A Fe 3+ Pre-coordinated lignocellulose nanofiber reinforced and toughened TPS / PBAT fully biodegradable composite film and its preparation method

By using Fe³⁺ pre-coordinated modified LCNF to form coordination bonds with the lignin phenolic hydroxyl and cellulose hydroxyl groups in the TPS/PBAT composite material, a dynamic metal ion crosslinking network is constructed, which solves the problems of insufficient interfacial compatibility and strength of the TPS/PBAT composite material and prepares a high-performance biodegradable composite film.

CN123152180APending Publication Date: 2026-11-24NINGBO UNIV +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611398117.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-09
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing TPS/PBAT composite materials suffer from poor interfacial compatibility, insufficient strength and toughness, and traditional chemical modification methods are complex and environmentally unfriendly.

Method used

Fe³⁺ pre-coordinated modified LCNF was used as a reinforcing agent to form coordination bonds with the lignin phenolic hydroxyl and cellulose hydroxyl groups in the TPS/PBAT composite material, thereby constructing a dynamic metal ion crosslinking network, improving interfacial compatibility and enhancing material properties.

Benefits of technology

The TPS/PBAT composite material exhibits high mechanical strength, thermal stability, and UV blocking properties. It is uniformly dispersed, possesses good aging resistance, and is suitable for applications such as green packaging and biodegradable film bags.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123152180A_ABST
    Figure CN123152180A_ABST
Patent Text Reader

Abstract

This invention discloses a Fe 3+ A pre-coordinated lignocellulose nanofiber reinforced and toughened TPS / PBAT fully biodegradable composite film and its preparation method are disclosed. The mass fraction of the film is: starch 100 parts, PBAT 80-150 parts, Fe... 3+ The mixture comprises 1-8 parts of coordination-modified lignocellulose nanofiber (Fe-LCNF), 10-30 parts of glycerol, 1-3 parts of lubricant, and 1-3 parts of stabilizer. The Fe-LCNF is LCNF prepared from straw through alkali treatment and mechanical ball milling, and then further processed using Fe... 3+ The LCNF is obtained by coordination with hydroxyl groups on the surface. It retains the lignin structure, with fiber diameters of 5–100 nm and lengths of 0.5–20 mm. This invention utilizes Fe... 3+ The metal ion bridging and dynamic coordination network structure formed between the composite material and the wood-based nanocellulose significantly improves the mechanical properties, thermal stability, water barrier properties, and UV barrier properties. This invention features a simple preparation process, utilizing a green aqueous phase system to complete the Fe... 3+ Pre-coordinated modification enables the high-value utilization of agricultural waste and straw resources. While maintaining the biodegradability of the material, it achieves a synergistic improvement in reinforcement and toughness, and can be widely used in the fields of green packaging materials, agricultural films and bio-based functional materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of biodegradable thin film technology, specifically relating to an Fe... 3+ Starch / PBAT biodegradable composite films synergistically reinforced with lignocellulose nanofibers and their preparation method. Background Technology

[0002] Starch is a natural biomolecule with wide availability, renewability, and low cost. Thermoplastic starch (TPS), obtained through plasticization modification, can be blended with biodegradable polyesters such as polybutylene adipate / terephthalate (PBAT) to produce starch-based biodegradable composites, significantly reducing the cost and performance of biodegradable materials. Furthermore, starch-based biodegradable plastics can be completely degraded into carbon dioxide and water through composting after their lifespan, making them environmentally friendly. TPS / PBAT composites are an important category of starch-based biodegradable plastics, applicable to various fields such as biodegradable agricultural films and disposable plastic bags. However, the blending of starch and PBAT presents a problem of poor interfacial compatibility. The hydrophilicity of starch and the hydrophobicity of PBAT hinder stress transfer at the interface, resulting in lower strength and modulus of TPS / PBAT composites, and the starch is prone to retrogradation. Therefore, improving interfacial compatibility, enhancing the mechanical properties of TPS / PBAT composites, and preventing starch retrogradation are key aspects driving the development of TPS / PBAT composites.

[0003] Nanofibrillated cellulose (NFC) possesses advantages such as high mechanical strength, tunable surface chemistry, and barrier properties, making it a promising interfacial modifier and reinforcing filler for TPS / PBAT composites. However, the high hydroxyl content on the surface of natural NFC limits its compatibility with PBAT, resulting in poor performance in TPS / PBAT systems. Furthermore, the nanoscale nature of NFC makes it difficult to disperse uniformly in the matrix, especially unmodified NFC, which exhibits significant aggregation due to intermolecular hydrogen bonding, negatively impacting the mechanical properties of TPS / PBAT composites. Fourati et al. (…) International Journal of Biological Macromolecules, (2021, 183: 267-275) This study employed esterification-modified nanofiber cellulose (NFC) followed by high-energy ball milling pretreatment to modify the TPS / PBAT blend system. Esterification modification allowed NFC to retain both hydrophilic hydroxyl groups and hydrophobic ester groups, forming an amphiphilic molecular structure. This structure could create an interfacial bridge between the hydrophilic TPS and hydrophobic PBAT phases, effectively reducing the size of the TPS dispersed phase, eliminating interfacial pores, and improving the interfacial compatibility between the two phases. While chemical modification (such as acetylation, oxidation, or grafting) can improve interfacial compatibility, it often involves complex processes, toxic reagents, or high costs, thereby compromising the sustainability and economic viability of the final product.

[0004] Recent studies have shown that retaining a certain amount of lignin can have positive effects on NFC, such as reducing polarity, improving UV blocking properties, and enhancing thermal stability. (Aouay et al.) Biomacromolecules 2023, 24(8): 3872-3886.) PBAT / TPS blends were modified with lignin-containing nanofibers (LCNF). Compared to traditional delignified pure CNF, the biggest advantage of LCNF is that it retains about 20 wt% hydrophobic lignin components, improving the interfacial compatibility between hydrophilic TPS and hydrophobic PBAT without additional chemical esterification modification. This can significantly reduce the water absorption rate of the material, solve the water sensitivity defect of TPS, and simultaneously enhance tensile strength and modulus while maintaining high ductility. Although LCNF is expected to improve the interfacial compatibility of TPS / PBAT composites and endow the material with certain functions, the interfacial improvement ability is limited, and the starch retrogradation problem still exists. In order to further improve the mechanical properties and durability of TPS / PBAT composite films, metal ion coordination (such as Fe) is used. 3+ Ca 2+ Zn 2+ This provides a better solution. He et al. ( ACS Sustainable Chemistry&Engineering, 2020, 8(23): 8655-8663.) Using zinc acetate and TPS to construct a metal-organic coordination network, only 3 wt% zinc acetate can increase the glass transition temperature of TPS from about 48℃ to 89℃ and the water contact angle from about 56° to 118°, while improving strength and shape stability. The coordination network is not only crosslinked, but can also change the movement of starch chains and supramolecular organization. Although a robust and reversible metal-organic supramolecular network structure can be constructed by adding multivalent metal ions as dynamic crosslinking agents to coordinate with the abundant hydroxyl groups on TPS and cellulose, for Fe 3+ The application of TPS / PBAT composites has not yet been reported, and the compounding system and preparation technology of the material still need to be studied.

