatoms like phosphorus, boron, and silicon), physical compounding with traditional intumescent flame retardants (such as simple mechanical mixing with ammonium polyphosphate), and simple metal / metal oxide physical loading. However, the above-mentioned existing technologies still have the following technical shortcomings: First, the interfacial compatibility is poor, and the filler agglomerates severely. The g-C3N4 surface is rich in amino groups and lone pairs of electrons, making it extremely hydrophilic; the PBAT matrix is a hydrophobic polymer, and the two have a huge difference in interfacial polarity. When pure carbon nitride is used as filler, it is very easy to agglomerate, resulting in uneven dispersion of the filler in the matrix and weak interfacial bonding, which directly leads to a decrease in the mechanical properties of the composite material and the failure to achieve the expected flame retardant efficiency.
[0004] Secondly, pure g-C3N4 has poor char-forming properties and a low flame retardant rating. The char layer produced by the combustion of unmodified carbon nitride is loose and porous with extremely low mechanical strength and numerous gaps, making it unable to effectively insulate against heat, combustible gases, and oxygen. The material is difficult to self-extinguish and can only achieve a V-2 or even no flame retardant rating, failing to meet the standards for products with high fire resistance requirements.
[0005] Third, traditional modification methods have insufficient synergistic flame retardant effects. Heteroatom doping, physical blending with ammonium polyphosphate, and simple metal oxide loading only achieve simple composites without chemically anchoring the metal components; metal particles are prone to detachment and loss, resulting in weak synergistic effects in catalytic char formation and limited improvement in char layer densification.
[0006] Fourth, traditional modification processes have obvious drawbacks, limiting their industrialization. Existing doping and metal precipitation modifications often require high temperatures and pressures, toxic organic solvents, harsh reaction conditions, high equipment investment, and high waste treatment costs, making large-scale industrial production difficult.
[0007] Fifth, the composite material exhibits poor high-temperature thermal stability and low char residue. Pure PBAT decomposes rapidly at high temperatures, resulting in a low char residue at 800℃; ordinary modified carbon nitride fillers offer only limited improvement in char residue, and the matrix rapidly decomposes at high temperatures, posing a high risk of continued combustion in a fire. Summary of the Invention
[0008] To address at least one of the aforementioned technical problems, this invention proposes a method for preparing a graphite-phase carbon nitride-based composite flame retardant, the flame retardant itself, its application in PBAT flame-retardant composite materials, and the preparation method thereof. The method involves a three-step modification process: gradient thermal polymerization to prepare a thin layer of g-C3N4, in-situ coating of polydopamine (PDA) surface, and metal ion coordination composite to construct an integrated composite flame retardant system. This significantly improves the technology across multiple dimensions, including preparation process, filler dispersibility, interfacial bonding, thermal stability, charring ability, flame retardant properties, material mechanical compatibility, and industrial suitability.
[0009] To achieve the above objectives, the present invention adopts the following technical solution: The first aspect of this invention provides a method for preparing a graphite-phase carbon nitride-based composite flame retardant, comprising the following steps: S1: Place 5-10 parts by weight of nitrogen-rich precursor in a covered crucible, and polymerize and exfoliate the nitrogen-rich precursor by two-stage gradient temperature controlled calcination to obtain thin g-C3N4 nanosheets. S2: Take 0.2-0.5 parts by weight of thin-layer g-C3N4 nanosheets and disperse them in 100 parts by weight of deionized water. After stirring and ultrasonic treatment in an ice-water bath, a uniform suspension is prepared. S3: Tris powder was added to the homogeneous suspension in S2 to prepare a 200 mM Tris buffer solution, and the pH was adjusted to 8.5 with hydrochloric acid; then dopamine hydrochloride was added, and the mass ratio of the thin-layer g-C3N4 nanosheets to dopamine hydrochloride was controlled. The mixture was stirred at room temperature to allow dopamine hydrochloride to polymerize in situ on the surface of the graphitic carbon nitride nanosheets to form a continuous polydopamine coating layer; after the reaction was completed, the mixture was centrifuged, washed, dried, and ground to obtain the g-C3N4@PDA intermediate; S4: Dissolve the g-C3N4@PDA intermediate in S3 with two transition metal salts in deionized water at a mass ratio of 1:(1-3):(1-3). Stir at room temperature and use the chelating coordination effect of polydopamine to anchor the two transition metal ions on the polydopamine surface in the form of coordination bonds. After the reaction is completed, wash with deionized water and anhydrous ethanol alternately, dry and grind to obtain a graphite phase carbon nitride-based composite flame retardant.
[0010] Preferably, the nitrogen-rich precursor in S1 is any one or more of urea, melamine, thiourea, or dicyandiamide.
