A high-resilience low-damping billiard table rubber edge and a preparation method thereof

By combining the A-section compound rubber with the B-section vulcanizing material, the problem of inconsistent rebound of the billiard table rubber edge after repeated impacts is solved, achieving a high initial rebound rate and good cycle retention capability, which is suitable for existing production equipment.

CN123152182APending Publication Date: 2026-11-24FOSHAN MEIRUN RUBBER TECH DEV CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611244071.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-17
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

The existing pool table rubber edges exhibit inconsistent rebound after repeated impacts, making it difficult to balance initial rebound rate, tensile performance, and rebound retention after cyclic impacts.

Method used

The combination of A-section compound rubber and B-section vulcanizing material, including No. 3 smoke rubber, carbon black N774, naphthenic oil, zinc oxide, antioxidant, etc., is used to form a high-resilience and low-fading billiard table rubber edge through specific mixing, rubber turning and vulcanization processes.

Benefits of technology

It achieves a high initial rebound rate and good rebound retention after cyclic impact, balancing hardness and elasticity, and is compatible with existing production equipment without the need for new equipment development.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123152182A_ABST
    Figure CN123152182A_ABST
Patent Text Reader

Abstract

This invention discloses a high-resilience, low-attenuation billiard table edge and its preparation method. The edge uses No. 3 smoked rubber, N774 carbon black, naphthenic oil, 99.7% zinc oxide, SA1801 stearic acid, antioxidant RD, antioxidant 4010NA, rubber binder, and Modified 935P as the A-stage compound, and sulfur IS-60, accelerator DM, accelerator D, and accelerator CZ as the B-stage vulcanizing agent. The resulting edge has a high initial rebound rate, balancing the required hardness and elasticity for billiard table edges. It exhibits good rebound retention after cyclic impact and good tensile properties, capable of withstanding tensile and compressive deformation during installation and repeated impacts. Furthermore, the formulation has good coordination, using natural rubber, low amounts of N774 carbon black, low amounts of naphthenic oil, a composite stabilizing system, and a composite vulcanizing system. This avoids performance imbalances caused by simply increasing fillers, softeners, or the degree of vulcanization. The equipment used in the production process is conventional, requiring no additional development of new equipment and adapting to existing production equipment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of rubber materials technology, and in particular to a high-resilience, low-attenuation billiard table rubber edge and its preparation method. Background Technology

[0002] The rubber edge of a billiard table is a key elastic component installed at the edge of the table, affecting the rebound speed, rebound angle, and rebound consistency of the ball after impact.

[0003] The rubber edges of a billiard table need to possess suitable hardness, high rebound rate, sufficient tensile strength, and good deformation recovery ability. In addition to initial rebound performance, the rubber edges should also maintain stable rebound after repeated impacts; otherwise, inconsistent rebound effects may occur at different stages of use.

[0004] Natural rubber possesses good elasticity, but the reinforcement, softening, and vulcanization levels in the edge formulation are mutually restrictive: excessive carbon black content may make the edge too hard and reduce resilience, excessive softener content may weaken strength and cycle retention, and inappropriate vulcanization level may result in insufficient strength or decreased dynamic performance. Therefore, comprehensive performance cannot be obtained by simply adding one material.

[0005] Existing rubber edge formulations and testing methods typically focus on initial hardness, initial rebound rate, and tensile properties, while paying insufficient attention to rebound changes after multiple impacts. Therefore, there is a need for a billiard table rubber edge material with a clearly defined composition and process, capable of stable compression molding, and which balances initial rebound, tensile properties, and rebound retention after cyclic impacts at an appropriate hardness. Summary of the Invention

[0006] To address the shortcomings of existing technologies, the present invention aims to provide a high-resilience, low-attenuation billiard table edge with superior performance that is compatible with existing production equipment, as well as a method for its preparation.