[0005] In summary, to address the shortcomings of TPS / PBAT composites in terms of mechanical and physical properties, this invention utilizes LCNF with its unique morphology and function as a reinforcing agent and functional agent, combined with Fe... 3+ The coordination advantage of ions led to the development of a Fe 3+ A TPS / PBAT composite film synergistically reinforced with LCNF and its preparation method. The biodegradable film prepared using this method exhibits uniform dispersion of all components, high mechanical strength, good aging resistance, and UV blocking properties, enabling its wide application in green packaging, biodegradable bags, and food preservation. Summary of the Invention

[0006] The technical problem to be solved by the present invention is to provide a metal ion Fe, which addresses the shortcomings of the prior art. 3+ A TPS / PBAT composite film synergistically reinforced with LCNF and its preparation method. The TPS / PBAT composite film of this invention exhibits high mechanical strength, thermal stability, and thermoplasticity, and is a novel, non-toxic, environmentally friendly, and biodegradable nanocomposite film material. The preparation method of this invention utilizes Fe... 3+ Synergistic enhancement of TPS / PBAT with LCNF, utilizing the depolarization and metal coordination mechanism of LCNF to improve interfacial compatibility, achieving good dispersibility of LCNF in starch matrix, while simultaneously mixing low-cost TPS with PBAT, and in Fe 3+ With the coordination effect of LCNF and the nanofiber reinforcement of LCNF, the reinforcing and toughening effect of LCNF in TPS / PBAT is fully utilized, and starch recrystallization is inhibited, thereby preparing a high-performance fully biodegradable composite film.

[0007] The technical solution adopted by the present invention to solve the above-mentioned technical problems is: a Fe 3+ A pre-coated lignocellulose nanofiber reinforced and toughened TPS / PBAT fully biodegradable composite film, the mass fraction of which is: starch 100 parts, PBAT 80-150 parts, Fe 3+ The mixture comprises 1-8 parts of coordination-modified lignocellulose nanofiber (Fe-LCNF), 10-30 parts of glycerol, 1-3 parts of lubricant, and 1-3 parts of stabilizer, wherein the Fe... 3+ Coordination-modified LCNF satisfies the following condition (a), the Fe 3+ The crosslinking agent meets the following condition (b): (a) The Fe 3+ It forms a coordination bond with the hydroxyl group on LCNF; (b) The LCNF has a network structure or a branched multidimensional structure, with a single fiber diameter of 5~100 nm, a length of 0.5~20 mm, and a lignin content of 5~20 wt%.

[0008] In the preparation method of LCNF, the concentration of NaOH ranges from 5 wt% to 20 wt%.

[0009] The Fe 3+ Fe in coordination-modified lignocellulose nanofibers 3+ The ratio of mol to LCNF was 0.031 mol: 100 g.

[0010] Optimal ratio: 100 parts TPS, 100 parts PBAT, 4 parts Fe-LCNF, 20 parts glycerin, 1 part lubricant, and 1 part stabilizer.

[0011] The LCNF used in this invention has a unique network or branched multidimensional structure, with a high aspect ratio and high specific surface area. Its surface simultaneously contains cellulose hydroxyl and lignin phenolic hydroxyl functional groups. Fe 3+ It can form coordination bonds with phenolic hydroxyl groups in lignin and hydroxyl groups in cellulose, and subsequently form coordination crosslinking structures with hydroxyl groups on the TPS surface, constructing a dynamic metal ion crosslinking network within the TPS / PBAT composite material. This is key to optimizing performance. The Fe used in this invention... 3+ It preferentially forms a metal-phenol network structure with the ortho-phenolic hydroxyl groups in the residual lignin, and further connects the starch phase and the PBAT phase through coordination bonds and hydrogen bonds, thereby improving interfacial compatibility, stress transfer efficiency, and the strength, toughness and barrier properties of the composite material.

[0012] Preferably, the Fe 3+ It is derived from at least one of anhydrous ferric chloride, ferric nitrate, or ferric sulfate.

[0013] Preferably, the Fe 3+ The raw materials for coordination-modified LCNF are derived from at least one of wood flour, bamboo flour, corn stalks, wheat stalks, rice stalks, and sugarcane bagasse, with a particle size of 40-200 mesh.

[0014] Preferably, the starch is one or a combination of two or more of the following: corn starch, tapioca starch, pea starch, potato starch, wheat starch, sweet potato starch, and lotus root starch.

[0015] Preferably, the glycerol is a food-grade plasticizer that breaks the hydrogen bonds within starch molecules, giving the system thermoplastic processing fluidity.

[0016] Preferably, the stabilizer is one or a combination of two or more of antioxidants 1010, 168, 1076, and 1790.

[0017] Preferably, the thickness of the starch film is 0.03~0.5 mm.

[0018] The above Fe 3+ A method for preparing TPS / PBAT composite films synergistically reinforced with LCNF includes the following steps: 1) Take 5-10 parts of straw raw material and place it in 70-80 parts of a 5-20 wt% sodium hydroxide solution. Treat at 70-80℃ for 5-6 hours to partially remove lignin and hemicellulose. After treatment, wash repeatedly with pure water until neutral and dry. Prepare a 10 wt% solution from the obtained powder and perform wet ball milling. The ball milling conditions are: rotation speed 400-600 rpm, ball-to-material ratio 18-20:1, and milling time 7-10 hours. After ball milling, an LCNF suspension is obtained.

[0019] 2) Dilute the LCNF suspension obtained in 1) to a mass concentration of 1 wt%. Sonicate the solution for 15-30 min to disperse the fibers. Then prepare a 0.05 mol / L solution of FeCl3, Fe(NO3)3, or Fe2(SO4)3. At 40℃, place the Fe-containing... 3+ The solution was slowly added dropwise to the LCNF suspension until Fe... 3+ The ratio of FeCl3 to LCNF was 0.031 mol: 100 g (corresponding to 5 wt% FeCl3, 7.5 wt% Fe(NO3)3, and 6.2 wt% Fe2(SO4)3 of LCNF). The reaction was continuously magnetically stirred for 2–3 h, allowing Fe to... 3+ It reacts fully with LCNF to form Fe 3+ Coordination. After the reaction, wash three times with pure water to remove unreacted Fe. 3+ Ions. The resulting product was freeze-dried to obtain Fe. 3+ Coordinated LCNF (i.e., Fe-LCNF) powder.

[0020] Because LCNF contains a large number of active groups such as alcohol hydroxyl and phenolic hydroxyl groups on its surface, it has a high surface energy and is prone to aggregation through hydrogen bonding. This results in insufficient dispersion in its TPS / PBAT matrix and poor interfacial compatibility, limiting the full realization of the reinforcing and toughening effect of LCNF. Therefore, in step 2), this invention uses Fe 3+ The pre-coordination modification strategy enables Fe 3+ It preferentially coordinates with phenolic hydroxyl, alcoholic hydroxyl, and carboxyl groups on the surface of LCNF. This coordination effectively inhibits the aggregation of LCNFs and also enhances the interfacial bonding between LCNFs and TPS and PBAT matrices. This invention not only retains some of the amphiphilic LCNFs with lignin but also utilizes Fe... 3+ A coordination network structure with dynamic and reversible characteristics is constructed between lignin and phenolic hydroxyl groups, thereby doubly enhancing the interfacial affinity of LCNF.

[0021] 3) Mix 100 parts of starch with 20-30 parts of glycerol and stir for 30-60 minutes to obtain a pre-plasticized starch system. Perform melt plasticizing and granulation in a twin-screw extruder at an extrusion temperature of 90-120℃ and a screw speed of 80-150 rpm to obtain thermoplastic starch (TPS) granules.

[0022] 4) The 100 parts of TPS particles obtained in step 3) are premixed with 1-4 parts of Fe-LCNF powder, 80-150 parts of PBAT particles, 1-3 parts of lubricant, and 1-3 parts of stabilizer at high speed for 15-30 min. Then, the mixture is put into a twin-screw extruder for melt blending and granulation. The extrusion temperature is 90-130℃ and the screw speed is 80-150 rpm.

