High-strength low-temperature-resistant rubber material and preparation method thereof

By combining cis-butadiene rubber, ethylene propylene diene monomer (EPDM) rubber, and modified phenyl silicone rubber, and introducing UPy-modified vinyl incomplete cage-like silsesquioxane, the problems of strength and compatibility of rubber materials at low temperatures were solved, and a high-strength, low-temperature resistant rubber material with excellent low-temperature performance and good interfacial bonding strength was prepared.

CN123152188APending Publication Date: 2026-11-24TAICANG GUANLIAN POLYMERIC MATERIAL
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611554962.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-09
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing rubber materials cannot simultaneously meet the requirements of high strength and excellent low-temperature resistance. Furthermore, conventional low-temperature resistant silicone rubber and diene rubber have compatibility issues when used together, requiring complex solvent-based grafting processes or solvent-based wet mixing processes. The interfacial bonding depends on a single grafting site.

Method used

A ternary system combining cis-butadiene rubber, ethylene propylene diene monomer (EPDM) rubber, and modified phenyl silicone rubber was adopted. Through the chemical bonding between the aminopropylsiloxane chain segments in the modified phenyl silicone rubber and the epoxidized liquid polybutadiene, combined with the introduction of reversible quadruple hydrogen bond crosslinking points in the rubber matrix by UPy modified vinyl incomplete cage-like silsesquioxane, multiple binding sites were formed, improving compatibility and interfacial bonding strength. High-strength low-temperature resistant rubber materials were prepared by conventional internal mixing-open milling-compression vulcanization process.

Benefits of technology

It achieves good mechanical properties in low-temperature environments, with tensile strength exceeding 16 MPa, high tear strength, low low-temperature compression set, and low brittle temperature. The material can still maintain excellent elasticity and mechanical properties at low temperatures.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

This invention relates to the field of rubber materials technology, specifically to a high-strength, low-temperature resistant rubber material and its preparation method. The invention discloses a high-strength, low-temperature resistant rubber material and its preparation method. This rubber material is mainly composed of butadiene rubber, ethylene propylene diene monomer (EPDM) rubber, and modified phenyl silicone rubber, combined with UPy-modified vinyl incomplete cage-like silsesquioxane, silica, carbon black, silane coupling agent, cold-resistant plasticizer, epoxidized liquid polybutadiene, and vulcanization system additives. In this invention, the UPy-modified vinyl incomplete cage-like silsesquioxane possesses both reversible hydrogen bonding crosslinking and co-crosslinking effects; the resulting high-strength, low-temperature resistant rubber material exhibits excellent mechanical properties and low-temperature resistance, making it suitable for sealing and vibration damping products in extremely cold environments.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of rubber materials technology, specifically to a high-strength, low-temperature resistant rubber material and its preparation method. Background Technology

[0002] Rubber seals and vibration damping products are widely used in aerospace, rail transportation, polar equipment, and industrial equipment in high-altitude and cold regions. These applications require rubber materials to maintain their elasticity and mechanical properties over long periods in low-temperature environments. However, most rubbers will vitrify at low temperatures due to the freezing of molecular chain segments or crystallization due to the regular arrangement of molecular chains, resulting in loss of elasticity, a sharp increase in hardness, and seal failure.

[0003] Existing rubber materials struggle to simultaneously meet the requirements of high strength and excellent low-temperature resistance. Furthermore, the compatibility issues inherent in conventional low-temperature resistant silicone rubbers blended with diene rubbers typically necessitate complex solvent-based grafting or wet compounding processes, with interfacial bonding relying solely on a single grafting site. Therefore, developing a rubber material that combines high strength, excellent low-temperature resistance, strong interfacial bonding, and simple processing remains a pressing technical challenge in this field. Summary of the Invention

[0004] The purpose of this invention is to provide a high-strength, low-temperature resistant rubber material and its preparation method, so as to solve the problems mentioned in the background art.

[0005] To solve the above-mentioned technical problems, the present invention provides the following technical solution: a method for preparing a high-strength, low-temperature resistant rubber material, comprising the following steps:

[0006] Butadiene rubber, ethylene propylene diene monomer (EPDM) rubber, and modified phenyl silicone rubber are added to a mixer and plasticized for 2-4 minutes. Then, zinc oxide, stearic acid, and antioxidant are added and mixed evenly. Silica, carbon black, and silane coupling agent are added, and the mixture is heated to 140-150℃ for 3-5 minutes. The temperature is then lowered to below 100℃, and UPy modified vinyl incomplete cage-like silsesquioxane, epoxidized liquid polybutadiene, and cold-resistant plasticizer are added. After mixing evenly, the mixture is discharged. The resulting rubber compound is transferred to a two-roll mill, and a peroxide crosslinking agent is added. The mixture is mixed evenly at a roll temperature not exceeding 110℃, and then sheeted to obtain a compound. The compound is then molded and vulcanized at 150-160℃, followed by a second-stage vulcanization at 170-180℃ for 1-2 hours to obtain a high-strength, low-temperature resistant rubber material.

[0007] Further, the preparation method of the modified phenyl silicone rubber is as follows: octamethylcyclotetrasiloxane, tetramethyltetraphenylcyclotetrasiloxane, tetramethyltetravinylcyclotetrasiloxane, N-(β-aminoethyl)-γ-aminopropylmethyldimethoxysilane, and tetramethyldivinyldisiloxane are added to a reaction vessel and mixed. Under nitrogen protection, tetramethylammonium hydroxide silanolate catalyst is added, and polymerization is carried out at 105°C. The temperature is then raised to 150°C for equilibrium reaction. Finally, the temperature is raised to 190°C to decompose the catalyst and remove low molecular weight substances under reduced pressure. The modified phenyl silicone rubber raw material is then discharged.

