An ethyl cellulose-based intelligent active packaging film based on synergistic effect of polyethylene glycol and titanium dioxide hybrid nanocrystals, and a preparation method and application thereof

By leveraging the synergistic effect of ethyl cellulose, polyethylene glycol, and titanium dioxide hybrid nanocrystals, an ethyl cellulose-based smart active packaging film was prepared. This solved the problems of single-function packaging materials, slow response, and easy oxidation and deactivation of the ferrous system, achieving high biocompatibility, rapid ammonia-sensitive response, and long-term stability, making it suitable for the food preservation field.

CN123152178APending Publication Date: 2026-11-24GUILIN UNIVERSITY OF TECHNOLOGY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611411754.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-11
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing packaging materials suffer from limited functionality, slow response, degraded processing performance, and easy oxidation and deactivation of ferrous systems. They also lack biocompatibility, high sensitivity and fast response, and structural stability, which restricts the application of smart packaging materials.

Method used

By utilizing the synergistic effect of hybrid nanocrystals of ethyl cellulose, polyethylene glycol, and titanium dioxide, organic-inorganic hybrid modified nanoparticles are formed in situ on the surface of titanium dioxide nanocrystals to prepare ethyl cellulose-based smart active packaging films. The synergistic effect of polyethylene glycol and titanium dioxide hybrid nanocrystals enhances the biosafety, rapid ammonia-sensitive response characteristics, and long-term stability of the materials.

Benefits of technology

It achieves high biocompatibility, sensitive and rapid ammonia sensitivity response, excellent processing performance and long-term storage stability, and possesses outstanding mechanical strength, ultraviolet shielding and broad-spectrum antibacterial properties, enabling timely and effective monitoring of changes in food freshness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123152178A_ABST
    Figure CN123152178A_ABST
Patent Text Reader

Abstract

This invention discloses an ethyl cellulose-based smart active packaging film based on the synergistic effect of polyethylene glycol and titanium dioxide hybrid nanocrystals, its preparation method, and its applications, belonging to the field of food packaging materials technology. This material utilizes the synergistic effect of polyethylene glycol and titanium dioxide hybrid nanocrystals, exhibiting good biocompatibility, highly sensitive and rapid ammonia-sensitive response characteristics, excellent processing performance, and superior long-term storage stability and service reliability. The packaging film also possesses outstanding mechanical strength, UV shielding, and broad-spectrum antibacterial properties, while maintaining high visible light transmittance. It can serve as a smart colorimetric indicator material, enabling timely and effective visual monitoring of freshness changes in meat products such as shrimp, pork, and fish during storage, and has broad application prospects in the field of smart active food packaging.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of food packaging materials technology, and in particular to an ethyl cellulose-based smart active packaging film based on the synergistic effect of polyethylene glycol and titanium dioxide hybrid nanocrystals, its preparation method and application. Background Technology

[0002] Animal-derived foods (including meat and seafood) are rich in protein, making them highly susceptible to spoilage due to bacterial contamination. This process typically produces alkaline compounds such as volatile ammonia. Therefore, developing smart active packaging materials that combine antibacterial properties with colorimetric ammonia sensitivity is crucial for maintaining food freshness and monitoring spoilage in real time.

[0003] Due to their high stability, ultraviolet absorption, antibacterial properties, and biocompatibility, titanium dioxide nanoparticles are often used as functional fillers in bio-based polymer (such as ethyl cellulose and starch) membrane materials to develop active packaging materials, showing broad application prospects in pharmaceutical and food packaging materials. However, titanium dioxide nanoparticles lack ammonia-sensitive color-changing functionality, which hinders their application in ammonia-sensitive intelligent active packaging materials. In recent years, organometallic complex materials have attracted widespread attention due to their tunable structure and function. Among them, various metal-based complexes such as cobalt, nickel, manganese, and ferrous metals have shown great potential in developing functional materials with antibacterial and ammonia-sensitive color-changing properties. Therefore, modifying the surface of titanium dioxide nanoparticles with organometallic complexes holds promise for developing multifunctional composite nanofillers with both antibacterial and ammonia-sensitive color-changing functions, thus overcoming the performance limitations of single materials.

[0004] Organometallic complex-based ammonia-sensitive smart active packaging materials often face problems such as slow response speed and limited ammonia sensitivity. Furthermore, during film preparation and molding, organometallic complex powders are prone to agglomeration, structural collapse, and coordination bond breakage, directly leading to a significant decrease in the material's ammonia-sensitive sensing performance and a degradation in colorimetric effects. Crucially, among various organometallic complex systems, ferrous complexes exhibit lower biotoxicity and superior biosafety compared to cobalt, nickel, and manganese complexes, making them more suitable for food packaging applications. However, this system often suffers from a core defect of poor intrinsic stability: ferrous ions are highly susceptible to oxidative deactivation by oxidizing media such as oxygen in the environment, leading to complex structural damage and loss of sensing and antibacterial functions. This severely reduces the long-term storage stability and service reliability of smart packaging materials, becoming a key technical challenge restricting the commercialization of ferrous-based ammonia-sensitive materials.

