Long-acting salt-storing and slow-release hydraulic asphalt anticoagulant modifier, hydraulic asphalt and preparation method thereof

A long-acting salt-storing and slow-release hydraulic asphalt anti-crystallization modifier was prepared by using a porous adsorption carrier and fluidized bed coating method. This method solved the problems of easy volatility and excessively rapid release of calcium formate and magnesium formate, and achieved long-acting antifreeze and crack-resistant properties and stable anti-icing effect of hydraulic asphalt, making it suitable for water conservancy projects in cold regions.

CN123152177APending Publication Date: 2026-11-24XIAN UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611538410.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-30
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

In existing technologies, calcium formate and magnesium formate are easily volatile and have a rapid release rate, which leads to a rapid decline in the anti-icing performance of hydraulic asphalt, making it difficult to achieve long-term antifreeze and crack-resistant effects.

Method used

A long-acting salt-storing slow-release hydraulic asphalt anticoagulant modifier was prepared by combining a porous adsorption carrier with a fluidized bed coating method. The release rate of calcium formate and magnesium formate was controlled by the adsorption of the porous adsorption carrier and the formation of a uniform and dense slow-release layer by fluidized bed coating, thus forming a continuous and uniform coating layer and avoiding the loss of active ingredients.

Benefits of technology

It achieves stable release of calcium formate and magnesium formate, long-lasting anti-icing performance, improves the freeze-thaw resistance and service life of hydraulic asphalt, reduces production costs, and is suitable for water conservancy projects in cold regions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

This invention discloses a long-acting, salt-storing, slow-release hydraulic asphalt anti-coagulation modifier, hydraulic asphalt, and its preparation method. The steps are as follows: A composite active powder and a porous adsorption carrier are prepared; the composite active powder and the porous adsorption carrier are added to anhydrous ethanol for reflux reaction to obtain an adsorption-supported intermediate; a coating liquid is prepared, and the coating liquid is mixed with the adsorption-supported intermediate and then coated using a fluidized bed coating method to obtain modifier particles; a hydrophobic modifier, dispersant, and toughening agent are added to the modifier particles, mixed, dried, pulverized, and sieved to obtain the long-acting, salt-storing, slow-release hydraulic asphalt anti-coagulation modifier; the matrix hydraulic asphalt is heated and melted, an anti-aging agent is added and stirred, and then the long-acting, salt-storing, slow-release hydraulic asphalt anti-coagulation modifier is preheated and added, stirred until uniformly dispersed to obtain a freeze-thaw resistant, crack-resistant, low-freezing-point hydraulic asphalt material. This invention solves the problems of easy volatility and excessively rapid release rate of calcium formate and magnesium formate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of hydraulic asphalt modification technology, specifically relating to the preparation method of long-acting salt-storing slow-release hydraulic asphalt anti-crystallizing modifier, as well as antifreeze and crack-resistant low-freezing-point hydraulic asphalt materials, and the preparation method of antifreeze and crack-resistant low-freezing-point hydraulic asphalt materials. Background Technology

[0002] Hydraulic asphalt, a core material in water conservancy projects, is widely used in reservoir seepage prevention. However, in cold regions, low temperatures can easily cause defects such as freezing cracks and peeling in hydraulic asphalt, and surface icing can seriously affect the safety and performance of engineering structures. Calcium formate and magnesium formate, as environmentally friendly anti-icing materials, have advantages such as low freezing point, low corrosivity to concrete and metals, strong high-temperature stability, and low volatility, making them ideal active ingredients for modifying hydraulic asphalt to prevent icing.

[0003] However, there are significant drawbacks in the existing technology of directly adding calcium formate and magnesium formate to hydraulic asphalt: First, calcium formate and magnesium formate are prone to volatilization during high-temperature mixing and use, resulting in the loss of active ingredients and rapid decay of anti-icing performance; Second, the release rate of calcium formate and magnesium formate is too fast, and the excessive release in the early stage can easily damage the bonding performance of asphalt, and the lack of effective ingredients in the later stage will make it impossible to maintain the long-term anti-icing effect. Currently, slow-release treatments for calcium formate and magnesium formate mostly employ single-carrier adsorption or simple coating methods. However, single-carrier adsorption capacity is limited, making it difficult to effectively prevent the loss of active ingredients; while simple polymer coating can achieve slow release, the coating layer is easily damaged by the swelling of the asphalt matrix, resulting in unstable slow-release effects. Therefore, developing a highly efficient anti-icing modifier for hydraulic asphalt that effectively inhibits the loss of active ingredients and provides controllable slow release is crucial for improving the freeze-thaw resistance and crack resistance of hydraulic asphalt. Summary of the Invention

[0004] The first objective of this invention is to provide a method for preparing a long-acting, slow-release, salt-absorbing anti-coagulant modifier for hydraulic asphalt, thereby solving the problems of easy volatility and excessively rapid release rate of calcium formate and magnesium formate in existing methods.

[0005] The second objective of this invention is to provide a frost-resistant, crack-resistant, low-freezing-point hydraulic asphalt material.

[0006] The third objective of this invention is to provide a method for preparing frost-resistant, crack-resistant, low-freezing-point hydraulic asphalt materials.

[0007] The first technical solution adopted in this invention is a method for preparing a long-acting salt-storing slow-release hydraulic asphalt anti-coagulant modifier, the steps of which are as follows: Step 1: Prepare composite active powder and porous adsorption carrier; Step 2: Add the composite active powder and porous adsorption carrier to anhydrous ethanol, stir and mix, then reflux the mixture, filter and dry to obtain the adsorption-supported intermediate. Step 3: Prepare coating solution. Mix the coating solution with the adsorption-supported intermediate and then perform coating treatment using a fluidized bed coating method to obtain modifier particles. Step 4: Add hydrophobic modifier, dispersant and toughening agent to the modifier particles, stir and mix, then dry, pulverize and sieve to obtain long-acting salt-storing slow-release hydraulic asphalt anti-crystallizing modifier.

[0008] The invention is further characterized by: In step 1, the process of preparing the composite active powder is as follows: calcium formate and magnesium formate with a mass ratio of 0.83~1.2:1 are added to deionized water and stirred at 40℃~60℃ for 1.5h~3h until completely dissolved to obtain a mixed solution. The obtained mixed solution is filtered, and the filtrate is concentrated by vacuum distillation to a solid content of 40%~50%. The concentrated solid is dried, pulverized and sieved to obtain the composite active powder. In the mixed solution, the sum of the masses of calcium formate and magnesium formate accounts for 15% to 25% of the sum of the masses of calcium formate, magnesium formate, and deionized water. The pressure of vacuum distillation is -0.08MPa to -0.1MPa, the temperature is 50℃ to 70℃, and the time is 1h to 3h.

[0009] In step 1, the process of preparing the porous adsorption carrier is as follows: diatomaceous earth and bentonite in a mass ratio of 1~3:1 are added to water and ultrasonically dispersed at a power of 200W~300W for 20min~30min, then dried at a temperature of 80℃~100℃ for 12h~24h, and after drying, they are ground and sieved to obtain the porous adsorption carrier.

[0010] In step 2, the amount of composite active powder added is 30 to 50 parts, the amount of porous adsorption carrier added is 15 to 30 parts, and the total mass ratio of composite active powder and porous adsorption carrier to anhydrous ethanol is 1:2 to 3. The stirring rate is 300 r / min to 500 r / min, the stirring time is 30 min to 60 min, the reflux reaction temperature is 60℃ to 80℃, the reflux reaction time is 2 h to 4 h, the drying temperature is 50℃ to 60℃, and the drying time is 8 h to 12 h.

[0011] In step 3, the coating solution is prepared by dissolving polylactic acid and chitosan in ethyl acetate at a mass ratio of 0.5 to 2:1 to obtain the coating solution. In the coating solution, the total mass of polylactic acid and chitosan accounts for 5% to 10% of the total mass of polylactic acid, chitosan and ethyl acetate.

