Elastomeric composition based on topologically restricted networks, process for its preparation and use

By introducing macrocyclic compounds into elastomer materials to form a topologically confined non-uniform physical cross-linked network, the performance trade-offs and processing compatibility issues in existing technologies are resolved, and the overall performance is improved.

CN123152185APending Publication Date: 2026-11-24SICHUAN UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611409685.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-11
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing technologies often face performance trade-offs when improving the strength, toughness, and fatigue resistance of elastomer materials. Furthermore, the preparation methods are incompatible with industrial processing, resulting in high costs and limiting industrial applications.

Method used

By introducing macrocyclic compounds to form topologically confined structures such as entanglement or interring with elastomers, a non-uniform physical cross-linked network is constructed, which, combined with a chemical network, enhances the overall performance of the material.

Benefits of technology

It achieves simultaneous improvement in tensile strength, tear strength, fracture toughness, puncture resistance and fatigue resistance, while reducing dynamic heat generation, breaking through the bottleneck of multiple properties in traditional modification strategies where one increases while the other decreases.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123152185A_ABST
    Figure CN123152185A_ABST
Patent Text Reader

Abstract

This invention belongs to the field of elastomer composite material technology, specifically relating to an elastomer composition based on a topologically confined network, its preparation method, and its applications. The elastomer composition comprises an elastomer matrix and a macrocyclic compound. The macrocyclic compound has a cyclic cavity or rigid cyclic skeleton structure and forms a non-uniform topologically confined structure with the polymer chains of the elastomer matrix. By introducing a macrocyclic compound with a cyclic cavity or rigid cyclic skeleton structure into the elastomer matrix, forming entangled or interlocking non-uniform topologically confined structures with the elastomer, this invention achieves a simultaneous and significant improvement in the tensile strength, elongation at break, tear strength, fracture toughness, puncture resistance, and fatigue resistance of the elastomer product, while reducing dynamic heat generation. This overcomes the trade-off bottleneck of multiple performance trade-offs in traditional elastomer reinforcement strategies.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of elastomer composite material technology, specifically relating to an elastomer composition based on a topologically restricted network, its preparation method, and its application. Background Technology

[0002] Crack initiation and propagation in elastomer products under dynamic cyclic loading due to the accumulation of micro-damage is a core issue limiting their service life. Improving the tear resistance, fracture toughness, and dynamic fatigue life of elastomers has been a long-term goal in the field of high-performance elastomers.

[0003] However, traditional modification strategies face an inherent performance trade-off: while increasing crosslinking density can increase stiffness, it often sacrifices elongation at break and fatigue life; while increasing the amount of reinforcing filler can improve tear strength, it leads to processing difficulties and increased dynamic heat generation. How to simultaneously improve the strength, toughness, and fatigue resistance of elastomer materials without excessively sacrificing other properties is a technical challenge that urgently needs to be solved in this field.

[0004] In recent years, research on the topological interactions between macrocyclic molecules (such as columnar aromatics and cyclodextrins) and polymer chains has provided new insights into overcoming the aforementioned bottlenecks. For example, by pre-constructing interlocking structures such as polyrotaxanes, molecular knots, and cord hydrocarbons and introducing them into the polymer matrix, topological entanglement can be introduced into the system. However, existing technologies typically rely on pre-constructing interlocking structures or forming "ring-through / interlocking" structures through long-term solution blending or melt blending. The preparation conditions are demanding and completely incompatible with industrial processing; moreover, the cost of the synthetic macrocyclic molecules (such as polyrotaxanes, molecular knots, and cord hydrocarbons) is high, limiting their prospects for industrial application.

[0005] Therefore, there is an urgent need in this field for a technical solution that is simple in process, cost-controllable, compatible with existing elastomer industrial processing systems, and can simultaneously improve multiple mechanical properties of elastomers. Summary of the Invention

[0006] To address the aforementioned problems, this invention provides an elastomer composition based on a topologically confined network. This composition constructs a non-uniform physical cross-linked network by introducing macrocyclic compounds to form entangled or interlocking topologically confined structures with the elastomer. This network exhibits excellent energy dissipation capabilities, preventing stress concentration and delaying crack propagation. Furthermore, it synergizes with the covalent network of the elastomer to comprehensively enhance overall performance, significantly improving tensile strength, tear strength, fracture toughness, puncture resistance, and fatigue resistance.

[0007] In a first aspect, the present invention provides an elastomer composition based on a topologically confined network, comprising an elastomer matrix and a macrocyclic compound having a cyclic cavity or a rigid cyclic skeleton structure, and forming a non-uniform topologically confined structure with the polymer chains of the elastomer matrix.

[0008] Furthermore, the macrocyclic compound is selected from at least one of cyclodextrin and its derivatives, polycyclodextrin and its derivatives, cyclodextrin tetramer, calixarene and its derivatives, monomodified calixarene and its derivatives, calixarene tetramer, polycalixarene, calixarene dimer, columnar aromatics and their derivatives, dimer columnar aromatics, polycocolumnar aromatics, tetramer columnar aromatics, cucurbituril and its derivatives, and crown ether and its derivatives.

[0009] Further, the derivatives include: compounds in which a macrocyclic host molecule is grafted with compatibilizing side chains or groups; and / or, dimers, oligomers, cross-linked copolymers or three-dimensional network polymers formed by two or more macrocyclic host molecules connected by covalent cross-linking bridges.

[0010] Furthermore, the compatibilizing side chain or group is a graft group that can improve the compatibility between the macrocyclic compound and the elastomer matrix, preferably a long-chain alkyl group.

