A melt processable low dielectric composition and method of making and use thereof
By coating the surface of polytetrafluoroethylene (PTFE) micropowder with benzocyclobutene prepolymer with a prepolymer conversion rate of 20%~60% and using low-temperature blending technology, combined with a low-temperature initiator, the problem of weak interfacial bonding between PTFE and the resin matrix was solved. This enabled melt processing and interfacial bonding strengthening of low-dielectric composite materials, thereby improving the mechanical and dielectric properties of the materials.
Patent Information
- Application Number
- CN202611549189.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-08
- Publication Date
- 2026-11-24
AI Technical Summary
It is difficult to ensure the interfacial bonding between PTFE and the resin matrix while obtaining melt processing capability in low dielectric PTFE composites, resulting in poor mechanical properties and moisture heat resistance of the composites.
By coating the surface of polytetrafluoroethylene micropowder with a prepolymer conversion rate of 20%~60% benzocyclobutene prepolymer, and combining it with a hydrocarbon resin with a 1,2-vinyl content of not less than 50% and a free radical initiator with a half-life temperature of 1 minute lower than the ring-opening initiation temperature, the crosslinking reaction is controlled to concentrate on the particle surface during the molding stage, forming chemical bonds.
This method achieves enhanced interfacial bonding between polytetrafluoroethylene (PTFE) and the resin matrix, ensuring the uniformity of the phase structure of the composition after melt processing and curing, improving the stability of the material's mechanical and dielectric properties, and simplifying the processing steps.
Smart Images

Figure CN123152187A_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of high-frequency electronic materials technology, and in particular to a melt-processable low-dielectric composition, its preparation method, and its application. Background Technology
[0002] The development of technologies such as 5G / 6G communication and millimeter-wave radar has placed demands on substrate and structural materials for low dielectric constants and low dielectric losses. Polytetrafluoroethylene (PTFE) has excellent dielectric properties, but its melt viscosity is very high, making it difficult to melt and process. It is generally formed by powder sintering or emulsion impregnation-lamination, which makes it difficult to manufacture complex-shaped components, and also limits dimensional accuracy and production efficiency.
[0003] Hydrocarbon resins (such as polybutadiene and styrene-butadiene copolymers) have low polarity, good dielectric properties, and can be melt-processed. However, polytetrafluoroethylene (PTFE) has low surface energy and lacks chemical affinity with non-fluoropolymers. When the two are blended, the interfacial bonding is weak, and the mechanical properties and moisture-heat resistance of the composite material are easily affected. Related technologies include crosslinking modifications to the fluoropolymer itself to improve interfacial bonding.
[0004] Benzocyclobutene resins are thermosetting low-dielectric resins that can undergo ring-opening crosslinking upon heating. Related technologies include formulating benzocyclobutene resins with other resins into a solution, followed by solution coating and lamination to produce copper-clad laminates; this method lacks melt processing capability. Another approach involves pre-grafting benzocyclobutene groups onto the resin molecular chain before formulation, but this requires additional synthesis steps.
[0005] In summary, the polytetrafluoroethylene low-dielectric composite materials in related technologies are difficult to ensure the interfacial bonding between polytetrafluoroethylene and the resin matrix while achieving melt processing capability. Summary of the Invention
[0006] In order to ensure the interfacial bonding between polytetrafluoroethylene and the resin matrix while achieving melt processability in polytetrafluoroethylene low-dielectric composite materials, this application provides a melt processable low-dielectric composition, its preparation method, and its application.
[0007] To achieve the above objectives, the technical solution adopted in this application is as follows: A melt-processable low-dielectric composition is provided, comprising, by weight: 15-45 parts of benzocyclobutene prepolymer, 30-60 parts of hydrocarbon resin, 15-40 parts of polytetrafluoroethylene micropowder, and 0.1-3 parts of free radical initiator; The benzocyclobutene prepolymer is obtained by partial prepolymerization of a difunctional benzocyclobutene monomer, and the prepolymerization conversion rate of the benzocyclobutene prepolymer is 20%~60%. The hydrocarbon resin is a polybutadiene with a 1,2-vinyl content of not less than 50% and / or a styrene-butadiene copolymer with a 1,2-vinyl content of not less than 50%. The free radical initiator is an organic peroxide, and the 1-minute half-life temperature of the organic peroxide is at least 20 °C lower than the ring-opening initiation temperature of the benzocyclobutene prepolymer. The surface of the polytetrafluoroethylene micropowder is coated with the benzocyclobutene prepolymer.
[0008] This technique allows benzocyclobutene prepolymers with a prepolymer conversion rate of 20%–60% to be low-viscosity melts at molding temperatures, enabling the composition to be melt-molded. After molding, ring-opening crosslinking occurs, and the flowability disappears. The prepolymer is pre-coated onto the surface of polytetrafluoroethylene (PTFE) micropowder, concentrating the crosslinking reaction on the particle surface and forming a crosslinked shell. Hydrocarbon resins with a 1,2-vinyl content of at least 50% can gel first under the action of an initiator and react with the o-quinone dimethane intermediate generated during ring-opening, forming chemical bonds between the shell and the matrix. The initiator's 1-minute half-life temperature is at least 20 °C lower than the ring-opening initiation temperature, ensuring that the hydrocarbon resin gels first, fixes the phase, and locks the shell in situ. The benzocyclobutene prepolymer then undergoes in-situ ring-opening crosslinking. This simultaneously solves the problems of weak interfacial bonding between PTFE and non-fluorinated resins, the inability to melt-process PTFE-vinyl composites, and the tendency for phase separation during curing of blends.
[0009] In some embodiments, the difunctional benzocyclobutene monomer is divinylsiloxane-bridged bisbenzocyclobutene.
[0010] In some embodiments, the number-average molecular weight of the hydrocarbon resin is 1,000 to 50,000; and the particle size D50 of the polytetrafluoroethylene micropowder is 0.5 to 15 μm.
[0011] In some embodiments, the gel content of the solidified product is not less than 85%, and the gel content is determined by boiling toluene Soxhlet extraction for 24 h.
[0012] In some embodiments, the mixture also includes 0.1 to 1 part of a hindered phenolic antioxidant and 0.1 to 30 parts of an inorganic filler and / or flame retardant, wherein the hindered phenolic antioxidant is used to inhibit the oxidative degradation of the hydrocarbon resin during the curing process.
[0013] This application also provides a method for preparing the melt-processable low-dielectric composition as described above, comprising the following steps: S1: The difunctional benzocyclobutene monomer is prepolymerized under a protective atmosphere to obtain a benzocyclobutene prepolymer with a prepolymerization conversion rate of 20%~60%. S2: The benzocyclobutene prepolymer is coated onto the surface of polytetrafluoroethylene micro powder to obtain coated micro powder; S3: The coated micropowder is blended with hydrocarbon resin and free radical initiator to obtain the melt-processable low-dielectric composition; S4: The melt-processable low-dielectric composition is melt-molded at a molding temperature and held at that temperature, which is lower than the ring-opening initiation temperature of the benzocyclobutene prepolymer; during the holding process, the free radical initiator decomposes and initiates the cross-linking gelation of the hydrocarbon resin to obtain a preform; S5: The blank is kept at a temperature higher than the ring-opening initiation temperature of the benzocyclobutene prepolymer to cause the benzocyclobutene prepolymer to undergo ring-opening crosslinking, thereby obtaining a cured part.