[0012] In step 3, the coating process using the fluidized bed coating method is as follows: The adsorbent-loaded intermediate is placed in the fluidized bed equipment hopper. The feed inlet is closed, and the equipment's airtightness is checked. The hot air system is turned on to preheat the fluidized bed, stabilizing the temperature of the adsorbent-loaded intermediate at 40℃~60℃. The fluidizing air velocity is adjusted to 0.8m / s~1.6m / s, ensuring the adsorbent-loaded intermediate is in a suspended, dispersed, and non-agglomerated fluidized state under the action of the airflow. The coating solution is then loaded into the supply device and pumped at a rate of 10mL / min using a peristaltic pump. A constant rate of ~30 mL / min is used to deliver the coating liquid to the atomizing nozzle. The spraying pressure is adjusted to between 0.15 and 0.3 MPa to atomize the coating liquid into fine droplets and spray them evenly onto the fluidized adsorbent-supported intermediate. The droplets evaporate and solidify rapidly under the action of hot air, forming a continuous and uniform coating layer on the surface of the fluidized adsorbent-supported intermediate. The spraying is repeated 2 to 3 times. After the spraying is completed, the fluidized state is maintained and the product is dried for 10 to 15 minutes. The hot air system is then stopped, the material is discharged and collected to obtain the modifier particles. The mass ratio of the coating solution to the adsorption-supported medium is 1:5~10.

[0013] In step 4, the mass ratio of hydrophobic modifier, dispersant, toughening agent to modifier particles is 2~8:1~5:1~3:100; The drying temperature is 40℃~50℃, and the drying time is 4h~6h.

[0014] The second technical solution adopted in this invention is a freeze-resistant, crack-resistant, low-freezing-point hydraulic asphalt material, which uses the above-mentioned long-acting salt-storing slow-release hydraulic asphalt anti-coagulation modifier and is composed of the following components by weight fraction: 70-85 parts of base hydraulic asphalt, 15-30 parts of long-acting salt-storing slow-release hydraulic asphalt anti-coagulation modifier, and 0.5-2 parts of anti-aging agent. The anti-aging agent consists of antioxidant 1010 and ultraviolet absorber UV-531 in a mass ratio of 1:1.

[0015] The third technical solution adopted in this invention is a method for preparing frost-resistant, crack-resistant, low-freezing-point hydraulic asphalt material, the steps of which are as follows: Step 1: Weigh the following raw materials by weight: 70-85 parts of base hydraulic asphalt, 15-30 parts of long-acting salt-storing slow-release hydraulic asphalt anti-coagulant modifier, and 0.5-2 parts of anti-aging agent. The anti-aging agent is composed of antioxidant 1010 and ultraviolet absorber UV-531 in a mass ratio of 1:1. The anti-aging agent can be obtained by stirring and mixing antioxidant 1010 and ultraviolet absorber UV-531 evenly at room temperature. Step 2: Heat and melt the base hydraulic asphalt, then add the anti-aging agent and stir to obtain a mixture. Add the long-acting salt-storing slow-release hydraulic asphalt anti-crystallization modifier after preheating to the mixture and stir until it is evenly dispersed to obtain a freeze-thaw resistant, crack-resistant, low-freezing-point hydraulic asphalt material.

[0016] The invention is further characterized by: The heating and melting temperature is 130℃~150℃, the heating and melting time is 15min~20min, the preheating temperature is 60℃~80℃, and the stirring speed is 500 r / min~800 r / min.

[0017] The beneficial effects of this invention are: (1) The preparation method of the long-acting salt storage slow-release hydraulic asphalt anticoagulant modifier of the present invention, through the dual protection of porous carrier adsorption and fluidized bed dense coating, the dissolution rate of calcium formate and magnesium formate is greatly reduced, the active ingredients are effectively retained, and the anticoagulant performance is stable and does not decay under low freezing point conditions. (2) The preparation method of the long-acting salt storage slow-release hydraulic asphalt anti-crystallization modifier of the present invention forms a uniform and complete slow-release layer through fluidized bed coating, which matches the adsorption rate of the carrier, so as to achieve uniform and stable release of active components. It does not damage the asphalt bonding performance in the early stage, and provides anti-icing effect in the later stage, and the long-acting effect is significantly improved. (3) The preparation method of the long-acting salt storage slow-release hydraulic asphalt anti-coagulant modifier of the present invention achieves particle non-adhesion and breakage by adopting fluidized bed coating process. The process is simple, the conditions are mild, and it can be produced on a large scale without complicated equipment modification. The production cost is controllable and it has good prospects for industrial application. (4) The antifreeze and crack-resistant low freezing point hydraulic asphalt material prepared by the method of the present invention can be reduced to -20℃~-26℃. After 50 freeze-thaw cycles, the residual penetration ratio is ≥87%. The antifreeze and crack-resistant, water damage-resistant and anti-aging properties are comprehensively improved, and the service life of hydraulic asphalt structures is greatly extended. Detailed Implementation

[0018] The present invention will now be described in detail with reference to specific embodiments.

[0019] The preparation method of the long-acting salt-storing slow-release hydraulic asphalt anti-coagulant modifier of the present invention comprises the following steps: Step 1: Prepare composite active powder and porous adsorption carrier; The process for preparing the composite active powder is as follows: calcium formate and magnesium formate in a mass ratio of 0.83 to 1.2:1 are added to deionized water and stirred at 40°C to 60°C for 1.5 to 3 hours until completely dissolved to obtain a mixed solution. The mixed solution is then filtered, and the filtrate is concentrated by vacuum distillation to a solid content of 40% to 50%. The concentrated solid is then dried, pulverized, and passed through an 80-mesh sieve to obtain the composite active powder. In the mixed solution, the sum of the masses of calcium formate and magnesium formate accounts for 15% to 25% of the sum of the masses of calcium formate, magnesium formate, and deionized water. The pressure of vacuum distillation is -0.08MPa to -0.1MPa, the temperature of vacuum distillation is 50℃ to 70℃, and the time of vacuum distillation is 1h to 3h. The process of preparing porous adsorption carrier is as follows: diatomaceous earth and bentonite in a mass ratio of 1~3:1 are added to water, ultrasonically dispersed at a power of 200W~300W for 20min~30min, and then dried at a temperature of 80℃~100℃ for 12h~24h. After drying, the material is ground through a 100-mesh sieve to obtain porous adsorption carrier. A porous adsorption carrier was prepared by using diatomaceous earth and bentonite. The synergistic advantages of the high porosity of diatomaceous earth and the high adsorption of bentonite were utilized, which significantly improved the adsorption capacity compared with a single carrier. It can also firmly fix calcium formate and magnesium formate, and greatly reduce the leaching loss under high temperature mixing, water immersion and freeze-thaw conditions. Step 2: Add the composite active powder and porous adsorption carrier to anhydrous ethanol, stir and mix, then reflux the mixture, filter and dry to obtain the adsorption-supported intermediate. The amount of composite active powder added is 30 to 50 parts, the amount of porous adsorption carrier added is 15 to 30 parts, and the total mass ratio of composite active powder and porous adsorption carrier to anhydrous ethanol is 1:2 to 3. The stirring rate is 300 r / min to 500 r / min, the stirring time is 30 min to 60 min, the reflux reaction temperature is 60℃ to 80℃, the reflux reaction time is 2 h to 4 h, the drying temperature is 50℃ to 60℃, and the drying time is 8 h to 12 h. Step 3: Prepare coating solution. Mix the coating solution with the adsorption-supported intermediate and then perform coating treatment using a fluidized bed coating method to obtain modifier particles. The coating solution is prepared by dissolving polylactic acid and chitosan in ethyl acetate at a mass ratio of 0.5 to 2:1 to obtain the coating solution. Polylactic acid and chitosan are used as coating materials, which have biodegradable properties; In the coating solution, the combined mass of polylactic acid and chitosan accounts for 5% to 10% of the combined mass of polylactic acid, chitosan, and ethyl acetate. The coating process using the fluidized bed coating method is as follows: The adsorbent-loaded intermediate is placed in the fluidized bed equipment hopper. The feed inlet is closed, and the equipment's airtightness is checked. The hot air system is turned on to preheat the fluidized bed, stabilizing the temperature of the adsorbent-loaded intermediate at 40℃~60℃. The fluidizing air velocity is adjusted to 0.8m / s~1.6m / s, ensuring the adsorbent-loaded intermediate is in a suspended, dispersed, and non-agglomerated fluidized state under the action of the airflow. The coating solution is then loaded into the supply device and pumped through a peristaltic pump at a constant rate of 10mL / min~30mL / min. The solution is fed to the atomizing nozzle, and the spraying pressure is adjusted to 0.15MPa~0.3MPa. The coating liquid is atomized into fine droplets and evenly sprayed onto the fluidized adsorbent-supported intermediate. The droplets evaporate and solidify rapidly under the action of hot air, forming a continuous and uniform coating layer on the surface of the fluidized adsorbent-supported intermediate. The spraying is repeated 2 to 3 times. After the spraying is completed, the fluidized state is maintained and the particles are dried for 10 to 15 minutes to ensure that the particles are completely dry and do not stick together. The hot air system is stopped, the material is discharged and collected, and modified agent particles with complete coating and stable slow-release performance are obtained. The mass ratio of the coating solution to the adsorption-supported intermediate is 1:5~10; The coating process using fluidized bed coating method results in a coating layer on the modifier particles that is continuous, uniform, dense, undamaged, and leak-free. This coating layer can prevent rapid water penetration that could lead to a sudden release of active ingredients, while also enabling long-term, uniform release, thus avoiding problems such as excessive initial release and subsequent failure. Step 4: Add hydrophobic modifier, dispersant and toughening agent to the modifier particles, stir and mix for 20 min to 40 min, then dry, pulverize and sieve through an 80 mesh to obtain long-lasting salt-storing slow-release hydraulic asphalt anti-crystallizing modifier; The mass ratio of hydrophobic modifier, dispersant, toughening agent and modifier particles is 2~8:1~5:1~3:100; The drying temperature is 40℃~50℃, and the drying time is 4h~6h.