[0008] Furthermore, the preparation method of the UPy modified vinyl incomplete cage-like silsesquioxane is as follows:

[0009] S1: Disperse vinyltrichlorosilane in acetone, add distilled water dropwise while stirring, and reflux at 40~60℃ for 24~30h. The reaction solution is filtered, washed with acetone, and dried to obtain vinyl incomplete cage-like silsesquioxane containing silanol groups.

[0010] S2: UPy-NCO monomer and silanol-containing vinyl incomplete cage silsesquioxane are dispersed in anhydrous acetone and reacted at 40-50℃ for 3-4 hours with dibutyltin dilaurate as catalyst to obtain UPy modified vinyl incomplete cage silsesquioxane.

[0011] Furthermore, in S1, the mass ratio of distilled water to vinyltrichlorosilane is 5~5.5:1.

[0012] Furthermore, in S2, UPy-NCO reacts with a vinyl incomplete cage-like silsesquioxane containing silanol groups at a molar ratio of isocyanate groups to silanol groups of (1.0~1.1):1.

[0013] Furthermore, in S2, the UPy-NCO monomer is prepared by reacting hexamethylene diisocyanate with 2-amino-4-hydroxy-6-methylpyrimidine.

[0014] Furthermore, the epoxidized liquid polybutadiene has a molecular weight of 2000~4000 and an epoxy value of 2.0~4.0 mmol / g.

[0015] Furthermore, in the high-strength low-temperature resistant rubber material, the content of each component by weight is as follows: 60-80 parts of butadiene rubber, 10-20 parts of ethylene propylene diene monomer (EPDM) rubber, 10-20 parts of modified phenyl silicone rubber, 3-6 parts of UPy modified vinyl incomplete cage-like silsesquioxane, 20-40 parts of silica, 5-15 parts of carbon black, 1-4 parts of silane coupling agent, 5-15 parts of cold-resistant plasticizer, 5-12 parts of epoxidized liquid polybutadiene, 3-5 parts of zinc oxide, 1-2 parts of stearic acid, 2-4 parts of antioxidant, and 1.5-3 parts of peroxide crosslinking agent; wherein, the sum of the weight parts of butadiene rubber, EPDM rubber, and modified phenyl silicone rubber is 100 parts.

[0016] Furthermore, the silane coupling agent is at least one of vinyltrimethoxysilane, vinyltris(β-methoxyethoxy)silane, and methacryloxypropyltrimethoxysilane.

[0017] Furthermore, the antioxidant is at least one of antioxidant 445, antioxidant MB, antioxidant RD, and antioxidant 4010NA; the cold-resistant plasticizer is at least one of dioctyl sebacate and dioctyl adipate.

[0018] Furthermore, the peroxide crosslinking agent is at least one of dicumyl peroxide and 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane.

[0019] Compared with the prior art, the beneficial effects achieved by the present invention are:

[0020] This invention employs a ternary system of butadiene rubber, ethylene propylene diene monomer (EPDM) rubber, and modified phenyl silicone rubber: the butadiene rubber has a flexible molecular chain and a low glass transition temperature, giving the material excellent low-temperature elasticity; the EPDM rubber has a saturated main chain, giving the material excellent weather resistance; the phenylsiloxane segments introduced into the modified phenyl silicone rubber can disrupt the regularity of the polysiloxane molecular chain and inhibit its low-temperature crystallization. The synergistic effect of the three components enables the material to maintain good performance for a long time in low-temperature environments.

[0021] In this invention, the aminopropylsiloxane segments in the modified phenyl silicone rubber can chemically bond with the epoxy groups of epoxidized liquid polybutadiene. The polybutadiene segments of the epoxidized liquid polybutadiene can then be co-cured with cis-butadiene rubber and EPDM rubber under the action of peroxides. Furthermore, the hydrogen bonding between the UPy groups and each component creates multiple bonding sites of "chemical bonds + hydrogen bonds" at the interface between the silicone rubber phase and the diene rubber phase, significantly improving the compatibility and interfacial bonding strength between the silicone rubber and the diene rubber. Simultaneously, the pre-reaction of the epoxidized liquid polybutadiene with the aminopropyl groups blocks the active amino groups, reducing the capture of peroxide free radicals by the amino groups and ensuring vulcanization efficiency.

[0022] This invention introduces reversible quadruple hydrogen bond crosslinking points into a rubber matrix by modifying vinyl-based incomplete cage-like silsesquioxanes with UPy (ureidopyrimidinone). The UPy groups can form quadruple hydrogen bond dimers, and under external force, these hydrogen bonds preferentially undergo "breakage-reorganization," effectively dissipating energy, passivating and deflecting crack tips. Simultaneously, the cage-like silsesquioxane nanoparticles exert physical reinforcement and pinning effects, resulting in a tensile strength exceeding 16 MPa, achieving a balance between high strength and excellent low-temperature resistance. Furthermore, the UPy-modified vinyl-based incomplete cage-like silsesquioxanes also act as a co-crosslinking agent: the vinyl groups retained on the cage-like structure surface undergo co-crosslinking with the rubber molecular chains under the action of a peroxide crosslinking agent, anchoring the nanoparticles in the crosslinking network through chemical bonds. This significantly increases the crosslinking density, preventing nanoparticle migration and aggregation in the matrix, further enhancing the material's mechanical properties and dimensional stability. In preparing vinyl incomplete cage-like silsesquioxanes containing silanol groups, this invention controls the mass ratio of distilled water to vinyltrichlorosilane to be 5~5.5:1. This ensures that the hydrolysis-condensation reaction proceeds fully while avoiding the problems of uncontrolled hydrolysis-condensation, reduced graftable silanol sites, and decreased product stability caused by excessive distilled water. The resulting intermediate has good stability, controllable grafting reaction, and high batch-to-batch stability of the product.