[0011] Preferably, the two-stage gradient temperature-controlled calcination in S1 includes: the first stage heating to 550-600℃ at a heating rate of 2-5℃ / min, holding at that temperature for 3-5 hours, naturally cooling, and grinding to obtain yellow coarse powder; the second stage heating to 450-550℃ at a heating rate of 5-10℃ / min, holding at that temperature for 2-3 hours, cooling, and grinding.
[0012] Preferably, the mixture in step S2 is stirred for 30 minutes and then ultrasonicated in an ice-water bath for 0.5 to 1 hour.
[0013] Preferably, the mass ratio of thin-layer g-C3N4 nanosheets to dopamine hydrochloride in S3 is 1:3-1:10; and the mixture is stirred at room temperature for 8-12 hours.
[0014] Preferably, the mass ratio of the thin g-C3N4 nanosheets to dopamine hydrochloride in S3 is 1:4-1:8 or 1:6.
[0015] Preferably, in S4, the g-C3N4@PDA intermediate and the two transition metal salts are in a mass ratio of 1:(1.5-2.5):(1.5-2.5) or 1:2:2.
[0016] Preferably, the transition metal salt in S4 is a combination of cobalt salt and zinc salt, or a combination of iron salt and nickel salt.
[0017] A second aspect of the present invention provides a flame retardant prepared by the method described in the first aspect.
[0018] The third aspect of the present invention provides a PBAT flame-retardant composite material, comprising: 90-99 parts by weight of PBAT matrix and 1-10 parts by weight of graphite-phase carbon nitride-based composite flame retardant prepared by the method of the second aspect.
[0019] A fourth aspect of the present invention provides a method for preparing the PBAT flame-retardant composite material as described in the third aspect, comprising the following steps: SS1, after melting the PBAT matrix at 130°C, a graphite-phase carbon nitride-based composite flame retardant is added and stirred continuously for 2 hours to obtain a uniform melt; SS2 was degassed in a vacuum drying oven at 130℃ for 15 minutes to remove air bubbles, and then naturally cooled and molded to obtain PBAT flame-retardant composite material.
[0020] Compared with the prior art, the present invention has the following beneficial effects: 1. This invention employs a two-stage gradient thermal polymerization process to prepare thin-layer g-C3N4, resulting in thinner layers and significantly reduced layer stacking compared to conventional one-step calcined carbon nitride sheets. This significantly increases the specific surface area, providing ample active sites for subsequent modification. In-situ polymerization of polydopamine (PDA) coats the g-C3N4 surface, forming a continuous organic interfacial bridging layer. This alters the inherently strong hydrophilic surface properties of carbon nitride, significantly reducing the interfacial tension with the hydrophobic PBAT matrix and fundamentally improving the interfacial compatibility between the two phases. The PDA layer is rich in phenolic hydroxyl and amino coordination sites, which can uniformly chelate bimetallic ions such as cobalt, zinc, iron, and nickel. The active metal components exhibit no local agglomeration and are uniformly distributed on the sheet surface, forming a complete composite functional layer. This improves the microstructure and dispersion performance of the filler, solves the agglomeration problem, and achieves uniform dispersion of the matrix.
[0021] 2. In this invention, polydopamine itself is rich in aromatic carbon structures, which can be rapidly carbonized at high temperatures to provide a char source. The loaded metal ions have a highly efficient catalytic char-forming function. The two work synergistically to catalyze the cross-linking and carbonization of the PBAT matrix, generating a continuous, dense, highly graphitized, and stable char layer without large pores or cracks after combustion, resulting in a significant leap in flame retardancy. The dense char layer plays multiple barrier roles: preventing the diffusion of external oxygen inward, blocking the release of internal combustible pyrolysis gases outward, and blocking the bidirectional transfer of heat, thus inhibiting the continuous combustion chain reaction and achieving self-extinguishing of the material. The bimetallic synergistic modified flame retardant of this invention can achieve the highest flame retardancy rating of UL-94V-0 with a low addition amount of only 3wt%. The three flame retardant mechanisms of two-dimensional thin-layer g-C3N4 sheet physical barrier + PDA char source + metal catalytic char formation work synergistically, and the flame retardant efficiency is far higher than that of single carbon nitride and simple physical compound flame retardant systems. At the same time, it effectively avoids problems such as decreased toughness, reduced tensile strength, and poor processing fluidity of PBAT caused by high filler addition, and retains the original mechanical, flexible, and processable properties of PBAT biodegradable substrate to the greatest extent. It can be used for environmentally friendly flame-retardant products such as disposable packaging, agricultural mulch film, and biodegradable injection molded products.
[0022] 3. The entire flame retardant preparation process of this invention uses deionized water as the reaction medium, eliminating the need for toxic organic solvents, high-temperature, high-pressure, or highly corrosive conditions, and requiring no high-end precision equipment. It uses inexpensive nitrogen-rich precursors such as urea and melamine, dopamine hydrochloride, and conventional metal nitrates / chlorides as raw materials, which are readily available and inexpensive. Gradient calcination, aqueous phase dispersion, and centrifugal drying are all mature chemical unit operations with a wide range of reaction parameters and high tolerance, allowing for direct scale-up to industrial continuous production.