[0005] In summary, the industry currently lacks an integrated intelligent packaging modification system that can simultaneously ensure biosafety, high sensitivity and rapid response to ammonia sensitivity, and excellent processability and structural stability.

[0006] In view of this, the present invention is proposed. Summary of the Invention

[0007] The purpose of this invention is to provide an ethyl cellulose-based smart active packaging film based on the synergistic effect of polyethylene glycol and titanium dioxide hybrid nanocrystals, its preparation method and application, in order to solve the technical problems of traditional packaging materials such as single function, slow response, degradation of processing performance and easy oxidation and deactivation of ferrous system.

[0008] To achieve the above objectives, the present invention provides the following solution: This invention provides an ethyl cellulose-based smart active packaging film, comprising the following raw materials: ethyl cellulose, polyethylene glycol, and titanium dioxide hybrid nanocrystals; The mass ratio of the ethyl cellulose, polyethylene glycol and titanium dioxide hybrid nanocrystals is 80:20:0.5-2; The titanium dioxide hybrid nanocrystals are organic-inorganic hybrid modified nanoparticles formed by in-situ coordination of arbutin and ferrous salt on the surface of titanium dioxide nanocrystals.

[0009] Furthermore, the preparation method of the titanium dioxide hybrid nanocrystals includes the following steps: (1) Titanium dioxide nanocrystals and arbutin are mixed in solution to obtain a blend; (2) Add ferrous salt to the blended liquid. After the reaction is completed, separate, wash and dry to obtain the titanium dioxide hybrid nanocrystals.

[0010] Furthermore, the ferrous salt is ferrous sulfate.

[0011] This invention also provides a method for preparing the above-mentioned ethyl cellulose-based smart active packaging film, comprising the following steps: (1) Titanium dioxide nanocrystals and arbutin are mixed in solution to obtain a blend; (2) Add ferrous salt to the blended liquid. After the reaction is completed, separate, wash and dry to obtain the titanium dioxide hybrid nanocrystals. (3) Ethyl cellulose, polyethylene glycol and titanium dioxide hybrid nanocrystals are mixed in an organic solvent to obtain a film-forming solution; (4) The film-forming liquid is subjected to film-forming treatment and dried to obtain the ethyl cellulose-based smart active packaging film.

[0012] Furthermore, the mixing temperature in step (3) is 25-70℃.

[0013] Furthermore, the ferrous salt is ferrous sulfate.

[0014] This invention also provides the application of the above-mentioned ethyl cellulose-based smart active packaging film in the field of food preservation.

[0015] Furthermore, the food is an animal-derived food.

[0016] The present invention discloses the following technical effects: This invention provides an ethyl cellulose-based smart active packaging film material. This material, through the synergistic effect of polyethylene glycol and titanium dioxide hybrid nanocrystals, possesses excellent biocompatibility, highly sensitive and rapid ammonia-sensitive response characteristics, superior processing performance, and excellent long-term storage stability and service reliability. Simultaneously, the packaging film exhibits outstanding mechanical strength, UV shielding, and broad-spectrum antibacterial properties, while maintaining high visible light transmittance. It can be used as a smart colorimetric indicator material to achieve timely and effective visual monitoring of freshness changes in meat products such as shrimp, pork, and fish during storage, and has broad application prospects in the field of smart active food packaging. Attached Figure Description

[0017] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0018] Figure 1 This is a scanning electron microscope image of the titanium dioxide hybrid nanocrystals of the present invention; Figure 2 This is a scanning electron microscope (SEM) image of the cross-sectional morphology of the membrane material prepared in Example 3 of the present invention; Figure 3 Fourier transform infrared spectra of titanium dioxide nanocrystals, iron-arbutin complexes, and titanium dioxide hybrid nanocrystals of the present invention. Figure 4 These are comparative images of the discoloration of the titanium dioxide hybrid nanocrystals of the present invention after ammonia fumigation. Figure 5 The graphs show the color difference ΔE over time of the membrane materials in Examples 1-3 and Comparative Examples 1 and 2 during the ammonia response process of this invention. Figure 6 The image shows a comparison of the color difference stability of the film materials of Examples 1-3 and Comparative Example 1 after storage at 25°C and 57% relative humidity for 45 days. Figure 7 This is a bar chart comparing the tensile strength of the membrane materials in Examples 1-3 and Comparative Examples 1, 3, and 4 of the present invention. Figure 8 The bar chart shows the comparison of the elongation at break of the membrane materials in Examples 1-3 and Comparative Examples 1, 3, and 4 of this invention. Detailed Implementation

[0019] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as a limitation of the present invention, but rather as a more detailed description of certain aspects, features, and embodiments of the present invention.

[0020] It should be understood that the terminology used in this invention is merely for describing particular embodiments and is not intended to limit the invention. Furthermore, with respect to numerical ranges in this invention, it should be understood that each intermediate value between the upper and lower limits of the range is also specifically disclosed. Any stated value or intermediate value within a stated range, as well as each smaller range between any other stated value or intermediate value within said range, is also included in this invention. The upper and lower limits of these smaller ranges may be independently included or excluded from the range.