[0023] This invention adds carbon black and silica in the same batch at a high temperature and heat-treats them. The filler is evenly dispersed under high shear and high temperature conditions, avoiding the problem of poor dispersion of inorganic fillers in the rubber matrix and further ensuring the mechanical properties of the material. The invention adopts a conventional internal mixing-open milling-compression vulcanization process, which is simple to operate and suitable for industrial production. Detailed Implementation

[0024] The technical solutions of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.

[0025] Materials and their sources used in this invention: UPy-NCO monomer was prepared by reacting hexamethylene diisocyanate with 2-amino-4-hydroxy-6-methylpyrimidine and purchased from Xi'an Ruixi Biotechnology Co., Ltd.; BR9000 butadiene rubber was purchased from Daqing Petrochemical Branch of China National Petroleum Corporation; EPDM 4045 ethylene propylene diene monomer was purchased from Jilin Petrochemical Branch of China National Petroleum Corporation; silica (HB-151 type) was purchased from Hubei Huifu Nanomaterials Co., Ltd.; carbon black was N550 carbon black (wet process) and purchased from Shandong Wanhua Tianhe New Materials Co., Ltd.; silane coupling agent was vinyltrimethoxysilane; cold-resistant plasticizer was dioctyl sebacate; epoxidized liquid polybutadiene was purchased from Kunshan Castel Polymer Materials Co., Ltd., type M; antioxidant was antioxidant 445; peroxide crosslinking agent was dicumyl peroxide; and the remaining raw materials were all commercially available industrial-grade products.

[0026] Example 1: A method for preparing a high-strength, low-temperature resistant rubber material, comprising the following steps:

[0027] Butadiene rubber, ethylene propylene diene monomer (EPDM) rubber, and modified phenyl silicone rubber were added to a mixer and plasticized for 2 minutes. Then, zinc oxide, stearic acid, and antioxidant were added and mixed evenly. Silica, carbon black, and silane coupling agent were added, and the mixture was heated to 140°C for 5 minutes. The temperature was lowered to below 100°C, and UPy modified vinyl incomplete cage-like silsesquioxane, epoxidized liquid polybutadiene, and cold-resistant plasticizer were added. After mixing evenly, the mixture was discharged. The resulting rubber compound was transferred to a two-roll mill, and a peroxide crosslinking agent was added. The mixture was mixed evenly at a roll temperature not exceeding 110°C, and then sheeted to obtain a compound. The compound was molded and vulcanized at 150°C, and then vulcanized in a second stage at 170°C for 2 hours to obtain a high-strength, low-temperature resistant rubber material.

[0028] The high-strength, low-temperature resistant rubber material comprises: 60 kg of butadiene rubber, 20 kg of ethylene propylene diene monomer (EPDM) rubber, 20 kg of modified phenyl silicone rubber, 3 kg of UPy modified vinyl incomplete cage-like silsesquioxane, 20 kg of silica, 5 kg of carbon black, 1 kg of silane coupling agent, 5 kg of cold-resistant plasticizer, 5 kg of epoxidized liquid polybutadiene, 3 kg of zinc oxide, 1 kg of stearic acid, 2 kg of antioxidant, and 1.5 kg of peroxide crosslinking agent.

[0029] The modified phenyl silicone rubber is prepared by:

[0030] 100g of octamethylcyclotetrasiloxane, 20g of tetramethyltetraphenylcyclotetrasiloxane, 8g of tetramethyltetravinylcyclotetrasiloxane, 6g of N-(β-aminoethyl)-γ-aminopropylmethyldimethoxysilane and 0.5g of tetramethyldivinyldisiloxane were added to a reaction vessel and mixed. Under nitrogen protection, 0.02g of tetramethylammonium hydroxide silanolate catalyst was added, and polymerization was carried out at 105℃ for 2h. Then the temperature was raised to 150℃ for equilibration reaction for 2h. Finally, the temperature was raised to 190℃ to decompose the catalyst and remove low molecular weight substances under reduced pressure for 2h. The modified phenyl silicone rubber raw material was then discharged.

[0031] The preparation method of the UPy modified vinyl incomplete cage-like silsesquioxane is as follows:

[0032] S1: Vinyltrichlorosilane is dispersed in acetone, and distilled water is slowly added dropwise while stirring. The mass ratio of distilled water to vinyltrichlorosilane is 5:1. The mixture is refluxed at 40°C for 30 h. The reaction solution is filtered, washed with acetone, and dried at 40°C to obtain vinyl incomplete cage-like silsesquioxane containing silanol groups.

[0033] S2: UPy-NCO monomer and silanol-containing vinyl incomplete cage silsesquioxane are dispersed in anhydrous acetone and reacted at 40°C for 4 h with dibutyltin dilaurate as catalyst to obtain UPy-modified vinyl incomplete cage silsesquioxane; wherein, the molar ratio of UPy-NCO to silanol-containing vinyl incomplete cage silsesquioxane is 1.0:1.