[0023] The flame retardant system of this invention is compatible with a variety of transition metal ions (Co). 2+ Zn 2+ Fe 2+ Ni 2+(etc.), the bimetallic synergistic system has the best catalytic carbonization effect and can achieve the V-0 high flame retardancy standard; the formula is highly adjustable and can be adapted to the flame retardancy index requirements of different downstream products. Attached Figure Description
[0024] Figure 1 This is a schematic diagram of the preparation process of the graphite phase carbon nitride-based composite flame retardant in an embodiment of the present invention; Figure 2 Scanning electron microscope (SEM) images of g-C3N4 prepared by a one-time calcination method; Figure 3 Scanning electron microscope (SEM) images of g-C3N4 prepared by the secondary calcination method; Figure 4 XPS full spectra of g-C3N4 and g-C3N4@PDA-Co / Zn, and O1s, Co2p and Zn2p spectra of g-C3N4@PDA-Co / Zn from high-magnification XPS analysis; Figure 5 XRD diffraction patterns of pure phase g-C3N4, g-C3N4@PDA, and g-C3N4@PDA-Co / Zn; Figure 6 This is a scanning electron microscope (SEM) image of the composite flame retardant g-C3N4@PDA-Co / Zn of the present invention; Figure 7 The thermogravimetric (TG) curves show a comparison of the residual carbon content after thermal decomposition at 800℃ for pure PBAT, PBAT / g-C3N4, PBAT / g-C3N4@PDA-Zn, PBAT / g-C3N4@PDA-Fe / Ni, and PBAT / g-C3N4@PDA-Co / Zn samples. Detailed Implementation
[0025] To enable those skilled in the art to better understand the technical solutions of the present invention, the technical solutions of the present invention will be clearly and completely described below with reference to the accompanying drawings of the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments of the present invention.
[0026] Example 1 For ease of understanding, the relevant chemical symbols and their corresponding Chinese names in the text are explained as follows: g-C3N4: Graphitic carbon nitride, a two-dimensional conjugated planar carbon-nitrogen material composed only of carbon (C) and nitrogen (N); PBAT: Polybutylene adipate terephthalate, a fully biodegradable thermoplastic; PDA: Polydopamine, a polymer formed by the self-polymerization of dopamine hydrochloride under weakly alkaline conditions; Tris: Tris(hydroxymethyl)aminomethane, a commonly used biological buffer; Co: Cobalt; Zn: Zinc; Fe: Iron; Ni: Nickel; Co 2+Divalent cobalt ions; Zn 2+ : Divalent zinc ion; Fe 3+ : Trivalent iron ion; Ni 2+ Nickel ions: divalent nickel ions; UL-94: Underwriters Laboratories' standard for testing the flammability of plastic materials; V-0: the highest flame retardant rating in the UL-94 standard, indicating that the material can self-extinguish within 10 seconds in a vertical burning test without igniting cotton with molten droplets; TG: Thermogravimetric analysis, a thermal analysis method that measures the relationship between sample mass change and temperature through programmed temperature control; XRD: X-ray diffraction, a characterization method used to analyze the crystal structure of materials; SEM: Scanning electron microscopy, a characterization method used to observe the microstructure of materials; XPS: X-ray photoelectron spectroscopy, a characterization method used to analyze the elemental composition and chemical state of the surface of materials.
[0027] Please refer to Figure 1 As shown in the figure, this embodiment provides a method for preparing a graphite-phase carbon nitride-based composite flame retardant, comprising the following steps: S1: Preparation of thin-layer g-C3N4 nanosheets Five to ten parts by weight (exemplarily, the parts by weight can be 5, 6, 7, 8, 9, 10, or any combination of two of the above values, or any value within the range of two of the above values) of nitrogen-rich precursor are placed in a covered crucible. The nitrogen-rich precursor is polymerized and exfoliated through a two-stage gradient temperature-controlled calcination process to obtain thin-layer g-C3N4 nanosheets. Specifically, the nitrogen-rich precursor is any one or more of urea, melamine, thiourea, or dicyandiamide. Urea is preferred in this embodiment.
[0028] Specifically, in this embodiment, the parameters for the first stage of calcination are: heating rate of 2-5℃ / min (preferably 2℃ / min in this embodiment), heating to 550-600℃ (preferably 550℃ in this embodiment), and holding at that temperature for 3-5 hours (preferably 4 hours in this embodiment), allowing the precursor to fully thermally condense and form graphitic carbon nitride. After holding at that temperature, the mixture is naturally cooled to room temperature and then ground to obtain yellow coarse carbon nitride powder.