[0014] In the above preparation method, step S1 controls the prepolymer conversion rate to make the prepolymer viscosity suitable for coating and retain the ring-opening structure; step S2 coats the prepolymer onto the surface of polytetrafluoroethylene micropowder, limiting the cross-linking reaction to the particle surface; step S3 blends at low temperature to obtain a thermoplastic composition that does not gel prematurely; step S4 utilizes the low viscosity of the prepolymer to melt and mold the composition, while the initiator initiates the hydrocarbon resin gelation, fixing the shape and locking the shell in situ; step S5 heats up to cause the prepolymer to open the ring and cross-link in situ, forming an overall cross-linked network. Thus, without prior chemical modification of the components, the composition can be melt-molded and then cured to obtain a low-dielectric component with strong interfacial bonding and a uniform phase structure.
[0015] In some implementations, step S2 includes: S201: Dissolve the benzocyclobutene prepolymer in an organic solvent to obtain a prepolymer solution; S202: The prepolymer solution is mixed with the polytetrafluoroethylene micro powder and sheared and dispersed to coat the surface of the polytetrafluoroethylene micro powder with the benzocyclobutene prepolymer, thereby obtaining a coated dispersion. S203: Remove the organic solvent from the coating dispersion to obtain the coated micro powder.
[0016] In some embodiments, in step S201, the organic solvent is toluene or xylene; In step S202, the shearing and dispersion time is 10~60 min; In step S203, the removal is carried out under reduced pressure, and the removal temperature is at least 30 °C lower than the ring-opening initiation temperature of the benzocyclobutene prepolymer.
[0017] In some embodiments, in step S1, the protective atmosphere is nitrogen, and the prepolymerization temperature is 150~180 ℃; in step S3, the blending temperature is 100~130 ℃; in step S4, the molding temperature is 160~185 ℃, and the holding time is 3~15 min; step S5 is carried out under nitrogen protection, with a holding temperature of 220~250 ℃ and a holding time of 1~3 h.
[0018] This application also provides the use of the melt-processable low-dielectric compositions described above in the preparation of high-frequency copper-clad laminates, millimeter-wave antenna components, or low-dielectric structural parts.
[0019] In summary, the beneficial effects of this application include: 1. By pre-coating the surface of polytetrafluoroethylene (PTFE) micropowder with a benzocyclobutene prepolymer of controlled prepolymer conversion rate, and combining it with a hydrocarbon resin containing at least 50% 1,2-vinyl alcohol and a free radical initiator with a half-life temperature below the ring-opening initiation temperature (1 minute), the composition can be melt-flowed and molded during the molding stage. During the curing stage, a cross-linked structure chemically bonded to the hydrocarbon resin matrix is formed in situ on the PTFE micropowder surface. Therefore, the composition balances melt processing capability with interfacial bonding after curing, resulting in a more uniform phase structure in the cured product, which is beneficial for maintaining the stability of the mechanical and dielectric properties of the molded part.
[0020] 2. By arranging the steps of prepolymerization, pre-coating, low-temperature blending, melt molding and in-mold gelation, and high-temperature ring-opening and curing, the location, timing and sequence of the crosslinking reaction can be controlled. No chemical grafting modification of any components is required beforehand, and the molding and curing of the composition can be completed on conventional processing equipment. The process steps are relatively simple.
[0021] 3. When this composition is used to prepare high-frequency copper-clad laminates, millimeter-wave antenna components or low-dielectric structural components, the millimeter-wave antenna components and low-dielectric structural components can be directly obtained in complex shapes through melt molding, and the high-frequency copper-clad laminates can be prepared by impregnation lamination, making the application methods more flexible. Attached Figure Description
[0022] The accompanying drawings, which form part of this application, are used to provide a further understanding of this application. The illustrative embodiments and descriptions of this application are used to explain this application and do not constitute an undue limitation of this application. In the drawings: Figure 1 This is a calibration curve of the prepolymerization conversion rate versus Brookfield viscosity of the benzocyclobutene prepolymer of Example 1 of this application; Figure 2 This is a schematic diagram of the first process of a method for preparing a melt-processable low-dielectric composition, which is an optional embodiment of this application. Figure 3This is a schematic diagram of the second process of a method for preparing a melt-processable low-dielectric composition, which is an optional embodiment of this application. Figure 4 These are the DSC temperature rise curves of the compositions of Examples 1, 2, and 3 provided in this application; Figure 5 These are the storage modulus-temperature curves and tanδ-temperature curves of the cured products of Example 1 and Comparative Example 3 provided in this application; Figure 6 These are the FTIR spectra of the composition of Example 1 provided in this application before and after curing; Figure 7 This is the viscosity-time curve of the composition of Example 1 provided in this application at 130 °C; Figure 8 This is the TGA curve of the gel content extraction residue and pure polytetrafluoroethylene micro powder of Example 1 provided in this application; Figure 9 This is a scanning electron microscope image of the cross-section of the high-frequency copper-clad laminate obtained in Embodiment 2 of this application; Figure 10 These are the DSC temperature rise curves of the compositions obtained by procedures (a) and (c) in Example 3 provided in this application; Figure 11 This is a graph showing the relationship between the prepolymer conversion rate, melt index, and interfacial bonding strength of Example 4 provided in this application. Detailed Implementation
[0023] To enable those skilled in the art to better understand the technical solutions of this application, the technical solutions of this application will be further described below in conjunction with the accompanying drawings and embodiments.
[0024] Polytetrafluoroethylene (PTFE) is one of the polymer matrices with excellent dielectric properties, with a dielectric constant of approximately 2.1 and a dielectric loss as low as below 0.001. However, PTFE has extremely high melt viscosity (approximately 10). 10 ~10 11The dielectric strength of PTFE (on the order of Pa·s) is practically non-melt-processable, requiring powder sintering or emulsion impregnation-lamination processes for molding. This makes it difficult to fabricate complex shapes, and limits dimensional accuracy and production efficiency. Hydrocarbon resins (such as polybutadiene and styrene-butadiene copolymers) have low polarity, excellent dielectric properties, and are melt-processable. However, when blended with PTFE micropowder, the extremely low surface energy of PTFE (approximately 18 mN / m) and lack of chemical affinity with non-fluoropolymers result in weak interfacial bonding, leading to poor mechanical properties and damp heat resistance in the composite material. Benzocyclobutene (BCB) resins are high-performance thermosetting low-dielectric resins. Their four-membered rings open at temperatures above approximately 200 °C, generating highly reactive o-quinone dimethane intermediates, which can undergo self-polymerization or react with compounds containing double bonds. In related technologies, some crosslink the fluororesin itself to improve the interface, some formulate BCB resin with polyphenylene ether, PTFE, etc. to form an adhesive solution and then coat and laminate it to produce copper-clad laminates, and some pregraft BCB groups onto the hydrocarbon resin backbone before formulating the adhesive solution; among them, the adhesive solution coating-lamination route does not have melt processability, while the pregrafting route has more process steps and higher costs.
[0025] Research has revealed that three long-standing unresolved issues in PTFE-based low-dielectric composite systems—weak interfacial bonding between PTFE and non-fluorinated resins, non-melt processability of the composite system, and easy phase separation during the curing of the thermoplastic hydrocarbon phase and the thermosetting crosslinked phase—can be simultaneously addressed in a one-pot blending system by uniformly controlling the "reaction location, reaction timing, and reaction sequence": pre-coating controls the preferential occurrence of crosslinking reactions on the PTFE particle surface (location); low-temperature non-crosslinking during molding and in-situ crosslinking after molding controls the reaction timing (timing); and initiator selection and temperature grading control the reaction sequence of free radical curing and phase locking followed by ring-opening bridging (sequence). Based on this concept, this application provides a melt-processable low-dielectric composition, its preparation method, and its applications, which are detailed below.