[0020] This invention relates to a long-acting, slow-release, salt-absorbing anti-freezing modifier for hydraulic asphalt. By adding a methyltriethoxysilane hydrophobic modifier to the modifier particles, the freezing point of hydraulic asphalt can be significantly reduced, improving its antifreeze and crack-resistant properties and extending the service life of the hydraulic asphalt structure. It is suitable for anti-freezing modification treatment in hydraulic engineering projects in cold regions. Simultaneously, the introduction of dispersants and toughening agents significantly improves the compatibility between the modifier and the asphalt matrix, prevents particle agglomeration, and enhances the low-temperature toughness and anti-aging properties of the asphalt. Therefore, this invention achieves slow dissolution and controlled release of calcium formate and magnesium formate through the adsorption of composite active powder on a porous adsorption carrier and the formation of a dense coating on the porous adsorption carrier with adsorbed composite active powder using a fluidized bed coating method. This combination of factors improves the antifreezing performance and antifreeze and crack-resistant durability of hydraulic asphalt.

[0021] The frost-resistant, crack-resistant, low-freezing-point hydraulic asphalt material is composed of the following components by weight: 70-85 parts of base hydraulic asphalt, 15-30 parts of long-lasting salt-storing and slow-release hydraulic asphalt anti-coagulation modifier, and 0.5-2 parts of anti-aging agent. The anti-aging agent is composed of antioxidant 1010 and ultraviolet absorber UV-531 in a mass ratio of 1:1. The anti-aging agent can be obtained by stirring and mixing antioxidant 1010 and ultraviolet absorber UV-531 evenly at room temperature.

[0022] The preparation method of freeze-thaw resistant, crack-resistant, low-freezing-point hydraulic asphalt material includes the following steps: Step 1: Weigh the following raw materials by weight: 70-85 parts of base hydraulic asphalt, 15-30 parts of long-acting salt-storing slow-release hydraulic asphalt anti-coagulant modifier, and 0.5-2 parts of anti-aging agent. Step 2: Heat the base hydraulic asphalt at 130℃~150℃ for 15min~20min, then add the anti-aging agent and stir for 10min~15min to obtain a mixture. Add the long-acting salt-storing slow-release hydraulic asphalt anti-crack modifier after preheating at 60℃~80℃ to the mixture, and stir at 500 r / min~800 r / min for 30min~45min until uniformly dispersed to obtain a freeze-thaw resistant, crack-resistant, low-freezing-point hydraulic asphalt material.

[0023] Example 1 The preparation method of the long-acting salt-storing slow-release hydraulic asphalt anti-coagulant modifier of the present invention comprises the following steps: Step 1: Prepare composite active powder and porous adsorption carrier; The process for preparing the composite active powder is as follows: calcium formate and magnesium formate in a mass ratio of 1:1.1 are added to deionized water and stirred at 50°C for 2 hours until completely dissolved to obtain a mixed solution. The mixed solution is filtered, and the filtrate is concentrated by vacuum distillation to a solid content of 45%. The concentrated solid is dried, pulverized, and passed through an 80-mesh sieve to obtain the composite active powder. In the mixed solution, the sum of the masses of calcium formate and magnesium formate accounts for 20% of the sum of the masses of calcium formate, magnesium formate, and deionized water. The pressure of vacuum distillation is -0.09 MPa, the temperature of vacuum distillation is 60℃, and the time of vacuum distillation is 2 hours. The process of preparing the porous adsorption carrier is as follows: diatomaceous earth and bentonite in a mass ratio of 1:1 are added to water, ultrasonically dispersed at a power of 250W for 25 minutes, and then dried at 90℃ for 18 hours. After drying, the mixture is ground through a 100-mesh sieve to obtain the porous adsorption carrier. Step 2: Add the composite active powder and porous adsorption carrier to anhydrous ethanol, stir and mix, then reflux the mixture, filter and dry to obtain the adsorption-supported intermediate. The amount of composite active powder added is 35 parts, the amount of porous adsorption carrier added is 20 parts, and the total mass ratio of composite active powder and porous adsorption carrier to anhydrous ethanol is 1:2. The stirring rate was 400 r / min, the stirring time was 45 min, the reflux reaction temperature was 70℃, the reflux reaction time was 3 h, the drying temperature was 55℃, and the drying time was 10 h. Step 3: Prepare coating solution. Mix the coating solution with the adsorption-supported intermediate and then perform coating treatment using a fluidized bed coating method to obtain modifier particles. The coating solution is prepared by dissolving polylactic acid and chitosan in ethyl acetate at a mass ratio of 2:1 to obtain the coating solution. In the coating solution, the combined mass of polylactic acid and chitosan accounts for 8% of the combined mass of polylactic acid, chitosan, and ethyl acetate. The coating process using the fluidized bed coating method is as follows: The adsorbent-loaded intermediate is placed in the fluidized bed equipment hopper. The feed inlet is closed, and the equipment's airtightness is checked. The hot air system is turned on to preheat the fluidized bed, stabilizing the temperature of the adsorbent-loaded intermediate at 50℃. The fluidizing air velocity is adjusted to 1.2 m / s, ensuring the adsorbent-loaded intermediate is in a suspended, dispersed, and non-clumping fluidized state under the airflow. The coating liquid is loaded into the supply device and delivered to the atomizing nozzle at a constant rate of 20 mL / min via a peristaltic pump. The spraying pressure is adjusted to 0.2 MPa, atomizing the coating liquid into fine droplets and uniformly spraying it onto the fluidized adsorbent-loaded intermediate. The droplets rapidly evaporate and solidify under the action of hot air, forming a continuous and uniform coating layer on the surface of the fluidized adsorbent-loaded intermediate. This process is repeated twice. After spraying, the fluidized state is maintained for another 12 minutes to ensure the particles are completely dry and do not stick together. The hot air system is then stopped, and the material is discharged and collected, yielding modified agent particles with complete coating and stable slow-release properties. The mass ratio of the coating solution to the adsorption-supported intermediate is 1:7. Step 4: Add hydrophobic modifier, dispersant and toughening agent to the modifier particles, stir and mix for 25 minutes, dry at 45℃ for 5 hours, pulverize and sieve through an 80-mesh screen to obtain long-acting salt-storing slow-release hydraulic asphalt anti-crystallizing modifier. The mass ratio of hydrophobic modifier, dispersant, toughening agent and modifier particles is 5:3:2:100; The hydrophobic modifier is methyltriethoxysilane, the dispersant is polyethylene glycol 4000, and the toughening agent is nano-silica.