[0007] To achieve the above objectives, the present invention provides a high-resilience, low-fading billiard table rubber edge, comprising a mixture of A-section compound rubber and B-section vulcanizing material. The A-section compound rubber comprises the following parts by weight: 90-110 parts of 3# smoked rubber; 15-25 parts of carbon black N774; 4-6 parts of naphthenic oil; 4-6 parts of 99.7% zinc oxide; 0.5-1.5 parts of stearic acid SA1801; 1-3 parts of antioxidant RD; 2-3 parts of antioxidant 4010NA; 1-3 parts of adhesive sizing agent; and 1-3 parts of Modified 935P. The B-section vulcanizing material is in the following mass proportions: sulfur IS-60 1.5-2 parts; accelerator DM 0.5-1 part; accelerator D 0.1-0.3 parts; accelerator CZ 0.5-1.5 parts.

[0008] Further, the A-section compound is prepared in the following proportions by weight: 100 parts of No. 3 smoked rubber; 20 parts of carbon black N774; 5 parts of naphthenic oil; 5 parts of 99.7% zinc oxide; 1 part of stearic acid SA1801; 2 parts of antioxidant RD; 2.5 parts of antioxidant 4010NA; 2 parts of rubber binder; and 2 parts of Modeli 935P.

[0009] Further, the B-section vulcanizing material is in the following mass proportions: 1.8 parts of sulfur IS-60; 0.8 parts of accelerator DM; 0.2 parts of accelerator D; and 1.0 part of accelerator CZ.

[0010] This invention also includes a method for preparing high-resilience, low-fading billiard table rubber edges, comprising the following steps: S1. Weigh out the following components by weight: No. 3 smoked rubber, carbon black N774, naphthenic oil, 99.7% zinc oxide, stearic acid SA1801, antioxidant RD, antioxidant 4010NA, rubber binder, and molded rubber 935P. Then, put No. 3 smoked rubber into a mixer and add carbon black N774, naphthenic oil, 99.7% zinc oxide, stearic acid SA1801, antioxidant RD, antioxidant 4010NA, rubber binder, and molded rubber 935P. Mix until the rubber temperature reaches 125℃, then discharge the rubber to form section A. The mixing time is 600-840s. S2. Cool and let stand the A-section compound obtained in step S1, and then put the A-section compound into the open mill for turning, wherein the open milling time is 220-260s; S3. Weigh out sulfur IS-60, accelerator DM, accelerator D, and accelerator CZ by mass percentage, then add them to the open mill for powdering. After powdering, turn the mixture until it is evenly mixed and forms a rubber compound. The powdering time is 4-5 minutes, and the turning time is 5-6 minutes. S4. The rubber material from step S3 is processed by a two-roll mill, then cut and weighed in sequence to form a rubber blank, and then the rubber blank is placed into a multi-cavity mold. S5. Place the mold containing the rubber material from step S4 into a vulcanizing machine for vulcanization. The mold closing pressure is set to 110-130 bar, the air is vented 3 times during vulcanization, the temperature of the upper and lower mold plates is set to 160℃, and the vulcanization time is 850-950 s. S6. After vulcanization, open the mold and remove the rubber edge. Then, cool, trim, shape, and inspect the appearance in sequence to obtain a high-resilience, low-attenuation billiard table rubber edge.

[0011] Furthermore, in step S1, the mixing time is 720s.

[0012] Furthermore, in step S4, the weight of a single plastic blank is 540±20g, and 30 plastic blanks are placed in each mold.

[0013] Furthermore, in step S5, the vulcanizing machine is a 1200T flat vulcanizing machine.

[0014] Furthermore, in step S3, production pigments are fed into the open mill, and then the pigments are absorbed. After the pigment absorption is completed, the mixture is turned over until it is evenly mixed and the color of the rubber compound is uniform.

[0015] The beneficial effects of this invention are as follows: It exhibits a high initial rebound rate and excellent rebound retention after cyclic impact. The rubber edge is manufactured using No. 3 smoked rubber, N774 carbon black, naphthenic oil, 99.7% zinc oxide, SA1801 stearic acid, antioxidant RD, antioxidant 4010NA, rubber binder, and Modified 935P as the A-stage compound, and sulfur IS-60, accelerator DM, accelerator D, and accelerator CZ as the B-stage vulcanizing agent. This results in a rubber edge with a high initial rebound rate, balancing the hardness and elasticity required for billiard table edges. It also demonstrates excellent rebound retention after cyclic impact and good tensile properties, capable of withstanding tensile and compressive deformation during installation and repeated impacts. Furthermore, the formulation exhibits good coordination, employing natural rubber, low-dosage N774 carbon black, low-dosage naphthenic oil, a composite stabilizing system, and a composite vulcanizing system. This avoids performance imbalances caused by simply increasing fillers, softeners, or the degree of vulcanization. The equipment used in the production process is all conventional, eliminating the need for additional equipment development and adapting to existing production equipment. Attached Figure Description