[0034] Example 2: A method for preparing a high-strength, low-temperature resistant rubber material, comprising the following steps:

[0035] Butadiene rubber, ethylene propylene diene monomer (EPDM) rubber, and modified phenyl silicone rubber are added to a mixer and plasticized for 3 minutes. Then, zinc oxide, stearic acid, and antioxidant are added and mixed evenly. Silica, carbon black, and silane coupling agent are added, and the mixture is heated to 145°C for 4 minutes. The temperature is then lowered to below 100°C, and UPy-modified vinyl incomplete cage-like silsesquioxane, epoxidized liquid polybutadiene, and cold-resistant plasticizer are added. After mixing evenly, the mixture is discharged. The resulting rubber compound is transferred to a two-roll mill, and a peroxide crosslinking agent is added. The mixture is mixed evenly at a roll temperature not exceeding 110°C, and then sheeted to obtain a compound. The compound is then molded and vulcanized at 155°C, followed by a second-stage vulcanization at 175°C for 1.5 hours to obtain a high-strength, low-temperature resistant rubber material. The high-strength, low-temperature resistant rubber material includes:

[0036] 70 kg of butadiene rubber, 18 kg of ethylene propylene diene monomer (EPDM) rubber, 12 kg of modified phenyl silicone rubber, 5 kg of UPy modified vinyl incomplete cage-type silsesquioxane, 35 kg of silica, 10 kg of carbon black, 3 kg of silane coupling agent, 9 kg of cold-resistant plasticizer, 10 kg of epoxidized liquid polybutadiene, 4 kg of zinc oxide, 1.5 kg of stearic acid, 3 kg of antioxidant, and 2 kg of peroxide crosslinking agent;

[0037] The modified phenyl silicone rubber is prepared by:

[0038] 100g of octamethylcyclotetrasiloxane, 20g of tetramethyltetraphenylcyclotetrasiloxane, 8g of tetramethyltetravinylcyclotetrasiloxane, 6g of N-(β-aminoethyl)-γ-aminopropylmethyldimethoxysilane and 0.5g of tetramethyldivinyldisiloxane were added to a reaction vessel and mixed. Under nitrogen protection, 0.02g of tetramethylammonium hydroxide silanolate catalyst was added, and polymerization was carried out at 105℃ for 2h. Then the temperature was raised to 150℃ for equilibration reaction for 2h. Finally, the temperature was raised to 190℃ to decompose the catalyst and remove low molecular weight substances under reduced pressure for 2h. The modified phenyl silicone rubber raw material was then discharged.

[0039] The preparation method of the UPy modified vinyl incomplete cage-like silsesquioxane is as follows:

[0040] S1: Vinyltrichlorosilane is dispersed in acetone, and distilled water is slowly added dropwise while stirring. The mass ratio of distilled water to vinyltrichlorosilane is 5.25:1. The mixture is refluxed at 50°C for 28 hours. The reaction solution is filtered, washed with acetone, and dried at 45°C to obtain vinyl incomplete cage-like silsesquioxane containing silanol groups.

[0041] S2: UPy-NCO monomer and silanol-containing vinyl incomplete cage silsesquioxane are dispersed in anhydrous acetone and reacted at 45°C for 3.5 h with dibutyltin dilaurate as catalyst to obtain UPy modified vinyl incomplete cage silsesquioxane.

[0042] Example 3: A method for preparing a high-strength, low-temperature resistant rubber material, comprising the following steps:

[0043] Butadiene rubber, ethylene propylene diene monomer (EPDM) rubber, and modified phenyl silicone rubber are added to a mixer and plasticized for 4 minutes. Then, zinc oxide, stearic acid, and antioxidant are added and mixed evenly. Silica, carbon black, and silane coupling agent are added, and the mixture is heated to 150°C for 5 minutes. The temperature is then lowered to below 100°C, and UPy modified vinyl incomplete cage-like silsesquioxane, epoxidized liquid polybutadiene, and cold-resistant plasticizer are added. After mixing evenly, the mixture is discharged. The resulting rubber compound is transferred to a two-roll mill, and a peroxide crosslinking agent is added. The mixture is mixed evenly at a roll temperature not exceeding 110°C, and then sheeted to obtain a compound. The compound is then molded and vulcanized at 160°C, followed by a second-stage vulcanization at 180°C for 1 hour to obtain a high-strength, low-temperature resistant rubber material. The high-strength, low-temperature resistant rubber material includes:

[0044] 80 kg of butadiene rubber, 10 kg of ethylene propylene diene monomer (EPDM) rubber, 10 kg of modified phenyl silicone rubber, 6 kg of UPy modified vinyl incomplete cage-like silsesquioxane, 40 kg of silica, 15 kg of carbon black, 4 kg of silane coupling agent, 15 kg of cold-resistant plasticizer, 12 kg of epoxidized liquid polybutadiene, 5 kg of zinc oxide, 2 kg of stearic acid, 4 kg of antioxidant, and 3 kg of peroxide crosslinking agent;

[0045] The modified phenyl silicone rubber is prepared by:

[0046] 100g of octamethylcyclotetrasiloxane, 20g of tetramethyltetraphenylcyclotetrasiloxane, 8g of tetramethyltetravinylcyclotetrasiloxane, 6g of N-(β-aminoethyl)-γ-aminopropylmethyldimethoxysilane and 0.5g of tetramethyldivinyldisiloxane were added to a reaction vessel and mixed. Under nitrogen protection, 0.02g of tetramethylammonium hydroxide silanolate catalyst was added, and polymerization was carried out at 105℃ for 2h. Then the temperature was raised to 150℃ for equilibration reaction for 2h. Finally, the temperature was raised to 190℃ to decompose the catalyst and remove low molecular weight substances under reduced pressure for 2h. The modified phenyl silicone rubber raw material was then discharged.