[0024] The frost-resistant, crack-resistant, low-freezing-point hydraulic asphalt material is composed of the following components by weight: 75 parts of base hydraulic asphalt, 23 parts of long-lasting salt-storing and slow-release hydraulic asphalt anti-crystallizing modifier, and 2 parts of anti-aging agent. The anti-aging agent consists of 1 part antioxidant 1010 and 1 part ultraviolet absorber UV-531.

[0025] The preparation method of freeze-thaw resistant, crack-resistant, low-freezing-point hydraulic asphalt material includes the following steps: Step 1: Weigh the following raw materials by weight: 75 parts of base hydraulic asphalt, 23 parts of long-acting salt-storing slow-release hydraulic asphalt anti-coagulant modifier, and 2 parts of anti-aging agent. The anti-aging agent consists of 1 part antioxidant 1010 and 1 part ultraviolet absorber UV-531; Step 2: Heat the base hydraulic asphalt at 140℃ for 17 minutes to melt it, then add the anti-aging agent and stir for 12 minutes to obtain a mixture. Add the long-acting salt-storing slow-release hydraulic asphalt anti-crack modifier after preheating at 70℃ to the mixture, and stir at 600 r / min for 40 minutes until it is evenly dispersed to obtain a freeze-thaw resistant, crack-resistant, low-freezing-point hydraulic asphalt material.

[0026] Example 2 The preparation method of the long-acting salt-storing slow-release hydraulic asphalt anti-coagulant modifier of the present invention comprises the following steps: Step 1: Prepare composite active powder and porous adsorption carrier; The process for preparing the composite active powder is as follows: calcium formate and magnesium formate in a mass ratio of 1:1.14 are added to deionized water and stirred at 40°C for 1.5 hours until completely dissolved to obtain a mixed solution. The mixed solution is filtered, and the filtrate is concentrated by vacuum distillation to a solid content of 40%. The concentrated solid is dried, pulverized, and passed through an 80-mesh sieve to obtain the composite active powder. In the mixed solution, the sum of the masses of calcium formate and magnesium formate accounts for 15% of the sum of the masses of calcium formate, magnesium formate, and deionized water. The pressure of vacuum distillation is -0.08 MPa, the temperature of vacuum distillation is 50℃, and the time of vacuum distillation is 1 hour. The process of preparing the porous adsorption carrier is as follows: diatomaceous earth and bentonite in a mass ratio of 1.5:1 are added to water, ultrasonically dispersed at a power of 200W for 20 minutes, and then dried at 80℃ for 24 hours. After drying, the mixture is ground through a 100-mesh sieve to obtain the porous adsorption carrier. Step 2: Add the composite active powder and porous adsorption carrier to anhydrous ethanol, stir and mix, then reflux the mixture, filter and dry to obtain the adsorption-supported intermediate. The amount of composite active powder added is 30 parts, the amount of porous adsorption carrier added is 15 parts, and the total mass ratio of composite active powder and porous adsorption carrier to anhydrous ethanol is 1:3. The stirring rate was 300 r / min, the stirring time was 60 min, the reflux reaction temperature was 60℃, the reflux reaction time was 2 h, the drying temperature was 60℃, and the drying time was 12 h. Step 3: Prepare coating solution. Mix the coating solution with the adsorption-supported intermediate and then perform coating treatment using a fluidized bed coating method to obtain modifier particles. The coating solution is prepared by dissolving polylactic acid and chitosan in ethyl acetate at a mass ratio of 1:1 to obtain the coating solution. In the coating solution, the combined mass of polylactic acid and chitosan accounts for 5% of the combined mass of polylactic acid, chitosan, and ethyl acetate; The coating process using the fluidized bed coating method is as follows: The adsorbent-loaded intermediate is placed in the fluidized bed equipment hopper. The feed inlet is closed, and the equipment's airtightness is checked. The hot air system is turned on to preheat the fluidized bed, stabilizing the temperature of the adsorbent-loaded intermediate at 45℃. The fluidizing air velocity is adjusted to 0.8 m / s, ensuring the adsorbent-loaded intermediate is in a suspended, dispersed, and non-clumping fluidized state under the airflow. The coating liquid is loaded into the supply device and delivered to the atomizing nozzle at a constant rate of 15 mL / min via a peristaltic pump. The spraying pressure is adjusted to 0.18 MPa, atomizing the coating liquid into fine droplets and uniformly spraying it onto the fluidized adsorbent-loaded intermediate. The droplets rapidly evaporate and solidify under the action of hot air, forming a continuous and uniform coating layer on the surface of the fluidized adsorbent-loaded intermediate. This process is repeated three times. After spraying, the fluidized state is maintained for another 10 minutes of drying to ensure the particles are completely dry and do not stick together. The hot air system is then stopped, and the material is discharged and collected, yielding modified agent particles with complete coating and stable slow-release properties. The mass ratio of the coating solution to the adsorption-supported medium is 1:7. Step 4: Add hydrophobic modifier, dispersant and toughening agent to the modifier particles, stir and mix for 20 minutes, dry at 40℃ for 6 hours, pulverize and sieve through an 80-mesh screen to obtain long-acting salt-storing slow-release hydraulic asphalt anti-crystallizing modifier. The mass ratio of hydrophobic modifier, dispersant, toughening agent and modifier particles is 5:3:2:100. The hydrophobic modifier is methyltriethoxysilane, the dispersant is polyethylene glycol 4000, and the toughening agent is nano-silica.

[0027] The freeze-thaw resistant, crack-resistant, low-freezing-point hydraulic asphalt material is composed of the following components by weight: 70 parts of base hydraulic asphalt, 29.5 parts of long-lasting salt-storing and slow-release hydraulic asphalt anti-crystallizing modifier, and 0.5 parts of anti-aging agent. The anti-aging agent consists of antioxidant 1010 and ultraviolet absorber UV-531 in a mass ratio of 1:1. The preparation method of freeze-thaw resistant, crack-resistant, low-freezing-point hydraulic asphalt material includes the following steps: Step 1: Weigh the following raw materials by weight: 70 parts of base hydraulic asphalt, 29.5 parts of long-acting salt-storing slow-release hydraulic asphalt anti-coagulant modifier, and 0.5 parts of anti-aging agent. The anti-aging agent consists of antioxidant 1010 and ultraviolet absorber UV-531 in a mass ratio of 1:1. Step 2: Heat the base hydraulic asphalt at 140℃ for 18 minutes, then add the anti-aging agent and stir for 12 minutes to obtain a mixture. Add the long-acting salt-storing slow-release hydraulic asphalt anti-crack modifier after preheating at 70℃ to the mixture, and stir at 650 r / min for 40 minutes until uniformly dispersed to obtain a freeze-thaw resistant, crack-resistant, low-freezing-point hydraulic asphalt material.