[0016] Figure 1 This is a curve showing the change in the elasticity of the adhesive edge according to the present invention. Detailed Implementation

[0017] The technical solution of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are some embodiments of the present invention, but not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0018] In the description of this invention, it should be noted that the terms "center," "upper," "lower," "left," "right," "vertical," "horizontal," "inner," and "outer," etc., indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings. They are used only for the convenience of describing the invention and for simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation. Therefore, they should not be construed as limitations on the invention. Furthermore, the terms "first," "second," and "third" are used for descriptive purposes only and should not be construed as indicating or implying relative importance. Example 1:

[0019] A high-resilience, low-fading billiard table rubber edge and its preparation method are disclosed, comprising mixing a section A compound rubber with a section B vulcanizing agent. The section A compound rubber is prepared in the following mass proportions: 90 parts of No. 3 smoked rubber; 15 parts of carbon black N774; 4 parts of naphthenic oil; 4 parts of 99.7% zinc oxide; 0.5 parts of stearic acid SA1801; 1 part of antioxidant RD; 2 parts of antioxidant 4010NA; 1 part of rubber sizing agent; and 1 part of Modified 935P.

[0020] The B-section vulcanizing material is in the following parts by weight: 1.5 parts of sulfur IS-60; 0.5 parts of accelerator DM; 0.1 parts of accelerator D; and 0.5 parts of accelerator CZ.

[0021] This embodiment also includes a method for preparing high-resilience, low-attenuation billiard table rubber edges, comprising the following steps: S1. Weigh out the following components by weight: #3 smoked rubber, carbon black N774, naphthenic oil, 99.7% zinc oxide, stearic acid SA1801, antioxidant RD, antioxidant 4010NA, rubber binder, and molded rubber 935P. Then, put the #3 smoked rubber into a mixer and add carbon black N774, naphthenic oil, 99.7% zinc oxide, stearic acid SA1801, antioxidant RD, antioxidant 4010NA, rubber binder, and molded rubber 935P. Mix until the rubber temperature reaches 125℃, then discharge the rubber to form section A. The mixing time is 600s.

[0022] S2. Cool and let stand the A-section compound obtained in step S1, and then put the A-section compound into a two-roll mill for turning, wherein the two-roll mill time is 220-260s.

[0023] S3. Weigh out sulfur IS-60, accelerator DM, accelerator D, and accelerator CZ by mass percentage, then add them to the open mill for powdering. After powdering, turn the mixture until it is evenly mixed and forms a rubber compound. The powdering time is 4-5 minutes, and the turning time is 5-6 minutes.

[0024] S4. The rubber material from step S3 is processed by an open mill, then cut and weighed sequentially to form rubber blanks, and then the rubber blanks are placed into a multi-cavity mold; wherein, the weight of a single rubber blank is 540±20g, and 30 rubber blanks are placed in each mold.

[0025] S5. Place the mold containing the rubber material from step S4 into a vulcanizing machine for vulcanization. The mold closing pressure is set to 110-130 bar, the air is vented 3 times during vulcanization, the temperature of the upper and lower plates of the mold is set to 160℃, and the vulcanization time is 850-950s. The vulcanizing machine is a 1200T flat vulcanizing machine.

[0026] S6. After vulcanization, open the mold and remove the rubber edge. Then, cool, trim, shape, and inspect the appearance in sequence to obtain a high-resilience, low-attenuation billiard table rubber edge. Example 2:

[0027] A high-resilience, low-fading billiard table rubber edge and its preparation method are disclosed. The rubber edge is prepared by mixing a section A compound rubber with a section B vulcanizing agent. The section A compound rubber is prepared in the following proportions by weight: 110 parts of No. 3 smoked rubber; 25 parts of carbon black N774; 6 parts of naphthenic oil; 6 parts of 99.7% zinc oxide; 1.5 parts of stearic acid SA1801; 3 parts of antioxidant RD; 3 parts of antioxidant 4010NA; 3 parts of rubber binder; and 3 parts of Modified 935P.