[0011] Furthermore, the polycyclodextrin and its derivatives, polycalixarene, and polypillararene are formed by a cross-linking reaction between macrocyclic molecules and cross-linking molecules, exhibiting a hierarchical porous structure. The macrocyclic molecules themselves possess inherent cavities, forming primary pores with a diameter of 0.5–0.9 nm. Multiple macrocyclic molecules are connected by cross-linking arms, which enclose secondary channels of adjustable size. By adjusting the length and connection method of the cross-linking arms, the size of the secondary channels can be controlled: short cross-linking arms form smaller channels, long cross-linking arms form larger channels, and the star-shaped connection structure can further expand the central cavity, allowing its pore size to reach the several nanometer scale. A schematic diagram is shown below. Figure 1 As shown.

[0012] Furthermore, the macrocyclic compound is selected from:

[0013] ,

[0014] Wherein, R1 is an alkyl chain with H atoms and 1 to 20 carbon atoms, or a long alkyl functional group with an unsaturated double bond, hydroxyl group, amino group, carboxyl group, or amide group at the end; R2 is a tert-butyl group, primary amino group, sulfonic acid group, nitro group, amide group, etc.; R3 is a long alkyl functional group with an unsaturated double bond, hydroxyl group, amino group, carboxyl group, or amide group at the end.

[0015] Furthermore, the macrocyclic compound is preferably:

[0016] , , , , , , , , , , , Methylated β-cyclodextrin, 4-tert-butylcalix[6] aromatics, 4-tert-butylcalix[8] aromatics, dibenzo-30-crown-10, cucurbit[7] urea.

[0017] Furthermore, the elastomer matrix is ​​selected from one or more of the following: natural rubber, isoprene rubber, styrene-butadiene rubber, butyl rubber, cis-butadiene rubber, nitrile rubber, ethylene propylene rubber, fluororubber, silicone rubber, fluorosilicone rubber, thermoplastic polyurethane, polyamide, and polyether block amide.

[0018] Furthermore, based on 100 parts by weight of the elastomer matrix, the content of the macrocyclic compound is 0.5-5 parts by weight.

[0019] Furthermore, the elastomer composition may also contain fillers.

[0020] Furthermore, the filler is selected from at least one of carbon black and silica.

[0021] Furthermore, based on 100 parts by weight of the elastomer matrix, the content of the filler is 30-80 parts by weight.

[0022] Furthermore, the elastomer composition also includes a vulcanizing agent and optional elastomer additives.

[0023] As used herein, the vulcanizing agent and optional elastomer additives can be any suitable vulcanizing agent and elastomer additive well known in the field of elastomers, and those skilled in the art can make conventional selections based on actual needs.

[0024] In a second aspect, the present invention provides a method for preparing an elastomer composition as described herein, comprising the steps of: uniformly mixing a macrocyclic compound with an elastomer matrix, thereby dispersing the macrocyclic compound in the elastomer matrix and forming a non-uniform topologically confined structure with the polymer chains of the elastomer matrix.

[0025] Furthermore, the mixing method is selected from at least one of solution blending, melt blending, and mechanical blending.

[0026] Furthermore, the preparation method further includes the step of mixing fillers, vulcanizing agents, and optional elastomer additives.

[0027] Furthermore, the preparation method also includes a sulfidation step.

[0028] In a third aspect, the present invention provides the use of the elastomeric compositions as described herein in the preparation of elastomeric articles.

[0029] Furthermore, the elastomer articles include tires, seals, shock absorbers, conveyor belts, or hoses.

[0030] Beneficial effects of the present invention

[0031] This invention constructs a non-uniform topologically confined physical cross-linked network outside the covalent network of the elastomer by introducing macrocyclic compounds and their derivatives with ring-shaped cavities or rigid ring-shaped skeleton structures. This physical network exhibits reversible dissociation-recombination properties and can synergize with the chemical network: under small strain, it jointly bears load to increase modulus; under large deformation, it preferentially dissociates to dissipate energy and delay covalent network failure; and during fatigue, it recombines to recover and inhibit microcrack propagation. Compared with existing technologies, this invention eliminates the need for pre-prepared interlocking structures; direct in-situ homogenization is sufficient. It achieves a simultaneous and significant improvement in tensile strength, elongation at break, tear strength, fracture toughness, puncture resistance, and fatigue resistance, while reducing dynamic heat generation. This overcomes the trade-off bottleneck of multiple performance trade-offs in traditional elastomer reinforcement strategies. Attached Figure Description

[0032] Figure 1 The diagram shows the structure of a polymer formed by the cross-linking reaction of macrocyclic molecules and cross-linked molecules.

[0033] Figure 2 Tensile curves of rubber products prepared in some examples and comparative examples are shown: (a) stress-strain curves of rubber products prepared in Examples 1-2, Comparative Examples 1 and 3; (b) stress-strain curves of rubber products prepared in Examples 9 and 8; (c) stress-strain curves of rubber products prepared in Examples 10 and 9; (d) stress-strain curves of rubber products prepared in Examples 11 and 10.

[0034] Figure 3 TPU (Comparative Example 12) and TPU-PCD are shown. 11 (a) Stress-strain curve, (b) Temperature-storage modulus curve, and (c) Temperature-loss factor curve of Example 13.

[0035] Figure 4 The images show (a) NR (Comparative Example 1) and (b) NR-CD. 11 (Example 1), (c) NR-PCD 11 Fracture toughness curves of (Example 2) and (d) NR (Comparative Example 1) and NR-PCD 11 (Example 2) Fracture toughness at different loading speeds.

[0036] Figure 5 The images show (a) NR (Comparative Example 1) and (b) NR-CD. 11 (Example 1), (c) NR-PCD 11 (Example 2) and (D)NR-cyclen 11 (Comparative Example 3) Low-magnification SEM cross-sectional view.

[0037] Figure 6 The images show (a) NR (Comparative Example 1) and (b) NR-CD. 11 (Example 1), (c) NR-PCD 11 (Example 2) and (D)NR-cyclen 11 (Comparative Example 3) High-magnification SEM cross-sectional view.