[0028] Example 3 The preparation method of the long-acting salt-storing slow-release hydraulic asphalt anti-coagulant modifier of the present invention comprises the following steps: Step 1: Prepare composite active powder and porous adsorption carrier; The process for preparing the composite active powder is as follows: calcium formate and magnesium formate in a mass ratio of 1.08:1 are added to deionized water and stirred at 60°C for 3 hours until completely dissolved to obtain a clear liquid with a mass fraction of 25%. The clear liquid is filtered, and the filtrate is concentrated by vacuum distillation to a solid content of 50%. The concentrated solid is dried, pulverized, and passed through an 80-mesh sieve to obtain the composite active powder. In the mixed solution, the sum of the masses of calcium formate and magnesium formate accounts for 25% of the sum of the masses of calcium formate, magnesium formate, and deionized water. The pressure of vacuum distillation is -0.1 MPa, the temperature of vacuum distillation is 70℃, and the time of vacuum distillation is 3 hours. The process of preparing the porous adsorption carrier is as follows: diatomaceous earth and bentonite in a mass ratio of 3:1 are added to water, ultrasonically dispersed at a power of 300W for 30 minutes, and then dried at 100℃ for 12 hours. After drying, the mixture is ground through a 100-mesh sieve to obtain the porous adsorption carrier. Step 2: Add the composite active powder and porous adsorption carrier to anhydrous ethanol, stir and mix, then reflux the mixture, filter and dry to obtain the adsorption-supported intermediate. The amount of composite active powder added is 50 parts, the amount of porous adsorption carrier added is 30 parts, and the total mass ratio of composite active powder and porous adsorption carrier to anhydrous ethanol is 1:3. The stirring rate was 500 r / min, the stirring time was 30 min, the reflux reaction temperature was 80℃, the reflux reaction time was 4 h, the drying temperature was 60℃, and the drying time was 8 h. Step 3: Prepare coating solution. Mix the coating solution with the adsorption-supported intermediate and then perform coating treatment using a fluidized bed coating method to obtain modifier particles. The coating solution is prepared by dissolving polylactic acid and chitosan in ethyl acetate at a mass ratio of 2:1 to obtain the coating solution. In the coating solution, the combined mass of polylactic acid and chitosan accounts for 10% of the combined mass of polylactic acid, chitosan, and ethyl acetate. The coating process using the fluidized bed coating method is as follows: The adsorbent-loaded intermediate is placed in the fluidized bed equipment hopper. The feed inlet is closed, and the equipment's airtightness is checked. The hot air system is turned on, and the fluidized bed is preheated to stabilize the temperature of the adsorbent-loaded intermediate at 55℃. The fluidizing air velocity is adjusted to 1.2 m / s, ensuring the adsorbent-loaded intermediate is in a suspended, dispersed, and non-clumping fluidized state under the airflow. The coating liquid is loaded into the supply device and delivered to the atomizing nozzle at a constant rate of 15 mL / min via a peristaltic pump. The spraying pressure is adjusted to 0.18 MPa, atomizing the coating liquid into fine droplets and uniformly spraying it onto the fluidized adsorbent-loaded intermediate. The droplets rapidly evaporate and solidify under the action of hot air, forming a continuous and uniform coating layer on the surface of the fluidized adsorbent-loaded intermediate. This process is repeated twice. After spraying, the fluidized state is maintained for 15 minutes to ensure the particles are completely dry and do not stick together. The hot air system is then stopped, and the material is discharged and collected, yielding modified agent particles with complete coating and stable slow-release properties. The mass ratio of the coating solution to the adsorption-supported medium is 1:8. Step 4: Add hydrophobic modifier, dispersant and toughening agent to the modifier particles, stir and mix for 20 minutes, dry at 50°C for 4 hours, pulverize and sieve through an 80-mesh screen to obtain long-acting salt-storing slow-release hydraulic asphalt anti-crystallizing modifier. The mass ratio of hydrophobic modifier, dispersant, toughening agent to modifier particles is 8: 5: 3:100. The hydrophobic modifier is methyltriethoxysilane, the dispersant is polyethylene glycol 4000, and the toughening agent is nano-silica.

[0029] The antifreeze and crack-resistant low freezing point hydraulic asphalt material is composed of the following components by weight: 85 parts of base hydraulic asphalt, 15 parts of long-acting salt-storing slow-release hydraulic asphalt anti-crystallizing modifier, and 2 parts of anti-aging agent. The anti-aging agent consists of antioxidant 1010 and ultraviolet absorber UV-531 in a mass ratio of 1:1.

[0030] The preparation method of freeze-thaw resistant, crack-resistant, low-freezing-point hydraulic asphalt material includes the following steps: Step 1: Weigh the following raw materials by weight: 85 parts of base hydraulic asphalt, 15 parts of long-acting salt-storing slow-release hydraulic asphalt anti-coagulant modifier, and 2 parts of anti-aging agent. The anti-aging agent consists of antioxidant 1010 and ultraviolet absorber UV-531 in a mass ratio of 1:1. Step 2: Heat the base hydraulic asphalt at 145℃ for 15 minutes to melt it, then add the anti-aging agent and stir for 14 minutes to obtain a mixture. Add the long-acting salt-storing slow-release hydraulic asphalt anti-crack modifier after preheating at 75℃ to the mixture, and stir at 750 r / min for 35 minutes until it is evenly dispersed to obtain a freeze-thaw resistant, crack-resistant, low-freezing-point hydraulic asphalt material.

[0031] Example 4 The preparation method of the long-acting salt-storing slow-release hydraulic asphalt anti-coagulant modifier of the present invention comprises the following steps: Step 1: Prepare composite active powder and porous adsorption carrier; The process for preparing the composite active powder is as follows: calcium formate and magnesium formate in a mass ratio of 0.83:1 are added to deionized water and stirred at 40°C for 3 hours until completely dissolved to obtain a mixed solution. The mixed solution is then filtered, and the filtrate is concentrated by vacuum distillation to a solid content of 40%. The concentrated solid is then dried, pulverized, and passed through an 80-mesh sieve to obtain the composite active powder. In the mixed solution, the sum of the masses of calcium formate and magnesium formate accounts for 20% of the sum of the masses of calcium formate, magnesium formate, and deionized water. The pressure of vacuum distillation is -0.09 MPa, the temperature of vacuum distillation is 60℃, and the time of vacuum distillation is 2 hours. The process of preparing the porous adsorption carrier is as follows: diatomaceous earth and bentonite in a mass ratio of 1:1 are added to water, ultrasonically dispersed at a power of 250W for 25 minutes, and then dried at 90℃ for 18 hours. After drying, the mixture is ground through a 100-mesh sieve to obtain the porous adsorption carrier. Step 2: Add the composite active powder and porous adsorption carrier to anhydrous ethanol, stir and mix, then reflux the mixture, filter and dry to obtain the adsorption-supported intermediate. The amount of composite active powder added is 35 parts, the amount of porous adsorption carrier added is 20 parts, and the total mass ratio of composite active powder and porous adsorption carrier to anhydrous ethanol is 1:2. The stirring rate was 400 r / min, the stirring time was 45 min, the reflux reaction temperature was 70℃, the reflux reaction time was 3 h, the drying temperature was 50℃, and the drying time was 12 h. Step 3: Prepare coating solution. Mix the coating solution with the adsorption-supported intermediate and then perform coating treatment using a fluidized bed coating method to obtain modifier particles. The coating solution is prepared by dissolving polylactic acid and chitosan in ethyl acetate at a mass ratio of 0.5:1 to obtain the coating solution. In the coating solution, the combined mass of polylactic acid and chitosan accounts for 10% of the combined mass of polylactic acid, chitosan, and ethyl acetate. The coating process using the fluidized bed coating method is as follows: The adsorbent-loaded intermediate is placed in the fluidized bed equipment hopper. The feed inlet is closed, and the equipment's airtightness is checked. The hot air system is turned on, and the fluidized bed is preheated to stabilize the temperature of the adsorbent-loaded intermediate at 40℃. The fluidizing air velocity is adjusted to 1.6 m / s, ensuring the adsorbent-loaded intermediate is in a suspended, dispersed, and non-clumping fluidized state under the airflow. The coating liquid is loaded into the supply device and delivered to the atomizing nozzle at a constant rate of 10 mL / min via a peristaltic pump. The spraying pressure is adjusted to 0.15 MPa, atomizing the coating liquid into fine droplets and uniformly spraying it onto the fluidized adsorbent-loaded intermediate. The droplets rapidly evaporate and solidify under the action of hot air, forming a continuous and uniform coating layer on the surface of the fluidized adsorbent-loaded intermediate. This process is repeated twice. After spraying, the fluidized state is maintained for another 12 minutes to ensure the particles are completely dry and do not stick together. The hot air system is then stopped, and the material is discharged and collected, yielding modified agent particles with complete coating and stable slow-release properties. The mass ratio of the coating solution to the adsorption-supported intermediate is 1:5. Step 4: Add hydrophobic modifier, dispersant and toughening agent to the modifier particles, stir and mix for 40 minutes, dry at 45°C for 5 hours, pulverize and sieve through an 80-mesh screen to obtain long-acting salt-storing slow-release hydraulic asphalt anti-crystallizing modifier. The mass ratio of hydrophobic modifier, dispersant, toughening agent and modifier particles is 2:1:1:100; The hydrophobic modifier is methyltriethoxysilane, the dispersant is polyethylene glycol 4000, and the toughening agent is nano-silica.