[0021] Unless otherwise stated, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art. While only preferred methods and materials have been described herein, any methods and materials similar or equivalent to those described herein may be used in the implementation or testing of this invention. All references to this specification are incorporated by way of citation to disclose and describe methods and / or materials associated with those references. In the event of any conflict with any incorporated reference, the content of this specification shall prevail.

[0022] Various modifications and variations can be made to the specific embodiments described in this specification without departing from the scope or spirit of the invention, as will be apparent to those skilled in the art. Other embodiments derived from this specification will also be readily apparent to those skilled in the art. This specification and embodiments are merely exemplary.

[0023] The terms “include,” “including,” “have,” “contain,” etc., used in this article are all open-ended terms, meaning that they include but are not limited to.

[0024] It should be noted that any aspects not described in detail in this invention are conventional practices in the field and are not the focus of this invention.

[0025] Unless otherwise specified, "room temperature" in this invention refers to 20±10℃.

[0026] This invention provides an ethyl cellulose-based smart active packaging film material based on the synergistic effect of polyethylene glycol and titanium dioxide hybrid nanocrystals, comprising the following raw materials: ethyl cellulose, polyethylene glycol and titanium dioxide hybrid nanocrystals; The mass ratio of ethyl cellulose, polyethylene glycol and titanium dioxide hybrid nanocrystals is 80:20:0.5-2.

[0027] The titanium dioxide hybrid nanocrystals are organic-inorganic hybrid modified nanoparticles formed by in-situ coordination of arbutin and ferrous salt on the surface of titanium dioxide nanocrystals.

[0028] The preferred preparation method includes the following steps: (1) Disperse 0.3 g of titanium dioxide nanocrystals in 40 mL of ethanol and stir at 25 °C for 30 min to obtain a uniform dispersion of titanium dioxide nanocrystals for later use. (2) Take 0.1362 g of arbutin and dissolve it in 30 mL of ethanol to obtain a homogeneous arbutin solution for later use. (3) Add the arbutin solution obtained in step (2) to the titanium dioxide nanocrystal dispersion obtained in step (1), stir at 25°C for 2 hours to obtain a uniform blend for later use. (4) Take 0.278 g of ferrous sulfate heptahydrate, dissolve it in 10 mL of deionized water to obtain a homogeneous ferrous sulfate solution for later use; (5) Add the ferrous sulfate solution obtained in step (4) to the blend obtained in step (3), stir and react at 25°C for 5 min, and then centrifuge, wash with ethanol and vacuum dry to obtain titanium dioxide hybrid nanocrystals. (6) Add 0.8 g of ethyl cellulose and 0.2 g of polyethylene glycol to 25 mL of ethanol, stir at 55 °C for 60 min to obtain a homogeneous blend solution for later use; (7) Disperse 0.005-0.02 g of titanium dioxide hybrid nanocrystals in 10 mL of ethanol and stir at room temperature for 60 min to obtain a uniform dispersion for later use; (8) Add the dispersion obtained in step (7) to the blend solution obtained in step (6), stir at 55°C for 60 min to obtain a uniform film-forming solution for later use; (9) Pour the film-forming liquid obtained in step (8) into a flat-bottomed plexiglass dish and dry it in an oven at 55°C for 24 hours to obtain an ethyl cellulose-based smart active packaging film material based on the synergistic effect of polyethylene glycol and titanium dioxide hybrid nanocrystals.

[0029] The following is a detailed explanation with reference to the embodiments: Unless otherwise specified, in the following embodiments and comparative examples of the present invention, "parts" refers to "parts by mass".

[0030] The reagents and specifications used in the following embodiments and comparative examples of this invention are as follows: Ethyl cellulose was a product purchased from Shanghai Yuanye Biotechnology Co., Ltd. (its number average molecular weight is 1.6 × 10⁻⁶). 5g / mol, with an ethoxy content of 48%; polyethylene glycol was purchased from Aladdin Reagent Co., Ltd. (its number average molecular weight is 20000 g / mol); titanium dioxide nanocrystals were Jin Hong hydrophilic high-purity reagent produced by Ron Reagent Co., Ltd., with a particle size of 40 nm; arbutin was purchased from Ron Reagent Co., Ltd. (CAS No.: 497-76-7); ferrous sulfate heptahydrate and ethanol were analytical grade reagents provided by Xilong Scientific Co., Ltd.; in addition, the plexiglass dishes used in the following examples and comparative examples of the present invention are square flat-bottomed plexiglass dishes with a specification of 10cm×10cm (dish height is 1.5 cm).