[0038] Figure 7 Showing NR (Comparative Example 1), NR-CD 11 (Example 1) and NR-PCD 11 Compression fatigue data for (Example 2): (a) dynamic stiffness variation curve, (b) fatigue variation curve, (c) compression permanent deformation and temperature rise, and (d) sample condition after fatigue test. Detailed Implementation

[0039] The present invention will be further illustrated below with reference to specific embodiments, but the embodiments do not limit the present invention in any way. Unless otherwise specified, the reagents, methods, and equipment used in the present invention are conventional reagents, methods, and equipment in this technical field.

[0040] The raw materials used in the embodiments of this invention and their sources are as follows:

[0041] Natural rubber and silica were supplied by Chongqing Double Coin Tire Group Co., Ltd.; isoprene rubber was purchased from Xinjiang Tianli Petrochemical; styrene-butadiene rubber and butadiene rubber were purchased from Sinopec; nitrile rubber was purchased from Lanzhou Petrochemical; ethylene propylene rubber was purchased from Lanxess GmbH, Germany; fluororubber was purchased from Inner Mongolia Sanai Fuwanhao Fluorochemical Co., Ltd.; silicone rubber was purchased from Dongjue Organosilicon Co., Ltd. Thermoplastic polyurethane (TPU) was purchased from BASF. Polyether block amide (PEBAX) was purchased from Arcoma. Macrocyclic compounds: β-cyclodextrin, β-cyclodextrin epichlorohydrin copolymer, methylated β-cyclodextrin, 4-tert-butylcalix[6] aromatics, 4-tert-butylcalix[8] aromatics, column[5] aromatics, dibenzo-30-crown-10 (DB30C10), cucurbit[7]urea, cycloalkyl oil, cyclohexane, etc. were purchased from Shanghai Titan Company. Vulcanization: Sulfur, vulcanization accelerator CZ, zinc oxide, stearic acid compound, antioxidant 4020, anti-aging agent RD, paraffin oil, hydroxyl silicone oil, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane, 2,2'-dibenzothiazole disulfide (accelerator DM), tetramethylthiuram disulfide, magnesium oxide, calcium hydroxide, carnauba wax, bisphenol AF, and benzyltriphenylphosphine chloride (BPP) were all purchased from Shanghai Titan Company. Carbon black was purchased from Black Cat Carbon Black Co., Ltd. All reagents were used directly without purification.

[0042] CD 11 PCD 11 PCD 6D Cyclen 11 PCD5, PCD 16 The synthesis was achieved by grafting long alkyl chains onto a macrocyclic host β-cyclodextrin, a β-cyclodextrin-epoxychloropropane copolymer, and cyclohexane-co ...

[0043] , , , .

[0044] The ATBC[6] reference (ACS Omega 2018, 3(1):229–239. DOI:10.1021 / acsomega.7b01852.) was synthesized, and the specific structure is as follows:

[0045] .

[0046] Tetrameric β-cyclodextrin (QCD) was synthesized according to the references (Polymers 2020, 12, 393, Biomacromolecules2023, 24, 2, 1022–1031, Chem. Commun, 2004, 4, 408-409.), and its specific structure is as follows:

[0047] .

[0048] The double-column[5]arene (DP5A) and the tetrameric column[5]arene (QP5A) were synthesized from the column[5]arene host molecule by the method described in the references (RSC Adv. 2013, 3, 21405-21408, Org. Lett. 2012, 14, 42-45, Chem. Commun. 2011, 47, 10290–10292, Chem. Commun. 2014, 50, 9122–9125.), and their specific structures are as follows:

[0049] , .

[0050] Dimeric-calix[6]arene (DC[6]) and poly-undecene-calix[6]arene (PTBC[6]) 11D The compound is synthesized using calix[6]arene and tert-butylcalix[6]arene as the main macrocycles, according to the method described in the references (Organic letters, 2013, 15(22): 5694-5697, ACS Omega 2018, 3(1):229–239.). The specific structure is as follows:

[0051] , .

[0052] Example 1

[0053] Mix 100 parts natural rubber and 1 part CD 11 First, mix in an internal mixer for 3 minutes. Then, add 5 parts zinc oxide, 2 parts stearic acid, 1 part antioxidant 4020, 1 part anti-aging agent RD, 40 parts carbon black, 1 part vulcanization accelerator CZ, and 2 parts sulfur in sequence. Mix and vulcanize in the internal mixer to obtain NR-CD. 11 .

[0054] Example 2

[0055] Mix 100 parts natural rubber and 1 part PCD 11First, mix in an internal mixer for 3 minutes. Then, add 5 parts zinc oxide, 2 parts stearic acid, 1 part antioxidant 4020, 1 part anti-aging agent RD, 40 parts carbon black, 1 part vulcanization accelerator CZ, and 2 parts sulfur in sequence. Mix and vulcanize in the internal mixer to obtain NR-PCD. 11 .

[0056] Example 3

[0057] Mix 100 parts natural rubber and 1 part PCD 6D First, mix in an internal mixer for 3 minutes. Then, add 5 parts zinc oxide, 2 parts stearic acid, 1 part antioxidant 4020, 1 part anti-aging agent RD, 40 parts carbon black, 1 part vulcanization accelerator CZ, and 2 parts sulfur in sequence. Mix and vulcanize in the internal mixer to obtain NR-PCD. 6D .

[0058] Example 4

[0059] 100 parts of natural rubber and 1 part of methylated β-cyclodextrin (MCD) were first mixed in an internal mixer for 3 minutes. Then, 5 parts of zinc oxide, 2 parts of stearic acid, 1 part of antioxidant 4020, 1 part of antioxidant RD, 40 parts of carbon black, 1 part of vulcanization accelerator CZ and 2 parts of sulfur were added in sequence and mixed and vulcanized in an internal mixer to obtain NR-MCD.

[0060] Example 5

[0061] 100 parts of isoprene rubber and 1.5 parts of DP5A were melt-blended at 90°C for 0.5 hours. Then, 5 parts of zinc oxide, 2 parts of stearic acid, 1 part of antioxidant 4020, 1 part of antioxidant RD, 40 parts of carbon black, 1 part of vulcanization accelerator CZ and 2 parts of sulfur were added sequentially and mixed and vulcanized in an internal mixer to obtain IR-2DP5A.