[0023] During the melt shearing process, shear force promotes the uniform dispersion of Fe-LCNF in the TPS / PBAT matrix and the formation of an entangled nanofiber network, which plays a role in physical reinforcement. Meanwhile, Fe... 3+ The six coordination structures simultaneously form a dynamic coordination crosslinking network with the hydroxyl groups of TPS and the phenolic hydroxyl groups on the surface of LCNF. The synergistic effect of the nanofiber physical network and the dynamic coordination bonds of metal ions improves the interfacial compatibility between TPS and PBAT, inhibits phase separation, and constructs multiple reversible interfacial forces, achieving efficient stress transfer and energy dissipation, ultimately forming a stable and synergistic interfacial reinforcement structure. This invention utilizes alkali-regulated amphiphilic LCNF that retains lignin to form a crosslinking network with Fe. 3+ The technical route of preparing Fe-LCNF through pre-coordination modification and further constructing a dynamic coordination network through melt blending allows Fe to... 3+ Prioritizing the surface of wood-based nanocellulose, it forms a metal ion bridging structure and a dynamic coordination crosslinking network within the composite material, achieving interfacial compatibility.

[0024] The composite particles obtained in step 4) are processed into thin films using hot pressing, blown film, or casting methods to obtain Fe. 3+ TPS / PBAT composite films synergistically reinforced with LCNF. Film thickness: 0.03~0.5 mm.

[0025] Compared with the prior art, the present invention has the following advantages: 1. This invention is the first to use Fe 3+ The method of pre-coordinated modification of LCNF, through Fe 3+ Stable coordination structures are formed between lignin phenolic hydroxyl groups, cellulose hydroxyl groups, and carboxyl groups, constructing a metal ion bridging layer on the surface of LCNF nanocellulose, effectively inhibiting LCNF aggregation and improving its dispersibility in the TPS / PBAT matrix. Furthermore, through Fe... 3+The pre-coordinated structure further forms a dynamic coordination network with the hydroxyl groups in the TPS matrix. Under the action of external force, it can undergo reversible dissociation and recombination, realizing the synergistic effect of stress transfer and energy dissipation, thereby simultaneously improving the tensile strength, elongation at break and toughness of the composite material.

[0026] 2. This invention uses amphiphilic LCNF that retains some lignin as a reinforcing phase. The hydrophobic groups in the residual lignin in LCNF can generate good interfacial interaction with the PBAT phase, while the hydroxyl groups on the surface of cellulose in LCNF can form hydrogen bonds with TPS, thereby playing an interfacial bridging role and significantly improving the interfacial compatibility between the TPS and PBAT phases.

[0027] 3. This invention constructs an "LCNF-reinforced framework-Fe". 3+ The "Dynamic Coordination Network-TPS / PBAT Interface Bridging" triple synergistic reinforcement structure effectively solves the problem of balancing strength and toughness in traditional starch-based composite materials, achieving simultaneous improvement in reinforcement and toughness. In this invention, Fe... 3+ Pre-coordinated structures can restrict polymer chain movement and improve the stability of the internal network structure of the material, thereby further enhancing the thermal stability and water resistance of the composite material. This invention utilizes Fe... 3+ The synergistic effect of pre-coordinated modification and amphiphilic LCNF significantly improves the overall performance of TPS / PBAT composite materials while maintaining the fully biodegradable properties of the materials, providing a new technical solution for high-performance fully biodegradable packaging materials, agricultural films and green functional materials.

[0028] 4. This invention uses agricultural waste (such as corn stalks) as raw materials to prepare LCNF, realizing the high-value utilization of biomass resources; at the same time, it adopts an aqueous phase coordination modification process, which does not require the introduction of a large amount of organic solvents. The preparation process is green and environmentally friendly, simple, and suitable for industrial promotion and utilization. Attached Figure Description

[0029] Figure 1 Mechanical properties of TPS / PBAT composite films with different Fe-LCNF addition amounts; Figure 2 WVP of TPS / PBAT composite films with different Fe-LCNF addition amounts; Figure 3 SEM images of TPS / PBAT composite films with different Fe-LCNF addition amounts; Figure 4 Mechanical properties of TPS / PBAT composite films with different PBAT addition amounts; Figure 5 WVP of TPS / PBAT composite films with different PBAT addition amounts; Figure 6 Mechanical properties of TPS / PBAT composite films with different FeCl3 addition amounts; Figure 7 WVP of TPS / PBAT composite films with different FeCl3 addition amounts; Figure 8 Mechanical properties of Fe-LCNF TPS / PBAT composite films treated with different concentrations of alkali; Figure 9 WVP of Fe-LCNF TPS / PBAT composite films treated with different concentrations of alkali; Figure 10 Thermal performance curves of TPS / PBAT composite films; Figure 11 UV-Vis transmission spectrum of TPS / PBAT composite film; Figure 12 Different Fe 3+ Mechanical properties of the source TPS / PBAT composite film; Figure 13 Different Fe 3+ WVP of the source TPS / PBAT composite film; Figure 14 Mechanical properties of TPS / PBAT composite films with different glycerol addition amounts; Figure 15 WVP of TPS / PBAT composite films with different glycerol additions. Detailed Implementation

[0030] The present invention will be further described in detail below with reference to the accompanying drawings and embodiments.

[0031] The mass composition of the composite films of Comparative Examples 1 to 4 is shown in Table 1. The composite films of Comparative Examples 1 to 4 are respectively represented by the numbers B1, B2, B3 and B4, and single-factor experiments were conducted.

[0032] Table 1 Serial Number serial number starch PBAT LCNF glycerin <![CDATA[FeCl3 addition amount]]> lubricant stabilizer Comparative Example 1 B1 100 100 0 0 0 1 1 Comparative Example 2 B2 100 100 0 20 0 1 1 Comparative Example 3 B3 100 100 0 20 5 1 1 Comparative Example 4 B4 100 100 4 20 0 1 1 The preparation method of the starch / PBAT composite film of Comparative Example 1 includes the following steps: 100 parts starch, 100 parts PBAT granules, 1 part lubricant, and 1 part stabilizer were premixed at high speed for 30 min, and then melt-blended and granulated in a twin-screw extruder at an extrusion temperature of 120℃ and a screw speed of 80 rpm.

[0033] The composite particles obtained in step 1) are processed into a film by hot pressing to obtain a starch / PBAT composite film.

[0034] The preparation method of the TPS / PBAT composite film of Comparative Example 2 includes the following steps: 1) Mix 100 parts starch with 20 parts glycerol and stir for 40 min to obtain a pre-plasticized starch system. Melt-plasticize and granulate the mixture in a twin-screw extruder at an extrusion temperature of 120℃ and a screw speed of 100 rpm to obtain TPS granules.

[0035] 2) Premix 100 parts of TPS granules, 100 parts of PBAT granules, 1 part of lubricant, and 1 part of stabilizer at high speed for 30 min, then put them into a twin-screw extruder for melt blending and granulation. The extrusion temperature is 120℃ and the screw speed is 100 rpm.

[0036] 3) The composite particles obtained in step 2) are processed into a thin film by hot pressing to obtain a TPS / PBAT composite film.

[0037] Comparative Example 3 Fe without LCNF 3+ A method for preparing separately reinforced TPS / PBAT composite films includes the following steps: 100 parts starch and 20 parts glycerol were mixed and stirred for 40 min to obtain a pre-plasticized starch system. The system was then melt-plasticized and granulated in a twin-screw extruder at an extrusion temperature of 120℃ and a screw speed of 100 rpm to obtain TPS granules.

[0038] Prepare a 0.05 mol / L FeCl3 solution. 3) The 100 parts of TPS particles obtained in step 1) are premixed with 5 parts of FeCl3 solution, 100 parts of PBAT particles, 1 part of lubricant and 1 part of stabilizer at high speed for 30 min. Then, the mixture is put into a twin-screw extruder for melt blending and granulation. The extrusion temperature is 120℃ and the screw speed is 100 rpm.

[0039] 4) The composite particles obtained in step 3) are processed into a thin film by hot pressing to obtain Fe without LCNF. 3+ TPS / PBAT composite film reinforced separately.