[0031] The titanium dioxide hybrid nanocrystals used in the following embodiments and comparative examples of the present invention were prepared through the following steps: (1) Disperse 0.3 g of titanium dioxide nanocrystals in 40 mL of ethanol and stir at 25 °C for 30 min to obtain a uniform dispersion of titanium dioxide nanocrystals for later use. (2) Take 0.1362 g of arbutin and dissolve it in 30 mL of ethanol to obtain a homogeneous arbutin solution for later use. (3) Add the arbutin solution obtained in step (2) to the titanium dioxide nanocrystal dispersion obtained in step (1), stir at 25°C for 2 hours to obtain a uniform blend for later use. (4) Take 0.278 g of ferrous sulfate heptahydrate, dissolve it in 10 mL of deionized water to obtain a homogeneous ferrous sulfate solution for later use; (5) Add the ferrous sulfate solution obtained in step (4) to the blend obtained in step (3), stir and react at 25°C for 5 min, and then centrifuge, wash with ethanol and vacuum dry to obtain titanium dioxide hybrid nanocrystals.

[0032] Example 1 This embodiment provides an ethyl cellulose-based smart active packaging film material based on the synergistic effect of polyethylene glycol and titanium dioxide hybrid nanocrystals, comprising the following raw materials: ethyl cellulose, polyethylene glycol, and titanium dioxide hybrid nanocrystals, wherein the mass ratio of ethyl cellulose, polyethylene glycol, and titanium dioxide hybrid nanocrystals is 80:20:0.5.

[0033] The preparation method of the packaging film material in this embodiment is as follows: (1) Add 0.8 g of ethyl cellulose and 0.2 g of polyethylene glycol to 25 mL of ethanol and stir at 55 °C for 60 min to obtain a homogeneous blend solution for later use; (2) Disperse 0.005 g of titanium dioxide hybrid nanocrystals in 10 mL of ethanol and stir at room temperature for 60 min to obtain a uniform dispersion for later use. (3) Add the dispersion obtained in step (2) to the blend solution obtained in step (1), stir at 55°C for 60 min to prepare a uniform film-forming solution for later use. (4) Pour the film-forming liquid obtained in step (3) into a square flat-bottomed organic glass dish with a specification of 10cm×10cm, and dry it in an oven at 55℃ for 24h to obtain an ethyl cellulose-based smart active packaging film material based on the synergistic effect of polyethylene glycol and titanium dioxide hybrid nanocrystals.

[0034] Example 2 This embodiment provides an ethyl cellulose-based smart active packaging film material based on the synergistic effect of polyethylene glycol and titanium dioxide hybrid nanocrystals, comprising the following raw materials: ethyl cellulose, polyethylene glycol, and titanium dioxide hybrid nanocrystals, wherein the mass ratio of ethyl cellulose, polyethylene glycol, and titanium dioxide hybrid nanocrystals is 80:20:1.

[0035] The preparation method of the packaging film material in this embodiment is as follows: (1) Add 0.8 g of ethyl cellulose and 0.2 g of polyethylene glycol to 25 mL of ethanol and stir at 55 °C for 60 min to obtain a homogeneous blend solution for later use; (2) Disperse 0.01 g of titanium dioxide hybrid nanocrystals in 10 mL of ethanol and stir at room temperature for 60 min to obtain a uniform dispersion for later use. (3) Add the dispersion obtained in step (2) to the blend solution obtained in step (1), stir at 55°C for 60 min to prepare a uniform film-forming solution for later use. (4) Pour the film-forming liquid obtained in step (3) into a square flat-bottomed organic glass dish with a specification of 10cm×10cm, and dry it in an oven at 55℃ for 24h to obtain an ethyl cellulose-based smart active packaging film material based on the synergistic effect of polyethylene glycol and titanium dioxide hybrid nanocrystals.

[0036] Example 3 This embodiment provides an ethyl cellulose-based smart active packaging film material based on the synergistic effect of polyethylene glycol and titanium dioxide hybrid nanocrystals, comprising the following raw materials: ethyl cellulose, polyethylene glycol, and titanium dioxide hybrid nanocrystals, wherein the mass ratio of ethyl cellulose, polyethylene glycol, and titanium dioxide hybrid nanocrystals is 80:20:2.

[0037] The preparation method of the packaging film material in this embodiment is as follows: (1) Add 0.8 g of ethyl cellulose and 0.2 g of polyethylene glycol to 25 mL of ethanol and stir at 55 °C for 60 min to obtain a homogeneous blend solution for later use; (2) Disperse 0.02 g of titanium dioxide hybrid nanocrystals in 10 mL of ethanol and stir at room temperature for 60 min to obtain a uniform dispersion for later use. (3) Add the dispersion obtained in step (2) to the blend solution obtained in step (1), stir at 55°C for 60 min to prepare a uniform film-forming solution for later use. (4) Pour the film-forming liquid obtained in step (3) into a square flat-bottomed organic glass dish with a specification of 10cm×10cm, and dry it in an oven at 55℃ for 24h to obtain an ethyl cellulose-based smart active packaging film material based on the synergistic effect of polyethylene glycol and titanium dioxide hybrid nanocrystals.

[0038] Comparative Example 1 This comparative example provides an ethyl cellulose / polyethylene glycol composite membrane material without the addition of titanium dioxide hybrid nanocrystals. The preparation steps are as follows: (1) Add 0.8 g of ethyl cellulose and 0.2 g of polyethylene glycol to 25 mL of ethanol and stir at 55 °C for 60 min to obtain a homogeneous blend solution for later use. (2) Add 10 mL of ethanol to the blended solution obtained in step (1), stir at 55 °C for 60 min to prepare a homogeneous film-forming solution for later use; (3) The film-forming liquid obtained in step (2) is poured into a square flat-bottomed organic glass dish with a specification of 10cm×10cm and placed in an oven at 55℃ for 24h to dry, thus obtaining ethyl cellulose / polyethylene glycol composite film material.