[0026] This application provides a melt-processable low-dielectric composition, comprising, by weight: 15-45 parts of benzocyclobutene prepolymer, 30-60 parts of hydrocarbon resin, 15-40 parts of polytetrafluoroethylene micropowder, and 0.1-3 parts of free radical initiator; the benzocyclobutene prepolymer is obtained by partial prepolymerization of a bifunctional benzocyclobutene monomer, and the prepolymerization conversion rate of the benzocyclobutene prepolymer is 20%-60%; the hydrocarbon resin is polybutadiene with a 1,2-vinyl content of not less than 50% and / or a styrene-butadiene copolymer with a 1,2-vinyl content of not less than 50%; the free radical initiator is an organic peroxide, and the 1-minute half-life temperature of the organic peroxide is at least 20 °C lower than the ring-opening initiation temperature of the benzocyclobutene prepolymer; the surface of the polytetrafluoroethylene micropowder is coated with the benzocyclobutene prepolymer.
[0027] The components of this composition are described below.
[0028] Regarding benzocyclobutene prepolymers: This component is obtained by partial prepolymerization of difunctional benzocyclobutene monomers, with a prepolymer conversion rate of 20%–60%. Prepolymerization refers to the partial ring-opening polymerization of difunctional benzocyclobutene monomers under conditions below their complete curing degree. The resulting prepolymer is a flowable liquid or a low-melting-point solid in the range of room temperature to 120 °C. The prepolymer conversion rate determines the subsequent coating viscosity and processing window: when the prepolymer conversion rate is below 20%, the prepolymer is too thin, and the coating layer on the surface of polytetrafluoroethylene micropowder is easily lost during subsequent processing; when the prepolymer conversion rate is above 60%, the prepolymer lacks fluidity at the molding processing temperature, and the composition loses its melt processability. The preferred prepolymer conversion rate is 30%–50%. In this application, the prepolymerization conversion rate was determined using Fourier transform infrared spectroscopy (FTIR): based on the characteristic absorption peak area of the benzocyclobutene four-membered ring at approximately 1460 cm⁻¹, it was calculated according to the formula: "Prepolymerization conversion rate (%) = (peak area before prepolymerization - peak area after prepolymerization) ÷ peak area before prepolymerization × 100%". During the prepolymerization process, Brookfield viscosity or refractive index was used for process monitoring, and the correspondence between viscosity or refractive index readings and prepolymerization conversion rate was pre-calibrated using the aforementioned FTIR method. The calibration curves for prepolymerization conversion rate and Brookfield viscosity are shown below. Figure 1 As shown.
[0029] The benzocyclobutene prepolymer in this application has a dual function: In the molding temperature range (160~185℃), the unopened benzocyclobutene prepolymer is a low-viscosity melt, acting as an internal lubricant for the PTFE micropowder / hydrocarbon resin blend system, enabling the originally non-melt-processable PTFE-containing composite system to acquire melt flowability. At this time, the benzocyclobutene prepolymer acts as a reactive processing aid. After molding, when the temperature is raised above the ring-opening temperature, the benzocyclobutene prepolymer undergoes in-situ ring-opening crosslinking and co-cures with the hydrocarbon resin, transforming into part of a covalent crosslinked network, and its flowability automatically shuts off. In other words, the same component performs both the functions of a processing aid and a crosslinking resin in the two processing stages.
[0030] Regarding hydrocarbon resins: This component consists of polybutadiene with a 1,2-vinyl content of not less than 50% and / or a styrene-butadiene copolymer with a 1,2-vinyl content of not less than 50%. The requirement of a 1,2-vinyl content of not less than 50% ensures that the molecular chain has a sufficient number of carbon-carbon double bonds. These double bonds serve two purposes: firstly, as crosslinking sites for free radicals generated by the decomposition of free radical initiators, allowing the hydrocarbon resin to crosslink and gel at lower temperatures; secondly, as Diels-Alder addition acceptors and / or free radical grafting sites for the o-quinone dimethane intermediate generated from the ring-opening of the benzocyclobutene prepolymer, enabling covalent bonding between the benzocyclobutene prepolymer and the hydrocarbon resin, rather than simple physical entanglement. Resins whose main chain does not contain aliphatic double bonds (such as polyphenylene ether, polyimide, etc.) do not possess the above-mentioned co-crosslinking function. The hydrocarbon resin can be made by using polybutadiene with a 1,2-vinyl content of not less than 50% alone, or by using styrene-butadiene copolymer with a 1,2-vinyl content of not less than 50% alone, or by mixing the two in any proportion. The 1,2-vinyl content can be determined by proton nuclear magnetic resonance spectroscopy according to conventional methods in the art.
[0031] Regarding polytetrafluoroethylene (PTFE) micropowder: This component is coated with benzocyclobutene prepolymer, meaning that before blending with hydrocarbon resin, the surface of the PTFE particles is pre-uniformly coated with a thin layer of benzocyclobutene prepolymer (based on the pre-coating step in the preparation method). This coating structure allows subsequent crosslinking reactions to preferentially occur on the PTFE particle surface: during curing, the benzocyclobutene prepolymer in the coating layer undergoes in-situ ring-opening crosslinking on the PTFE surface, forming a crosslinked shell tightly bound to the PTFE particles, transforming the PTFE from a free filler into an anchor point for the crosslinked network; the crosslinked shell and the hydrocarbon resin matrix are further covalently bridged through the covalent reaction of o-quinone dimethane and side-attached double bonds, making the entire composition a single covalent network. Thus, the cured composition forms a three-level structure of "coating-anchoring-bridging" at the particle scale. The following parameters can be used to verify: (1) The gel content of the cured composition is not less than 85% (determined by boiling toluene Soxhlet extraction for 24 h); (2) The thermogravimetric analysis of the extraction residue of gel content determination shows that the thermal decomposition initiation temperature of PTFE is shifted relative to that of pure PTFE micro powder, indicating that the PTFE surface is covered with a cross-linked layer; (3) In the dynamic thermomechanical analysis (DMA) spectrum, the tanδ transition peak of the polybutadiene phase is shifted and broadened relative to pure cured polybutadiene, and the storage modulus in the high temperature range of 150 ℃ is significantly higher than that of the binary system without benzocyclobutene prepolymer, indicating that there is an interaction between the two networks (it should be noted that because the glass transition temperatures of the two phases are significantly different, the DMA spectrum will necessarily show two transitions, and a single transition is not used as a criterion).