[0029] Take 0.5 to 2 parts by weight (exemplary parts by weight can be 0.5, 0.6, 0.7, 0.8, 0.9, 1.0, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9, 2.0, or any combination of the above values) and place the yellow coarse powder in an uncovered alumina crucible for a second calcination. The second calcination process parameters are: heating rate 5 to 10 °C / min (preferably 5 °C / min in this embodiment), heating to 450 to 550 °C (preferably 500 °C in this embodiment), holding for 2 to 3 hours (preferably 2 hours in this embodiment), and perform a second low-temperature exfoliation treatment on the first calcination product. After holding, allow it to cool naturally to room temperature and grind to obtain a light yellow thin layer of g-C3N4 nanosheet powder.
[0030] Please refer to Figure 2 The figure shows a scanning electron microscope (SEM) image of g-C3N4 prepared by a single calcination method. It can be seen from the figure that there is obvious stacking between the layers of g-C3N4, and few active sites are exposed, which is not conducive to modification treatment.
[0031] Compared to Figure 3 The SEM image of g-C3N4 prepared by the secondary calcination method shown clearly shows that the g-C3N4 sheets are more uniformly dispersed and have more exposed active sites, providing a large number of active sites for subsequent modification.
[0032] It is understandable that the core function of the two-stage gradient temperature-controlled calcination in this embodiment is: the first stage of high-temperature long-term heat preservation ensures that the precursor is fully polymerized to form a complete carbon nitride sheet structure; the second stage of secondary calcination at a lower temperature uses thermal stress to weaken the weak van der Waals forces between the sheets, thereby achieving sheet peeling, which significantly reduces the degree of sheet stacking, increases the specific surface area and surface active sites, and provides sufficient loading sites for subsequent PDA coating and metal coordination.
[0033] It should be noted that the process parameters are mainly based on the following considerations: In this embodiment, if the first-stage calcination temperature is below 550℃ or the holding time is less than 3 hours, the precursor polymerization is incomplete, resulting in low crystallinity of carbon nitride and numerous lamellar defects. If the first-stage calcination temperature is above 600℃ or the holding time exceeds 5 hours, excessive lamellar growth and severe stacking occur, making subsequent peeling difficult. If the second-stage calcination temperature is below 450℃, the thermal stress is insufficient to effectively peel off the lamellars; if it is above 550℃, secondary sintering and re-stacking of the lamellars may occur, increasing energy consumption and reducing economic efficiency.
[0034] Preparation of S2-S3: g-C3N4@PDA intermediate Take 0.2-0.5 parts by weight (exemplary, the weight value can be 0.2, 0.3, 0.4, 0.5 or any two of the above values or any value within the range of any two of the above values) of thin-layer g-C3N4 nanosheets and disperse them in 100 parts by weight of deionized water. Stir for 30 min and treat with sonication in an ice water bath for 0.5-1 h to prepare a uniform suspension.
[0035] Tris powder was added to the homogeneous suspension in S2 to prepare a 200 mM Tris buffer solution, and the pH was adjusted to 8.5 with hydrochloric acid. Dopamine hydrochloride was then added, controlling the mass ratio of the thin-layer g-C3N4 nanosheets to dopamine hydrochloride. The mixture was stirred at room temperature for 8-12 hours to allow dopamine hydrochloride to polymerize in situ on the surface of the graphitic carbon nitride nanosheets, forming a continuous polydopamine coating layer. The continuous polydopamine coating layer refers to the PDA coating layer extending along the surface of the g-C3N4 sheets and covering most of its surface, forming a complete organic interface bridging layer.
[0036] After the reaction was completed, the product was centrifuged, washed, dried, and ground to obtain the g-C3N4@PDA intermediate.
[0037] Specifically, the mass ratio of thin-layer g-C3N4 nanosheets to dopamine hydrochloride is 1:3-1:10; preferably 1:4-1:8, more preferably 1:6. In this embodiment, there are 0.5g of g-C3N4 nanosheets and 3.0g of dopamine hydrochloride.
[0038] It is understood that in this embodiment, PDA contains a large number of phenolic hydroxyl and amino groups. One end can form hydrogen bonds with the amino groups on the surface of g-C3N4, and the other end can form intermolecular forces with the hydrophobic PBAT matrix, acting as a continuous organic interface bridging layer between the g-C3N4 and PBAT phases, fundamentally improving interfacial compatibility and eliminating filler agglomeration.
[0039] Meanwhile, PDA is rich in phenolic hydroxyl and amino coordination sites, which can stably chelate and anchor transition metal ions in subsequent steps, preventing the physical shedding of metal components.
[0040] In addition, PDA itself is a carbon-rich organic polymer, which can be rapidly carbonized during high-temperature combustion to assist in char formation and improve the density of the char layer.