[0039] Comparative Example 2 This comparative example provides an ethyl cellulose / titanium dioxide hybrid nanocrystalline composite film material without the addition of polyethylene glycol. The preparation steps are as follows: (1) Add 0.8 g of ethyl cellulose to 25 mL of ethanol and stir at 55 °C for 60 min to obtain a homogeneous blend solution for later use; (2) Disperse 0.02 g of titanium dioxide hybrid nanocrystals in 10 mL of ethanol and stir for 60 min at room temperature to obtain a uniform dispersion for later use. (3) Add the dispersion obtained in step (2) to the blend solution obtained in step (1), stir at 55°C for 60 min to prepare a uniform film-forming solution for later use. (4) Pour the film-forming liquid obtained in step (3) into a square flat-bottomed organic glass dish with a specification of 10cm×10cm, and dry it in an oven at 55℃ for 24h to obtain the ethyl cellulose / titanium dioxide hybrid nanocrystalline composite film material.

[0040] Comparative Example 3 This comparative example provides an ethyl cellulose / polyethylene glycol / titanium dioxide composite membrane material, using unmodified titanium dioxide nanocrystals, and the preparation steps are as follows: (1) Add 0.8 g of ethyl cellulose and 0.2 g of polyethylene glycol to 25 mL of ethanol and stir at 55 °C for 60 min to obtain a homogeneous blend solution for later use. (2) Disperse 0.02 g of titanium dioxide nanocrystals in 10 mL of ethanol and stir for 60 min at room temperature to obtain a uniform dispersion for later use. (3) Add the dispersion obtained in step (2) to the blend solution obtained in step (1), stir at 55°C for 60 min to prepare a uniform film-forming solution for later use. (4) Pour the film-forming liquid obtained in step (3) into a square flat-bottomed organic glass dish with a specification of 10cm×10cm, and dry it in an oven at 55℃ for 24h to obtain the ethyl cellulose / polyethylene glycol / titanium dioxide composite film material.

[0041] Comparative Example 4 This comparative example provides an ethyl cellulose / polyethylene glycol / iron-arbutin complex composite membrane material, and the preparation steps are as follows: (1) Add 0.8 g of ethyl cellulose and 0.2 g of polyethylene glycol to 25 mL of ethanol and stir at 55 °C for 60 min to obtain a homogeneous blend solution for later use. (2) Disperse 0.02 g of iron-arbutin complex in 10 mL of ethanol and stir for 60 min at room temperature to obtain a uniform dispersion for later use. (3) Add the dispersion obtained in step (2) to the blend solution obtained in step (1), stir at 55°C for 60 min to prepare a uniform film-forming solution for later use. (4) Pour the film-forming liquid obtained in step (3) into a square flat-bottomed organic glass dish with a specification of 10cm×10cm, and dry it in an oven at 55℃ for 24h to obtain the ethyl cellulose / polyethylene glycol / iron-arbutin complex composite membrane material.

[0042] The preparation steps of the iron-arbutin complex are as follows: (1) Weigh 0.1362 g of arbutin, dissolve it in 30 mL of ethanol to prepare a homogeneous arbutin solution for later use; (2) Add the arbutin solution obtained in step (1) to 40 mL of ethanol and stir at 25 °C for 2 h to obtain a homogeneous solution for later use; (3) Weigh 0.278 g of ferrous sulfate heptahydrate, dissolve it in 10 mL of deionized water to prepare a ferrous sulfate solution for later use; (4) Add the ferrous sulfate solution obtained in step (3) to the solution obtained in step (2), stir and react at 25°C for 5 min; after the reaction is completed, centrifuge and separate, wash with ethanol, and then vacuum dry to obtain the iron-arbutin complex.

[0043] Structural and performance testing: 1. Structural characterization a. Microscopic morphological characterization: The morphology of titanium dioxide hybrid nanocrystals and film samples was characterized using scanning electron microscopy; the results are as follows: Figure 1 As shown in the figure, the prepared titanium dioxide hybrid nanocrystals are uniform small-sized particles with an average particle size of 55 nm (obtained by statistical calculation using ImageJ software).

[0044] Figure 2 This is a cross-sectional scanning electron microscope (SEM) image of the membrane material prepared in Example 3. As can be observed from the image, the composite membrane has a distinct porous structure, which facilitates the permeation and adsorption of gas molecules within the membrane.