[0028] The B-section vulcanizing material is in the following mass proportions: 2 parts of sulfur IS-60; 1 part of accelerator DM; 0.3 parts of accelerator D; and 1.5 parts of accelerator CZ.

[0029] This embodiment also includes a method for preparing high-resilience, low-attenuation billiard table rubber edges, comprising the following steps: S1. Weigh out the following components by weight: No. 3 smoked rubber, carbon black N774, naphthenic oil, 99.7% zinc oxide, stearic acid SA1801, antioxidant RD, antioxidant 4010NA, rubber binder, and Moldex 935P. Then, put No. 3 smoked rubber into a mixer and add carbon black N774, naphthenic oil, 99.7% zinc oxide, stearic acid SA1801, antioxidant RD, antioxidant 4010NA, rubber binder, and Moldex 935P. Mix until the rubber temperature reaches 125℃, then discharge the rubber to form section A. The mixing time is 600-840s.

[0030] S2. Cool and let stand the A-section compound obtained in step S1, and then put the A-section compound into a two-roll mill for turning, wherein the two-roll mill time is 220-260s.

[0031] S3. Weigh out sulfur IS-60, accelerator DM, accelerator D, and accelerator CZ by mass percentage, then add them to the open mill for powdering. After powdering, turn the mixture until it is evenly mixed and forms a rubber compound. The powdering time is 4-5 minutes, and the turning time is 5-6 minutes.

[0032] S4. The rubber material from step S3 is processed by an open mill, then cut and weighed sequentially to form rubber blanks, and then the rubber blanks are placed into a multi-cavity mold; wherein, the weight of a single rubber blank is 540±20g, and 30 rubber blanks are placed in each mold.

[0033] S5. Place the mold containing the rubber material from step S4 into a vulcanizing machine for vulcanization. The mold closing pressure is set to 110-130 bar, the air is vented 3 times during vulcanization, the temperature of the upper and lower plates of the mold is set to 160℃, and the vulcanization time is 850-950s. The vulcanizing machine is a 1200T flat vulcanizing machine.

[0034] S6. After vulcanization, open the mold and remove the rubber edge. Then, cool, trim, shape, and inspect the appearance in sequence to obtain a high-resilience, low-attenuation billiard table rubber edge. Example 3:

[0035] This embodiment is a preferred embodiment, a high-resilience, low-attenuation billiard table rubber edge and its preparation method, comprising mixing A-section compound rubber and B-section vulcanizing material. The A-section compound rubber is prepared in the following mass parts: 100 parts of 3# smoked rubber; 20 parts of carbon black N774; 5 parts of naphthenic oil; 5 parts of 99.7% zinc oxide; 1 part of stearic acid SA1801; 2 parts of antioxidant RD; 2.5 parts of antioxidant 4010NA; 2 parts of rubber sizing agent; and 2 parts of Modified 935P.

[0036] The B-section vulcanizing material is in the following parts by weight: 1.8 parts of sulfur IS-60; 0.8 parts of accelerator DM; 0.2 parts of accelerator D; and 1.0 part of accelerator CZ.

[0037] This embodiment also includes a method for preparing high-resilience, low-attenuation billiard table rubber edges, comprising the following steps: S1. Weigh out the following components by weight: No. 3 smoked rubber, carbon black N774, naphthenic oil, 99.7% zinc oxide, stearic acid SA1801, antioxidant RD, antioxidant 4010NA, rubber binder, and Moldex 935P. Then, put No. 3 smoked rubber into a mixer and add carbon black N774, naphthenic oil, 99.7% zinc oxide, stearic acid SA1801, antioxidant RD, antioxidant 4010NA, rubber binder, and Moldex 935P. Mix until the rubber temperature reaches 125℃, then discharge the rubber to form section A. The mixing time is 600-840s.

[0038] S2. Cool and let stand the A-section compound obtained in step S1, and then put the A-section compound into a two-roll mill for turning, wherein the two-roll mill time is 220-260s.