[0032] Regarding the free radical initiator: This component is an organic peroxide, whose 1-minute half-life temperature is at least 20 °C lower than the ring-opening initiation temperature of the benzo[a]cyclobutene prepolymer. The ring-opening initiation temperature is determined by differential scanning calorimetry (DSC), and the ring-opening initiation temperature of the bifunctional benzo[a]cyclobutene monomer and its prepolymer is generally around 200–220 °C. The 1-minute half-life temperature is a well-known characteristic parameter of organic peroxides, indicating the temperature required for the initiator to decompose by half within 1 minute, and can be obtained from the technical data of the initiator supplier or determined by conventional methods in the art. The aforementioned temperature difference allows the free radical crosslinking of the hydrocarbon resin to complete gelation (frozen phase, molded and ready for demolding) first in the lower temperature range of 160–185 °C, while the ring-opening polymerization of the benzo[a]cyclobutene prepolymer occurs only in the higher temperature range of 220–250 °C. The two reactions are represented on the DSC curve as two separate exothermic peaks with a peak temperature difference of not less than 40 °C. This prevents the molten benzocyclobutene prepolymer from migrating and flowing away from the surface of the polytetrafluoroethylene micropowder during the ring-opening process, thus preventing phase separation. Without a low-temperature gel segment, the spatial distribution advantage established by the pre-coating is destroyed before curing is complete. Organic peroxides that meet the above selection requirements include, for example, dicumyl peroxide (DCP, 1-minute half-life temperature approximately 171 °C) and 1,3-bis(tert-butylperoxyisopropyl)benzene (BIPB, 1-minute half-life temperature approximately 182 °C). Those skilled in the art can select commercially available organic peroxides with 1-minute half-life temperatures that meet the above temperature difference requirements based on the ring-opening initiation temperature of the selected benzocyclobutene prepolymer.
[0033] In some embodiments, the 1-minute half-life temperature of the organic peroxide is 150~195 °C. A 1-minute half-life temperature not lower than 150 °C ensures that the initiator decomposes slowly and does not cause premature gelation (scorching) during the blending process (100~130 °C); a 1-minute half-life temperature not higher than 195 °C and at least 20 °C lower than the ring-opening initiation temperature ensures that the initiator fully decomposes within the holding time (3~15 min) at the molding temperature (160~185 °C), allowing the hydrocarbon resin to complete cross-linking and gelation.
[0034] In some embodiments, differential scanning calorimetry (DSC) was performed on the melt-processable low-dielectric composition at a heating rate of 10 °C / min. The DSC curve showed two separate exothermic peaks, corresponding to the exothermic free radical crosslinking of the hydrocarbon resin and the exothermic ring-opening polymerization of the benzocyclobutene prepolymer, respectively. The temperature difference between the peaks of the two exothermic peaks was not less than 40 °C. The peak temperature difference of not less than 40 °C indicates that the two crosslinking reactions can be effectively separated in time, which is direct evidence of the feasibility of the "gel-lock-in first, then ring-opening bridging" temperature-graded curing procedure.
[0035] In some embodiments, the difunctional benzocyclobutene monomer is divinylsiloxane-bridged benzocyclobutene (DVS-BCB), with the chemical name 1,3-bis(2-bicyclo[4.2.0]oct-1,3,5-trien-3-ylvinyl)-1,1,3,3-tetramethyldisiloxane (CAS No.: 117732-87-3). DVS-BCB is commercially available or prepared using methods known in the art, such as the Heck coupling reaction of 4-bromobenzocyclobutene with 1,1,3,3-tetramethyl-1,3-divinyldisiloxane.
[0036] In some embodiments, the number-average molecular weight of the hydrocarbon resin is 1000-50000; the particle size D50 of the polytetrafluoroethylene (PTFE) micropowder is 0.5-15 μm. The number-average molecular weight can be determined using gel permeation chromatography (GPC) according to conventional methods in the art; for example, the number-average molecular weight of the hydrocarbon resin can be 1000, 3000, 10000, 30000, or 50000. The particle size D50 can be determined using a laser particle size analyzer according to conventional methods in the art; for example, the particle size D50 of the PTFE micropowder can be 0.5 μm, 5 μm, 10 μm, or 15 μm. Hydrocarbon resins with a number-average molecular weight within the above range have suitable melt viscosity at the blending temperature, ensuring both blendability and the mechanical properties of the cured part. PTFE micropowder with a particle size D50 within the above range is easily and uniformly coated by the prepolymer solution and dispersed in the matrix.
[0037] In some embodiments, the gel content of the cured product of the melt-processable low-dielectric composition is not less than 85%, and the gel content is determined by Soxhlet extraction with boiling toluene for 24 h. The gel content reflects the degree of formation of the covalent cross-linked network, and is determined as follows: a cured sample is weighed and placed in a Soxhlet extractor for continuous extraction with boiling toluene for 24 h. The residue is then removed, dried to constant weight, and weighed. The gel content is calculated as the percentage of the residue mass to the mass of the sample before extraction. A gel content of not less than 85% indicates that the composition has formed a substantially complete covalent cross-linked network after curing.
[0038] In some embodiments, the melt flow rate of the melt-processable low-dielectric composition, measured according to GB / T 3682.1-2018 at 150 °C and a load of 2.16 kg, is 0.5~10 g / 10 min. A melt flow rate within this range indicates that the composition has melt flowability suitable for injection molding, extrusion, or compression molding before molding, i.e., melt processability. A melt flow rate that is too low results in insufficient melt flowability and difficulty in molding, while a flow rate that is too high corresponds to a low prepolymer conversion rate of the benzocyclobutene prepolymer and easy loss of the coating layer during processing.
[0039] In some embodiments, the melt-processable low-dielectric composition further includes 0.1 to 1 part of a hindered phenolic antioxidant, which is used to inhibit the oxidative degradation of the hydrocarbon resin during the curing process. High-vinyl hydrocarbon resins contain numerous carbon-carbon double bonds in their molecular chains, making them prone to oxidative degradation in the high-temperature curing stage (especially the post-curing stage at 220-250 °C). The hindered phenolic antioxidant inhibits this degradation process by capturing oxidative free radicals, ensuring the stability of the dielectric and mechanical properties of the cured part. The hindered phenolic antioxidant can be a commercially available variety commonly used in the art, such as pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] (antioxidant 1010) or octadecyl β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate (antioxidant 1076).
[0040] In some embodiments, the melt-processable low-dielectric composition may further include other optional additives, such as inorganic fillers (silica, alumina, etc.), flame retardants, etc., and the amount of optional additives may be 0.1 to 30 parts by weight. It should be noted that in applications where dielectric performance is a priority, the use of inorganic fillers should be reduced or eliminated to avoid polarity loss introduced by the fillers.
[0041] The preparation method of the melt-processable low-dielectric composition provided in this application will be described below. For example... Figure 2 As shown, the preparation method includes the following steps S1 to S5, which will be described one by one in sequence below, and the specific implementation method of each step will be described immediately afterward.
[0042] S1: The difunctional benzocyclobutene monomer is prepolymerized under a protective atmosphere to obtain a benzocyclobutene prepolymer with a prepolymerization conversion rate of 20%~60%.
[0043] In step S1, the protective atmosphere is preferably nitrogen, and the prepolymerization temperature is preferably 150~180 ℃. During the prepolymerization process, the prepolymerization progress is monitored using Brookfield viscosity or refractive index, and the prepolymerization conversion rate is calculated according to the aforementioned FTIR calibration relationship. After reaching the target prepolymerization conversion rate, the material is cooled for later use. The selection of the prepolymerization conversion rate needs to consider both the subsequent coating quality and processing fluidity: if the prepolymerization conversion rate is too low, the coating layer will be too thin and easily lose fluidity; if it is too high, the fluidity will be insufficient at the molding processing temperature. The prepolymerization conversion rate is preferably 30%~50%, and more preferably around 40%.
[0044] S2: The benzocyclobutene prepolymer is coated onto the surface of polytetrafluoroethylene micropowder to obtain coated micropowder.