[0045] b. Characterization of functional group structure: Fourier transform infrared spectroscopy was used to test titanium dioxide nanocrystals, iron-arbutin complex (prepared in Comparative Example 4), and titanium dioxide hybrid nanocrystals to analyze the characteristic functional groups of the samples. The microstructure of titanium dioxide hybrid nanocrystals was observed using scanning electron microscopy. Fourier transform infrared spectroscopy was used to characterize the characteristic functional groups of the titanium dioxide nanocrystals, the iron-arbutin complex, and the titanium dioxide hybrid nanocrystals. The test results are as follows: Figure 3 The iron-arbutin complex at 3333 cm⁻¹ -1 The absorption peak at 1497 cm⁻¹ is attributed to the stretching vibration of the hydroxyl group (-OH); -1 The absorption peak at 1148 cm⁻¹ corresponds to the stretching vibration of the C=C bond in the benzene ring. -1 1016cm -1 The absorption peak is due to the CO bond stretching vibration, 526 cm⁻¹. -1 The absorption peak at this point is attributed to the stretching vibration of the Fe-O bond. Compared to the iron-arbutin complex, titanium dioxide hybrid nanocrystals also exhibit a hydroxyl stretching vibration peak (3425 cm⁻¹). -1 ), the C=C stretching vibration peak of the benzene ring (1493 cm⁻¹) -1 ) and CO bond stretching vibration peak (1157 cm⁻¹) -1 1016cm -1 ); at the same time at 451cm -1 A new absorption band appears nearby, which is attributed to the stretching vibration of the Ti-O bond and is similar to that of titanium dioxide at 459 cm⁻¹. -1The characteristic peaks at the specified locations match. These results demonstrate that the iron-arbutin complex has been successfully modified onto the surface of titanium dioxide nanocrystals, indicating the successful preparation of titanium dioxide hybrid nanocrystals.

[0046] 2. Characterization of the ammonia-sensitive color-changing properties of titanium dioxide hybrid nanocrystals The titanium dioxide hybrid nanocrystal sample prepared according to this invention was fixed in a sealed container with a diameter of 10 cm and a height of 10 cm. 10 mL of 25% ammonia solution was added to the container, with the sample positioned 5 cm vertically above the ammonia solution surface. The container was sealed to create an ammonia reaction environment. After standing for 1 minute, the ammonia-sensitive color change behavior of the sample was observed, and the results are shown in Figure 4. The titanium dioxide hybrid nanocrystals were initially off-white, but upon contact with volatile ammonia gas, the color rapidly changed to bluish-green, and further to brownish-yellow within 1 minute.

[0047] 3. Membrane material performance testing The structure and performance of the membrane materials prepared in each embodiment and comparative example were tested: The UV-Vis spectral performance was tested using a Shimadzu UV-2450 UV-Vis spectrometer, and the average UV transmittance was calculated according to GB / T 18830-2009 standard. Tensile mechanical properties were tested according to GB / T 1040-2006 standard; The water vapor transmission coefficient was determined according to ASTM E 96 standard; The antibacterial properties of the material were tested in accordance with the QB / T 2591-2003 standard. The ammonia response test method is as follows: Pre-cut the membrane material into 1cm diameter samples and fix them in a sealed container with a diameter of 10cm and a height of 10cm. Add 10mL of 25% ammonia solution to the sealed container, with the sample 5cm perpendicular to the ammonia solution surface. Seal the container to create an ammonia reaction environment. Then observe and measure the color change of the composite membrane within 0~600 seconds using a colorimeter (NR200, Shenzhen Sanenshi Co., Ltd.), and calculate the color difference ΔE of the membrane material after the ammonia response. The calculation formula is as follows: ,in, , and This is the initial color value of the membrane sample. , and This is the color value of the membrane sample after exposure to ammonia (Note: , and The values ​​are the core parameters for measuring color in a colorimeter, representing lightness, red-green axis, and yellow-blue axis, respectively. The long-term color stability test method is as follows: The membrane sample (1 cm in diameter) was stored at 25℃ and 57% humidity for 45 days. The color change of the membrane sample was then observed and measured using a colorimeter (NR200, Shenzhen Sanenshi Co., Ltd.), and the color difference ΔE after storage was calculated. ,in, , and This is the initial color value of the membrane sample. , and It is the color value of the membrane sample after storage.

[0048] Shrimp Freshness Monitoring Experiment: Fresh shrimp were purchased from the market. Shrimp of uniform size and weight were selected and divided into two groups of four shrimp each, with a total weight of 30g per group. The shrimp were placed in Petri dishes and sealed with the dish lids. The bottom of the petri dish lids of the two treatment groups were respectively attached with the ethyl cellulose / polyethylene glycol composite material prepared in Comparative Example 1 and the ethyl cellulose / polyethylene glycol-based nanocomposite material prepared in Example 3 (pre-cut into sample materials with a diameter of 1 cm). The shrimp samples were then stored in an oven at 25°C. Changes in shrimp freshness and color changes of the sample materials were observed and recorded. The value of volatile basic nitrogen (TVB-N) released by the shrimp samples during storage was tested according to the method of GB 5009.288-2016.

[0049] The above structural and performance test data are shown in Tables 1 and 2. Figures 1-6 As shown.

[0050] Table 1 Sample performance test data Table 2 Results of Shrimp Freshness Monitoring Experiment In Table 2, t represents the storage time of fresh shrimp.