[0039] S3. Weigh out sulfur IS-60, accelerator DM, accelerator D, and accelerator CZ by mass percentage. Then, add sulfur IS-60, accelerator DM, accelerator D, accelerator CZ, and production pigment to the open mill for powdering. After powdering, turn the mixture until it is evenly mixed and the rubber compound is uniform in color, forming a rubber compound. The powdering time is 4-5 minutes, and the turning time is 5-6 minutes.

[0040] S4. Cut and weigh the rubber material from step S3 in sequence to form a rubber blank, and then place the rubber blank into the mold; wherein, the weight of a single rubber blank is 540±20g, and 30 rubber blanks are placed in each mold.

[0041] S5. Place the mold containing the rubber material from step S4 into a vulcanizing machine for vulcanization. The mold closing pressure is set to 110-130 bar, the air is vented 3 times during vulcanization, the temperature of the upper and lower plates of the mold is set to 160℃, and the vulcanization time is 850-950s. The vulcanizing machine is a 1200T flat vulcanizing machine.

[0042] S6. After vulcanization, open the mold and remove the rubber edge. Then, cool, trim, shape, and inspect the appearance in sequence to obtain a high-resilience, low-attenuation billiard table rubber edge.

[0043] In this embodiment, fillers, softeners, activators, stabilizers and processing aids may be added to the A-section compound rubber, and vulcanizing agents and composite accelerators may be added to the B-section vulcanizing material. The billiard table rubber edge is then obtained through material preparation, molding, venting and pressure vulcanization.

[0044] This embodiment uses natural rubber as the matrix, with 100 parts of No. 3 smoked rubber as the single main elastic matrix. Natural rubber has cis-1,4-polyisoprene as its main structure, with regular molecular chains and good flexibility. It can recover quickly after being subjected to instantaneous compression, making it suitable for the characteristics of billiard table edges that withstand short-term, high-frequency, and repeated impacts. Natural rubber also has strain-induced crystallization properties under large deformation conditions, which helps to improve the load-bearing capacity when the edge of the rubber is subjected to impact and local tension, so that the material takes into account elastic recovery, tensile strength, and resistance to deformation.

[0045] This embodiment employs a low-filler reinforcement and softening system, consisting of 20 parts of carbon black N774 and 5 parts of naphthenic oil, with a nominal mass ratio of carbon black to naphthenic oil of 4:1. N774 is a relatively mild reinforcing carbon black, and at 20 parts, it forms the necessary rubber-filler effect, improving the tensile strength, compressive deformation resistance, molding dimensional stability, and edge integrity of the rubber compound. Simultaneously, it avoids using high-reinforcing carbon black or high filler content to form an excessively strong filler network, thereby reducing hysteresis loss of the rubber compound during rapid deformation.

[0046] This embodiment uses a vulcanization active system, consisting of 5 parts zinc oxide and 1 part stearic acid. During the mixing and heating process, stearic acid reacts with zinc oxide to form zinc soap-like active intermediates, which improves the dispersion and reactivity of zinc oxide in the rubber matrix and promotes the formation of complex structures with high reactivity between the vulcanizing agent and the accelerator, thereby accelerating the crosslinking reaction of natural rubber.

[0047] This embodiment employs a composite stabilization system, consisting of 2 parts of antioxidant RD and 2.5 parts of antioxidant 4010NA, for a total dosage of 4.5 parts. Antioxidant RD is mainly used to improve the performance retention of natural rubber under mixing, molding vulcanization, and heating conditions, and to reduce molecular chain changes caused by thermo-oxidative effects. Antioxidant 4010NA has a good inhibitory effect on oxidation reactions under dynamic conditions, making it suitable for applications involving repeated compression, bending, and recovery of the rubber edge.

[0048] This embodiment employs a composite vulcanization system, using 1.8 parts of pre-dispersed sulfur IS-60, combined with 0.8 parts of accelerator DM, 0.2 parts of accelerator D, and 1.0 part of accelerator CZ, for a nominal total vulcanization system volume of 3.8 parts. The pre-dispersed sulfur, carried by a carrier, helps reduce the dispersion, agglomeration, and localized concentration differences of powdered sulfur during the open milling process, resulting in a more uniform distribution of the vulcanizing agent within the natural rubber matrix. The effective sulfur content of IS-60 and the carrier composition should be further confirmed based on supplier information.