[0032] The frost-resistant, crack-resistant, low-freezing-point hydraulic asphalt material is composed of the following components by weight: 70 parts of base hydraulic asphalt, 30 parts of long-lasting salt-storing and slow-release hydraulic asphalt anti-crystallizing modifier, and 2 parts of anti-aging agent. The anti-aging agent consists of 1 part antioxidant 1010 and 1 part ultraviolet absorber UV-531.

[0033] The preparation method of freeze-thaw resistant, crack-resistant, low-freezing-point hydraulic asphalt material includes the following steps: Step 1: Weigh the following raw materials by weight: 70 parts of base hydraulic asphalt, 30 parts of long-acting salt-storing slow-release hydraulic asphalt anti-coagulant modifier, and 2 parts of anti-aging agent. The anti-aging agent consists of 1 part antioxidant 1010 and 1 part ultraviolet absorber UV-531; Step 2: Heat the base hydraulic asphalt at 130℃ for 20 minutes to melt it, then add the anti-aging agent and stir for 10 minutes to obtain a mixture. Add the long-acting salt-storing slow-release hydraulic asphalt anti-crack modifier after preheating at 60℃ to the mixture, and stir at 500r / min for 30 minutes until it is evenly dispersed to obtain a freeze-thaw resistant, crack-resistant, low-freezing-point hydraulic asphalt material.

[0034] Example 5 The preparation method of the long-acting salt-storing slow-release hydraulic asphalt anti-coagulant modifier of the present invention comprises the following steps: Step 1: Prepare composite active powder and porous adsorption carrier; The process for preparing the composite active powder is as follows: calcium formate and magnesium formate in a mass ratio of 1.2:1 are added to deionized water and stirred at 50°C for 2 hours until completely dissolved to obtain a mixed solution. The mixed solution is then filtered, and the filtrate is concentrated by vacuum distillation to a solid content of 45%. The concentrated solid is then dried, pulverized, and passed through an 80-mesh sieve to obtain the composite active powder. In the mixed solution, the sum of the masses of calcium formate and magnesium formate accounts for 20% of the sum of the masses of calcium formate, magnesium formate, and deionized water. The pressure of vacuum distillation is -0.09 MPa, the temperature of vacuum distillation is 60℃, and the time of vacuum distillation is 2 hours. The process of preparing the porous adsorption carrier is as follows: diatomaceous earth and bentonite in a mass ratio of 1:1 are added to water, ultrasonically dispersed at a power of 250W for 25 minutes, and then dried at 90℃ for 18 hours. After drying, the mixture is ground through a 100-mesh sieve to obtain the porous adsorption carrier. Step 2: Add the composite active powder and porous adsorption carrier to anhydrous ethanol, stir and mix, then reflux the mixture, filter and dry to obtain the adsorption-supported intermediate. The amount of composite active powder added is 35 parts, the amount of porous adsorption carrier added is 20 parts, and the total mass ratio of composite active powder and porous adsorption carrier to anhydrous ethanol is 1:2.5. The stirring rate was 400 r / min, the stirring time was 45 min, the reflux reaction temperature was 70℃, the reflux reaction time was 3 h, the drying temperature was 55℃, and the drying time was 10 h. Step 3: Prepare coating solution. Mix the coating solution with the adsorption-supported intermediate and then perform coating treatment using a fluidized bed coating method to obtain modifier particles. The coating solution is prepared by dissolving polylactic acid and chitosan in ethyl acetate at a mass ratio of 2:1 to obtain the coating solution. In the coating solution, the combined mass of polylactic acid and chitosan accounts for 8% of the combined mass of polylactic acid, chitosan, and ethyl acetate. The coating process using the fluidized bed coating method is as follows: The adsorbent-loaded intermediate is placed in the fluidized bed equipment hopper. The inlet is closed and the equipment's airtightness is checked. The hot air system is turned on to preheat the fluidized bed, stabilizing the temperature of the adsorbent-loaded intermediate at 60℃. The fluidizing air velocity is adjusted to 1.2 m / s, ensuring the adsorbent-loaded intermediate is in a suspended, dispersed, and non-clumping fluidized state under the airflow. The coating liquid is loaded into the supply device and delivered to the atomizing nozzle at a constant rate of 30 mL / min via a peristaltic pump. The spraying pressure is adjusted to 0.3 MPa, atomizing the coating liquid into fine droplets and uniformly spraying it onto the fluidized adsorbent-loaded intermediate. The droplets rapidly evaporate and solidify under the action of hot air, forming a continuous and uniform coating layer on the surface of the fluidized adsorbent-loaded intermediate. This process is repeated twice. After spraying, the fluidized state is maintained for another 12 minutes to ensure the particles are completely dry and do not stick together. The hot air system is then stopped, and the material is discharged and collected, yielding modified agent particles with complete coating and stable slow-release properties. The mass ratio of the coating solution to the adsorption-supported intermediate is 1:10. Step 4: Add hydrophobic modifier, dispersant and toughening agent to the modifier particles, stir and mix for 40 minutes, dry at 45°C for 5 hours, pulverize and sieve through an 80-mesh screen to obtain long-acting salt-storing slow-release hydraulic asphalt anti-crystallizing modifier. The mass ratio of hydrophobic modifier, dispersant, toughening agent and modifier particles is 5:3:2:100; The hydrophobic modifier is methyltriethoxysilane, the dispersant is polyethylene glycol 4000, and the toughening agent is nano-silica.

[0035] The frost-resistant, crack-resistant, low-freezing-point hydraulic asphalt material is composed of the following components by weight: 75 parts of base hydraulic asphalt, 23 parts of long-lasting salt-storing and slow-release hydraulic asphalt anti-crystallizing modifier, and 2 parts of anti-aging agent. The anti-aging agent consists of 1 part antioxidant 1010 and 1 part ultraviolet absorber UV-531.

[0036] The preparation method of freeze-thaw resistant, crack-resistant, low-freezing-point hydraulic asphalt material includes the following steps: Step 1: Weigh the following raw materials by weight: 75 parts of base hydraulic asphalt, 23 parts of long-acting salt-storing slow-release hydraulic asphalt anti-coagulant modifier, and 2 parts of anti-aging agent. The anti-aging agent consists of 1 part antioxidant 1010 and 1 part ultraviolet absorber UV-531; Step 2: Heat the base hydraulic asphalt at 150°C for 15 minutes to melt it, then add the anti-aging agent and stir for 15 minutes to obtain a mixture. Add the long-acting salt-storing slow-release hydraulic asphalt anti-crack modifier after preheating at 80°C to the mixture, and stir at 800 r / min for 45 minutes until it is evenly dispersed to obtain a freeze-thaw resistant, crack-resistant, low-freezing-point hydraulic asphalt material.