[0051] The ammonia response test results of Comparative Example 1, Comparative Example 2, and Examples 1-3 are as follows: Figure 5 As shown, it can be seen that: The ethyl cellulose / polyethylene glycol-based composite material prepared in Comparative Example 1 is colorless and transparent. After exposure to ammonia, the ΔE value of the membrane remained less than 1.0 throughout the entire test period, indicating almost no color change (Note: a ΔE value greater than 5 indicates a visually perceptible color change in the composite membrane). This is because neither ethyl cellulose nor polyethylene glycol possesses ammonia-sensitive color-changing properties. The ethyl cellulose / titanium dioxide hybrid nanocrystal composite membrane material prepared in Comparative Example 2 is light yellow. After exposure to ammonia, the ΔE value of the membrane remained less than 2.5 throughout the entire test period, indicating no visually perceptible color change. This suggests that the addition of titanium dioxide hybrid nanocrystals did not endow ethyl cellulose with good ammonia-sensitive color-changing properties. This may be attributed to the inherently poor stability of the ferrous complex (i.e., iron-arbutin complex) system modified on the surface of the titanium dioxide hybrid nanocrystals. Ferrous ions are easily oxidized and deactivated by oxidizing media such as oxygen in the environment during membrane preparation, leading to the destruction of the complex structure and the failure of the sensing function.

[0052] The composite membrane material prepared in Example 1 was a light off-white color. Upon exposure to ammonia, its color first changed to a light green and then to a light brownish-yellow. The ΔE value of this membrane increased from 0 at the initial stage to 3.7 at 5 seconds, 6.3 at 20 seconds, 8.8 at 60 seconds, 9.3 at 180 seconds, and 9.4 at 600 seconds throughout the test, indicating that a visually perceptible color change occurred within 20 seconds. The composite membrane material prepared in Example 2 was also a light off-white color. Upon exposure to ammonia, it first changed to a light green and then to a light brownish-yellow. The ΔE value of this membrane increased from 0 at the initial stage to 7.5 at 5 seconds, 7.5 at 20 seconds, 7.5 at 20 seconds, 7.7 at 3 ... The values ​​of 13.6, 18.3 at 60 seconds, 19.2 at 180 seconds, and 19.4 at 600 seconds indicate that the membrane underwent a visually perceptible color change within 5 seconds. The composite membrane material prepared in Example 3 was off-white. After being exposed to an ammonia environment, its color first turned green and then brownish-yellow. The ΔE value of the membrane increased from 0 at the beginning to 14.1 at 5 seconds, 19.6 at 20 seconds, 31.2 at 60 seconds, 32.4 at 180 seconds, and 32.6 at 600 seconds during the entire test period. This indicates that the membrane underwent a visually perceptible color change within 5 seconds, which means that the membrane has rapid and significant ammonia-sensitive color-changing properties.

[0053] Comparing the ammonia response behavior of the composite membrane materials in Example 3 of this invention with those in Comparative Examples 1 and 2, it can be seen that adding polyethylene glycol and titanium dioxide hybrid nanocrystals separately to the ethyl cellulose membrane matrix cannot effectively improve the ammonia-sensitive color-changing performance of the ethyl cellulose membrane. However, adding polyethylene glycol and titanium dioxide hybrid nanocrystals simultaneously to the ethyl cellulose membrane matrix can synergistically give the membrane material a rapid and significant ammonia-sensitive color-changing performance. This can be attributed to two factors: firstly, the addition of polyethylene glycol and titanium dioxide hybrid nanocrystals can make the membrane sample material exhibit a significant porous structure (which is conducive to the permeation and adsorption of gas molecules); secondly, the main chain of polyethylene glycol contains CO. The bonds possess a low internal rotation barrier and exhibit excellent chain segment flexibility, allowing them to adaptively adhere to the surface of titanium dioxide hybrid nanocrystals to form a coating layer. The flexible polyethylene glycol chains inhibit nanoparticle aggregation through steric hindrance, while simultaneously constructing a solvation shell with ether oxygen groups and ethanol molecules, effectively suppressing the attack of solvent molecules and oxygen on the metal centers (ferrous) on the surface of the titanium dioxide hybrid nanocrystals during membrane material preparation. Furthermore, the flexible polyethylene glycol polymer shell does not completely block active sites, allowing small molecules such as ammonia to penetrate the protective layer and coordinate with the internal titanium dioxide hybrid nanocrystals (ferrous metal complexes on the surface), thus improving material stability while retaining its ammonia-sensitive colorimetric functions.

[0054] The long-term color stability test results of Comparative Example 1 and Examples 1-3 (see) Figure 6 The results demonstrate that the membrane materials prepared in Examples 1, 2, and 3, after being stored at 25°C and 57% humidity for 45 days, did not exhibit significant color changes, and the color difference ΔE value after storage was less than 2 (i.e., the color difference was imperceptible to the human eye). These results indicate that the membrane materials prepared according to this invention possess excellent long-term storage stability.