[0049] This embodiment employs a processing aid system, using 2 parts each of Gum-Easy and Mold-Del 935P, for a total processing aid of 4 parts. Gum-Easy is mainly used to improve the internal lubrication of the rubber compound, the dispersion of carbon black and small particles, the open milling operation, and the molding filling state, so that the rubber compound still has the necessary processing fluidity even with a low amount of naphthenic oil. Mold-Del 935P is mainly used to improve the demolding state of the interface between the rubber compound and the mold and the surface quality of the product, reducing demolding scratches, sticking to the mold, and edge defects.

[0050] The formulation design in this embodiment does not rely on a single component to achieve high resilience, but rather establishes an overall balance of "continuous elastic phase of natural rubber - low-filler reinforcing system - low-dosage softening system - uniform cross-linking network - composite stabilization and processing system". Natural rubber provides the main elastic energy storage and release capacity; 20 parts of N774 provide the necessary load-bearing capacity and dimensional stability; 5 parts of naphthenic oil and two processing aids ensure the feasibility of mixing and molding; the active system and composite promoting system enable the cross-linked structure to form uniformly in the cross-section of the product; the RD / 4010NA system is used to reduce performance changes during production and dynamic use.

[0051] The aforementioned systems exhibit interrelationships: increasing carbon black or crosslinking levels can increase hardness and strength, but may restrict molecular chain movement and reduce springback; increasing naphthenic oil levels can reduce hardness and viscosity, but may weaken strength and cycle retention; processing aids can improve the process without significantly increasing the amount of softener, but their effects still need to be confirmed in conjunction with specific compositions and comparative samples. Therefore, this embodiment uses a Shore A hardness of 47, initial springback of 88.57%, tensile strength of 17.7 MPa, elongation at break of 577%, and a springback retention of 96.10% after 10,000 cycles as the equilibrium result of the existing formulation.

[0052] Basic performance tests were conducted on the high-resilience, low-fading billiard table rubber edge:

[0053] The Shore A hardness of this embodiment is 47, the initial rebound rate is 88.57%, the tensile strength is 17.7 MPa, and the elongation at break is 577%. The above results show that the formulation can form a molded billiard table edge that takes into account hardness, rebound and tensile properties.

[0054] Then, the high-resilience, low-attenuation billiard table rubber edge prepared in this embodiment was subjected to cyclic impact and rebound rate measurements: Cyclic impact testing equipment applies a specified number of repeated impacts to a sample using an impact head; a pendulum rebound tester is used to measure the rebound rate of vulcanized rubber before the start of a cycle and at different stages of the cycle. A single rebound rate measurement using a pendulum rebound tester is not equivalent to a cyclic impact test.

[0055] Each round of cyclic impact test used the rebound rate measured immediately before the start of that round of impact as the initial rebound rate R0, without using the rebound rates of other batches or other test rounds to replace R0 for this round. Impacts were paused at 100, 1000, 2500, 5000, 7500, and 10000 cycles, and the equipment was placed under the same recovery time and environmental conditions. The stage rebound rate R was then measured using the same pendulum rebound meter.

[0056] The rebound performance after each cycle is evaluated using rebound rate, rebound decrease, rebound retention rate, and rebound decay ratio. The specific formulas and their meanings are as follows: (1) Rebound decrease value:

[0057] In the formula, ΔR represents the cumulative decrease in rebound rate after n cyclic impacts, in percentage points; R0 represents the initial rebound rate measured immediately before the cyclic impacts; and R represents the rebound rate after n cyclic impacts. The smaller ΔR is, the less the rebound rate decreases due to the cyclic impacts.

[0058] (2) Rebound retention rate:

[0059] In the formula, K represents the percentage of the elastic energy retained after n cycles of impact relative to the initial elastic energy. The closer K is to 100%, the better the elasticity retention of the rubber edge after cyclic impacts.