[0045] In step S2, pre-coating is a crucial step to ensure that the cross-linking reaction preferentially occurs on the surface of the PTFE particles. If pre-coating is not performed and the components are directly blended, the benzocyclobutene prepolymer will be uniformly dispersed in the matrix, and after curing, the BCB cross-linking network will be uniformly distributed in the matrix. The PTFE surface will remain in non-bonded contact, resulting in limited interface improvement. (Refer to...) Figure 3 Step S2 is preferably implemented through the following sub-steps S201 to S203: S201: Dissolve the benzocyclobutene prepolymer in an organic solvent to obtain a prepolymer solution. The organic solvent is preferably toluene or xylene, which has good solubility for the benzocyclobutene prepolymer, a moderate boiling point, is easy to remove in subsequent processes, and will not cause the polytetrafluoroethylene micropowder to swell or degrade.
[0046] S202: The prepolymer solution is mixed with the polytetrafluoroethylene (PTFE) micropowder and sheared to disperse the benzocyclobutene prepolymer onto the surface of the PTFE micropowder, resulting in a coated dispersion. The shearing dispersion time is preferably 10-60 min, which can be performed using a high-speed shear disperser; if the shearing dispersion time is too short, the coating will be uneven, and if it is too long, energy consumption will increase without further improving the coating quality.
[0047] S203: Remove the organic solvent from the coated dispersion to obtain the coated micropowder. The removal is preferably carried out under reduced pressure, and the removal temperature is at least 30 °C lower than the ring-opening initiation temperature of the benzocyclobutene prepolymer, for example, 80-120 °C. Limiting the temperature difference between the removal temperature and the ring-opening initiation temperature is to prevent premature ring-opening and cross-linking of the benzocyclobutene prepolymer during solvent extraction, thereby maintaining its melt flowability in subsequent processing stages.
[0048] S3: The coated micropowder is blended with hydrocarbon resin and free radical initiator to obtain the melt-processable low-dielectric composition.
[0049] In step S3, the preferred blending temperature is 100-130 °C. Blending can be performed using a Banbury mixer or a twin-screw extruder, resulting in thermoplastic granules or rubber compounds. The blending temperature must be lower than both the ring-opening initiation temperature of the benzocyclobutene prepolymer and the rapid decomposition temperature of the free radical initiator. For example, dicumyl peroxide (DCP) has a 10-hour half-life temperature of approximately 117 °C. Blending at 120 °C for 15 minutes results in a decomposition rate of less than 5%, which will not cause premature gelation. If the blending temperature exceeds 140 °C, the initiator decomposition intensifies, posing a risk of scorching. In step S3, the aforementioned hindered phenolic antioxidants and other optional additives may also be added according to the formulation.
[0050] S4: The melt-processable low-dielectric composition is melt-formed at a molding temperature and held at that temperature, which is lower than the ring-opening initiation temperature of the benzocyclobutene prepolymer; during the holding process, the free radical initiator decomposes and initiates the cross-linking gelation of the hydrocarbon resin to obtain a preform.
[0051] In step S4, the molding temperature is preferably 160~185 ℃, and the holding time is preferably 3~15 min. The melt molding method can be injection molding, extrusion, or compression molding, which can be selected according to the shape of the target part, such as molding into an antenna radome, connector housing, waveguide component, or sheet. At this stage, the benzocyclobutene prepolymer has not yet opened its ring and acts as an internal lubricant for the blend system in the form of a low-viscosity melt. The composition can flow and be molded at a temperature much lower than the melting point of PTFE (327 ℃). PTFE is always carried by the reactive carrier in the form of a solid filler. At the same time, the free radical initiator decomposes and initiates free radical cross-linking of hydrocarbon resins. The system completes a first stage of gelation and solidification in the mold, that is, molding and solidification are completed in the same temperature range. Demolding yields a blank with a fixed shape. The cross-linked network formed by the first stage of gelation freezes the phase of the system and locks the pre-coated benzocyclobutene prepolymer shell on the surface of polytetrafluoroethylene micropowder, preventing it from migrating and being lost during subsequent heating. The melt index and pot life (viscosity-time characteristics) of the composition are indicators of the processability window, and their values are shown in the Examples section below.
[0052] S5: The blank is kept at a temperature higher than the ring-opening initiation temperature of the benzocyclobutene prepolymer to cause the benzocyclobutene prepolymer to undergo ring-opening crosslinking, thereby obtaining a cured part.
[0053] In step S5, the heat treatment is preferably carried out under nitrogen protection, with a preferred temperature of 220-250 °C and a preferred holding time of 1-3 h. Within this temperature range, the benzocyclobutene prepolymer undergoes ring-opening to generate an o-quinone dimethane intermediate, resulting in two types of reactions: (i) the benzocyclobutene prepolymer itself polymerizes into a network; (ii) the o-quinone dimethane intermediate undergoes Diels-Alder addition and / or free radical grafting co-crosslinking with the residual double bonds in the hydrocarbon resin crosslinking network (the free radical curing in step S4 only consumes a portion of the double bonds). This results in the in-situ formation of a benzocyclobutene crosslinking network covalently bridged to the hydrocarbon resin matrix on the surface of the polytetrafluoroethylene (PTFE) micropowder, yielding a cured part. Nitrogen protection is used to inhibit the oxidative degradation of the residual double bonds in the hydrocarbon resin at high temperatures.
[0054] In some embodiments, the preferred process conditions for each step of the preparation method are as follows: in step S1, the protective atmosphere is nitrogen, and the prepolymerization temperature is 150~180 ℃; in step S3, the blending temperature is 100~130 ℃; in step S4, the molding temperature is 160~185 ℃, and the holding time is 3~15 min; in step S5, the process is carried out under nitrogen protection, the holding temperature is 220~250 ℃, and the holding time is 1~3 h.
[0055] In addition to the melt molding route described above, the composition of this application can also be processed via a lamination route: the coated micro powder obtained in step S2 is dissolved in an organic solvent with hydrocarbon resin and free radical initiator to form an adhesive solution, which is then impregnated with low dielectric glass fiber cloth. After baking to remove the solvent, a semi-cured sheet is obtained. The semi-cured sheets are stacked and coated with copper foil on the surface. First, a first-stage gel is completed by hot pressing at a lower temperature, and then a second-stage curing is completed by hot pressing at 200~250 ℃ to obtain a high-frequency copper-clad laminate.
[0056] This application also provides the application of the above-mentioned melt-processable low-dielectric composition in the preparation of high-frequency copper-clad laminates, millimeter-wave antenna components, or low-dielectric structural parts. The millimeter-wave antenna component is, for example, a millimeter-wave radome; the low-dielectric structural part is, for example, a connector housing, waveguide components, or other complex-shaped components. Because the composition exhibits melt flowability during the molding stage and its flowability automatically closes after solidification, the aforementioned components can be directly molded into complex shapes via injection molding, extrusion, or compression molding, overcoming the process limitations of PTFE-based low-dielectric materials, which can only be sintered or laminated; high-frequency copper-clad laminates can be prepared via the aforementioned lamination route.
[0057] The present application will be further described below with reference to specific embodiments and comparative examples.