[0055] Figure 7 These are tensile strength diagrams of the composite membrane materials prepared in Comparative Examples 1, 3-4, and 1-3 of this invention. Figure 8 This is a graph showing the elongation at break of the composite membrane materials prepared in Comparative Examples 1, 3-4, and 1-3 of this invention. It can be seen that: In Comparative Example 1, the ethyl cellulose / polyethylene glycol composite membrane material had a tensile strength of 9.54 MPa and an elongation at break of 1.2%. In Comparative Example 3, the addition of titanium dioxide nanocrystals to the ethyl cellulose / polyethylene glycol composite membrane material resulted in a decrease in tensile strength to 8.73 MPa and an increase in elongation at break of 3.3%. In Comparative Example 4, the addition of an iron-arbutin complex to the ethyl cellulose / polyethylene glycol composite membrane material resulted in a decrease in tensile strength to 5.6 MPa and an elongation at break of 2.8%.

[0056] In Example 1 of this invention, 0.005 g of titanium dioxide hybrid nanocrystals were added to the ethyl cellulose / polyethylene glycol composite membrane material, resulting in a composite membrane material with a tensile strength of 11.1 and an elongation at break of 2.0%. In Example 2 of this invention, 0.01 g of titanium dioxide hybrid nanocrystals were added to the ethyl cellulose / polyethylene glycol composite membrane material, resulting in a composite membrane material with a tensile strength of 15.3 and an elongation at break of 2.6%. In Example 3 of this invention, 0.02 g of titanium dioxide hybrid nanocrystals were added to the ethyl cellulose / polyethylene glycol composite membrane material. g, the tensile strength of the resulting composite membrane material is 12.4 MPa, and the elongation at break is 1.9%. It can be seen that using pure titanium dioxide nanocrystals or pure iron-arbutin complexes as fillers for ethyl cellulose / polyethylene glycol composite membrane materials can slightly improve the elongation at break (i.e., ductility) of ethyl cellulose / polyethylene glycol composite membrane materials, but it leads to a significant decrease in tensile strength. In contrast, the embodiments of the present invention use titanium dioxide hybrid nanocrystals (i.e., titanium dioxide nanocrystals modified with iron-arbutin complexes) as fillers for ethyl cellulose / polyethylene glycol composite membrane materials, which can effectively improve both the tensile strength and elongation at break of the composite membrane material.

[0057] Furthermore, the sample performance test data in Tables 1 and 2 also show that the composite membrane material prepared by this invention has excellent ultraviolet shielding, high-energy blue light blocking, and antibacterial properties, while maintaining high visible light transparency. It can be used as a smart indicator material to indicate the freshness changes of shrimp and other meat products during storage in a timely and effective manner. Moreover, the preparation process of this composite material is simple, environmentally friendly, low-cost, and suitable for large-scale production, and has wide application value in food packaging, smart materials, ammonia detection, and other fields.

[0058] The embodiments described above are merely preferred embodiments of the present invention and are not intended to limit the scope of the present invention. Various modifications and improvements made by those skilled in the art to the technical solutions of the present invention without departing from the spirit of the present invention should fall within the protection scope defined by the claims of the present invention.

Claims

1. An ethyl cellulose-based smart active packaging film, characterized in that, The raw materials include: ethyl cellulose, polyethylene glycol, and titanium dioxide hybrid nanocrystals; The mass ratio of the ethyl cellulose, polyethylene glycol and titanium dioxide hybrid nanocrystals is 80:20:0.5-2; The titanium dioxide hybrid nanocrystals are organic-inorganic hybrid modified nanoparticles formed by in-situ coordination of arbutin and ferrous salt on the surface of titanium dioxide nanocrystals.

2. The ethyl cellulose-based smart active packaging film according to claim 1, characterized in that, The preparation method of the titanium dioxide hybrid nanocrystals includes the following steps: (1) Titanium dioxide nanocrystals and arbutin are mixed in solution to obtain a blend; (2) Add ferrous salt to the blended liquid. After the reaction is completed, separate, wash and dry to obtain the titanium dioxide hybrid nanocrystals.

3. The ethyl cellulose-based smart active packaging film according to claim 2, characterized in that, The ferrous salt is ferrous sulfate.

4. A method for preparing an ethyl cellulose-based smart active packaging film as described in claim 1, characterized in that, Includes the following steps: (1) Titanium dioxide nanocrystals and arbutin are mixed in solution to obtain a blend; (2) Add ferrous salt to the blended liquid. After the reaction is completed, separate, wash and dry to obtain the titanium dioxide hybrid nanocrystals. (3) Ethyl cellulose, polyethylene glycol and titanium dioxide hybrid nanocrystals are mixed in an organic solvent to obtain a film-forming solution; (4) The film-forming liquid is subjected to film-forming treatment and dried to obtain the ethyl cellulose-based smart active packaging film.

5. The preparation method according to claim 4, characterized in that, The mixing temperature in step (3) is 25-70℃.

6. The preparation method according to claim 4, characterized in that, The ferrous salt is ferrous sulfate.

7. The application of the ethyl cellulose-based smart active packaging film as described in any one of claims 1-3 in the field of food preservation.

8. The application according to claim 7, characterized in that, The food in question is an animal-derived food.