[0062] Example 6

[0063] 100 parts of EPDM and 3 parts of 4-tert-butylcalix[6] aromatics were mixed in a mixer for 5 minutes. Then, 5 parts of zinc oxide, 1 part of stearic acid, 50 parts of carbon black N330, 20 parts of paraffin oil, 1 part of accelerator CZ were added in sequence. Finally, 1.5 parts of sulfur were added and mixed for 8-10 minutes to obtain the compound. Then, it was vulcanized at 160℃ and 15 MPa to obtain EPDM-3TBC[6].

[0064] Example 7

[0065] 100 parts of silicone rubber and 1 part of dibenzo-30-crown-10 (DB30C10) were mixed in an internal mixer for 10 minutes. Then, 40 parts of silica and 6 parts of hydroxyl silicone oil were added and thoroughly mixed. The mixture was then poured out. After cooling, the rubber compound was re-milled in an open mill until the surface was smooth. Then, the vulcanizing agent 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane (bis(2,5-dimethyl)hexane) was added. Subsequently, a first-stage vulcanization (160°C, time determined by T90) and a second-stage vulcanization (200°C, 4 hours) were carried out on a flat vulcanizing mill to obtain SIR-DB30C10.

[0066] Example 8

[0067] 100 parts of NBR and 1.5 parts of cucurbita[7]urea were mixed in a mixer for 5 minutes. Then, 5 parts of zinc oxide, 1 part of stearic acid, 1.2 parts of 2,2'-dibenzothiazole disulfide (accelerator DM), 0.3 parts of tetramethylthiuram disulfide (accelerator TMTD), and 2 parts of antioxidant 4020 were added in sequence and mixed for 3-5 minutes. Then, 40 parts of carbon black N330 were added and mixed for 5-10 minutes. Finally, 1.5 parts of sulfur were added and mixed for 3-5 minutes to obtain the compound. Then, NBR-1.5CB[7] was obtained by vulcanization at 160℃ and 15 MPa.

[0068] Example 9

[0069] Mix 90 parts natural rubber, 10 parts butadiene rubber 9000, and 1 part PCD. 11 First, mix for 7 minutes. Then, add 10 parts of indirect zinc oxide, 2 parts of stearic acid, 2 parts of antioxidant 4010NA, 1 part of antioxidant RD, 1 part of heat stabilizer HS-80, 40 parts of carbon black N660, 1 part of coupling agent KH845-4, and 3.5 parts of aromatic oil in sequence and mix for 10-15 minutes. Next, add 1.1 parts of vulcanization accelerator NOBS, 2 parts of sulfur, 0.3 parts of anti-scorching agent, and 0.8 parts of anti-reversion agent WK-901 and mix for 5 minutes. Finally, vulcanize at 143℃ and 10MPa to obtain NR. 90 BR 10 -PCD 11 .

[0070] Example 10

[0071] Mix 100 parts butadiene rubber and 1 part PCD 11 First, mix in an internal mixer for 4 minutes. Then, add 5 parts zinc oxide, 2 parts stearic acid, 1 part antioxidant 4020, 1 part anti-aging agent RD, 40 parts carbon black, 1 part vulcanization accelerator CZ, and 2 parts sulfur in sequence. Mix and vulcanize in the internal mixer to obtain BR-PCD. 11 .

[0072] Example 11

[0073] Mix 100 parts styrene-butadiene rubber and 1 part PCD 11 First, the mixture is internally mixed for 4 minutes. Then, 5 parts zinc oxide, 2 parts stearic acid, 1 part antioxidant 4020, 1 part anti-aging agent RD, 40 parts carbon black, 1 part vulcanization accelerator CZ, and 2 parts sulfur are added sequentially and mixed and vulcanized in an internal mixer to obtain SBR-PCD. 11 .

[0074] Example 12

[0075] 100 parts of fluororubber and 2 parts of 4-tert-butylcalix[8] aromatic hydrocarbon were dissolved in ethyl acetate and stirred for 8-24 hours. After mixing evenly, the solvent was evaporated. The mixture was mixed in a mixer for 5 minutes, then 6 parts of magnesium oxide, 3 parts of calcium hydroxide, 2 parts of carnauba wax and 20 parts of carbon black 990 were added and mixed for 5-10 minutes. Finally, 3.2 parts of bisphenol AF and 1.8 parts of benzyltriphenylphosphine chloride (BPP) were added and mixed for 5 minutes. The mixed rubber was then placed on a flat vulcanizing machine for a first-stage vulcanization at a vulcanization temperature of 180 °C, a vulcanization pressure of 20 MPa and a vulcanization time of 1.5 times the normal vulcanization time. The second-stage vulcanization was carried out in a forced-air drying oven at 230 °C for 10 hours to obtain FKM-2TBC[8].

[0076] Example 13

[0077] Dissolve 100 parts TPU in an appropriate amount of THF until a clear, transparent solution is obtained; then dissolve 3 parts PCD 11 Dissolve in a small amount of THF, add to TPU solution, stir for 8 hours overnight, then pour into a petri dish to evaporate and form a film to obtain TPU-3PCD. 11 .

[0078] Example 14

[0079] 100 parts of natural rubber and 2 parts of PCD5 were first mixed in an internal mixer for 3 minutes. Then, 5 parts of zinc oxide, 2 parts of stearic acid, 1 part of antioxidant 4020, 1 part of anti-aging agent RD, 40 parts of carbon black, 1 part of vulcanization accelerator CZ and 2 parts of sulfur were added in sequence and mixed and vulcanized in an internal mixer to obtain NR-PCD5.