[0047] The preparation method of the UPy modified vinyl incomplete cage-like silsesquioxane is as follows:

[0048] S1: Vinyltrichlorosilane is dispersed in acetone, and distilled water is slowly added dropwise while stirring. The mass ratio of distilled water to vinyltrichlorosilane is 5.5:1. The mixture is refluxed at 60°C for 24 hours. The reaction solution is filtered, washed with acetone, and dried at 50°C to obtain vinyl incomplete cage-like silsesquioxane containing silanol groups.

[0049] S2: UPy-NCO monomer and silanol-containing vinyl incomplete cage silsesquioxane are dispersed in anhydrous acetone and reacted at 50°C for 3 h with dibutyltin dilaurate as catalyst to obtain UPy-modified vinyl incomplete cage silsesquioxane; wherein, the molar ratio of UPy-NCO to silanol-containing vinyl incomplete cage silsesquioxane is 1.1:1.

[0050] Comparative Example 1: An equal amount of silanol-containing vinyl incomplete cage silsesquioxane was used instead of UPy-modified vinyl incomplete cage silsesquioxane; the remaining parameters were the same as in Example 1.

[0051] Butadiene rubber, ethylene propylene diene monomer (EPDM) rubber, and modified phenyl silicone rubber were added to a mixer and plasticized for 2 minutes. Then, zinc oxide, stearic acid, and antioxidant were added and mixed evenly. Silica, carbon black, and silane coupling agent were added, and the mixture was heated to 140°C for 5 minutes. The temperature was lowered to below 100°C, and UPy modified vinyl incomplete cage-like silsesquioxane, epoxidized liquid polybutadiene, and cold-resistant plasticizer were added. After mixing evenly, the mixture was discharged. The resulting rubber compound was transferred to a two-roll mill, and a peroxide crosslinking agent was added. The mixture was mixed evenly at a roll temperature not exceeding 110°C, and then sheeted to obtain a compound. The compound was molded and vulcanized at 150°C, and then vulcanized in a second stage at 170°C for 2 hours to obtain a high-strength, low-temperature resistant rubber material.

[0052] The high-strength, low-temperature resistant rubber material comprises: 60 kg of butadiene rubber, 20 kg of ethylene propylene diene monomer (EPDM) rubber, 20 kg of modified phenyl silicone rubber, 3 kg of silanol-containing vinyl incomplete cage-like silsesquioxane, 20 kg of silica, 5 kg of carbon black, 1 kg of silane coupling agent, 5 kg of cold-resistant plasticizer, 5 kg of epoxidized liquid polybutadiene, 3 kg of zinc oxide, 1 kg of stearic acid, 2 kg of antioxidant, and 1.5 kg of peroxide crosslinking agent.

[0053] The modified phenyl silicone rubber is prepared by:

[0054] 100g of octamethylcyclotetrasiloxane, 20g of tetramethyltetraphenylcyclotetrasiloxane, 8g of tetramethyltetravinylcyclotetrasiloxane, 6g of N-(β-aminoethyl)-γ-aminopropylmethyldimethoxysilane and 0.5g of tetramethyldivinyldisiloxane were added to a reaction vessel and mixed. Under nitrogen protection, 0.02g of tetramethylammonium hydroxide silanolate catalyst was added, and polymerization was carried out at 105℃ for 2h. Then the temperature was raised to 150℃ for equilibration reaction for 2h. Finally, the temperature was raised to 190℃ to decompose the catalyst and remove low molecular weight substances under reduced pressure for 2h. The modified phenyl silicone rubber raw material was then discharged.

[0055] The method for preparing the silanol-containing vinyl incomplete cage-like silsesquioxane is as follows:

[0056] Vinyltrichlorosilane was dispersed in acetone, and distilled water was slowly added dropwise with stirring. The mass ratio of distilled water to vinyltrichlorosilane was 5:1. The mixture was refluxed at 40°C for 30 h. The reaction solution was filtered, washed with acetone, and dried at 40°C to obtain vinyl incomplete cage-like silsesquioxane containing silanol groups.

[0057] Comparative Example 2: In the preparation of vinyl incomplete cage-like silsesquioxanes containing silanol groups, the amount of distilled water was increased, and the other parameters were the same as in Example 1.

[0058] Butadiene rubber, ethylene propylene diene monomer (EPDM) rubber, and modified phenyl silicone rubber were added to a mixer and plasticized for 2 minutes. Then, zinc oxide, stearic acid, and antioxidant were added and mixed evenly. Silica, carbon black, and silane coupling agent were added, and the mixture was heated to 140°C for 5 minutes. The temperature was lowered to below 100°C, and UPy modified vinyl incomplete cage-like silsesquioxane, epoxidized liquid polybutadiene, and cold-resistant plasticizer were added. After mixing evenly, the mixture was discharged. The resulting rubber compound was transferred to a two-roll mill, and a peroxide crosslinking agent was added. The mixture was mixed evenly at a roll temperature not exceeding 110°C, and then sheeted to obtain a compound. The compound was molded and vulcanized at 155°C, and then vulcanized in a second stage at 175°C for 2 hours to obtain a high-strength, low-temperature resistant rubber material.

[0059] The high-strength, low-temperature resistant rubber material comprises: 60 kg of butadiene rubber, 20 kg of ethylene propylene diene monomer (EPDM) rubber, 20 kg of modified phenyl silicone rubber, 3 kg of UPy modified vinyl incomplete cage-like silsesquioxane, 20 kg of silica, 5 kg of carbon black, 1 kg of silane coupling agent, 5 kg of cold-resistant plasticizer, 5 kg of epoxidized liquid polybutadiene, 3 kg of zinc oxide, 1 kg of stearic acid, 2 kg of antioxidant, and 1.5 kg of peroxide crosslinking agent.

