A rubber composition for hard rubber of semi-steel radial tire and a method for preparing the same

By optimizing the formulation of natural rubber and butadiene rubber, and combining low rolling resistance modifiers and dispersants, the problems of high heat generation and insufficient safety in the hard rubber formulation of semi-steel radial tires have been solved, achieving low rolling resistance and high aging resistance, thereby improving tire service life and safety.

CN123152186APending Publication Date: 2026-11-24CHENG SHIN RUBBER (XIAMEN) IND LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611385231.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-08
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing hard rubber formulations for semi-steel radial tires suffer from high heat generation, insufficient safety, and poor wear resistance. Traditional modifiers cannot effectively improve the crosslinking reaction rate, leading to heat accumulation in the rubber compound, high rolling resistance, and affecting tire lifespan and safety.

Method used

Using natural rubber and butadiene rubber as a base, combined with low rolling resistance modifiers and dispersants, the reaction system of tetrazine compounds with carbon black and silica is optimized to reduce the amount of carbon black filler. A weak alkaline protectant is used to prevent the degradation of the modifier, thereby achieving a highly efficient crosslinking reaction and improving aging resistance and tear resistance.

Benefits of technology

It significantly reduces heat accumulation and rolling resistance, improves tear resistance, maintains the rigidity of hard rubber, extends tire life, and reduces the risk of bead cracking. It is suitable for hard rubber tires in semi-steel radial tires.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The application belongs to the technical field of rubber materials, and discloses a rubber composition for hard rubber of semi-steel radial tire and a preparation method thereof, wherein components of the rubber composition include, in terms of mass fractions, a base rubber system including 30-50 parts of natural rubber (NR) and 50-70 parts of butadiene rubber (BR); a reinforcing system including 30-60 parts of carbon black, 0-30 parts of white carbon black and 0-3 parts of a silane coupling agent; a vulcanization system including 2-4 parts of insoluble sulfur, 0.5-2.5 parts of a vulcanization accelerator, 3-5 parts of zinc oxide and 1-2 parts of stearic acid; a protection system including 2-3 parts of antioxidant A, 0.5-1.5 parts of antioxidant B and 1-2 parts of protective wax; and functional additives including 0.5-2 parts of a low-rolling-resistance modifier and 0.5-1.5 parts of a low-rolling-resistance dispersant. The application realizes the significant reduction of heat accumulation, rolling resistance and aging risk while maintaining or improving the rigidity of hard rubber, and improves the tear resistance, and the amount of carbon black in the formula is low, and the application is particularly suitable for hard rubber of semi-steel radial tire.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of rubber materials technology, and specifically relates to a rubber composition for hard rubber of semi-steel radial tires and its preparation method. Background Technology

[0002] Currently, the hard rubber formulations of semi-steel radial tires generally use butadiene rubber (BR) as the main raw material, relying on high-filler carbon black to ensure the rigidity and strength of the compound. Existing technologies, such as the composite formulation system of natural rubber, difunctional polybutadiene, carbon black, and silica disclosed in patent CN 114276586 A, while balancing the wear resistance and low heat generation characteristics of the hard rubber, still have significant technical defects in practical applications, seriously affecting tire life and driving safety. The core drawback of traditional formulation systems lies in severe heat accumulation and an imbalance in overall performance. Ordinary butadiene rubber itself lacks rigidity, requiring a large amount of carbon black for reinforcement. This not only significantly increases the heat generation and rolling resistance of the compound but also causes a substantial decrease in the compound's resistance to flexural cracking. During long-term high-speed, heavy-load driving, the continuous heat accumulation in the hard rubber leads to aging and failure, directly reducing the interfacial adhesion between the hard rubber and the anti-friction rubber, causing delamination. Simultaneously, the compound's shortcomings in heat resistance and flexural resistance easily lead to bead cracking, significantly increasing vehicle driving safety risks.

[0003] To address the issue of high heat generation in rubber compounds, the mainstream improvement method in the industry is to introduce tetrazine-based low-heat modifiers to optimize formulation performance. However, these modifiers have significant limitations in application; they only exhibit good reactivity with styrene-butadiene rubber and cannot undergo effective crosslinking reactions with ordinary butadiene rubber, making it difficult to achieve modified performance enhancement and reduce the amount of carbon black filler. This has become a key technical bottleneck restricting the performance upgrade of rigid rubber formulations.