[0080] Example 15

[0081] Mix 100 parts natural rubber and 1 part PCD 16 First, mix in an internal mixer for 5 minutes. Then, add 5 parts zinc oxide, 2 parts stearic acid, 1 part antioxidant 4020, 1 part anti-aging agent RD, 40 parts carbon black, 1 part vulcanization accelerator CZ, and 2 parts sulfur in sequence. Mix and vulcanize in the internal mixer to obtain NR-PCD. 16 .

[0082] Example 16

[0083] 100 parts of natural rubber and 1 part of PCD-COOH were first mixed in an internal mixer for 5 minutes. Then, 5 parts of zinc oxide, 2 parts of stearic acid, 1 part of antioxidant 4020, 1 part of anti-aging agent RD, 40 parts of carbon black, 1 part of vulcanization accelerator CZ and 2 parts of sulfur were added in sequence and mixed and vulcanized in an internal mixer to obtain NR-PCD-COOH.

[0084] Example 17

[0085] 100 parts of natural rubber and 1 part of QCD were first mixed in an internal mixer for 3 minutes. Then, 5 parts of zinc oxide, 2 parts of stearic acid, 1 part of antioxidant 4020, 1 part of anti-aging agent RD, 40 parts of carbon black, 1 part of vulcanization accelerator CZ and 2 parts of sulfur were added in sequence and mixed and vulcanized in an internal mixer to obtain NR-QCD.

[0086] Example 18

[0087] 100 parts of natural rubber and 5 parts of ATBC[6] were first mixed for 3 minutes, and then 5 parts of zinc oxide, 2 parts of stearic acid, 1 part of antioxidant 4020, 1 part of antioxidant RD, 40 parts of carbon black, 1 part of vulcanization accelerator CZ and 2 parts of sulfur were added in sequence and mixed and vulcanized in a mixer to obtain NR-5ATBC[6].

[0088] Example 19

[0089] Mix 100 parts of natural rubber and 1 part of QP5A in an internal mixer for 3 minutes. Then, add 5 parts of zinc oxide, 2 parts of stearic acid, 1 part of antioxidant 4020, 1 part of antioxidant RD, 40 parts of carbon black, 1 part of vulcanization accelerator CZ and 2 parts of sulfur in an internal mixer and vulcanize to obtain NR-QP5A.

[0090] Example 20

[0091] 100 parts of natural rubber and 1 part of DC[6] were first mixed for 3 minutes, and then 5 parts of zinc oxide, 2 parts of stearic acid, 1 part of antioxidant 4020, 1 part of antioxidant RD, 40 parts of carbon black, 1 part of vulcanization accelerator CZ and 2 parts of sulfur were added in sequence and mixed and vulcanized in a mixer to obtain NR-DC[6].

[0092] Example 21

[0093] Mix 100 portions of PEBAX and 3 portions of PCD 11 The mixture was kneaded at 170°C for 10 minutes, and then molded to obtain PEBAX-3PCD. 11 .

[0094] Example 22

[0095] Mix 100 parts natural rubber with 1 part PTBC[6]11D First, mix for 5 minutes, then add 5 parts zinc oxide, 2 parts stearic acid, 1 part antioxidant 4020, 1 part anti-aging agent RD, 40 parts carbon black, 1 part vulcanization accelerator CZ and 2 parts sulfur in a mixing mill and vulcanize to obtain NR-PTBC[6]. 11D .

[0096] Comparative Example 1

[0097] 100 parts of natural rubber were first mixed in an internal mixer for 3 minutes. Then, 5 parts of zinc oxide, 2 parts of stearic acid, 1 part of antioxidant 4020, 1 part of antioxidant RD, 40 parts of carbon black, 1 part of vulcanization accelerator CZ and 2 parts of sulfur were added in sequence and mixed and vulcanized in an internal mixer to obtain NR.

[0098] Comparative Example 2

[0099] 100 parts of natural rubber and 1 part of NAP (naphthenic oil) are first mixed in an internal mixer for 3 minutes. Then, 5 parts of zinc oxide, 2 parts of stearic acid, 1 part of antioxidant 4020, 1 part of antioxidant RD, 40 parts of carbon black, 1 part of vulcanization accelerator CZ and 2 parts of sulfur are added in sequence and mixed and vulcanized in an internal mixer to obtain NR-NAP.

[0100] Comparative Example 3

[0101] 100 parts of natural rubber and 1 part of Cyclen11 (a modified product of Cyclen) were first mixed in an internal mixer for 3 minutes. Then, 5 parts of zinc oxide, 2 parts of stearic acid, 1 part of antioxidant 4020, 1 part of antioxidant RD, 40 parts of carbon black, 1 part of vulcanization accelerator CZ, and 2 parts of sulfur were added sequentially and mixed and vulcanized in an internal mixer to obtain NR-Cyclen. 11 .

[0102] Comparative Example 4

[0103] 100 parts of isoprene rubber were heated for 0.5 hours under the same conditions. Then, 5 parts of zinc oxide, 2 parts of stearic acid, 1 part of antioxidant 4020, 1 part of antioxidant RD, 40 parts of carbon black, 1 part of vulcanization accelerator CZ and 2 parts of sulfur were added sequentially and mixed and vulcanized in an internal mixer to obtain IR.

[0104] Comparative Example 5

[0105] 100 parts of EPDM were mixed in an internal mixer for 5 minutes. Then, 5 parts of zinc oxide, 1 part of stearic acid, 50 parts of carbon black N330, 20 parts of paraffin oil, and 1 part of accelerator CZ were added in sequence. Finally, 1.5 parts of sulfur were added, and the mixture was mixed for 8-10 minutes to obtain the compound. The compound was then vulcanized at 160℃ and 15 MPa to obtain EPDM.

[0106] Comparative Example 6

[0107] 100 parts of silicone rubber were internally mixed in a mixer for 10 minutes, then 40 parts of silica and 6 parts of hydroxyl silicone oil were added and thoroughly mixed before being poured out. After the rubber compound cooled, it was re-milled in an open mill until the surface was smooth, and then a vulcanizing agent (D25) was added. Subsequently, a first-stage vulcanization (160℃, time determined by T90) and a second-stage vulcanization (200℃, 4h) were carried out on a flat vulcanizing mill to obtain SIR.