[0040] Comparative Example 4 (Fe-free) 3+ The method for preparing LCNF-reinforced TPS / PBAT composite films includes the following steps: 1) Take 10 parts of straw raw material and place it in 80 parts of a 10 wt% sodium hydroxide solution. Treat at 80℃ for 6 h to partially remove lignin and hemicellulose. After treatment, wash repeatedly with pure water until neutral and dry. Prepare a 10 wt% solution of the obtained powder and perform wet ball milling. The ball milling conditions are: rotation speed 600 rpm, ball-to-material ratio 20:1, and ball milling time 10 h. After ball milling, an LCNF suspension is obtained. Subsequently, centrifuge and wash with deionized water until neutral, and freeze-dry to obtain LCNF powder. 2) Mix 100 parts starch with 20 parts glycerol and stir for 60 min to obtain a pre-plasticized starch system. Melt-plasticize and granulate the mixture in a twin-screw extruder at an extrusion temperature of 120℃ and a screw speed of 100 rpm to obtain TPS granules.

[0041] 3) The 100 parts of TPS granules obtained in step 2) are premixed with the 4 parts of LCNF powder, 100 parts of PBAT granules, 1 part of lubricant and 1 part of stabilizer obtained in step 1) at high speed for 30 min. Then, the mixture is put into a twin-screw extruder for melt blending and granulation. The extrusion temperature is 120℃ and the screw speed is 100 rpm.

[0042] 4) The composite particles obtained in step 3) are processed into a thin film by hot pressing to obtain an LCNF-reinforced TPS / PBAT composite film.

[0043] The mass fraction composition of the composite films of Examples 1 to 8 is shown in Table 2. The composite films of Examples 1 to 8 are respectively represented by the numbers C1, C2, C3, C4, C5, C6, C7, and C8, and single-factor experiments were conducted.

[0044] Table 2 Serial Number serial number starch PBAT Fe-LCNF glycerin lubricant stabilizer Example 1 C1 100 100 1 20 1 2 Example 2 C2 100 100 2 20 1 2 Example 3 C3 100 100 3 20 1 2 Example 4 C4 100 100 4 20 1 2 Example 5 C5 100 100 5 20 1 2 Example 6 C6 100 100 6 20 1 2 Example 7 C7 100 100 7 20 1 2 Example 8 C8 100 100 8 20 1 2 The preparation method of the TPS / PBAT / Fe-LCNF composite film in Example 1 includes the following steps: Ten parts of straw raw material were placed in 80 parts of a 10 wt% sodium hydroxide solution and treated at 80℃ for 6 h to partially remove lignin and hemicellulose. After treatment, the material was repeatedly washed with pure water until neutral and dried. The resulting powder was prepared into a 10 wt% solution and wet ball-milled. The ball-milling conditions were: 600 rpm, ball-to-material ratio 20:1, and milling time 10 h. After ball milling, an LCNF suspension was obtained.

[0045] 2) Dilute the LCNF suspension obtained in 1) to a mass concentration of 1 wt%. Sonicate the solution for 30 min to disperse the fibers. Then prepare a 0.05 mol / L FeCl3 solution and, at 40℃, dissolve the Fe...3+ The solution was slowly added dropwise to the LCNF suspension, allowing Fe to... 3+ The ratio of FeCl3 to LCNF was 0.031 mol: 100 g (corresponding to FeCl3 added at 5 wt% of the mass of LCNF), and the reaction was continuously magnetically stirred for 2-3 h, allowing FeCl3 to... 3+ It reacts with LCNF to form Fe 3+ Coordination. After the reaction, wash three times with pure water to remove unreacted Fe. 3+ Ions. The resulting product was freeze-dried to obtain Fe. 3+ Coordinated LCNF (i.e., Fe-LCNF) powder.

[0046] 3) Mix 100 parts starch with 20 parts glycerol and stir for 60 min to obtain a pre-plasticized starch system. Melt-plasticize and granulate the mixture in a twin-screw extruder at an extrusion temperature of 120℃ and a screw speed of 100 rpm to obtain TPS granules.

[0047] 4) The 100 parts of TPS particles obtained in step 3) are premixed with the 1 part of Fe-LCNF powder, 100 parts of PBAT particles, 1 part of lubricant and 2 parts of stabilizer obtained in step 2) at high speed for 30 min. Then, the mixture is put into a twin-screw extruder for melt blending and granulation. The extrusion temperature is 120℃ and the screw speed is 100 rpm.

[0048] 5) The composite particles obtained in step 4) are processed into a thin film by hot pressing to obtain an LCNF-reinforced TPS / PBAT composite film.

[0049] The preparation methods of the composite films in Examples 2 to 8 are basically the same as those in Example 1, except that the mass fractions of Fe-LCNF in step 4) of the preparation of Examples 2 to 8 are 2 parts, 3 parts, 4 parts, 5 parts, 6 parts, 7 parts, and 8 parts, respectively, to prepare the TPS / PBAT / Fe-LCNF composite films of Examples 2 to 8.

[0050] For the composite films of Comparative Examples 1-4 and Examples 1-8, tensile test samples were prepared using a cutting tool. The mechanical properties of the composite films of Comparative Examples 1-4 and Examples 1-8 were tested in groups according to the method of national standard GB / T1040.1-2018. The tensile test samples were dumbbell-shaped specimens, 50 mm in length and 4 mm in width at the center. The tensile speed was 10 mm / min, and at least 5 specimens were tested in each group. The average tensile strength and elongation at break of the samples were taken. The results are shown in Table 3. Figure 1 As shown.

[0051] From Table 3 and Figure 1It can be seen that the starch / PBAT composite film of Comparative Example 1 has the lowest tensile strength, only 5.68 MPa, and a tensile breaking rate of 152%. The TPS / PBAT composite film of Comparative Example 2 has a tensile strength of 5.88 MPa and a tensile breaking rate of 378%. This is because the intermolecular forces of starch decrease after plasticization, making it easier for the molecular chains to slip relative to each other under tensile stress, thus increasing the tensile breaking rate. Comparative Example 3, Fe without LCNF... 3+ The tensile strength of the TPS / PBAT composite film reinforced alone is 6.69 MPa, and the tensile breaking rate is 403%. This is due to the free Fe... 3+ It can form chelate crosslinks with starch molecules, restricting chain segment movement and simultaneously improving the material's strength and toughness. Comparative Example 4, which does not contain Fe... 3+ The LCNF-reinforced TPS / PBAT composite film exhibited a tensile strength of 7.03 MPa and a tensile breaking rate of 309%. Compared to the TPS / PBAT / Fe-LCNF composite films of Examples 1-8, the mechanical properties of these comparative examples are relatively low because the comparative examples lacked Fe. 3+ Alternatively, the absence of LCNF prevents the formation of a stable metal ion coordination structure on the surface, resulting in limited improvement in the mechanical properties of the composite film. In Examples 1-8, the tensile strength and tensile breaking rate of the TPS / PBAT / Fe-LCNF composite films showed a trend of first increasing and then decreasing with increasing Fe-LCNF content. When the Fe-LCNF content was 4 parts, both the tensile strength and tensile breaking rate of the composite film reached their maximum values, with a maximum tensile strength of 19.34 MPa, approximately four times that of pure starch film, and a maximum tensile breaking rate of 1109%. These results indicate that Fe-LCNF has a significant reinforcing and toughening effect on the TPS / PBAT composite material. This is because LCNF has abundant alcohol and phenolic hydroxyl active sites, which, in Fe... 3+ Under pre-coordination, a stable metal ion coordination structure is formed on the surface of LCNF, which can form strong interfacial forces with the hydroxyl groups in TPS and the ester groups in PBAT, thereby constructing a continuous and stable reinforcing network structure. This network structure can not only effectively transfer external loads but also inhibit the slippage of polymer molecular chains, improving the load-bearing capacity of the material, thus significantly improving the tensile strength of the composite material. When the amount of Fe-LCNF added continues to increase, the strength of the composite material shows a decreasing trend. This is mainly because excessive Fe-LCNF is prone to agglomeration in the matrix, leading to a decrease in its dispersion uniformity and thus weakening the reinforcing effect.