[0004] In summary, existing hard rubber compounds for semi-steel radial tires suffer from numerous problems, including poor compatibility, high heat generation, and insufficient safety. Traditional modification methods cannot overcome these technical limitations. Therefore, there is an urgent need to develop a novel tread rubber compound for semi-steel radial tires and its corresponding preparation process. Summary of the Invention

[0005] The purpose of this invention is to overcome the defects of the existing technology and provide a rubber composition for hard rubber of semi-steel radial tires and its preparation method. Without adding styrene-butadiene rubber, the reaction system of tetrazine compounds and ordinary cis-butadiene rubber is optimized to improve the crosslinking reaction rate of the two. Through modification and adaptation optimization, the amount of carbon black filler in the formulation can be effectively reduced, thereby reducing the heat accumulation and rolling resistance of the rubber compound from the source, improving the aging resistance and flexural crack resistance of the rubber compound, avoiding the problems of hard rubber delamination and bead cracking, and taking into account the wear resistance, low heat generation and structural stability of the formulation to meet the requirements of tire safety.

[0006] To achieve the above objectives, one of the technical solutions of the present invention is: a rubber composition for hard rubber in semi-steel radial tires, the components of which, by mass parts, include:

[0007] Base rubber system: includes 30-50 parts of natural rubber (NR) and 50-70 parts of butadiene rubber (BR);

[0008] Reinforcing system: includes 30-60 parts carbon black, 0-30 parts silica, and 0-3 parts silane coupling agent;

[0009] Vulcanization system: including 2-4 parts insoluble sulfur, 0.5-2.5 parts vulcanization accelerator, 3-5 parts zinc oxide and 1-2 parts stearic acid;

[0010] The protective system includes 2-3 parts of antioxidant A, 0.5-1.5 parts of antioxidant B, and 1-2 parts of protective wax.

[0011] Functional additives, including 0.5 to 2 parts of low rolling resistance modifier and 0.5 to 1.5 parts of low rolling resistance dispersant.

[0012] In a preferred embodiment of the present invention, the low rolling resistance modifier is a tetrazine compound, and the low rolling resistance dispersant is an acylhydrazine compound; the mechanism of action of the tetrazine compound is to react with both rubber double bonds and the functional groups of silica simultaneously, thereby helping silica dispersion to achieve low heat generation; the mechanism of action of the acylhydrazine compound is to react with both rubber double bonds and the functional groups on the surface of carbon black simultaneously, thereby helping carbon black dispersion to achieve low heat generation and resistance to dynamic fatigue.

[0013] In a preferred embodiment of the present invention, the natural rubber is smoked sheet rubber; the butadiene rubber is a highly crystalline isotactic 1,2-polyethylene glycol (SPB) reinforced butadiene rubber with an SPB content of 12-20%; and the silica is a silica with a sieve residue of ≤0.50% (325 mesh) and a specific surface area of ​​≤160 m². 2 Silicon dioxide materials of / g or higher.

[0014] In a preferred embodiment of the present invention, the vulcanization accelerator is sulfenamide.

[0015] In a preferred embodiment of the present invention, antioxidant A is a p-phenylenediamine antioxidant, and antioxidant B is a quinoline polymeric ketone amine antioxidant.

[0016] Because low rolling resistance dispersants readily form complex structures with Zn, they must be added separately from ZnO. Low rolling resistance modifiers are easily adsorbed by silica and have high activity, allowing them to react pre-react with natural rubber to ensure their modification effect. The melting point of low rolling resistance dispersants is approximately 150℃, which facilitates dispersion and increases their reaction rate with rubber under high-temperature conditions. Adding a weakly alkaline substance (pH 7–8.5) during the mixing process effectively protects the low rolling resistance modifier, as it is prone to decomposition in acidic environments, leading to performance degradation. Weakly alkaline conditions (pH 7–8.5) inhibit this adverse reaction, thereby improving the modifier's stability. The mechanism of action is as follows:

[0017] Under acidic conditions (pH<5), nitrogen atoms on the ring are protonated, which reduces the ring electron density, causing the ring to crack and remove N2, further decomposing into ammonia or other fragments, and the low rolling resistance modifier quickly becomes ineffective.

[0018] Under weakly acidic conditions (pH 5–9), tetrazine compounds generally maintain their structural stability and reactivity without significant decomposition or failure. Among them, under weakly alkaline conditions (pH 7–9), the reactivity of tetrazine compounds is better than that under weakly acidic conditions (pH 5–7). The nitrogen atoms on the ring remain in a deprotonated state, the structure is stable, and it can react directly with the rubber matrix to form a robust modified network. The modifier is effectively protected and its performance is maintained.