[0108] Comparative Example 7

[0109] 100 parts of NBR were mixed in an internal mixer for 5 minutes. Then, 5 parts of zinc oxide, 1 part of stearic acid, 1.2 parts of 2,2'-dibenzothiazole disulfide (accelerator DM), 0.3 parts of tetramethylthiuram disulfide (accelerator TMTD), and 2 parts of antioxidant 4020 were added sequentially and mixed for 3-5 minutes. Then, 40 parts of carbon black N330 were added and mixed for 5-10 minutes. Finally, 1.5 parts of sulfur were added and mixed for 3-5 minutes to obtain the compound. The compound was then vulcanized at 160℃ and 10 MPa to obtain NBR.

[0110] Comparative Example 8

[0111] 90 parts natural rubber and 10 parts butadiene rubber 9000 were first mixed for 7 minutes. Then, 10 parts of indirect zinc oxide, 2 parts of stearic acid, 2 parts of antioxidant 4010NA, 1 part of antioxidant RD, 1 part of heat stabilizer HS-80, 40 parts of carbon black N660, 1 part of coupling agent KH845-4, and 3.5 parts of aromatic oil were added and mixed for 10-15 minutes. Then, 1.1 parts of vulcanization accelerator NOBS, 2 parts of sulfur, 0.3 parts of scorch inhibitor, and 0.8 parts of anti-reversion agent WK-901 were added and mixed for 5 minutes. Finally, the mixture was vulcanized at 143℃ and 10MPa to obtain NR. 90 BR 10 .

[0112] Comparative Example 9

[0113] 100 parts of butadiene rubber were first mixed in an internal mixer for 4 minutes. Then, 5 parts of zinc oxide, 2 parts of stearic acid, 1 part of antioxidant 4020, 1 part of antioxidant RD, 40 parts of carbon black, 1 part of vulcanization accelerator CZ and 2 parts of sulfur were added in sequence and mixed and vulcanized in an internal mixer to obtain BR.

[0114] Comparative Example 10

[0115] 100 parts of styrene-butadiene rubber were first mixed in an internal mixer for 4 minutes. Then, 5 parts of zinc oxide, 2 parts of stearic acid, 1 part of antioxidant 4020, 1 part of antioxidant RD, 40 parts of carbon black, 1 part of vulcanization accelerator CZ and 2 parts of sulfur were added in sequence and mixed and vulcanized in an internal mixer to obtain SBR.

[0116] Comparative Example 11

[0117] 100 parts of fluororubber were mixed for 5 minutes, followed by the addition of 6 parts magnesium oxide, 3 parts calcium hydroxide, 2 parts carnauba wax, and 20 parts carbon black 990, and mixed for 5-10 minutes. Finally, 3.2 parts bisphenol AF and 1.8 parts BPP were added and mixed for 5 minutes. The mixture was then placed on a flat vulcanizing machine for a first-stage vulcanization at a temperature of 180 °C, a pressure of 20 MPa, and a vulcanization time 1.5 times the normal vulcanization time. A second-stage vulcanization was then carried out in a forced-air drying oven at 230 °C for 10 h to obtain FKM.

[0118] Comparative Example 12

[0119] Dissolve 100 parts of TPU in an appropriate amount of THF until a clear and transparent solution is obtained. Stir for 8 hours overnight, then pour into a petri dish to evaporate and form a film to obtain TPU.

[0120] Comparative Example 13

[0121] 100 parts of PEBAX were mixed at 170°C for 10 minutes and then molded to obtain PEBAX.

[0122] Performance Analysis:

[0123] 1. Mechanical performance testing: The instrument used was an Instron 5966, and the test sample was dumbbell-shaped, with dimensions of 35×2×1 mm. 3 The test rate was 100 mm / min, and the test temperature was room temperature; each sample was tested in parallel three times, and the average value was taken as the final data point.

[0124] Fracture toughness and notch resistance tests were performed using 35×6×0.5 mm steel. 3 Rectangular splines, with or without a 1.5 mm wide notch, were stretched at a rate of 6 mm / min. Tensile curves were measured for samples with and without the notch, and the fracture toughness value was calculated using the integrated area and Equation 1.

[0125] Formula 1

[0126] Where Gc represents fracture toughness, with units of kJ / m. 2 W represents the fracture energy of the unnotched sample at λc, which is the integral area of ​​the stress-strain curve, expressed in MJ / m². 2 C represents the notch depth in mm. λc represents the fracture strain of the notched sample.

[0127] Experimental subjects: rubber products obtained in Examples 1-22 and rubber products obtained in Comparative Examples 1-13.

[0128] Experimental results: From Table 1 and Appendix Figure 2 Appendix Figure 3 a and appendix Figure 4 It can be seen that the addition of macrocyclic compounds to rubber / filler composites significantly improves their mechanical properties, tear resistance, fracture toughness, and puncture resistance. Furthermore, due to the different structures of the macrocyclic compounds, different samples exhibit a wide range of tunability. Based on the low polarity and complex topological structure of macrocyclic compounds, they can effectively adjust the network structure in most rubbers, demonstrating a certain degree of universality.