[0058] The specifications and sources of the main raw materials used in the examples are as follows: the difunctional benzocyclobutene monomer is divinylsiloxane-bridged benzocyclobutene (DVS-BCB, CAS No.: 117732-87-3), which is commercially available; the hydrocarbon resin is liquid polybutadiene with a 1,2-vinyl content of about 70% and a number average molecular weight of about 3000. A specific grade of commercially available high-vinyl liquid polybutadiene with a 1,2-vinyl content and number average molecular weight meeting the requirements can be selected, or it can be prepared by anionic polymerization (using a polar structure modifier to control the 1,2-vinyl content). The 1,2-vinyl content is determined by 1H NMR spectroscopy, and the number average molecular weight is determined by gel permeation chromatography; the polytetrafluoroethylene micropowder has a particle size D50 of about 5 μm and is commercially available; the free radical initiator is dicumyl peroxide (DCP, with a 1-minute half-life temperature of about 171°C). The 1-minute half-life temperature of the benzo[a]cyclobutene prepolymer (BIPB, with a half-life temperature of approximately 182 °C) and 1,3-bis(tert-butylperoxyisopropyl)benzene (BIPB, with a half-life temperature of approximately 182 °C) were selected to be at least 20 °C lower than the ring-opening initiation temperature of the benzo[a]cyclobutene prepolymer (as determined by DSC, the ring-opening initiation temperature of the benzo[a]cyclobutene prepolymer used in the embodiments of this application is approximately 215 °C). The tert-butyl hydroperoxide (TBHP, with a half-life temperature of approximately 230 °C), the hindered phenolic antioxidant (antioxidant 1010), toluene, xylene, low dielectric fiber cloth, and copper foil were all conventional commercially available products. Example 1
[0059] The melt-processable low-dielectric composition of this embodiment is prepared according to the aforementioned preparation method, and the specific preparation parameters are as follows: S1: Prepolymerize DVS-BCB monomers at 165 °C under nitrogen protection, monitor with Brookfield viscosity and convert according to FTIR calibration relationship until the prepolymerization conversion rate reaches 40%, then cool for later use.
[0060] S2: Dissolve 30 parts by weight of the obtained benzocyclobutene prepolymer in toluene, add 25 parts by weight of polytetrafluoroethylene micro powder with a particle size of about 5 μm (D50), and disperse at high speed for 30 min to make the prepolymer uniformly coat the surface of the polytetrafluoroethylene micro powder. Remove toluene under reduced pressure at 100℃ to obtain coated micro powder.
[0061] S3: The obtained coated micro powder is mixed with 45 parts by weight of liquid polybutadiene with a 1,2-vinyl content of about 70% and a number average molecular weight of about 3000, 1 part by weight of dicumyl peroxide, and 0.3 parts by weight of antioxidant 1010 at 120 °C for 15 min, and then granulated to obtain thermoplastic composition granules.
[0062] S4: The obtained composition granules were injection molded at 170 °C and kept in the mold for 8 min to complete a gelation stage. The sample strip and antenna radome blank were then demolded.
[0063] S5: The obtained blank is kept at 240 ℃ for 2 h under nitrogen protection to complete the two-stage curing and obtain the cured part. Example 2
[0064] The melt-processable low-dielectric composition of this embodiment is prepared according to the aforementioned lamination route: Steps S1 and S2 are the same as in Example 1. The obtained coated micro powder is dissolved in xylene with 50 parts by weight of liquid polybutadiene and 0.8 parts by weight of 1,3-bis(tert-butylperoxyisopropyl)benzene to prepare an adhesive solution. The adhesive solution is then impregnated with low dielectric glass fiber cloth and baked at 120 °C to remove the solvent, resulting in a prepreg. Eight prepregs are stacked and double-sided coated with copper foil. The first stage of gelation is completed by hot pressing at 175 °C and 10 MPa for 30 min, followed by heating to 245 °C and holding for 1.5 h to complete the second stage of curing, resulting in a high-frequency copper-clad laminate. Example 3
[0065] Specifically, a temperature-graded curing verification example is provided.
[0066] The remaining conditions were the same as in Example 1. Three curing procedures were compared: (a) staged curing, i.e., holding at 170 °C for 8 min followed by holding at 240 °C for 2 h; (b) curing directly at 240 °C for 2 h without in-mold heat preservation gel after molding; (c) staged curing according to procedure (a) after replacing dicumyl peroxide with tert-butyl hydroperoxide (TBHP, half-life temperature of about 230 °C at 1 minute, higher than 195 °C). The independent contribution of the low-temperature pre-gel lock to the performance of the cured part was verified by using DSC exothermic peak resolution, gel content, storage modulus at 150 °C, and interfacial bonding strength as comparative indicators. Example 4
[0067] Specifically, an example of verifying the prepolymerization conversion rate window is provided.
[0068] In step S1, the prepolymerization conversion rates of the benzocyclobutene prepolymer were set to 20%, 40%, and 60%, respectively, with the remaining conditions the same as in Example 1. The effect of the prepolymerization conversion rate on the coating quality and processing fluidity was investigated, and the prepolymerization conversion rate window of 20% to 60% was verified.
[0069] Comparative Example 1 Without performing the pre-coating step S2, the benzocyclobutene prepolymer, polytetrafluoroethylene micropowder, liquid polybutadiene, dicumyl peroxide, and antioxidant 1010 were directly blended according to the proportions of Example 1, with all other conditions the same as in Example 1. This comparative example was used to verify the contribution of pre-coating to the interfacial anchoring structure.
[0070] Comparative Example 2 The hydrocarbon resin was replaced with an equal amount of commercially available polyphenylene oxide (PPO) powder, with all other conditions the same as in Example 1. This comparative example was used to verify the indispensability of a hydrocarbon resin with a 1,2-vinyl content of not less than 50% and its co-crosslinking mechanism.
[0071] Comparative Example 3 Without the addition of benzocyclobutene prepolymer, a binary filled system consisting only of liquid polybutadiene, polytetrafluoroethylene micropowder, dicumyl peroxide, and antioxidant 1010 was constructed. The amounts of each component were the same as in Example 1, and all other conditions were the same as in Example 1. This comparative example was used to verify the dual function of the benzocyclobutene prepolymer (reactive processing aid and covalently bridged resin).
[0072] Comparative Example 4 The composition was injection molded at 170 °C and then cured in one step by directly heating to 240 °C for 2 h without in-mold thermal insulation gelation, with other conditions the same as in Example 1. This comparative example was used to verify the performance degradation caused by shell migration and phase separation of benzocyclobutene prepolymer without a low-temperature phase-locking stage.
[0073] The performance testing methods for the samples obtained in the above embodiments and comparative examples are as follows.
[0074] Gel content: The solidified sample was weighed (recorded as m0) and placed in a Soxhlet extractor. It was continuously extracted with boiling toluene for 24 h. The residue was then vacuum dried at 80 °C to constant weight and weighed (recorded as m1). The gel content (%) was calculated according to the formula: "Gel content (%) = m1 ÷ m0 × 100%". This indicator characterizes the degree of covalent cross-linking network formation. It should be noted that because polytetrafluoroethylene (PTFE) micropowder is insoluble in boiling toluene, the mass of the residue includes the mass of PTFE micropowder. If the degree of cross-linking of the organic phase needs to be characterized separately, it can be calculated by deducting the mass fraction of PTFE micropowder in the formulation from the mass of the residue. The data in Table 1 of this application are the measured values without deducting the PTFE micropowder content.
[0075] DSC curing behavior: Approximately 5-10 mg of the composition granules were heated from 50 °C to 300 °C at a heating rate of 10 °C / min under a nitrogen atmosphere, and the exothermic peak was recorded. The DSC heating curves of Example 1, Comparative Example 2, and Comparative Example 3 are shown below. Figure 4 As shown, the two exothermic peaks correspond to the exothermic free radical crosslinking of the hydrocarbon resin and the exothermic ring-opening polymerization of the benzocyclobutene prepolymer, respectively. The difference in the peak temperatures of the two peaks characterizes the feasibility of temperature-stage curing. A peak temperature difference of not less than 40 °C indicates that the two reactions can be effectively separated in time.