[0019] Under strongly alkaline conditions (pH>9), although protonation can be suppressed, the strongly alkaline environment will degrade the modifier itself, resulting in a shortened lifespan and the modifier is still prone to failure.

[0020] Both p-phenylenediamine antioxidants and quinoline polymeric ketone amine antioxidants are weakly alkaline substances and can be used alone or in combination as alkaline protective agents.

[0021] To achieve the above objectives, the second technical solution of the present invention is: a method for preparing a rubber composition for hard rubber in semi-steel radial tires, the core of which lies in preventing the degradation of tetrazine compounds by using an alkaline protective agent and avoiding premature complexation of hydrazine compounds with zinc oxide, thereby achieving efficient reaction and full dispersion, and ultimately obtaining a rubber system with low hysteresis and low rolling resistance; including the following steps:

[0022] (1) Pre-dispersion and preliminary mixing: Natural rubber, butadiene rubber, carbon black, low rolling resistance modifier, low rolling resistance dispersant, antioxidant A and antioxidant B are added to the mixer according to the ratio and pre-dispersed at 155~165℃ and 5~25rpm for 0.5~1.5min. Then continue mixing for a total mixing time of 3~5min. After mixing, unload the material at 160~170℃ to obtain the first stage rubber compound, ensuring that all active components have reacted completely and dispersed fully, thereby maximizing low hysteresis and rolling resistance performance.

[0023] (2) Adding additives and mixing: Add silica, silane coupling agent, zinc oxide, stearic acid and protective wax to the first stage rubber compound obtained in step (1) according to the ratio and mix. The mixing temperature is 140~150℃ and the speed is 5~25rpm. Higher speed can achieve stronger shearing and uniform mixing. Maintain constant temperature mixing for 1~3min to allow zinc oxide to be evenly dispersed and obtain the second stage rubber compound.

[0024] (3) Adding accelerator to the rubber compound obtained in step (2): Add vulcanization accelerator and insoluble sulfur to the second stage rubber compound according to the ratio, and mix at 90~105℃ and 15~35rpm to obtain the accelerator rubber, namely the rubber composition for hard rubber of semi-steel radial tires.

[0025] Uncured vulcanized rubber is loaded into a vulcanizing mold or calender and vulcanized at 155~165℃ with secondary venting, venting pressure set at 10.0~15.0MPa, vulcanizing pressure set at 15.0~20.0MPa, and vulcanization for 15~25 min to obtain a vulcanized rubber composition with excellent low hysteresis and low rolling resistance properties.

[0026] Compared with the prior art, the present invention has the following beneficial effects:

[0027] This invention achieves significant reduction in heat accumulation, rolling resistance, and aging risks while maintaining or improving the rigidity of hard rubber through the synergistic effect of low rolling resistance dispersants, low rolling resistance modifiers, and weakly alkaline protective agents. At the same time, it improves tear resistance, requires less carbon black in the formulation, and the process is easy to promote. It is particularly suitable for hard rubber of semi-steel radial tires. Detailed Implementation

[0028] To make the objectives, technical solutions and advantages of the present invention clearer, the present invention will be described in more detail below with reference to specific embodiments, but the scope of protection of the present invention is not limited to these embodiments.

[0029] The sources of each raw material in the following examples and comparative examples are as follows:

[0030] Natural rubber: Smoked sheet rubber manufactured by Sheng Yufeng Rubber;

[0031] Butadiene rubber: Highly crystalline isotactic 1,2-polyethylene glycol (SPB) reinforcing butadiene rubber manufactured by Ube Rubber Co., Ltd. of Japan;

[0032] Carbon Black A: Manufactured by Ningbo Detai, with an oil absorption value (DBP) of 83~93.10. -5 m 3 / kg, nitrogen adsorption specific surface area is 73~83 10 --5 m 3 / kg;

[0033] Carbon Black B: Manufactured by Qingdao Zunshun, with an oil absorption value (DBP) of 80-90. --5 m 3 / kg, nitrogen adsorption specific surface area is 35~45 10 --5 m 3 / kg;

[0034] White carbon black: White carbon soot manufactured by Evonik United Silica Inc. Ltd.

[0035] Silane coupling agent: bis(triethoxysilylpropyl)tetrasulfide manufactured by Evonik, with a sulfur content of 21.7~23.3 parts;

[0036] A: N-(1,3-dimethylbutyl)-N'phenyl-1,4-phenylenediamine manufactured by Shandong Shangshun Chemical Co., Ltd. has a purity of over 97%.