[0060] (3) Rebound attenuation ratio:

[0061] In the formula, D represents the percentage decrease in rebound rate after n cycles of impact relative to the initial rebound rate. The smaller D is, the lower the degree of rebound attenuation of the rubber edge.

[0062] (4) Relationship between rebound retention rate and rebound decay ratio:

[0063] K represents the percentage of performance still retained, and D represents the percentage of performance lost; therefore, their sum is 100%. The rebound decrease value ΔR is expressed as a percentage point, while the rebound attenuation ratio D is expressed as a percentage; the two have different meanings.

[0064] The meanings of the symbols in the above formula are as follows:

[0065] The results of the cyclic shock phase are as follows:

[0066] refer to Figure 1 After 10,000 cycles of impact, the rebound rate of this embodiment was 85.12%, a decrease of 3.45 percentage points from the initial rebound rate of 88.57%; the rebound attenuation rate was 3.90%, and the rebound retention rate was 96.10%. The results show that the rubber edge can still maintain high rebound performance under the specified cyclic impact conditions.

[0067] Comparative Example 1 The difference between this comparative example and Example 3 is that: 30 parts of carbon black N774.

[0068] Comparative Example 2 The difference between this comparative example and Example 3 is that: 10 parts of naphthenic oil.

[0069] Comparative Example 3 The difference between this comparative example and Example 3 is that accelerator DM and accelerator D are removed.

[0070] Comparative Example 4 The difference between this comparative example and Example 3 is that SCR20 / N550 is used instead of #3 smoke adhesive.

[0071] Comparative Example 5 The difference between this comparative example and Example 3 is that the adhesive is removed.

[0072] Comparative Example 6 The difference between this comparative example and Example 3 is that the Modalite 935P is removed.

[0073] Comparative Example 7 The difference between this comparative example and Example 3 is that the adhesive and Moldex 935P are removed.

[0074] The performance results of Example 3 and the comparative examples are as follows:

[0075] In Comparative Example 1, increasing the amount of carbon black resulted in improved hardness and tensile strength, but lower initial resilience and cycle retention compared to Example 1.

[0076] In Comparative Example 2, increasing the amount of naphthenic oil resulted in decreased hardness and increased elongation, but decreased tensile strength, initial resilience, and cycle retention.

[0077] After simplifying the promoting system in Comparative Example 3, the hardness, strength, and cycle retention performance were all lower than those in Example 3.

[0078] Comparative Example 4 uses a common natural rubber compound formulation with a higher filler content, resulting in higher hardness and significantly lower initial rebound rate and cycle retention rate compared to Example 3.

[0079] Comparative Example 5 showed relatively little change in performance after the removal of the adhesive.

[0080] After removing the mold from the Deli 935P in Comparative Example 6, the performance change was relatively small.

[0081] In Comparative Example 7, the tensile properties, initial resilience, and cycle retention all decreased after the removal of both processing aids.

[0082] Specific analysis: (1) The combination of natural rubber, low amount of N774 carbon black, low amount of naphthenic oil, composite stabilization system and composite vulcanization system is the basis for achieving an initial rebound rate of 88.57% under the condition of Shore A hardness of 47 in Example 1.

[0083] (2) After 10,000 cycles of impact, the rebound rate is still 96.10%, indicating that the existing formula has low rebound decay under the specified cycle conditions.

[0084] (3) Example 3 has both a tensile strength of 17.7 MPa and an elongation at break of 577%, indicating that the high resilience does not come at the cost of significantly sacrificing tensile performance.

[0085] (4) The results of Example 3 and Comparative Examples 1, 2, 3, 4, 5, 6 and 7 show that carbon black, naphthenic oil, composite accelerator system and two processing aids have different effects on hardness, tensile properties, initial rebound rate and cycle retention performance, and there are synergistic relationships among the components.

[0086] The embodiments described above are merely preferred embodiments of the present invention and are not intended to limit the present invention in any way. Any person skilled in the art can make more possible variations and modifications to the technical solutions of the present invention, or modify them into equivalent embodiments, without departing from the scope of the present invention. Therefore, all equivalent changes made based on the concept of the present invention without departing from the scope of the present invention should be covered within the protection scope of the present invention.