[0060] The modified phenyl silicone rubber is prepared by:

[0061] 100g of octamethylcyclotetrasiloxane, 20g of tetramethyltetraphenylcyclotetrasiloxane, 8g of tetramethyltetravinylcyclotetrasiloxane, 6g of N-(β-aminoethyl)-γ-aminopropylmethyldimethoxysilane and 0.5g of tetramethyldivinyldisiloxane were added to a reaction vessel and mixed. Under nitrogen protection, 0.02g of tetramethylammonium hydroxide silanolate catalyst was added, and polymerization was carried out at 105℃ for 2h. Then the temperature was raised to 150℃ for equilibration reaction for 2h. Finally, the temperature was raised to 190℃ to decompose the catalyst and remove low molecular weight substances under reduced pressure for 2h. The modified phenyl silicone rubber raw material was then discharged.

[0062] The preparation method of the UPy modified vinyl incomplete cage-like silsesquioxane is as follows:

[0063] S1: Vinyltrichlorosilane is dispersed in acetone, and distilled water is slowly added dropwise while stirring. The mass ratio of distilled water to vinyltrichlorosilane is 7.5:1. The mixture is refluxed at 40°C for 30 hours. The reaction solution is filtered, washed with acetone, and dried at 40°C to obtain vinyl incomplete cage-like silsesquioxane containing silanol groups.

[0064] S2: UPy-NCO monomer and silanol-containing vinyl incomplete cage silsesquioxane are dispersed in anhydrous acetone and reacted at 40°C for 4 h with dibutyltin dilaurate as catalyst to obtain UPy-modified vinyl incomplete cage silsesquioxane; wherein, the molar ratio of UPy-NCO to silanol-containing vinyl incomplete cage silsesquioxane is 1.0:1.

[0065] Comparative Example 3: No epoxidized liquid polybutadiene was added to the raw materials, and the other parameters were the same as in Example 1.

[0066] Butadiene rubber, ethylene propylene diene monomer (EPDM) rubber, and modified phenyl silicone rubber were added to a Banbury mixer and plasticized for 2 minutes. Then, zinc oxide, stearic acid, and antioxidant were added and mixed evenly. Silica, carbon black, and silane coupling agent were added, and the mixture was heated to 140°C for 5 minutes. The temperature was then lowered to below 100°C, and UPy modified vinyl incomplete cage-like silsesquioxane and cold-resistant plasticizer were added. After mixing evenly, the mixture was discharged. The resulting rubber compound was transferred to a two-roll mill, and a peroxide crosslinking agent was added. The mixture was mixed evenly at a roll temperature not exceeding 110°C, and then sheeted to obtain a compound. The compound was then molded and vulcanized at 160°C, followed by a two-stage vulcanization at 180°C for 2 hours to obtain a high-strength, low-temperature resistant rubber material.

[0067] The high-strength, low-temperature resistant rubber material comprises: 60 kg of butadiene rubber, 20 kg of ethylene propylene diene monomer (EPDM) rubber, 20 kg of modified phenyl silicone rubber, 3 kg of UPy modified vinyl incomplete cage-like silsesquioxane, 20 kg of silica, 5 kg of carbon black, 1 kg of silane coupling agent, 5 kg of cold-resistant plasticizer, 3 kg of zinc oxide, 1 kg of stearic acid, 2 kg of antioxidant, and 1.5 kg of peroxide crosslinking agent.

[0068] The modified phenyl silicone rubber is prepared by:

[0069] 100g of octamethylcyclotetrasiloxane, 20g of tetramethyltetraphenylcyclotetrasiloxane, 8g of tetramethyltetravinylcyclotetrasiloxane, 6g of N-(β-aminoethyl)-γ-aminopropylmethyldimethoxysilane and 0.5g of tetramethyldivinyldisiloxane were added to a reaction vessel and mixed. Under nitrogen protection, 0.02g of tetramethylammonium hydroxide silanolate catalyst was added, and polymerization was carried out at 105℃ for 2h. Then the temperature was raised to 150℃ for equilibration reaction for 2h. Finally, the temperature was raised to 190℃ to decompose the catalyst and remove low molecular weight substances under reduced pressure for 2h. The modified phenyl silicone rubber raw material was then discharged.

[0070] The preparation method of the UPy modified vinyl incomplete cage-like silsesquioxane is as follows:

[0071] S1: Vinyltrichlorosilane is dispersed in acetone, and distilled water is slowly added dropwise while stirring. The mass ratio of distilled water to vinyltrichlorosilane is 5:1. The mixture is refluxed at 40°C for 30 h. The reaction solution is filtered, washed with acetone, and dried at 40°C to obtain vinyl incomplete cage-like silsesquioxane containing silanol groups.

[0072] S2: UPy-NCO monomer and silanol-containing vinyl incomplete cage silsesquioxane are dispersed in anhydrous acetone and reacted at 40°C for 4 h with dibutyltin dilaurate as catalyst to obtain UPy-modified vinyl incomplete cage silsesquioxane; wherein, the molar ratio of UPy-NCO to silanol-containing vinyl incomplete cage silsesquioxane is 1.0:1.

[0073] Comparative Example 4: No UPy-modified vinyl incomplete cage silsesquioxane was added, and the other parameters were the same as in Example 1.