[0052] Referring to GB / T 1037-2021 standard, the water vapor transmission rate (WVP) of the composite films of Comparative Examples 1 to 4 and Examples 1 to 8 was tested (Table 3 and...). Figure 2 The water vapor transmission rates of Comparative Examples 1 to 4 all exceeded 10 × 10⁻⁶. -5 ·g·m -1 ·s -1 ·Pa -1 Among them, the pure starch film had the highest water vapor permeability of 13.45 × 10⁻⁶. -5 ·g·m -1 ·s -1 ·Pa -1 The water vapor transmission rate of the TPS / PBAT / Fe-LCNF composite films in Examples 1 to 8 after adding different amounts of Fe-LCNF showed a trend of first decreasing and then increasing, with the lowest C4 being 3.89 × 10⁻⁶. -5 ·g·m -1 ·s -1 ·Pa -1 This is because the uniformly dispersed LCNF scaffold acts as a water-impermeable and rigid physical labyrinth within the soft starch matrix. However, when the amount of Fe-LCNF added exceeds 4 parts, the forced micro-aggregation of nanoparticles begins, creating localized gaps and voids. These voids promote rapid water penetration, leading to a slight rebound in the WVP value.

[0053] Figure 3 Comparative Example 1 is shown. Figure 3 a) Comparative Example 2 ( Figure 3 b) Comparative Example 3 Figure 3 c) Example 1 ( Figure 3 d) Example 4 Figure 3 e), Example 7 ( Figure 3 f) SEM image of the quenched cross section of the composite thin film. Figure 3 As can be seen from (ac), the characteristic of the unbroken surface of the Fe-LCNF composite film is the presence of obvious voids and gaps around the dispersed phase. This phase separation indicates that there is thermodynamic incompatibility between the recrystallized starch particles and between the hydrophilic starch and the hydrophobic PBAT, resulting in stress concentration points and premature failure. When the Fe-LCNF addition amount is 4 parts ( Figure 3 e), the microstructure of the interface has undergone a fundamental transformation. For example... Figure 3 As shown in (df), the sharp phase boundaries disappear, replaced by a continuous and integrated morphology, with the surface exhibiting extensive plastic deformation rather than brittle fracture characteristics. This indicates that the interface is strong enough to transfer stress, yet flexible enough to withstand significant tension.

[0054] Table 3 Serial Number serial number Tensile strength (MPa) Tensile fracture rate (%) <![CDATA[Water vapor transmission rate (×10 -5 ·g·m -1 ·s -1 ·Pa -1 )]]> Comparative Example 1 B1 5.68 ± 0.1 152 ± 10 13.45 ± 0.11 Comparative Example 2 B2 5.88 ± 0.2 378 ± 12 12.48 ± 0.12 Comparative Example 3 B3 6.69 ± 0.1 403 ± 15 11.29 ± 0.11 Comparative Example 4 B4 7.03 ± 0.1 309 ± 13 12.92 ± 0.11 The mass fraction composition of the TPS / PBAT / Fe-LCNF composite films of Examples 9 to 12 is shown in Table 4. The composite films of Examples 9 to 12 are designated as D1, D2, D3, and D4, respectively, and single-factor experiments were conducted.

[0055] Table 4 Serial Number serial number starch PBAT Fe-LCNF glycerin lubricant stabilizer Example 9 D1 100 80 4 20 3 1 Example 10 D2 100 100 4 20 3 1 Example 11 D3 100 120 4 20 3 1 Example 12 D4 100 150 4 20 3 1 The preparation methods of the TPS / PBAT / Fe-LCNF composite films in Examples 9 to 12 are basically the same as those in Example 4, except that in step 4) of Examples 9 to 12, the number of PBAT parts is 80 parts, 100 parts, 120 parts and 150 parts respectively, and the TPS / PBAT / Fe-LCNF composite films of Examples 9 to 12 are prepared respectively.

[0056] For the composite films of Examples 9 to 12, tensile test samples were prepared using a cutting tool. The mechanical properties of the composite films of Examples 9 to 12 were tested in groups according to the method of national standard GB / T1040.1-2018. The tensile test samples were dumbbell-shaped specimens, 50 mm in length and 4 mm in width at the center. The tensile speed was 10 mm / min, and at least 5 specimens were tested in each group. The average value of the tensile strength and elongation at break of the samples was taken. The results are as follows: Figure 4 As shown.

[0057] from Figure 4 As can be seen, with the increase of PBAT addition, the tensile strength of the TPS / PBAT / Fe-LCNF composite film first increases and then decreases. The maximum tensile strength is 19.45 MPa when the PBAT addition is 100 parts, with a tensile fracture rate exceeding 1000%. This is because PBAT forms a continuous load-bearing matrix, improves the interfacial compatibility of the TPS two phases, and refines the grains to reduce stress defects. However, when PBAT is excessive, the rigid reinforcing skeleton of starch and Fe-LCNF is diluted, the density of the metal coordination crosslinking network decreases, and a large number of weak phase interfaces reduce the tensile strength. With the increase of PBAT addition, the elongation at break of the TPS / PBAT / Fe-LCNF composite film continuously increases. This is because PBAT molecules are rich in flexible aliphatic chains, acting as the dominant material in the continuous phase for plastic deformation, while simultaneously isolating rigid TPS and nanofillers, preventing rapid crack propagation, inhibiting starch retrogradation, and allowing the film to achieve greater tensile deformation.

[0058] According to GB / T 1037-2021 standard, the water vapor transmission rate of the composite films in Examples 9 to 12 was tested. Figure 5 As the amount of PBAT added increases, the water vapor transmission rate first decreases and then increases. When the amount of PBAT added is 100 parts, the water vapor transmission rate of the composite film is the lowest, at 3.50 × 10⁻⁶.-5 ·g·m -1 ·s -1 ·Pa -1 This is because an appropriate amount of hydrophobic PBAT can interrupt the continuous water-permeable channels of hydrophilic starch, and in conjunction with the LCNF labyrinth structure, extend the water vapor diffusion path, thereby increasing the film density and decreasing the water vapor permeability. However, when too much PBAT is added, the dense barrier framework is diluted, the free volume of the matrix increases, the number of micropores at the two-phase interface increases, the resistance to water molecule diffusion decreases, and the water vapor permeability increases.

[0059] The mass fraction composition of the TPS / PBAT / Fe-LCNF composite films of Examples 13 to 17 is shown in Table 5. The composite films of Examples 13, 14, 16 and 17 are designated as E1, E2, E4 and E5, respectively, and single-factor experiments were conducted.

[0060] Table 5 Serial Number serial number starch PBAT Fe-LCNF glycerin <![CDATA[FeCl3]]> lubricant stabilizer Example 13 E1 100 100 4 20 1 2 1 Example 14 E2 100 100 4 20 5 2 1 Example 16 E4 100 100 4 20 7 2 1 Example 17 E5 100 100 4 20 9 2 1 The preparation methods of the starch composite films in Examples 13 to 17 are basically the same as those in Example 4, except that in step 2) of Examples 13 to 17, the amount of FeCl3 added is 1 wt%, 5 wt%, 7 wt%, and 9 wt% of the mass of LCNF, respectively, and TPS / PBAT / Fe-LCNF composite films of Examples 13 to 17 are prepared respectively.

[0061] For the composite films of Examples 13-17, tensile test samples were prepared using a cutting tool. The mechanical properties of the composite films of Examples 13-17 were tested in groups according to the method of national standard GB / T1040.1-2018. The tensile test samples were dumbbell-shaped specimens, 50 mm in length and 4 mm in width at the center. The tensile speed was 10 mm / min, and at least 5 specimens were tested in each group. The average tensile strength and elongation at break of the samples were taken. The results are as follows: Figure 6 As shown.