[0037] B: 2,2,4-trimethyl-1,2-dihydroquinoline polymers manufactured by Comai Chemical, in dimer, trimer, and tetramer forms, with a purity of over 75%;

[0038] Microcrystalline wax: Microcrystalline wax manufactured by Shandong Yanggu Huatai Chemical Co., Ltd., with a molecular weight of 500~700;

[0039] Vulcanization accelerator: N-cyclohexyl-benzothiazole sulfenamide manufactured by Tianjin Kemai, melting point 98℃;

[0040] Stearic acid, zinc oxide, and sulfur are all commercially available.

[0041] Low rolling resistance dispersant: Acroad® DC-01T manufactured by Otsuka Chemicals;

[0042] Low rolling resistance modifier: Acroad® DS01 manufactured by Otsuka Chemicals.

[0043] The performance tests in the following examples and comparative examples include:

[0044] 1. Low heat generation performance test

[0045] The heat generation properties of each vulcanized rubber composition sample under dynamic load were measured using a compression heat generation tester (HBU).

[0046] Under the conditions of fixed initial temperature of 50~60℃, frequency of 8~12Hz, dynamic load of 900~1100N, and test time of 10min~30min, the core temperature T of the sample is recorded. The lower the final core temperature (Tf) of the sample, the lower the heat generation. According to the following calculation formula, the compression heat generation characteristics are expressed by an exponent. The larger the exponent, the lower the heat generation.

[0047] (Compression heat generation index) = (1 - (Tf of each formulation - Tf of the reference formulation (Comparative Example 1)) / (Tf of the reference formulation (Comparative Example 1)) × 100

[0048] 2. Tear resistance:

[0049] The crack growth test of each vulcanized rubber composition sample was measured using a De Mattia testing machine. The number of flexing cycles was set on the control panel according to the formulation properties. The testing machine was turned on, and the crack length was checked each time it was stopped. The measurement and recording were done using a low-magnification magnifying glass. The end of the test was determined according to the needs of the batch test.

[0050] 3. Rolling resistance performance test

[0051] The dynamic mechanical properties of each vulcanized rubber composition sample were measured using a viscoelastic analyzer. The tan(δ) value at 0°C was recorded during a temperature scan under dynamic strain conditions at a frequency of 10 Hz. In a manner well-known to those skilled in the art, the tan(δ)60°C value represents the rolling resistance of the material; a smaller tan(δ)60°C value indicates better hysteresis performance and lower rolling resistance.

[0052] (Rolling resistance index) = (1 - (tanδ of each formulation - tanδ of the reference formulation (Comparative Example 1)) / (tanδ of the reference formulation (Comparative Example 1)) × 100

[0053] Example 1

[0054] A rubber composition for hard rubber in semi-steel radial tires, the composition of which is shown in Table 1, is prepared by the following process:

[0055] (1) Pre-dispersion and preliminary mixing: Natural rubber, butadiene rubber, carbon black, low rolling resistance modifier, low rolling resistance dispersant, antioxidant A and antioxidant B are added to the mixer according to the ratio, and pre-dispersion is carried out at 155~165℃ and 5~35 rpm for 1 min. Then, mixing is continued, and the total mixing time reaches 4 min. After the mixing is completed, the material is discharged at 165℃ to obtain the first stage rubber compound.

[0056] (2) Adding additives and mixing: Add silica, silane coupling agent, zinc oxide, stearic acid and microcrystalline wax to the first stage rubber compound obtained in step (1) according to the ratio and mix. The mixing temperature is 145~155℃, the rotation speed is 5~25 rpm, and the constant temperature mixing is maintained for 2 min to obtain the second stage rubber compound.

[0057] (3) Adding accelerator to the rubber compound obtained in step (2): Add vulcanization accelerator and insoluble sulfur to the second stage rubber compound according to the ratio, and mix at 30°C to 100°C and 25 rpm to obtain the accelerator rubber, namely the rubber composition for hard rubber of semi-steel radial tires.

[0058] Comparative Example 1

[0059] A rubber composition, the composition of which is shown in Table 1, is prepared by the same method as in Example 1.

[0060] Comparative Example 2

[0061] A rubber composition, the composition of which is shown in Table 1, is prepared by the same method as in Example 1.

[0062] Comparative Example 3

[0063] A rubber composition, the composition of which is shown in Table 1, is prepared by the same method as in Example 1.