[0076] DMA: Using a three-point bending mode at a frequency of 1 Hz, the temperature was increased from -100 ℃ to 250 ℃ at a heating rate of 3 ℃ / min. The changes in storage modulus and loss factor tanδ with temperature were recorded. The interaction between the two networks was characterized by the shift of the peak temperature of the polybutadiene phase tanδ transition relative to pure cured polybutadiene (peak temperature approximately -20 ℃) and the degree of peak broadening. The storage modulus at 150 ℃ was recorded to characterize the mechanical retention capability at high temperatures. The storage modulus-temperature curves and tanδ-temperature curves of Example 1 and Comparative Example 3 are shown below. Figure 5 As shown.
[0077] FTIR: Infrared spectra of the composition before and after curing were measured. The intensity changes of the vinyl absorption peak (approximately 910 cm⁻¹) and the characteristic absorption peak of the benzocyclobutene four-membered ring (approximately 1460 cm⁻¹) before and after curing were compared. The depletion of these two characteristic peaks was used as evidence of co-curing of hydrocarbon resin free radical crosslinking and benzocyclobutene ring-opening. The FTIR spectra before and after curing are shown below. Figure 6 As shown.
[0078] Pot life: Particles of the composition were placed in a rotational rheometer at 130 °C (upper limit of blending temperature), and the viscosity-time curve was recorded. The time required for the viscosity to double from the initial viscosity was defined as the viscosity doubling time. A viscosity doubling time of not less than 30 min indicates that the composition has a processing window that meets the requirements for blending, storage, transportation, and melt molding operations. The viscosity-time curve of the composition in Example 1 at 130 °C is shown below. Figure 7 As shown.
[0079] Melt flow index: According to GB / T 3682.1-2018, the melt mass flow rate of the composition granules before molding is determined at 150 ℃ and 2.16 kg load. The test is started after preheating for 1 min after loading to avoid the rapid decomposition of the initiator during the test due to excessively high test temperature, which would lead to premature gelation. This index characterizes the melt processability of the composition.
[0080] Interfacial bonding strength: For cured parts, laminated shear test specimens were prepared according to GB / T 7124-2008, and the tensile shear strength (MPa) was measured; for copper clad laminates, the copper foil peel strength (N / mm) was measured according to GB / T 4722-2017; both were used to characterize the interfacial bonding strength between the PTFE phase and the matrix.
[0081] Dielectric constant and dielectric loss: measured at 10 GHz using the separated dielectric resonant cavity method. Copper-clad laminate samples can also be measured according to GB / T 4722-2017.
[0082] Water absorption rate: The sample was placed in an environment of 85 ℃ and 85% relative humidity for 96 h. After being removed and dried, the sample was weighed. The percentage increase in mass before and after moisture absorption was used to characterize the reliability of moisture heat resistance.
[0083] Thermogravimetric analysis (TGA) of the extraction residue: The extraction residue obtained from gel content determination was subjected to thermogravimetric analysis (nitrogen atmosphere, 10℃ / min), and its thermal decomposition onset temperature was compared with that of pure PTFE micropowder. The thermal decomposition onset temperature of PTFE in the residue shifted relative to that of pure PTFE micropowder, indicating that the PTFE particles are covered with a cross-linked shell. The TGA curves of the extraction residue and pure PTFE micropowder are shown below. Figure 8 As shown.
[0084] Cross-sectional morphology characterization: The copper-clad laminate obtained in Example 2 was cut, mounted, and polished. Its cross-sectional morphology was observed using a scanning electron microscope in backscattered electron imaging (BSE) mode with an accelerating voltage of 20 kV. The fluorinated polytetrafluoroethylene (PTFE) micropowder appeared brighter than the hydrocarbon resin matrix, while the glass fibers appeared light gray. This indicated the dispersion state and interfacial bonding of the PTFE micropowder within the resin region between the glass fiber bundles. The obtained cross-sectional SEM images are shown below. Figure 9 As shown.
[0085] The test results for each embodiment and comparative example are shown in Table 1.
[0086] Table 1 Performance test results of each embodiment and comparative example
[0087] Note: Example 2 is a copper-clad laminate sample; melt flow index and DMA-related indicators (three-point bending method for molding compound strips) are not applicable. The DSC curves of Comparative Examples 2 and 3 show only one exothermic peak, with no peak temperature difference. The transformation behavior of the polyphenylene ether phase in Comparative Example 2 is different from that of the polybutadiene phase; therefore, the tanδ peak displacement indicator is not applicable. In the interfacial bonding strength column, Examples 1, 3, 4, and Comparative Examples 1-4 show tensile shear strength (MPa), while Example 2 shows copper foil peel strength of the copper-clad laminate (N / mm).
[0088] The technical effects of the technical solution in this application will be analyzed below in conjunction with the data in Table 1.
[0089] (1) Regarding interfacial bonding. Example 1 uses a pre-coating and in-situ co-curing process. The gel content of the cured product reaches 92%, and the tensile shear strength reaches 6.5 MPa, which is significantly higher than that of Comparative Example 1 (2.8 MPa) which was directly blended. Comparative Example 1 and Example 1 have the same chemical composition and similar gel content (90% vs. 92%), but the interfacial bonding strength differs by more than double. This indicates that the gel content reflects the total amount of network, while the significant improvement in interfacial bonding strength comes from the spatial distribution established by the pre-coating - the cross-linking reaction preferentially occurs on the PTFE surface, transforming PTFE from a free filler into an anchor point of the covalent network. Comparative Example 3, which does not contain benzocyclobutene prepolymer, has a gel content reduced to 84% (below 85%) and an interfacial bonding strength of only 2.1 MPa. Comparative Example 2, which uses polyphenylene ether instead of high-vinyl hydrocarbon resin, cannot co-crosslink with o-quinone dimethane intermediate because the main chain does not contain aliphatic double bonds. The gel content is significantly reduced to 55% and the interfacial bonding strength is only 2.5 MPa. Furthermore, the DSC only shows a single exothermic peak of benzocyclobutene self-polymerization, proving that the co-crosslinking mechanism of high-vinyl hydrocarbon resin is indispensable.
[0090] (2) Regarding melt processability. The composition of Example 1 had a melt index of 3.2 g / 10 min (150 ℃ / 2.16 kg) before molding, and a viscosity doubling time of approximately 95 min (not less than 30 min) at 130 ℃ (the upper limit of the blending temperature). The processing window was ample, and it could be successfully injection molded into complex shapes such as test strips and antenna radome blanks. After molding, the flowability was automatically shut off after two-stage curing, and the parts were heat-set. Comparative Example 3, lacking the low-viscosity benzocyclobutene prepolymer that provides internal lubrication, had a melt index of only 0.4 g / 10 min, making it difficult to melt mold. This indicates that the reactive processing aid function of the benzocyclobutene prepolymer is the key to achieving melt processability.