[0129] Table 1: Summary of Sample Performance

[0130] project Tensile strength (MPa) Elongation at break (%) Young's modulus (MPa) <![CDATA[Toughness (MJ / m 3 )]]> Tear resistance (KN / m) <![CDATA[Fracture toughness (KJ / m 2 )]]> Puncture resistance (KN / m) Dynamic heat generation (tanδ60℃) <![CDATA[NR-CD 11 (Example 1) 29.90 489.21 3.63 52.96 113.26 142.95 46 0.095 <![CDATA[NR-PCD 11 (Example 2) 31.09 507.07 3.53 62.55 85.91 177.59 53 0.095 <![CDATA[NR-PCD 6D (Example 3) 31.12 509.98 3.73 60.48 82.07 82.79 50 0.110 NR-MCD (Example 4) 29.96 491.23 3.96 58.37 67.44 72.51 48 0.095 NR (Comparative Example 1) 27.85 465.5 3.81 51.83 59.39 64.11 42 0.095 NR+NAP (Comparative Example 2) 28.25 484.24 3.71 54.54 65.14 68.29 40 0.104 <![CDATA[NR+Cyclen 11 (Comparative Example 3) 26.79 451.23 4.31 50.54 49.44 55.43 43 0.114 IR-2DP5A (Example 5) 27.78 550.14 3.24 58.32 45.96 \ \ \ IR (Comparative Example 4) 23.14 450.29 3.12 41.98 32.78 \ \ \ EPDM-3TBC[6] (Example 6) 16.78 380.79 5.62 25.71 \ \ \ \ EPDM (Comparative Example 5) 13.64 320.65 5.79 17.62 \ \ \ \ SIR-DB30C10 (Example 7) 8.73 538.73 1.31 18.93 \ \ \ \ SIR (Comparative Example 6) 5.89 415.26 1.24 9.45 \ \ \ \ NBR-1.5CB[7] (Example 8) 17.29 390.74 4.12 27.20 45.78 \ \ \ NBR (Comparative Example 7) 13.76 350.35 3.93 18.27 38.29 \ \ \ <![CDATA[NR 90 BR 10 -PCD 11 (Example 9) 32.80 540.19 4.71 74.38 56.95 \ \ 0.084 <![CDATA[NR 90 BR 10 (Comparative Example 8) 29.20 578.13 3.84 65.68 44.51 \ \ 0.101 <![CDATA[BR-PCD 11 (Example 10) 24.92 511.33 5.27 53.99 48.88 \ \ 0.090 BR (Comparative Example 9) 15.15 342.96 5.16 22.81 45.10 \ \ 0.092 <![CDATA[SBR-PCD 11 (Example 11) 36.92 525.30 5.69 79.35 60.71 \ \ 0.142 SBR (Comparative Example 10) 31.91 459.07 5.99 60.63 46.71 \ \ 0.152 FKM-2TBC[8] (Example 12) 14.78 260.29 5.02 17.69 \ \ \ \ FKM (Comparative Example 11) 10.23 210.37 4.85 10.78 \ \ \ \ <![CDATA[TPU-3PCD 11 (Example 13) 41.47 827.23 21.50 153.84 90.52 \ \ 0.101 TPU (Comparative Example 12) 40.49 868.01 18.72 150.82 84.49 \ \ 0.072 <![CDATA[NR-PCD5 (Example 14)]]> 29.85 465.5 3.87 55.58 67.59 120.15 \ \ <![CDATA[NR-PCD 16 (Example 15) 32.59 512.36 3.96 66.79 85.93 132.15 \ \ NR-PCD-COOH (Example 16) 33.54 523.69 3.80 70.25 90.69 145.29 \ \ NR-QCD (Example 17) 30.27 490.13 4.21 59.34 66.31 89.26 \ \ NR-5ATBC[6] (Example 18) 31.69 536.24 4.03 67.97 78.69 123.04 \ \ NR-QP5A (Example 19) 32.50 501.34 4.36 65.17 85.34 92.14 \ \ NR-DC[6] (Example 20) 29.15 498.15 3.90 58.08 62.38 78.35 \ \ PEBAX-3PCD11 (Example 21) 23.54 650.34 58.21 108.69 108.43 \ \ \ PEBAX (Comparative Example 13) 18.51 550.59 63.41 72.52 93.01 \ \ \ <![CDATA[NR-PTBC[6] 11D (Example 22) 35.78 584.67 4.31 83.67 112.35 135.47 \ \

[0131] Note: In Table 1, "\" indicates that it was not measured.

[0132] 2. Tear resistance test: The instrument used was Instron 5966. The test sample was a right-angled crescent shape. The test speed was 500 mm / min. The test temperature was room temperature. Each sample was tested in parallel three times and the average value was taken as the final data point.

[0133] 3. Puncture resistance test: The instrument used was Instron 5966. The test sample was a circular film with a size of φ50*0.5mm. The test rate was 50mm / min and the test temperature was room temperature. Each sample was tested in parallel three times and the average value was taken as the final data point.

[0134] 4. SEM Testing (Rubber Cross-Section and Filler Dispersion): The instrument used was a ZEISS Sigma 300 (Germany). The vulcanized rubber samples were fractured in liquid nitrogen, and the fracture surfaces were then sputter-coated with gold before SEM observation. The cross-sectional morphology was photographed at different magnifications to analyze the overall fracture characteristics, filler dispersion, and local interface structure of the samples. The sample dimensions were 10 mm × 5 mm × 1 mm.

[0135] Experimental subjects: Examples 1 and 2, Comparative Examples 1 and 3.

[0136] Experimental results: as attached Figure 5 As shown, compared to Comparative Examples 1 and 3, Examples 1-2 exhibit a rougher fracture surface and more tear lines, indicating more efficient energy dissipation during fracture. (See attached...) Figure 6 As shown, the filler dispersion in Examples 1-2 and Comparative Examples 1 and 3 is basically similar, indicating that the addition of macrocyclic compounds to NR / carbon black composite materials does not cause filler aggregation.

[0137] 5. Rolling resistance test (dynamic heat generation): Instrument model: TA Q850 dynamic mechanical analyzer. Test conditions: scanning temperature range -20℃ to 100℃, heating rate 10℃ / min, strain 5%. Specimen size: 10mm*4mm*1mm.

[0138] 6. Fatigue testing: Instrument model is E1000 fatigue tester. Experimental conditions are: pre-compression to 4.8mm, amplitude 1.5mm, frequency 5Hz, number of tests 500,000. Sample size: φ25*12mm.