[0041] Understandably, the selection of key process parameters is primarily based on the following considerations: If the amount of dopamine hydrochloride (DA) added is too low (the mass ratio of g-C3N4 to DA is greater than 1:10), the PDA coating layer will be discontinuous, failing to form a complete interfacial bridging layer and sufficient metal coordination sites; if the amount added is too high (the mass ratio is less than 1:3), the PDA layer will be too thick, potentially leading to severe adhesion of the g-C3N4 sheets, and excessive PDA coating will reduce the thermal stability of the final flame retardant. If the reaction time is less than 8 hours, dopamine polymerization will be incomplete and the PDA layer thickness will be insufficient; if it exceeds 12 hours, polymerization will tend to saturate and increase the production cycle, which is detrimental to industrial efficiency.
[0042] Preparation of S4: g-C3N4@PDA-Co / Zn composite flame retardant The g-C3N4@PDA intermediate in S3 was dissolved in deionized water with two transition metal salts at a mass ratio of 1:(1-3):(1-3). The mixture was stirred at room temperature for 0.5–2 hours (preferably 1 hour in this embodiment). The two transition metal ions were anchored to the polydopamine surface by coordination bonds using the chelating coordination effect of polydopamine. Specifically, the oxygen atom of the phenolic hydroxyl group and the nitrogen atom of the amino group in the PDA molecule contain lone pairs of electrons, which can form coordination bonds with the empty orbitals of the transition metal ions, achieving chemical bonding and anchoring. This coordination chemical anchoring method differs from the simple physical mixing or physical precipitation loading in the prior art. Metal ions are uniformly anchored on the PDA surface in a molecular-level dispersion form, forming a nanoscale metal catalytic layer. During high-temperature combustion, the metal ions will not be lost due to physical shedding and can continue to play a catalytic char formation role, promoting the rapid graphitization of PBAT and PDA, generating a continuous, dense, and high-strength char layer, strengthening the condensed phase barrier flame retardancy, and significantly improving the char rate and UL-94 flame retardancy rating. After the reaction was completed, the product was washed alternately with deionized water and anhydrous ethanol, dried and ground to obtain a graphite-phase carbon nitride-based composite flame retardant.
[0043] To demonstrate coordinate bond formation, please refer to Figure 4 As shown in the figure, the XPS full spectrum of g-C3N4 and g-C3N4@PDA-Co / Zn is displayed, as well as the O1s, Co2p and Zn2p spectra of g-C3N4@PDA-Co / Zn obtained from high-magnification XPS analysis.
[0044] Specifically, XPS analysis was performed on the original sample g-C3N4 and g-C3N4@PDA-Co / Zn hybrid. Figure 4 a shows that XPS full spectrum reveals that both materials contain C, N, and O elements, with Co and Zn additionally detected in the hybrid.
[0045] like Figure 4b shows that the O1s spectrum at 530.55 eV corresponds to the Co-O / Zn-O bond, at 531.94 eV corresponds to the C-OH (phenolic hydroxyl group) in PDA, at 533.33 eV corresponds to the C=O / COC bond (derived from the carbonyl group, ether bond and coordinated oxygen in PDA), and at 535.44 eV is surface adsorbed water.
[0046] like Figure 4 c shows that the Co 2p spectrum can be fitted to two sets of spin-orbit double peaks and their satellite peaks, with 780.44 eV and 796.33 eV corresponding to Co 2p and 796.33 eV respectively. 2+ Co 2p 3 / 2 and Co 2p 1 / 2 The spin-orbit splitting energy is 15.89 eV, and satellite peaks confirm that cobalt is represented by Co. 2+ It exists in the form of a substance and is stabilized by coordination with N and O atoms in PDA and g-C3N4.
[0047] like Figure 4 d shows that the Zn 2p spectrum exhibits a pair of double peaks at 1021.25 eV (Zn 2p 3 / 2 ) and 1044.35 eV (Zn 2p 1 / 2 The peak spacing of 23.1 eV indicates that Zn 2+ Successful load.
[0048] It should be noted that in this embodiment, the transition metal salt is a combination of cobalt and zinc salts, specifically cobalt nitrate hexahydrate (Co(NO3)2·6H2O) and zinc nitrate hexahydrate (Zn(NO3)2·6H2O). The g-C3N4@PDA intermediate is mixed with the two transition metal salts in a mass ratio of 1:(1.5-2.5):(1.5-2.5) or 1:2:2. Specifically, in this embodiment, the intermediate is 0.2g, cobalt nitrate hexahydrate is 0.4g, and zinc nitrate hexahydrate is 0.4g.