[0091] (3) Regarding the uniformity of phase structure and high-temperature performance. In Example 3, the graded curing procedure (a) had a gel content of 91%, a storage modulus of 415 MPa at 150 ℃, and an interfacial bonding strength of 6.3 MPa, which were all superior to the direct one-step high-temperature curing procedure (b) (90%, 305 MPa, and 4.6 MPa, respectively) and the procedure (c) using the high half-life temperature initiator TBHP (78%, 235 MPa, and 3.8 MPa, respectively). In procedure (b), the two crosslinking reactions were carried out simultaneously at high temperature, and the molten benzocyclobutene prepolymer had migrated and lost from the PTFE surface before gelation; in procedure (c), TBHP decomposed slowly at 170 ℃ (the half-life at this temperature is on the order of several hours), and the hydrocarbon resin hardly crosslinked during the 8-minute heat preservation time. The low-temperature section could not form a gel network to lock the phase state, and the DSC peak temperature difference was only 23 ℃ (below 40 ℃). The two reactions could not be effectively separated. The DSC temperature rise curves of procedure (a) and procedure (c) are as follows. Figure 10As shown. In Comparative Example 4, after the low-temperature gelation segment was removed, the storage modulus at 150 °C decreased from 420 MPa to 300 MPa, and the interfacial bonding strength decreased from 6.5 MPa to 4.2 MPa. This results corroborate those of Example 3, jointly demonstrating that the temperature grading procedure of "first gelation and phase locking, then ring-opening bridging" has an independent contribution to the performance of the cured part.
[0092] (4) Regarding the prepolymer conversion window. The relationship between prepolymer conversion and melt index and interfacial bonding strength is as follows: Figure 11 As shown in Example 4, the results indicate that at a prepolymer conversion rate of 20%, the prepolymer exhibits low viscosity and good processing fluidity (melt index 6.4 g / 10min), but the coating layer is relatively thin, and the interfacial bonding strength decreases to 4.9 MPa after curing. At a prepolymer conversion rate of 60%, the coating quality and cross-linked network integrity are optimal (gel content 93%, storage modulus at 150 °C 430 MPa), but the melt index decreases to 0.6 g / 10min, and the processing fluidity deteriorates significantly. At a prepolymer conversion rate of 40%, the coating quality and processing fluidity achieve the best balance (melt index 3.3 g / 10min, interfacial bonding strength 6.5 MPa). Therefore, 20%–60% is a feasible window, and 30%–50% is the preferred range.
[0093] (5) Regarding dielectric properties, resistance to damp heat, and process simplicity. The composition of this application consists entirely of low-polarity components. The dielectric constant of the cured product of Example 1 is 2.38, the dielectric loss is 0.0021 (10 GHz), and the water absorption rate is only 0.08% after 96 hours at 85 ℃ / 85%RH, demonstrating excellent dielectric properties and resistance to damp heat. In contrast, Comparative Example 2, due to the inability to form a complete co-crosslinked network, poor interfacial bonding, and the presence of unreacted residual components, has a dielectric constant of 2.52 and a dielectric loss of 0.0035, exceeding the expected low dielectric window. Furthermore, the entire preparation process does not require pre-chemical grafting or surface grafting modification of any components; a one-pot blending method is sufficient. The process steps and costs are significantly superior to pre-grafted molecular design routes.
[0094] The foregoing has shown and described the basic principles, main features, and advantages of this application. Those skilled in the art should understand that this application is not limited to the above embodiments. The embodiments and descriptions in the specification are merely illustrative of the principles of this application. Various changes and modifications can be made to this application without departing from the spirit and scope thereof, and all such changes and modifications fall within the scope of this application as claimed. The scope of protection of this application is defined by the appended claims and their equivalents.
Claims
1. A melt-processable low-dielectric composition, characterized in that, By weight, it comprises: 15-45 parts of benzocyclobutene prepolymer, 30-60 parts of hydrocarbon resin, 15-40 parts of polytetrafluoroethylene micro powder, and 0.1-3 parts of free radical initiator; The benzocyclobutene prepolymer is obtained by partial prepolymerization of a difunctional benzocyclobutene monomer, and the prepolymerization conversion rate of the benzocyclobutene prepolymer is 20%~60%. The hydrocarbon resin is a polybutadiene with a 1,2-vinyl content of not less than 50% and / or a styrene-butadiene copolymer with a 1,2-vinyl content of not less than 50%. The free radical initiator is an organic peroxide, and the 1-minute half-life temperature of the organic peroxide is at least 20 °C lower than the ring-opening initiation temperature of the benzocyclobutene prepolymer. The surface of the polytetrafluoroethylene micropowder is coated with the benzocyclobutene prepolymer.
2. The melt-processable low-dielectric composition according to claim 1, characterized in that, The difunctional benzocyclobutene monomer is a divinylsiloxane-bridged benzocyclobutene.
3. The melt-processable low-dielectric composition according to claim 1 or 2, characterized in that, The number average molecular weight of the hydrocarbon resin is 1000~50000; the particle size D50 of the polytetrafluoroethylene micro powder is 0.5~15 μm.
4. The melt-processable low-dielectric composition according to claim 1 or 2, characterized in that, The gel content of the solidified product is not less than 85%, and the gel content is determined by boiling toluene Soxhlet extraction for 24 h.
5. The melt-processable low-dielectric composition according to claim 1 or 2, characterized in that, It also includes 0.1 to 1 part of hindered phenolic antioxidant and 0.1 to 30 parts of inorganic filler and / or flame retardant, wherein the hindered phenolic antioxidant is used to inhibit the oxidative degradation of the hydrocarbon resin during the curing process.
6. A method for preparing a melt-processable low-dielectric composition according to any one of claims 1 to 5, characterized in that, Includes the following steps: S1: The difunctional benzocyclobutene monomer is prepolymerized under a protective atmosphere to obtain a benzocyclobutene prepolymer with a prepolymerization conversion rate of 20%~60%. S2: The benzocyclobutene prepolymer is coated onto the surface of polytetrafluoroethylene micro powder to obtain coated micro powder; S3: The coated micropowder is blended with hydrocarbon resin and free radical initiator to obtain the melt-processable low-dielectric composition; S4: The melt-processable low-dielectric composition is melt-formed at a molding temperature and held at that temperature, wherein the molding temperature is lower than the ring-opening initiation temperature of the benzocyclobutene prepolymer; During the heat preservation process, the free radical initiator decomposes and initiates the cross-linking gelation of the hydrocarbon resin to obtain a blank; S5: The blank is kept at a temperature higher than the ring-opening initiation temperature of the benzocyclobutene prepolymer to allow the benzocyclobutene prepolymer to undergo ring-opening crosslinking, thereby obtaining a cured part.
7. The preparation method according to claim 6, characterized in that, Step S2 includes: S201: Dissolve the benzocyclobutene prepolymer in an organic solvent to obtain a prepolymer solution; S202: The prepolymer solution is mixed with the polytetrafluoroethylene micro powder and sheared and dispersed to coat the surface of the polytetrafluoroethylene micro powder with the benzocyclobutene prepolymer, thereby obtaining a coated dispersion. S203: Remove the organic solvent from the coating dispersion to obtain the coated micro powder.
8. The preparation method according to claim 7, characterized in that, In step S201, the organic solvent is toluene or xylene; In step S202, the shearing and dispersion time is 10~60 min; In step S203, the removal is carried out under reduced pressure, and the removal temperature is at least 30 °C lower than the ring-opening initiation temperature of the benzocyclobutene prepolymer.
9. The preparation method according to any one of claims 6 to 8, characterized in that, In step S1, the protective atmosphere is nitrogen, and the prepolymerization temperature is 150~180 ℃; in step S3, the blending temperature is 100~130 ℃; in step S4, the molding temperature is 160~185 ℃, and the holding time is 3~15 min; in step S5, the process is carried out under nitrogen protection, with a holding temperature of 220~250 ℃ and a holding time of 1~3 h.
10. The use of the melt-processable low-dielectric composition according to any one of claims 1 to 5 in the preparation of high-frequency copper-clad laminates, millimeter-wave antenna components or low-dielectric structural parts.