[0074] Polybutadiene rubber, ethylene propylene diene monomer (EPDM) rubber, and modified phenyl silicone rubber were added to a mixer and plasticized for 2 minutes. Then, zinc oxide, stearic acid, and antioxidant were added and mixed evenly. Silica, carbon black, and silane coupling agent were added, and the mixture was heated to 140°C for 5 minutes. The temperature was lowered to below 100°C, and epoxidized liquid polybutadiene and a cold-resistant plasticizer were added. After mixing evenly, the mixture was discharged. The resulting rubber compound was transferred to a two-roll mill, and a peroxide crosslinking agent was added. The mixture was mixed evenly at a roll temperature not exceeding 110°C, and then sheeted to obtain a compound. The compound was then molded and vulcanized at 150°C, followed by a two-stage vulcanization at 170°C for 2 hours to obtain a high-strength, low-temperature resistant rubber material.

[0075] The high-strength, low-temperature resistant rubber material comprises: 60 kg of butadiene rubber, 20 kg of ethylene propylene diene monomer (EPDM) rubber, 20 kg of modified phenyl silicone rubber, 20 kg of silica, 5 kg of carbon black, 1 kg of silane coupling agent, 5 kg of cold-resistant plasticizer, 5 kg of epoxidized liquid polybutadiene, 3 kg of zinc oxide, 1 kg of stearic acid, 2 kg of antioxidant, and 1.5 kg of peroxide crosslinking agent.

[0076] The modified phenyl silicone rubber is prepared by:

[0077] 100g of octamethylcyclotetrasiloxane, 20g of tetramethyltetraphenylcyclotetrasiloxane, 8g of tetramethyltetravinylcyclotetrasiloxane, 6g of N-(β-aminoethyl)-γ-aminopropylmethyldimethoxysilane and 0.5g of tetramethyldivinyldisiloxane were added to a reactor and mixed. Under nitrogen protection, 0.02g of tetramethylammonium hydroxide silanolate catalyst was added, and polymerization was carried out at 105℃ for 2h. Then, the temperature was raised to 150℃ for equilibration reaction for 2h. Finally, the temperature was raised to 190℃ to decompose the catalyst and remove low molecular weight substances under reduced pressure for 2h. The modified phenyl silicone rubber raw material was then discharged.

[0078] The materials prepared in Examples 1-3 and Comparative Examples 1-4 were subjected to performance tests, and the test results are shown in Table 1. The testing methods are as follows:

[0079] Tensile strength and elongation at break were tested according to GB / T 528-2009, using type 1 dumbbell-shaped specimens, with a tensile rate of 500 mm / min;

[0080] Tear strength was tested according to GB / T 529-2008, using a right-angled specimen;

[0081] The low-temperature compression set was tested according to GB / T 7759.2-2014, with test conditions of -40℃×72h and a compression rate of 25%.

[0082] The brittleness temperature was tested according to GB / T 1682-2014.

[0083] Table 1.

[0084] Test Project Example 1 Example 2 Example 3 Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 Tensile strength / MPa 16.8 18.5 17.6 13.2 14.0 15.0 12.1 Elongation at break / % 450 495 520 385 400 415 365 Tear strength (kN / m) 38.2 43.1 41.5 31.5 33.0 34.8 29.2 Low-temperature compression set / % (-40℃×72h) 21.5 17.2 15.8 28.6 33.4 24.3 30.8 Brittleness temperature / °C -45 -48 -50 -43 -40 -42 -41

[0085] Conclusion: As can be seen from the test results in Table 1, the high-strength low-temperature resistant rubber materials prepared in Examples 1 to 3 all possess excellent mechanical properties and low-temperature resistance. Among them, Example 2 exhibits the best overall performance: tensile strength reaches 18.5 MPa, tear strength reaches 43.1 kN / m, low-temperature compression set at -40℃ for 72 hours is only 17.2%, and brittle temperature reaches -48℃. This indicates that within the formulation and process range described in this invention, each component can fully exert its synergistic effect.

[0086] Comparing Example 1 with Comparative Example 1, it can be seen that after replacing the UPy modified product with an equal amount of unmodified silanol-containing vinyl incomplete cage-like silsesquioxane, the tensile strength of the material decreased from 16.8 MPa to 13.2 MPa, the tear strength decreased from 38.2 kN / m to 31.5 kN / m, and the low-temperature compression set at -40℃ for 72 h increased from 21.5% to 28.6%. This indicates that the reversible cross-linked network of quadruple hydrogen bonds formed between the UPy groups plays a key role in improving the material strength and elastic recovery at low temperatures.

[0087] Comparing Example 1 and Comparative Example 2, it can be seen that when the mass ratio of distilled water to vinyltrichlorosilane is increased from 5:1 to 7.5:1, the tensile strength of the material decreases to 14.0 MPa, the low-temperature compression set at -40℃ for 72 hours increases to 33.4%, and the brittle temperature increases to -40℃. This is because the hydrolysis of vinyltrichlorosilane produces hydrochloric acid, which accelerates the condensation reaction between silanol groups. Excessive condensation also significantly reduces the number of silanol groups on the surface of the product, reducing the sites for grafting UPy-NCO, decreasing the grafting rate and making it unstable, ultimately deteriorating the performance of the rubber material.

[0088] Comparing Example 1 and Comparative Example 3, it can be seen that without the addition of epoxidized liquid polybutadiene, the tensile strength of the material decreased from 16.8 MPa to 15.0 MPa, the tear strength decreased from 38.2 kN / m to 34.8 kN / m, and the low-temperature compression set at -40℃ for 72 hours increased from 21.5% to 24.3%. This indicates that the epoxidized liquid polybutadiene forms a chemical anchor at the interface of the three phases of the blended adhesive through the reaction between epoxy groups and aminoalkyl and silanol groups, which significantly enhances the interfacial bonding. Without this component, the interfacial bonding of the components weakens, and the mechanical properties and low-temperature properties decrease accordingly.