[0139] Target subjects: Examples 1-2 and Comparative Example 1

[0140] Experimental results: as attached Figure 7 As shown, after 500,000 compression cycles, the final fatigue performance of Examples 1 and 2 remained at around 88%, while that of the control sample was around 78%. At the same time, the compression set and fatigue heat generation of the examples were also reduced compared with the control sample 1, showing a significant improvement in fatigue resistance.

[0141] 7. Dynamic Mechanical Performance Testing: Tests were conducted using a TA Instruments Q850 Dynamic Mechanical Analyzer (DMA). Temperature scanning mode was employed, with a test temperature range of -80 to 100 °C, a heating rate of 5 °C / min, a frequency of 1 Hz, and an amplitude of 15 μm.

[0142] Implementation targets: Example 13 and Comparative Example 12.

[0143] like Figure 3 As shown in b and 3c, a small amount of PCD is added to the TPU. 11 Subsequently, the energy storage modulus of the composite material increases across the entire temperature range, and its loss factor also increases significantly, exhibiting stronger dynamic mechanical strength and energy absorption capacity.

[0144] It should be noted that the preferred embodiments of the present invention are given in the specification and figures. However, the present invention can be implemented in many different forms and is not limited to the embodiments described in this specification. These embodiments are not intended to impose additional limitations on the content of the present invention, and are provided to provide a more thorough and comprehensive understanding of the disclosure of the present invention. Furthermore, the above-mentioned technical features can be combined with each other to form various embodiments not listed above, all of which are considered to be within the scope of the present invention specification. Moreover, those skilled in the art can make improvements or modifications based on the above description, and all such improvements and modifications should fall within the protection scope of the appended claims.

Claims

1. An elastomer composition based on a topologically restricted network, characterized in that, The elastomer composition comprises an elastomer matrix and a macrocyclic compound having a cyclic cavity or a rigid cyclic skeleton structure and forming a non-uniform topologically confined structure with the polymer chains of the elastomer matrix.

2. The elastomer composition according to claim 1, characterized in that, The macrocyclic compound is selected from at least one of cyclodextrin and its derivatives, polycyclodextrin and its derivatives, cyclodextrin tetramer, calixarene and its derivatives, monomodified calixarene and its derivatives, calixarene tetramer, polycalixarene, calixarene dimer, columnar aromatics and their derivatives, dimer columnar aromatics, polycocolumnar aromatics, tetramer columnar aromatics, cucurbituril and its derivatives, and crown ether and its derivatives.

3. The elastomer composition according to claim 2, characterized in that, The derivatives include: compounds with compatibilizing side chains or groups grafted onto macrocyclic main molecules; and / or dimers, oligomers, cross-linked copolymers or three-dimensional network polymers formed by two or more macrocyclic main molecules linked by covalent cross-linking bridges. Furthermore, the compatibilizing side chain or group is a graft group that can improve the compatibility between the macrocyclic compound and the elastomer matrix, preferably a long-chain alkyl group.

4. The elastomer composition according to claim 2, characterized in that, The polycyclodextrin and its derivatives, polycalixarene and polycolumnararene are formed by cross-linking reaction of macrocyclic molecules and cross-linking molecules, and have a hierarchical porous structure. The macrocyclic molecules themselves have inherent cavities, forming primary pores with a pore size of 0.5 to 0.9 nm. Multiple macrocyclic molecules are connected by cross-linking arms, and the cross-linking arms enclose and form secondary channels with adjustable size.

5. The elastomer composition according to any one of claims 2-4, characterized in that, The macrocyclic compounds are selected from: , Wherein, R1 is an alkyl chain with H atoms and 1 to 20 carbon atoms, or a long alkyl functional group with an unsaturated double bond, hydroxyl group, amino group, carboxyl group, or amide group at the end; R2 is a tert-butyl group, primary amino group, sulfonic acid group, nitro group, amide group, etc.; R3 is a long alkyl functional group with an unsaturated double bond, hydroxyl group, amino group, carboxyl group, or amide group at the end. Furthermore, the macrocyclic compound is selected from: , , , , , , , , , , , Methylated β-cyclodextrin, 4-tert-butylcalix[6] aromatics, 4-tert-butylcalix[8] aromatics, dibenzo-30-crown-10, cucurbit[7] urea.

6. The elastomer composition according to claim 1, characterized in that, The elastomer matrix is ​​selected from one or more of the following: natural rubber, isoprene rubber, styrene-butadiene rubber, butyl rubber, cis-butadiene rubber, nitrile rubber, ethylene propylene rubber, fluororubber, silicone rubber, fluorosilicone rubber, thermoplastic polyurethane, polyamide, and polyether block amide. Preferably, the content of the macrocyclic compound is 0.5-5 parts by weight, based on 100 parts by weight of the elastomer matrix.

7. The elastomer composition according to claim 1, characterized in that, The elastomer composition may also contain fillers; Preferably, the filler is selected from at least one of carbon black and silica; Preferably, the filler content is 30-80 parts by weight, based on 100 parts by weight of the elastomer matrix; Preferably, the elastomer composition further comprises a vulcanizing agent and optional elastomer additives.

8. A method for preparing an elastomer composition according to any one of claims 1-7, characterized in that, Includes the following steps: The macrocyclic compound is mixed uniformly with the elastomer matrix, so that the macrocyclic compound is dispersed in the elastomer matrix and forms a non-uniform topologically confined structure with the polymer chains of the elastomer matrix.

9. The preparation method according to claim 8, characterized in that, The mixing method is selected from at least one of solution blending, melt blending, and mechanical blending; Preferably, the preparation method further includes a step of mixing fillers, vulcanizing agents, and optional elastomer additives; Preferably, the preparation method further includes a sulfidation step.

10. The use of the elastomeric composition according to any one of claims 1-7 in the preparation of elastomeric articles; Preferably, the elastomer product includes tires, seals, shock absorbers, conveyor belts, or hoses.