Claims

1. A high-resilience, low-fading billiard table edge, comprising a mixture of A-section compound rubber and B-section vulcanizing agent, characterized in that: The A-section compound is composed of the following parts by weight: 90-110 parts of No. 3 smoked rubber; 15-25 parts of carbon black N774; and 4-6 parts of naphthenic oil. 4-6 parts of 99.7% zinc oxide; Stearic acid SA1801 0.5-1.5 parts; antioxidant RD 1-3 parts; antioxidant 4010NA 2-3 parts; gelling agent 1-3 parts; Modified 935P 1-3 parts; The B-section vulcanizing material is in the following mass proportions: sulfur IS-60 1.5-2 parts; accelerator DM 0.5-1 part; accelerator D 0.1-0.3 parts; accelerator CZ 0.5-1.5 parts.

2. The high-resilience, low-attenuation billiard table edge according to claim 1, characterized in that: The A-section compound is composed of the following parts by weight: 100 parts of No. 3 smoked rubber; 20 parts of carbon black N774; and 5 parts of naphthenic oil. 5 parts of 99.7% zinc oxide; 1 part of stearic acid SA1801; Antioxidant RD 2 parts; Antioxidant 4010NA 2.5 parts; 2 parts of Jiaoyisu; 2 parts of Modeli 935P.

3. The high-resilience, low-attenuation billiard table edge according to claim 2, characterized in that: The B-section vulcanizing material is in the following parts by weight: 1.8 parts of sulfur IS-60; 0.8 parts of accelerator DM; 0.2 parts of accelerator D; and 1.0 part of accelerator CZ.

4. A method for preparing the high-resilience, low-attenuation billiard table rubber edge as described in any one of claims 1-3, characterized in that: Includes the following steps: S1. Weigh out the following components by weight: No. 3 smoked rubber, carbon black N774, naphthenic oil, 99.7% zinc oxide, stearic acid SA1801, antioxidant RD, antioxidant 4010NA, rubber binder, and molded rubber 935P. Then, put No. 3 smoked rubber into a mixer and add carbon black N774, naphthenic oil, 99.7% zinc oxide, stearic acid SA1801, antioxidant RD, antioxidant 4010NA, rubber binder, and molded rubber 935P. Mix until the rubber temperature reaches 125℃, then discharge the rubber to form section A. The mixing time is 600-840s. S2. Cool and let stand the A-section compound obtained in step S1, and then put the A-section compound into the open mill for turning, wherein the open milling time is 220-260s; S3. Weigh out sulfur IS-60, accelerator DM, accelerator D, and accelerator CZ by mass percentage, then add them to the open mill for powdering. After powdering, turn the mixture until it is evenly mixed and forms a rubber compound. The powdering time is 4-5 minutes, and the turning time is 5-6 minutes. S4. The rubber material from step S3 is processed by a two-roll mill, then cut and weighed in sequence to form a rubber blank, and then the rubber blank is placed into a multi-cavity mold. S5. Place the mold containing the rubber material from step S4 into a vulcanizing machine for vulcanization. The mold closing pressure is set to 110-130 bar, the air is vented 3 times during vulcanization, the temperature of the upper and lower mold plates is set to 160℃, and the vulcanization time is 850-950 s. S6. After vulcanization, open the mold and remove the rubber edge. Then, cool, trim, shape, and inspect the appearance in sequence to obtain a high-resilience, low-attenuation billiard table rubber edge.

5. The method for preparing a high-resilience, low-attenuation billiard table edge according to claim 4, characterized in that: In step S1, the mixing time is 720s.

6. The method for preparing a high-resilience, low-attenuation billiard table edge according to claim 4, characterized in that: In step S4, the weight of a single plastic preform is 540±20g, and 30 plastic preforms are placed in each mold.

7. The method for preparing a high-resilience, low-attenuation billiard table edge according to claim 4, characterized in that: In step S5, the vulcanizing machine is a 1200T flat vulcanizing machine.

8. The method for preparing a high-resilience, low-attenuation billiard table edge according to claim 4, characterized in that: In step S3, production pigments are fed into the open mill, and then the pigments are absorbed. After the pigment absorption is completed, the mixture is turned over until it is evenly mixed and the color of the rubber compound is uniform.