[0037] Example 6 The preparation method of the long-acting salt-storing slow-release hydraulic asphalt anti-coagulant modifier of the present invention comprises the following steps: Step 1: Prepare composite active powder and porous adsorption carrier; The process of preparing composite active powder is as follows: calcium formate and magnesium formate in a mass ratio of 1:1 are added to deionized water and stirred at 45°C for 3 hours until completely dissolved to obtain a mixed solution. The mixed solution is filtered, and the filtrate is concentrated by vacuum distillation to a solid content of 40%. The concentrated solid is dried, pulverized and passed through an 80-mesh sieve to obtain composite active powder. In the mixed solution, the sum of the masses of calcium formate and magnesium formate accounts for 20% of the sum of the masses of calcium formate, magnesium formate, and deionized water. The pressure of vacuum distillation is -0.09 MPa, the temperature of vacuum distillation is 60℃, and the time of vacuum distillation is 2 hours. The process of preparing the porous adsorption carrier is as follows: diatomaceous earth and bentonite in a mass ratio of 1:1 are added to water, ultrasonically dispersed at a power of 250W for 25 minutes, and then dried at 90℃ for 18 hours. After drying, the mixture is ground through a 100-mesh sieve to obtain the porous adsorption carrier. Step 2: Add the composite active powder and porous adsorption carrier to anhydrous ethanol, stir and mix, then reflux the mixture, filter and dry to obtain the adsorption-supported intermediate. The amount of composite active powder added is 35 parts, the amount of porous adsorption carrier added is 20 parts, and the total mass ratio of composite active powder and porous adsorption carrier to anhydrous ethanol is 1:2. The stirring rate was 400 r / min, the stirring time was 45 min, the reflux reaction temperature was 70℃, the reflux reaction time was 3 h, the drying temperature was 55℃, and the drying time was 10 h. Step 3: Prepare coating solution. Mix the coating solution with the adsorption-supported intermediate and then perform coating treatment using a fluidized bed coating method to obtain modifier particles. The coating solution is prepared by dissolving polylactic acid and chitosan in ethyl acetate at a mass ratio of 2:1 to obtain the coating solution. In the coating solution, the combined mass of polylactic acid and chitosan accounts for 8% of the combined mass of polylactic acid, chitosan, and ethyl acetate. The coating process using the fluidized bed coating method is as follows: The adsorbent-loaded intermediate is placed in the fluidized bed equipment hopper. The feed inlet is closed, and the equipment's airtightness is checked. The hot air system is turned on to preheat the fluidized bed, stabilizing the temperature of the adsorbent-loaded intermediate at 50℃. The fluidizing air velocity is adjusted to 1.2 m / s, ensuring the adsorbent-loaded intermediate is in a suspended, dispersed, and non-clumping fluidized state under the airflow. The coating liquid is loaded into the supply device and delivered to the atomizing nozzle at a constant rate of 20 mL / min via a peristaltic pump. The spraying pressure is adjusted to 0.2 MPa, atomizing the coating liquid into fine droplets and uniformly spraying it onto the fluidized adsorbent-loaded intermediate. The droplets rapidly evaporate and solidify under the action of hot air, forming a continuous and uniform coating layer on the surface of the fluidized adsorbent-loaded intermediate. This process is repeated twice. After spraying, the fluidized state is maintained for another 12 minutes to ensure the particles are completely dry and do not stick together. The hot air system is then stopped, and the material is discharged and collected, yielding modified agent particles with complete coating and stable slow-release properties. The mass ratio of the coating solution to the adsorption-supported intermediate is 1:10. Step 4: Add hydrophobic modifier, dispersant and toughening agent to the modifier particles, stir and mix for 25 minutes, dry at 45℃ for 5 hours, pulverize and sieve through an 80-mesh screen to obtain long-acting salt-storing slow-release hydraulic asphalt anti-crystallizing modifier. The mass ratio of hydrophobic modifier, dispersant, toughening agent and modifier particles is 6:3:2:100; The hydrophobic modifier is methyltriethoxysilane, the dispersant is polyethylene glycol 4000, and the toughening agent is nano-silica.

[0038] The frost-resistant, crack-resistant, low-freezing-point hydraulic asphalt material is composed of the following components by weight: 83 parts of base hydraulic asphalt, 15 parts of long-lasting salt-storing and slow-release hydraulic asphalt anti-crystallizing modifier, and 2 parts of anti-aging agent. The anti-aging agent consists of 1 part antioxidant 1010 and 1 part ultraviolet absorber UV-531.

[0039] The preparation method of freeze-thaw resistant, crack-resistant, low-freezing-point hydraulic asphalt material includes the following steps: Step 1: Weigh the following raw materials by weight: 75 parts of base hydraulic asphalt, 23 parts of long-acting salt-storing slow-release hydraulic asphalt anti-coagulant modifier, and 2 parts of anti-aging agent. The anti-aging agent consists of 1 part antioxidant 1010 and 1 part ultraviolet absorber UV-531; Step 2: Heat the base hydraulic asphalt at 150℃ for 17 minutes to melt it, then add the anti-aging agent and stir for 10 minutes to obtain a mixture. Add the long-acting salt-storing slow-release hydraulic asphalt anti-crack modifier after preheating at 70℃ to the mixture, and stir at 600 r / min for 45 minutes until it is evenly dispersed to obtain a freeze-thaw resistant, crack-resistant, low-freezing-point hydraulic asphalt material.

[0040] Comparative Example 1 The preparation methods for the comparative modifier are as follows: Step 1: Weigh the following raw materials according to the following weight proportions: 18 parts calcium formate, 17 parts magnesium formate, 8 parts polylactic acid, and 4 parts chitosan; Step 2: Prepare the composite powder of calcium formate and magnesium formate according to the preparation method of composite active powder in Example 1; Step 3: Prepare the coating solution according to the preparation method of the coating solution in Example 1; Step 4, Coating Treatment: The calcium formate and magnesium formate composite powder obtained in Step 2 is fed into the fluidized bed equipment hopper. The feed inlet is closed, and the equipment's airtightness is checked. The hot air system is turned on to preheat the fluidized bed and stabilize the powder temperature at 50℃. The fluidizing air velocity is adjusted to 1.2 m / s to ensure the calcium formate and magnesium formate composite powder is in a suspended, dispersed, and non-agglomerated fluidized state. The coating liquid is loaded into the supply device and delivered to the atomizing nozzle at a constant rate of 20 mL / min via a peristaltic pump. The spraying pressure is adjusted to 0.2 MPa, and the spraying is repeated twice. After spraying, the fluidized state is maintained for 12 minutes to ensure the powder is completely dry and free of adhesion. After stopping the hot air system, the material is discharged and collected to obtain carrier-free coated modifier particles. In the coating process, the mass ratio of the composite powder of calcium formate and magnesium formate to the coating solution is 7:1. Step 5: Add 5 parts hydrophobic modifier, 3 parts dispersant, and 2 parts toughening agent to 100 parts modifier particles, stir and mix for 25 minutes, dry at 45°C for 5 hours, pulverize and sieve through an 80-mesh sieve to obtain the comparative modifier.

[0041] The preparation methods of hydraulic asphalt are compared as follows: The difference from Example 1 is that the long-acting salt-storing slow-release hydraulic asphalt anti-crystallizing modifier is replaced with the comparative modifier, while the rest is exactly the same as in Example 1, and comparative asphalt is prepared.

[0042] Comparative Example 2 The preparation methods for the comparative modifier are as follows: Step 1, prepare the materials according to the following mass proportions: 18 parts calcium formate, 17 parts magnesium formate, 10 parts diatomaceous earth, and 10 parts bentonite. Step 2: Prepare the composite powder of calcium formate and magnesium formate according to the preparation method of composite active powder in Example 1; A composite porous support was prepared according to the method for preparing porous adsorption supports in Example 1; Step 3, adsorption loading: 35 parts of the composite powder of calcium formate and magnesium formate and 20 parts of the composite porous carrier were added to anhydrous ethanol and mixed. After stirring and mixing, the mixture was refluxed and then filtered and dried to obtain the comparative adsorption loading intermediate. The stirring rate was 400 r / min, the stirring time was 45 min, the reflux reaction temperature was 70℃, the reflux reaction time was 3 h, the drying temperature was 55℃, and the drying time was 10 h. Step 4, Modification treatment: Add 5 parts of hydrophobic modifier, 3 parts of dispersant, and 2 parts of toughening agent to 100 parts of comparative adsorption-supported intermediate. After stirring and mixing for 25 minutes, dry at 45°C for 5 hours and pulverize through an 80-mesh sieve to obtain the comparative modifier.