[0062] Depend on Figure 6 It can be seen that with the increase of FeCl3 addition, the tensile strength of the TPS / PBAT composite film shows a trend of first increasing and then decreasing. When the FeCl3 addition is 5 wt%, the tensile strength of the composite film is relatively high at 19.05 MPa, and the tensile breaking rate is 1169%. This indicates that Fe... 3+ Pre-coordination can significantly enhance the interfacial bonding between LCNF and the TPS / PBAT matrix. The enhancement mechanism lies in the fact that Fe... 3+It can form stable coordination structures with phenolic hydroxyl, hydroxyl, and carboxyl groups on the LCNF surface, and simultaneously undergo dynamic coordination with hydroxyl groups in TPS, constructing a continuous and stable metal-ion bridging network. This network structure can preferentially transfer external stress, improve interfacial load transfer efficiency, and inhibit crack propagation, thereby significantly improving the strength and toughness of the composite material. When the FeCl3 addition amount is further increased to 9 wt%, the mechanical properties of the composite film show a decreasing trend. This is mainly due to the excess Fe... 3+ This leads to excessive local cross-linking and nanofiber aggregation, reducing the uniformity of the interfacial structure and causing stress concentration, thereby weakening the reinforcing effect. Therefore, the preferred FeCl3 addition amount in this invention is 5 wt% of the mass of LCNF.

[0063] According to GB / T 1037-2021 standard, the water vapor transmission rate of the composite films in Examples 13 to 17 was tested. Figure 7 As the amount of FeCl3 added increases, the water vapor transmission rate first decreases and then increases. When the amount of FeCl3 added is 5 wt%, the water vapor transmission rate of the composite film is the lowest, at 3.48 × 10⁻⁶. -5 ·g·m -1 ·s -1 ·Pa -1 This is due to Fe 3+ The bridging effect promotes the formation of a denser network structure between LCNF and the TPS / PBAT matrix, reduces the free volume inside the material, and lengthens the diffusion path of water molecules, thereby effectively improving water-blocking performance. However, when Fe... 3+ When an excessive amount is added, the barrier performance improvement effect tends to stabilize or even slightly decreases due to the occurrence of local aggregation.

[0064] The mass fraction composition of the TPS / PBAT / Fe-LCNF composite films of Examples 18 to 20 is shown in Table 6. The composite films of Examples 18 to 20 are respectively represented by the numbers F1, F2, and F3, and single-factor experiments were conducted.

[0065] Table 6 Serial Number serial number starch PBAT Fe-LCNF glycerin NaOH lubricant stabilizer Example 18 F1 100 100 4 20 5 1 3 Example 19 F2 100 100 4 20 10 1 3 Example 20 F3 100 100 4 20 20 1 3 The preparation methods of the composite films in Examples 18 to 20 are basically the same as those in Example 4, except that in step 1) of Examples 18 to 20, the concentrations of NaOH are 5 wt%, 10 wt%, and 20 wt%, respectively, to prepare the TPS / PBAT / Fe-LCNF composite films of Examples 18 to 20.

[0066] For the composite films of Examples 18-20, tensile test samples were prepared using a cutting tool. The mechanical properties of the composite films of Examples 18-20 were tested in groups according to the method of national standard GB / T1040.1-2018. The tensile test samples were dumbbell-shaped specimens, 50 mm in length and 4 mm in width at the center. The tensile speed was 10 mm / min, and at least 5 specimens were tested in each group. The average tensile strength and elongation at break of the samples were taken. The results are as follows: Figure 8 As shown.

[0067] from Figure 8 As can be seen, Fe-LCNF prepared by different alkali treatments can improve the mechanical properties of TPS / PBAT composite films. However, with the increase of NaOH treatment concentration, the tensile strength and elongation at break of the composite film show a trend of first increasing and then decreasing. Among them, Fe-LCNF prepared by treatment with 10 wt% NaOH has the most significant reinforcing effect, with a tensile strength of 19.67 MPa and an elongation at break of 1145%. The reason is that moderate alkali treatment can partially remove lignin and hemicellulose, increase the exposure of cellulose microfibrils, and at the same time retain an appropriate amount of lignin structure, so that Fe-LCNF has both hydrophilic and hydrophobic characteristics. 3+ Under the influence of pre-coordination, Fe 3+ It can form stable coordination structures with phenolic hydroxyl, hydroxyl, and carboxyl groups on the LCNF surface, and further dynamically coordinate with hydroxyl groups in the TPS matrix, thereby constructing a continuous and stable interfacial reinforcement network. This network structure can effectively transfer external stress, inhibit interfacial debonding and crack propagation, and thus improve the tensile strength of the composite film. When the NaOH treatment concentration continues to increase, excessive lignin removal leads to a weakening of the amphiphilic characteristics of LCNF and a decrease in interfacial control ability, thus reducing the mechanical properties of the composite material.

[0068] According to GB / T 1037-2021 standard, the water vapor transmission rate of the composite films in Examples 18 to 20 was tested. Figure 9 As the NaOH treatment concentration increased, the water vapor transmission rate first decreased and then increased. When the NaOH treatment concentration was 10 wt%, the composite film exhibited the lowest water vapor transmission rate, which was 3.35 × 10⁻⁶. -5 ·g·m -1 ·s -1 ·Pa -1 This is because moderate alkali treatment can partially remove lignin and hemicellulose from the raw material, fully exposing the cellulose microfibrils, while retaining an appropriate amount of lignin components, allowing Fe... 3+Fe-LCNF can form metal coordination bridges with the phenolic and hydroxyl groups on the LCNF surface, effectively improving the interfacial bonding between Fe-LCNF and the TPS / PBAT phases and reducing internal matrix defects. Uniformly dispersed Fe-LCNF constructs a labyrinthine barrier structure within the matrix, extending the water molecule diffusion path, reducing the matrix's free volume, and minimizing the composite film's water vapor permeability. However, when the NaOH concentration is too high, a large amount of lignin is removed, significantly weakening the amphiphilic interface control ability of LCNF, decreasing the compatibility between the filler and the matrix interface, and causing the regeneration of micro-gaps within the material. This disrupts the original dense barrier network structure, reducing water vapor diffusion resistance and ultimately causing the composite film's water vapor permeability to rebound. Furthermore, excessively high alkali concentrations also pose environmental problems, lacking environmental friendliness.

[0069] For the composite films of Comparative Example 2, Example 1, Example 4, Example 7, Example 18, and Example 20, the thermal properties of the films were tested using a thermogravimetric analyzer. The tests were conducted under a nitrogen atmosphere at a flow rate of 20 mL / min, with a temperature range of 25–600 °C and a heating rate of 10 °C / min. Differential scanning calorimetry (DSC) was used to evaluate the thermal transition, heating from 30 °C to 250 °C at a heating rate of 10 °C / min under a nitrogen atmosphere. The test results are as follows: Figure 10 As shown in (ab). The results show that all samples exhibit a typical multi-stage thermal degradation process. A small amount of weight loss occurs before 100℃, mainly due to the evaporation of adsorbed and bound water in the material; the second stage of weight loss corresponds mainly to the decomposition of glycerol and some low-molecular-weight components; when the temperature exceeds 300℃, the TPS and PBAT matrix undergo large-scale thermal decomposition, and the material mass rapidly decreases. With increasing Fe-LCNF content, the thermal decomposition initiation temperature of the composite material gradually increases. Among them, the material exhibits the highest thermal stability when the Fe-LCNF content is 4 parts. This is mainly attributed to Fe... 3+ Pre-coordinated Fe-LCNF formed a stable three-dimensional network structure in the TPS / PBAT matrix. On the one hand, LCNF itself possesses high thermal stability; on the other hand, Fe... 3+ Fe-LCNF forms coordination structures with the phenolic hydroxyl, hydroxyl, and carboxyl groups on the LCNF surface, further improving the interfacial bonding strength and restricting polymer chain segment movement, thereby delaying the thermal decomposition process. When the amount of Fe-LCNF added continues to increase to 7 parts, although the thermal stability is still better than the sample without Fe-LCNF, the improvement in thermal stability tends to plateau due to the decrease in network structure uniformity caused by the occurrence of local agglomeration. Therefore, an appropriate amount of Fe... 3+ Pre-coordinated LCNF can significantly improve the heat resistance of TPS / PBAT composites. For example... Figure 10As shown in (cd), X-ray diffraction calculations indicate a reduction in overall crystallite size. This is because the dense and interpenetrating LCNF network exerts a spatial confinement effect, restricting the mobility of PBAT molecular chains and hindering the diffusion of chain segments towards the crystal growth front. Therefore, the growth of large, perfect spherulites is suppressed, resulting in the formation of numerous smaller, imperfect crystals. This grain refinement is structurally beneficial because it creates a more uniform crystal morphology with a higher density of connecting molecules linking crystalline and amorphous regions.