[0049] Understandably, the selection of key process parameters is primarily based on the following considerations: If the amount of metal salt is too low (the mass ratio of intermediate to metal salt is less than 1:3), the metal coordination sites on the PDA surface cannot be fully utilized, resulting in insufficient density of catalytic active sites and limited synergistic catalytic carbonization effect; if the amount of metal salt is too high (the mass ratio is greater than 1:1), excessive metal ions may physically agglomerate on the PDA surface, forming large particles, leading to poor dispersibility and wasting raw materials. If the stirring time is less than 0.5 h, the coordination reaction between metal ions and PDA has not yet reached equilibrium, resulting in insufficient metal loading and uneven distribution; if it exceeds 2 h, the coordination reaction has been completed, but the production cycle is prolonged, which is detrimental to large-scale production.
[0050] Please refer to Figure 5 To verify the structure of the flame retardant at different preparation stages in this embodiment, Figure 5 The XRD diffraction patterns of pure phase g-C3N4, g-C3N4@PDA, and g-C3N4@PDA-Co / Zn are shown.
[0051] from Figure 5 It can be seen that the pure phase g-C3N4 exhibits a strong and sharp characteristic diffraction peak at 2θ≈27.5°, which belongs to the (002) crystal plane of the graphitic carbon nitride, reflecting its typical layered stacked structure; a weaker diffraction peak appears at 2θ≈13.0°, corresponding to the (100) crystal plane, which reflects the periodic arrangement of the tri-s-triazine structural units in the plane.
[0052] Compared with pure g-C3N4, the (002) and (100) characteristic peak positions of g-C3N4@PDA remain basically unchanged, indicating that the polydopamine (PDA) coating process does not damage the main crystal structure of g-C3N4; its diffraction peak intensity is reduced and the peak shape is broadened, mainly due to the coating effect of the amorphous PDA layer on the surface of g-C3N4, which reduces the overall crystallinity of the material and reduces the orderliness of the interlayer stacking to a certain extent.
[0053] In the final product g-C3N4@PDA-Co / Zn, the characteristic diffraction peaks of g-C3N4 can still be clearly identified, indicating that the main crystal phase structure remains stable after loading the Co / Zn bimetallic component; the diffraction peak intensity further decreases and the broadening phenomenon is more significant, indicating that the introduction of Co / Zn metal species has a more significant impact on the crystallinity and structural order of the material.
[0054] At the same time, combined Figure 6 Scanning electron microscopy (SEM) images of the composite flame retardant g-C3N4@PDA-Co / Zn are shown. It can be seen that the composite flame retardant g-C3N4@PDA-Co / Zn maintains the unique two-dimensional lamellar framework of g-C3N4, with the lamellars stacked and partially curled to form a three-dimensional network structure with a certain porosity. On the surface of the g-C3N4 lamellars, the PDA coating layer undergoes an in-situ coordination reaction with Co / Zn metal ions, generating porous nanoclusters of uneven size. These clusters are tightly anchored to the lamellar surface and edges, exhibiting a coral-like porous morphology in some areas, a typical characteristic of the chelation coordination between metal ions and functional groups such as catechol and amino groups in PDA.
[0055] Compared to the binary g-C3N4@PDA composite material, the surface roughness of the Co / Zn doped material is significantly improved, and the specific surface area is further optimized. This unique porous layered structure not only provides ample exposed sites for catalytic active sites, but also provides efficient channels for mass transport and charge transfer during the reaction process, providing reliable structural support for improving the performance of this composite material in the field of flame retardancy.
[0056] Example 2 Unlike Example 1, the transition metal salts used in this example are iron salts and nickel salts, specifically ferric chloride hexahydrate (FeCl3·6H2O) and nickel chloride hexahydrate (NiCl2·6H2O).
[0057] It should be noted that, in this application, the transition metal is preferably a fourth-period transition metal.
[0058] Of course, transition elements from other periods are based on the same flame retardant mechanism and can theoretically be adapted to the bimetallic flame retardant system in this application. However, considering cost, environmental protection and processing performance, transition elements from other periods are not the optimal choice compared to transition elements from the fourth period.
[0059] Meanwhile, from a technical perspective, there are no compatibility restrictions for multi-element composite flame retardant systems formed by three or more transition metals. However, compared to bimetallic systems, multi-element composite flame retardant systems do not offer a significant improvement in flame retardant performance. Therefore, considering production costs, process control difficulties, and the overall performance of the substrate, bimetallic composite flame retardant systems are the optimal combination.
[0060] Comparative Example 1 Unlike Example 1, this example uses a single metal salt, specifically zinc nitrate hexahydrate (Zn(NO3)2·6H2O).
[0061] Preparation Example 1 This preparation example provides a PBAT flame-retardant composite material, comprising: 90-99 parts by weight of PBAT matrix and 1-10 parts by weight of graphite-phase carbon nitride-based composite flame retardant prepared by the preparation method of Example 1.