[0064] Comparative Example 4

[0065] A rubber composition, the composition of which is shown in Table 1, is prepared by the same method as in Example 1.

[0066] Table 1. Composition ratios of rubber compositions in Example 1 and Comparative Examples 1-4

[0067]

[0068] The rubber compositions obtained in Example 1 and Comparative Examples 1-4 were loaded into a vulcanizing mold and vulcanized at 160°C with secondary venting, a venting pressure of 10.0 MPa, and a vulcanization pressure of 15.0 MPa. The vulcanized rubber compositions were obtained after 20 minutes of vulcanization. The low heat generation properties, tear resistance, and rolling resistance of the obtained vulcanized rubber compositions were tested, and the test results are shown in Table 2.

[0069] Table 2. Performance test results of the rubber compositions in Example 1 and Comparative Examples 1-4 after vulcanization.

[0070]

[0071] As can be seen from the above test results, the rubber composition prepared by the present invention has low heat generation, tear resistance and low rolling resistance after vulcanization, and is particularly suitable for semi-steel radial tires.

[0072] The above embodiments are only used to illustrate the technical solutions of the present invention, and are not intended to limit it. Although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some or all of the technical features therein. Such modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A rubber composition for use in hard rubber of semi-steel radial tires, characterized in that, Its components, by mass parts, include: Base rubber system: includes 30-50 parts natural rubber and 50-70 parts butadiene rubber; Reinforcing system: includes 30-60 parts carbon black, 0-30 parts silica, and 0-3 parts silane coupling agent; Vulcanization system: including 2-4 parts insoluble sulfur, 0.5-2.5 parts vulcanization accelerator, 3-5 parts zinc oxide and 1-2 parts stearic acid; The protective system includes 2-3 parts of antioxidant A, 0.5-1.5 parts of antioxidant B, and 1-2 parts of protective wax. Functional additives, including 0.5 to 2 parts of low rolling resistance modifier and 0.5 to 1.5 parts of low rolling resistance dispersant.

2. The rubber composition for semi-steel radial tire tread as described in claim 1, characterized in that, The low rolling resistance modifier is a tetrazine compound, and the low rolling resistance dispersant is an acylhydrazine compound.

3. The rubber composition for semi-steel radial tire tread as described in claim 1, characterized in that, The natural rubber is smoked sheet rubber; the butadiene rubber is a highly crystalline isotactic 1,2-polyethylene resin-reinforced butadiene rubber with an SPB content of 12-20%.

4. The rubber composition for semi-steel radial tire tread as described in claim 1, characterized in that, The vulcanization accelerator is sulfenamide.

5. The rubber composition for semi-steel radial tire tread as described in claim 1, characterized in that, Antioxidant A is a p-phenylenediamine antioxidant, and antioxidant B is a quinoline polymeric ketone amine antioxidant.

6. A method for preparing a rubber composition for hard rubber of semi-steel radial tires as described in any one of claims 1-5, characterized in that, Includes the following steps: (1) Pre-dispersion and preliminary mixing: Natural rubber, butadiene rubber, carbon black, low rolling resistance modifier, low rolling resistance dispersant, antioxidant A and antioxidant B are added to the mixer according to the ratio for pre-dispersion, and then mixing is continued. After the mixing is completed, the material is discharged to obtain the first stage rubber compound. (2) Adding additives and mixing: Add silica, silane coupling agent, zinc oxide, stearic acid and protective wax to the first stage rubber compound obtained in step (1) according to the proportion and mix to obtain the second stage rubber compound; (3) Adding accelerator to the rubber compound obtained in step (2): Add vulcanization accelerator and insoluble sulfur to the second stage rubber compound according to the ratio and mix to obtain the accelerator, namely the rubber composition for hard rubber of semi-steel radial tires.

7. The method for preparing the rubber composition for hard rubber of semi-steel radial tires as described in claim 6, characterized in that, In step (1), the pre-dispersion temperature is 155~165℃, the rotation speed is 5~25rpm, and the time is 0.5~1.5min.

8. The method for preparing the rubber composition for hard rubber of semi-steel radial tires as described in claim 6, characterized in that, The cumulative mixing time in step (1) is 3~5 minutes, and the unloading temperature is 160~170℃.

9. The method for preparing the rubber composition for hard rubber of semi-steel radial tires as described in claim 6, characterized in that, In step (2), the mixing temperature is 140~150℃, the rotation speed is 5~25rpm, and the mixing time is 1~3min.