[0070] The ultraviolet (UV) blocking performance of the composite films from Comparative Example 2, Example 1, Example 4, Example 7, Example 18, and Example 20 was tested. Figure 11 It can be seen that with the increase of Fe-LCNF addition, the transmittance of the composite material to ultraviolet light gradually decreases, while the ultraviolet blocking performance is significantly improved. Among them, the material exhibits the best ultraviolet shielding effect when the Fe-LCNF addition is 4 parts. This is because the lignin structure retained in Fe-LCNF contains a large number of aromatic rings and conjugated chromophores, which can effectively absorb ultraviolet light. Meanwhile, Fe... 3+ After forming a coordination structure with the phenolic hydroxyl groups in lignin, Fe-LCNF can further enhance ultraviolet light absorption and improve light energy dissipation efficiency. Furthermore, the uniformly dispersed Fe-LCNF network structure increases the scattering and reflection paths of ultraviolet light within the material, thereby further reducing ultraviolet light transmittance. When the Fe-LCNF content increases to 7 parts, the aggregation of some nanofibers leads to a decrease in the uniformity of the internal structure of the material, and the formation of light transmission channels in some areas weakens the improvement in ultraviolet blocking performance. Therefore, an appropriate amount of Fe... 3+ Pre-coordinated LCNF can not only enhance the mechanical properties and thermal stability of TPS / PBAT composites, but also significantly improve their UV barrier properties, which is beneficial for their application in food packaging and agricultural films.

[0071] The mass fraction composition of the TPS / PBAT / Fe-LCNF composite films of Examples 21 and 22 is shown in Table 7. The composite films of Examples 21 and 22 are respectively represented by the numbers G1 and G2, and single-factor experiments were conducted.

[0072] Table 7 Serial Number serial number starch PBAT Fe-LCNF glycerin <![CDATA[Fe 3+ ]]> lubricant stabilizer Example 21 G1 100 100 4 20 <![CDATA[Fe(NO3)3]]> 1 3 Example 22 G2 100 100 4 20 <![CDATA[Fe2(SO4)3]]> 1 3 The preparation methods of the composite films in Examples 21 and 22 are basically the same as those in Example 4, except that in step 1) of Examples 21 and 22, the Fe-containing films used are... 3+The solutions were Fe(NO3)3 and Fe2(SO4)3, with Fe(NO3)3 added at 7.5 wt% of the LCNF mass and Fe2(SO4)3 added at 6.2 wt% of the LCNF mass. TPS / PBAT / Fe-LCNF composite films of Examples 21 and 22 were prepared accordingly.

[0073] For the composite films of Examples 21 and 22, tensile test samples were prepared using a cutting tool. The mechanical properties of the composite films of Examples 21 and 22 were tested in groups according to the method of national standard GB / T1040.1-2018. The tensile test samples were dumbbell-shaped specimens, 50 mm in length and 4 mm in width at the center. The tensile speed was 10 mm / min, and at least 5 specimens were tested in each group. The average tensile strength and elongation at break of the samples were taken. The results are as follows: Figure 12 As shown.

[0074] from Figure 12 As can be seen, the tensile strengths of the three composite films, G1, G2, and C4, are 19.11 MPa, 20.45 MPa, and 19.34 MPa, respectively. This is because SO4... 2- As a high-valence anion, although it competes for coordination sites to a small extent, it can enhance the intermolecular cohesion of the matrix. Combined with the uniformly dispersed Fe-LCNF rigid fiber skeleton, it has the highest load transfer efficiency and the best tensile strength. Cl- coordination competition is weak, the system has a complete metal-bridged coordination network, and the tensile strength is slightly lower than that of ferric sulfate. Nitrate ions have slight coordination competition, reducing the number of effective crosslinking sites and decreasing the interfacial bonding strength between the two phases, so the tensile strength is the lowest of the three. The elongation at break of the three composite films of G1, G2, and C4 are 1209%, 1009%, and 1109%, respectively. This is because nitrate ions have the weakest coordination competition for hydroxyl groups, and the system can form a large number of reversible dynamic coordination bonds. During the stretching process, the coordination bonds continuously dissociate and recombine, continuously dissipating external forces, and the macromolecular chains can fully slide and stretch, resulting in the best film extensibility. Chloride ions bring a weakly acidic environment, slightly restricting chain segment movement. The dynamic stress dissipation structure is less than that of the ferric nitrate system, resulting in a moderate elongation at break. Sulfate ions have strong competition, grabbing a large amount of Fe. 3+ The active sites and reversible coordination network are sparse, lacking effective energy buffer channels. Under stress, cracks propagate rapidly, and the film is prone to premature brittle fracture, exhibiting the worst toughness.

[0075] According to GB / T 1037-2021 standard, the water vapor transmission rate of the composite films in Examples 21 and 22 was tested. Figure 13 The water vapor transmission rates of the three composite films, G1, G2, and C4, were 3.88 × 10⁻⁶. -5 ·g·m -1 ·s -1 ·Pa-1 3.77×10 -5 ·g·m -1 ·s -1 ·Pa -1 3.89×10 -5 ·g·m -1 ·s -1 ·Pa -1 This is because the Fe2(SO4)3 system has stronger intermolecular forces, forming a dense labyrinth barrier structure with uniformly distributed Fe-LCNF, which significantly extends the diffusion path of water molecules and has the greatest resistance to water vapor permeation. The coordination network constructed by Fe(NO3)3 is less dense, with more free volume inside the film, resulting in slightly poorer barrier performance. The cross-linking density of FeCl3 modified film is not as high as the former two, with more micro-permeation channels in the matrix, resulting in the highest water vapor permeability and weaker water vapor barrier effect than Fe2(SO4)3 and Fe(NO3)3.

[0076] The mass fraction composition of the TPS / PBAT / Fe-LCNF composite films of Examples 23 to 25 is shown in Table 8. The composite films of Examples 23 to 25 are respectively represented by the numbers H1, H2, and H3, and single-factor experiments were conducted.

[0077] Table 8 Serial Number serial number starch PBAT Fe-LCNF glycerin <![CDATA[FeCl3]]> lubricant stabilizer Example 23 H1 100 100 4 10 1 1 3 Example 24 H2 100 100 4 20 1 1 3 Example 25 H3 100 100 4 30 1 1 3 The preparation methods of the composite films in Examples 23 to 25 are basically the same as those in Example 4, except that in step 3) of Examples 23 to 25, the amount of glycerol is 10, 20 and 30 respectively, and the TPS / PBAT / Fe-LCNF composite films of Examples 23 to 25 are prepared respectively.

[0078] For the composite films of Examples 23-25, tensile test samples were prepared using a cutting tool. The mechanical properties of the composite films of Examples 23-25 ​​were tested in groups according to the method of national standard GB / T1040.1-2018. The tensile test samples were dumbbell-shaped specimens, 50 mm in length and 4 mm in width at the center. The tensile speed was 10 mm / min, and at least 5 specimens were tested in each group. The average tensile strength and elongation at break of the samples were taken. The results are as follows: Figure 14 As shown.