[0062] Preferably, the weight parts of the PBAT matrix can be 90, 91, 92, 93, 94, 95, 96, 97, 98, 99, or any range of any two of the above values, or any value within the range of any two of the above values; the weight parts of the corresponding graphite phase carbon nitride-based composite flame retardant can be 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, or any range of any two of the above values, or any value within the range of any two of the above values.
[0063] The preparation method of the above-mentioned PBAT flame-retardant composite material includes the following steps: SS1 involves melting the PBAT matrix at 130°C, adding a graphite-phase carbon nitride-based composite flame retardant, and continuously stirring for 2 hours to obtain a homogeneous melt. It is understood that the processing temperature of 130°C is lower than the thermal decomposition initiation temperature of PBAT, ensuring that PBAT does not undergo thermal degradation during processing. Simultaneously, this temperature is higher than the melting point of PBAT, giving the melt sufficient fluidity to achieve uniform dispersion of the flame retardant.
[0064] SS2 was degassed in a vacuum drying oven at 130℃ for 15 minutes to remove air bubbles, and then naturally cooled and molded to obtain PBAT flame-retardant composite material.
[0065] Preparation Example 2 Unlike Preparation Example 1, this preparation example uses the graphite-phase carbon nitride-based composite flame retardant prepared in Example 2.
[0066] Preparation Example 3 Unlike Preparation Example 1, this preparation example uses the graphite-phase carbon nitride-based composite flame retardant prepared in Comparative Example 1.
[0067] Please refer to Figure 7 As shown, in order to verify the flame retardant properties of different flame retardant materials, this application compares the residual char content of flame retardant materials prepared by pure PBAT resin, unmodified pure thin-layer g-C3N4, Preparation Example 1, Preparation Example 2 and Preparation Example 3 at 800℃.
[0068] The thermogravimetric (TG) curve shows that pure PBAT begins to decompose rapidly at around 400℃, and by 500℃, the mass loss exceeds 95%. It does not have a UL-94 flame retardant rating, and the char residue rate at 800℃ is only 2.24%, indicating that it degrades almost completely at high temperatures, making it difficult to form an effective protective char layer and exhibiting poor thermal stability.
[0069] After introducing g-C3N4, the final char residue of the PBAT / g-C3N4 composite material increased to 5.18%, achieving a UL-94 rating of V-2. This is mainly attributed to the thermal decomposition of g-C3N4, which releases inert gases such as NH3 and N2, diluting the concentration of combustible gases through a gas-phase flame-retardant effect. Simultaneously, the nitrogen-containing char residue formed during its decomposition can, to some extent, block heat and mass transfer. However, due to the low char content and porous structure, the improvement in thermal stability and flame retardancy is limited.
[0070] After PDA-supported Fe and Ni bimetallic modification to obtain g-C3N4@PDA-Fe / Ni filler, the final char residue of the PBAT / g-C3N4@PDA-Fe / Ni composite material was further improved to 6.96%, achieving a UL-94 rating of V-1. For the PBAT / g-C3N4@PDA-Co / Zn composite material, the final char residue reached 8.23%, achieving a UL-94 rating of V-0. 10% The thermal decomposition temperature is 382.6℃. In the high-temperature range above 500℃, the char retention rate of this sample is significantly higher than that of the other three groups of samples, exhibiting the best thermal stability and long-term barrier ability of the char layer. Compared with the Fe / Ni bimetallic modification system, Co / Zn transition metal ions have stronger catalytic carbonization activity during polymer thermal degradation, and can induce the matrix to generate more continuous, high-temperature resistant protective char.
[0071] Meanwhile, the composite material formed by the single-metal composite flame retardant g-C3N4@PDA-Zn, after flame retardancy testing, achieved a UL-94 flame retardancy rating of V-1 and a char residue rate of 5.22% at 800℃.
[0072] Therefore, the bimetallic composite material prepared in this application can form a dense, high-strength barrier char layer during combustion, exhibiting excellent char-forming and flame-retardant properties. Specifically, polydopamine itself is rich in aromatic carbon structures, which can rapidly carbonize at high temperatures to provide a char source; the supported metal ions have highly efficient catalytic char-forming functions, and the two synergistically catalyze the cross-linking and carbonization of the PBAT matrix, generating a continuous, dense, highly graphitized, and stable char layer without large pores or cracks after combustion, which is different from the loose, porous, and easily damaged char layer after combustion of pure g-C3N4.
[0073] At the same time, the dense carbon layer can not only isolate external oxygen from diffusing inward, block the release of internal combustible pyrolysis gases outward, and block the bidirectional transfer of heat, but also inhibit the continuous progress of the combustion chain reaction, thus enabling the material to self-extinguish.
[0074] Furthermore, in this preparation scheme, the bimetallic synergistic modified sample (Example 1, Co / Zn composite system) can achieve the highest flame retardant rating of UL-94 V-0 with a low addition amount of only 3wt%.