[0043] The preparation methods of hydraulic asphalt are compared as follows: The difference from Example 1 is that the long-acting salt-storing slow-release hydraulic asphalt anti-crystallizing modifier is replaced with the comparative modifier, while the rest is exactly the same as in Example 1, and comparative asphalt is prepared.

[0044] The performance tests of the hydraulic asphalt materials prepared in Examples 1-3 and Comparative Examples 1-2 are shown in Table 1. Table 1

[0045] As can be seen from Table 1, the long-acting salt-storing slow-release hydraulic asphalt anti-coagulation modifier and the freeze-thaw-resistant and crack-resistant low-freezing-point hydraulic asphalt material prepared by the method of the present invention are far superior to the comparative example in terms of freezing point reduction, inhibition of volatilization loss, and freeze-thaw resistance and crack resistance durability. Therefore, the freeze-thaw-resistant and crack-resistant low-freezing-point hydraulic asphalt material prepared by the present invention has better overall performance.

Claims

1. A method for preparing a long-acting, salt-storing, slow-release hydraulic asphalt anti-coagulant modifier, characterized in that, The steps are as follows: Step 1: Prepare composite active powder and porous adsorption carrier; Step 2: Add the composite active powder and porous adsorption carrier to anhydrous ethanol, stir and mix, then reflux the mixture, filter and dry to obtain the adsorption-supported intermediate. Step 3: Prepare coating solution. Mix the coating solution with the adsorption-supported intermediate and then perform coating treatment using a fluidized bed coating method to obtain modifier particles. Step 4: Add hydrophobic modifier, dispersant and toughening agent to the modifier particles, stir and mix, then dry, pulverize and sieve to obtain long-acting salt-storing slow-release hydraulic asphalt anti-crystallizing modifier.

2. The preparation method of the long-acting salt-storing slow-release hydraulic asphalt anti-coagulant modifier according to claim 1, characterized in that, In step 1, the process of preparing the composite active powder is as follows: calcium formate and magnesium formate with a mass ratio of 0.83~1.2:1 are added to deionized water and stirred at 40℃~60℃ for 1.5h~3h until completely dissolved to obtain a mixed solution. The obtained mixed solution is filtered, and the filtrate is concentrated by vacuum distillation to a solid content of 40%~50%. The concentrated solid is dried, pulverized and sieved to obtain the composite active powder. In the mixed solution, the sum of the masses of calcium formate and magnesium formate accounts for 15% to 25% of the sum of the masses of calcium formate, magnesium formate, and deionized water. The pressure of vacuum distillation is -0.08MPa to -0.1MPa, the temperature is 50℃ to 70℃, and the time is 1h to 3h.

3. The preparation method of the long-acting salt-storing slow-release hydraulic asphalt anti-coagulant modifier according to claim 1, characterized in that, In step 1, the process of preparing the porous adsorption carrier is as follows: diatomaceous earth and bentonite in a mass ratio of 1~3:1 are added to water and ultrasonically dispersed at a power of 200W~300W for 20min~30min, then dried at a temperature of 80℃~100℃ for 12h~24h, and after drying, they are ground and sieved to obtain the porous adsorption carrier.

4. The preparation method of the long-acting salt-storing slow-release hydraulic asphalt anti-coagulant modifier according to claim 1, characterized in that, In step 2, the amount of composite active powder added is 30 to 50 parts, the amount of porous adsorption carrier added is 15 to 30 parts, and the total mass ratio of composite active powder and porous adsorption carrier to anhydrous ethanol is 1:2 to 3. The stirring rate is 300 r / min to 500 r / min, the stirring time is 30 min to 60 min, the reflux reaction temperature is 60℃ to 80℃, the reflux reaction time is 2 h to 4 h, the drying temperature is 50℃ to 60℃, and the drying time is 8 h to 12 h.

5. The preparation method of the long-acting salt-storing slow-release hydraulic asphalt anti-coagulant modifier according to claim 1, characterized in that, In step 3, the coating solution is prepared by dissolving polylactic acid and chitosan in ethyl acetate at a mass ratio of 0.5 to 2:1 to obtain the coating solution. In the coating solution, the total mass of polylactic acid and chitosan accounts for 5% to 10% of the total mass of polylactic acid, chitosan and ethyl acetate.

6. The preparation method of the long-acting salt-storing slow-release hydraulic asphalt anti-coagulant modifier according to claim 1, characterized in that, In step 3, the coating process using the fluidized bed coating method is as follows: The adsorbent-loaded intermediate is placed in the fluidized bed equipment hopper. The feed inlet is closed, and the equipment's airtightness is checked. The hot air system is turned on to preheat the fluidized bed, stabilizing the temperature of the adsorbent-loaded intermediate at 40℃~60℃. The fluidizing air velocity is adjusted to 0.8m / s~1.6m / s, ensuring the adsorbent-loaded intermediate is in a suspended, dispersed, and non-agglomerated fluidized state under the action of the airflow. The coating solution is then loaded into the supply device and pumped at a rate of 10mL / min using a peristaltic pump. A constant rate of ~30 mL / min is used to deliver the coating liquid to the atomizing nozzle. The spraying pressure is adjusted to between 0.15 and 0.3 MPa to atomize the coating liquid into fine droplets and spray them evenly onto the fluidized adsorbent-supported intermediate. The droplets evaporate and solidify rapidly under the action of hot air, forming a continuous and uniform coating layer on the surface of the fluidized adsorbent-supported intermediate. The spraying is repeated 2 to 3 times. After the spraying is completed, the fluidized state is maintained and the product is dried for 10 to 15 minutes. The hot air system is then stopped, the material is discharged and collected to obtain the modifier particles. The mass ratio of the coating solution to the adsorption-supported medium is 1:5~10.

7. The preparation method of the long-acting salt-storing slow-release hydraulic asphalt anti-coagulant modifier according to claim 1, characterized in that, In step 4, the mass ratio of hydrophobic modifier, dispersant, toughening agent to modifier particles is 2~8:1~5:1~3:100; The drying temperature is 40℃~50℃, and the drying time is 4h~6h.

8. A freeze-thaw resistant, crack-resistant, low-freezing-point hydraulic asphalt material, characterized in that, The long-acting salt-storing slow-release hydraulic asphalt anti-coagulant modifier according to any one of claims 1 to 8 is composed of the following components by weight fraction: 70 to 85 parts of base hydraulic asphalt, 15 to 30 parts of long-acting salt-storing slow-release hydraulic asphalt anti-coagulant modifier, and 0.5 to 2 parts of anti-aging agent. The anti-aging agent consists of antioxidant 1010 and ultraviolet absorber UV-531 in a mass ratio of 1:

1.

9. A method for preparing frost-resistant, crack-resistant, low-freezing-point hydraulic asphalt material, characterized in that, The steps are as follows: Step 1: Weigh the following raw materials by weight: 70-85 parts of base hydraulic asphalt, 15-30 parts of long-acting salt-storing slow-release hydraulic asphalt anti-coagulant modifier, and 0.5-2 parts of anti-aging agent. The anti-aging agent is composed of antioxidant 1010 and ultraviolet absorber UV-531 in a mass ratio of 1:

1. The anti-aging agent can be obtained by stirring and mixing antioxidant 1010 and ultraviolet absorber UV-531 evenly at room temperature. Step 2: Heat and melt the base hydraulic asphalt, then add the anti-aging agent and stir to obtain a mixture. Add the long-acting salt-storing slow-release hydraulic asphalt anti-crystallization modifier after preheating to the mixture and stir until it is evenly dispersed to obtain a freeze-thaw resistant, crack-resistant, low-freezing-point hydraulic asphalt material.

10. The method for preparing the frost-resistant, crack-resistant, low-freezing-point hydraulic asphalt material according to claim 9, characterized in that, The heating and melting temperature is 130℃~150℃, the heating and melting time is 15min~20min, the preheating temperature is 60℃~80℃, and the stirring speed is 500 r / min~800 r / min.