[0079] from Figure 14As can be seen, the tensile strength of the TPS / PBAT composite film first increases and then decreases with increasing glycerol content. When the glycerol content is low, insufficient plasticization occurs, resulting in unmelted starch particles and interfacial defects, limiting load transfer in the coordination network and leading to low tensile strength. At 20 parts glycerol, the starch is sufficiently plasticized, the interface between the two phases is improved, and the fiber and coordination network work together to bear the load, achieving a peak strength of 20.45 MPa. Excessive glycerol dilutes the rigid framework, weakens coordination crosslinking, and generates vacuole defects, thus reducing tensile strength. With increasing glycerol content, the elongation at break of the TPS / PBAT composite film gradually increases to 1045%. This is because glycerol contains a large number of hydroxyl groups, which can form hydrogen bonds with starch and lignocellulose nanofibers, replacing the intermolecular hydrogen bonds in starch molecules, expanding the free volume of the molecular chains, lowering the glass transition temperature, enhancing chain segment slippage ability, and increasing the elongation at break of the composite film.

[0080] According to GB / T 1037-2021 standard, the water vapor transmission rate of the composite films in Examples 23 to 25 was tested. Figure 15 As the amount of glycerol added increases, the water vapor transmission rate first decreases and then increases. When the amount of glycerol added is 20 parts, the water vapor transmission rate of the composite film is the lowest, at 3.23 × 10⁻⁶. -5 ·g·m -1 ·s -1 ·Pa -1 This is because when the amount of glycerol is too low, the starch is not fully plasticized, resulting in aggregated particles and interfacial gaps inside the matrix. The hydrophilic starch forms continuous water-permeable channels, making it easy for water vapor to diffuse. An appropriate amount of glycerol can fully plasticize the starch, making the hydrophilic phase evenly dispersed. Combined with Fe-LCNF, it forms a labyrinth barrier structure, increasing the density of the film and increasing the resistance to water vapor diffusion. When glycerol is excessive, a large amount of hydrophilic free glycerol increases the overall hydrophilicity of the material. At the same time, it expands the molecular chains, increases the free volume of the matrix, and forms more water vapor permeation channels, resulting in a decrease in barrier performance.

Claims

1. A Fe 3+ The pre-coated lignocellulose nanofiber reinforced and toughened TPS / PBAT fully biodegradable composite film is characterized by, The mass fraction of the film is composed of starch 100 parts, PBAT 80~150 parts, Fe 3+ The coordination modified lignin nanocellulose (Fe-LCNF) 1~8 parts, glycerol 10~30 parts, lubricant 1~3 parts, stabilizer 1~3 parts, and the Fe 3+ The pre-coordination lignin nanocellulose meets the following conditions: (1) Fe 3+ forms a coordination structure with the hydroxyl group on the surface of the LCNF (2) The LCNF has a network structure or a branched multidimensional structure, with a single fiber diameter of 5~100 nm, a length of 0.5~20 mm, and a lignin content of 5~20 wt%.

2. The Fe according to claim 1 3+ The pre-coordinated lignocellulose nanofiber reinforced and toughened TPS / PBAT fully biodegradable composite film is characterized by: The Fe 3+ derived from at least one of FeCl3, Fe(NO3)3, Fe2(SO4)3.

3. The Fe according to claim 1 3+ The pre-coordinated lignocellulose nanofiber reinforced and toughened TPS / PBAT fully biodegradable composite film is characterized by: The LCNF is derived from at least one of wood flour, bamboo flour, corn stalks, wheat stalks, rice stalks, and sugarcane bagasse, with a particle size of 40-200 mesh.

4. The Fe according to claim 1 3+ The pre-coated lignocellulose nanofiber reinforced and toughened TPS / PBAT fully biodegradable composite film is characterized by, The starch is one or a combination of two or more of the following: corn starch, tapioca starch, pea starch, potato starch, wheat starch, sweet potato starch, and lotus root starch.

5. The Fe according to claim 1 3+ The pre-coated lignocellulose nanofiber reinforced and toughened TPS / PBAT fully biodegradable composite film is characterized by, The stabilizer is one or a combination of two or more of antioxidants 1010, 168, 1076, and 1790.

6. The Fe according to claim 1 3+ The pre-coordinated lignocellulose nanofiber reinforced and toughened TPS / PBAT fully biodegradable composite film is characterized by: The Fe 3+ The ratio of the addition amount to the LCNF is 0.031 mol: 100 g, which corresponds to an FeCl3 addition amount of 5 wt% of the mass of the LCNF, an Fe(NO3)3 addition amount of 7.5 wt% of the mass of the LCNF, and an Fe2(SO4)3 addition amount of 6.2 wt% of the mass of the LCNF.

7. The Fe according to claim 1 3+ The pre-coordinated lignocellulose nanofiber reinforced and toughened TPS / PBAT fully biodegradable composite film is characterized by: The Fe-LCNF forms a synergistic enhancement structure of nanofiber framework-metal ion bridging-dynamic coordination network in the TPS / PBAT matrix.

8. The Fe according to claim 1 3+ The pre-coordinated lignocellulose nanofiber reinforced and toughened TPS / PBAT fully biodegradable composite film is characterized by: The thickness of the film is 0.03~0.5 mm.

9. A method for preparing Fe as described in any one of claims 1 to 8 3+ A method for preparing a pre-coordinated lignocellulose nanofiber reinforced and toughened TPS / PBAT fully biodegradable composite film, characterized in that, Includes the following steps: 1) Take 5-10 parts of straw raw material and place it in 70-80 parts of a 5-20 wt% sodium hydroxide solution. Treat it at 70-80℃ for 5-6 h to partially remove lignin and hemicellulose. After treatment, wash it repeatedly with pure water until neutral and dry it. Prepare a 10 wt% solution from the obtained powder and perform wet ball milling. The ball milling conditions are: rotation speed 400-600 rpm, ball-to-material ratio 18-20:1, and ball milling time 7-10 h. After ball milling, an LCNF suspension is obtained. 2) Dilute the LCNF suspension obtained in 1) to a mass concentration of 1 wt%, and ultrasonically disperse it for 15-30 min to disperse the fibers. Then prepare a 0.05 mol / L FeCl3, Fe(NO3)3, or Fe2(SO4)3 solution. At 40℃, place the Fe... 3+ The solution was slowly added dropwise to the LCNF suspension, allowing Fe to... 3+ The ratio of FeCl3 to LCNF was 0.031 mol: 100 g (corresponding to 5 wt% FeCl3, 7.5 wt% Fe(NO3)3, and 6.2 wt% Fe2(SO4)3 of LCNF). The reaction was continuously magnetically stirred for 2–3 h, allowing Fe to... 3+ It reacts with LCNF to form Fe 3+ Coordination binding; after the reaction, wash three times with pure water to remove unreacted Fe. 3+ Ions, the resulting product was freeze-dried to obtain Fe 3+ Coordinated LCNF (Fe-LCNF) powder; 3) Mix 100 parts of starch with 20-30 parts of glycerol and stir for 30-60 min to obtain a pre-plasticized starch system. Then, melt-plasticize and granulate the system in a twin-screw extruder at an extrusion temperature of 90-120℃ and a screw speed of 80-150 rpm to obtain TPS granules. 4) The 100 parts of TPS particles obtained in step 3) are premixed with 1-8 parts of Fe-LCNF powder, 80-150 parts of PBAT particles, 1-3 parts of lubricant, and 1-3 parts of stabilizer at high speed for 15-30 min. Then, the mixture is put into a twin-screw extruder for melt blending and granulation. The extrusion temperature is 90-130℃ and the screw speed is 80-150 rpm. 5) The composite particles obtained in step 4) are processed into thin films by hot pressing, blown film blowing, or casting to obtain Fe. 3+ TPS / PBAT composite films synergistically reinforced with LCNF, with film thicknesses of 0.03~0.5 mm.