[0075] In this invention, deionized water is used as the solvent in the flame retardant preparation process, eliminating the need for toxic organic solvents. The reaction is carried out at room temperature or low temperature, requiring no high-pressure or high-temperature equipment. The process is simple, environmentally friendly, and suitable for industrial mass production. The flame-retardant composite material is prepared by low-temperature melt blending at 130℃, with mild processing conditions that do not compromise the biodegradability of PBAT.
[0076] The above description is a specific implementation of the embodiments of the present invention. It should be noted that for those skilled in the art, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications should also be considered within the scope of protection of this application.
Claims
1. A method for preparing a graphite-phase carbon nitride-based composite flame retardant, characterized in that, Includes the following steps: S1: Place 5-10 parts by weight of nitrogen-rich precursor in a covered crucible, and polymerize and peel off the nitrogen-rich precursor by two-stage gradient temperature controlled calcination to obtain thin g-C3N4 nanosheets. S2: Take 0.2-0.5 parts by weight of thin-layer g-C3N4 nanosheets and disperse them in 100 parts by weight of deionized water. After stirring and ultrasonic treatment in an ice-water bath, a uniform suspension is prepared. S3: Tris powder was added to the homogeneous suspension in S2 to prepare a 200 mM Tris buffer solution, and the pH was adjusted to 8.5 with hydrochloric acid; then dopamine hydrochloride was added, and the mass ratio of the thin-layer g-C3N4 nanosheets to dopamine hydrochloride was controlled. The mixture was stirred at room temperature to allow dopamine hydrochloride to polymerize in situ on the surface of the graphitic carbon nitride nanosheets to form a continuous polydopamine coating layer; after the reaction was completed, the mixture was centrifuged, washed, dried, and ground to obtain the g-C3N4@PDA intermediate; S4: Dissolve the g-C3N4@PDA intermediate in S3 with two transition metal salts in deionized water at a mass ratio of 1:(1-3):(1-3). Stir at room temperature and use the chelating coordination effect of polydopamine to anchor the two transition metal ions on the polydopamine surface in the form of coordination bonds. After the reaction is completed, wash with deionized water and anhydrous ethanol alternately, dry and grind to obtain a graphite phase carbon nitride-based composite flame retardant.
2. The preparation method of the graphite-phase carbon nitride-based composite flame retardant according to claim 1, characterized in that, The nitrogen-rich precursor in S1 is any one or more of urea, melamine, thiourea, or dicyandiamide.
3. The preparation method of the graphite-phase carbon nitride-based composite flame retardant according to claim 1, characterized in that, The two-stage gradient temperature-controlled calcination in S1 includes: the first stage heating to 550-600℃ at a heating rate of 2-5℃ / min, holding at that temperature for 3-5 hours, naturally cooling, and grinding to obtain yellow coarse powder; the second stage heating to 450-550℃ at a heating rate of 5-10℃ / min, holding at that temperature for 2-3 hours, cooling, and grinding.
4. The preparation method of the graphite-phase carbon nitride-based composite flame retardant according to claim 1, characterized in that, Stir in S2 for 30 minutes, then sonicate in an ice-water bath for 0.5 to 1 hour.
5. The method for preparing the graphite-phase carbon nitride-based composite flame retardant according to claim 1, characterized in that, The mass ratio of thin-layer g-C3N4 nanosheets to dopamine hydrochloride in S3 is 1:3-1:10; stir at room temperature for 8-12 hours.
6. The method for preparing the graphite-phase carbon nitride-based composite flame retardant according to claim 1, characterized in that, The mass ratio of the thin-layer g-C3N4 nanosheets to dopamine hydrochloride in S3 is 1:4-1:8 or 1:
6.
7. The method for preparing the graphite-phase carbon nitride-based composite flame retardant according to claim 1, characterized in that, In S4, the g-C3N4@PDA intermediate is mixed with two transition metal salts in a mass ratio of 1:(1.5-2.5):(1.5-2.5) or 1:2:2; the transition metal salts in S4 are a combination of cobalt salt and zinc salt, or a combination of iron salt and nickel salt.
8. The flame retardant prepared by the method for preparing the graphite phase carbon nitride-based composite flame retardant according to any one of claims 1-7.
9. A PBAT flame-retardant composite material, characterized in that, include: 90-99 parts by weight of PBAT matrix and 1-10 parts by weight of the flame retardant as described in claim 8.
10. A method for preparing the PBAT flame-retardant composite material as described in claim 9, characterized in that, Includes the following steps: SS1, after melting the PBAT matrix at 130°C, a graphite-phase carbon nitride-based composite flame retardant is added and stirred continuously for 2 hours to obtain a uniform melt; SS2 was degassed in a vacuum drying oven at 130℃ for 15 minutes to remove air bubbles, and then naturally cooled and molded to obtain PBAT flame-retardant composite material.