[0089] Comparing Example 1 and Comparative Example 4, it can be seen that when the raw material does not contain UPy-modified vinyl incomplete cage-like silsesquioxane, the tensile strength of the material decreases to 12.1 MPa, the elongation at break decreases to 365%, the tear strength decreases to 29.2 kN / m, and the low-temperature compression set at -40℃ for 72 hours increases to 30.8%, which is the worst among all groups. This further proves that the synergistic effect of the reversible hydrogen bond crosslinking and co-crosslinking of UPy-modified silsesquioxane is indispensable.

[0090] It should be noted that, in this document, relational terms such as "first" and "second" are used only to distinguish one entity or operation from another, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Furthermore, the terms "comprising," "including," or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, article, or apparatus that comprises a list of elements includes not only those elements but also other elements not expressly listed, or elements inherent to such process, method, article, or apparatus.

Claims

1. A method for preparing a high-strength, low-temperature resistant rubber material, characterized in that: Butadiene rubber, ethylene propylene diene monomer (EPDM) rubber, and modified phenyl silicone rubber are added to a mixer and plasticized for 2-4 minutes. Then, zinc oxide, stearic acid, and antioxidant are added and mixed evenly. Silica, carbon black, and silane coupling agent are added, and the mixture is heated to 140-150℃ for 3-5 minutes. The temperature is then lowered to below 100℃, and UPy modified vinyl incomplete cage-like silsesquioxane, epoxidized liquid polybutadiene, and cold-resistant plasticizer are added. After mixing evenly, the mixture is discharged. The resulting rubber compound is transferred to a two-roll mill, and a peroxide crosslinking agent is added. The mixture is mixed evenly at a roll temperature not exceeding 110℃, and then sheeted to obtain a compound. The compound is then molded and vulcanized at 150-160℃, followed by a second-stage vulcanization at 170-180℃ for 1-2 hours to obtain a high-strength, low-temperature resistant rubber material.

2. The preparation method according to claim 1, characterized in that: The preparation method of modified phenyl silicone rubber is as follows: Octamethylcyclotetrasiloxane, tetramethyltetraphenylcyclotetrasiloxane, tetramethyltetravinylcyclotetrasiloxane, N-(β-aminoethyl)-γ-aminopropylmethyldimethoxysilane, and tetramethyldivinyldisiloxane are added to a reaction vessel and mixed. Tetramethylammonium hydroxide silanolate catalyst is added under nitrogen protection, and polymerization is carried out at 105℃. The temperature is then raised to 150℃ for equilibrium reaction. Finally, the temperature is raised to 190℃ to decompose the catalyst and remove low molecular weight substances under reduced pressure. The modified phenyl silicone rubber raw material is then discharged.

3. The preparation method according to claim 1, characterized in that: The preparation method of UPy modified vinyl incomplete cage-like silsesquioxane is as follows: S1: Disperse vinyltrichlorosilane in acetone, add distilled water dropwise while stirring, and reflux at 40~60℃ for 24~30h. The reaction solution is filtered, washed with acetone, and dried to obtain vinyl incomplete cage-like silsesquioxane containing silanol groups. S2: UPy-NCO monomer and silanol-containing vinyl incomplete cage silsesquioxane are dispersed in anhydrous acetone and reacted at 40-50℃ for 3-4 hours with dibutyltin dilaurate as catalyst to obtain UPy modified vinyl incomplete cage silsesquioxane.

4. The preparation method according to claim 3, characterized in that: In S1, the mass ratio of distilled water to vinyltrichlorosilane is 5~5.5:

1.

5. The preparation method according to claim 3, characterized in that: In S2, UPy-NCO reacts with silanol-containing vinyl incomplete cage-like silsesquioxanes at a molar ratio of isocyanate group to silanol group of (1.0~1.1):

1.

6. The preparation method according to claim 3, characterized in that: In S2, the UPy-NCO monomer is prepared by reacting hexamethylene diisocyanate with 2-amino-4-hydroxy-6-methylpyrimidine.

7. The preparation method according to claim 1, characterized in that: The molecular weight of epoxidized liquid polybutadiene is 2000~4000, and the epoxy value is 2.0~4.0 mmol / g.

8. The preparation method according to claim 1, characterized in that: The high-strength, low-temperature resistant rubber material comprises the following components by weight: 60-80 parts butadiene rubber, 10-20 parts ethylene propylene diene monomer (EPDM) rubber, 10-20 parts modified phenyl silicone rubber, 3-6 parts UPy modified vinyl incomplete cage-like silsesquioxane, 20-40 parts silica, 5-15 parts carbon black, 1-4 parts silane coupling agent, 5-15 parts cold-resistant plasticizer, 5-12 parts epoxidized liquid polybutadiene, 3-5 parts zinc oxide, 1-2 parts stearic acid, 2-4 parts antioxidant, and 1.5-3 parts peroxide crosslinking agent; wherein the sum of the weight parts of butadiene rubber, EPDM rubber, and modified phenyl silicone rubber is 100 parts.

9. The preparation method according to claim 1, characterized in that: The silane coupling agent is at least one of vinyltrimethoxysilane, vinyltris(β-methoxyethoxy)silane, and methacryloxypropyltrimethoxysilane; the antioxidant is at least one of antioxidant 445, antioxidant MB, antioxidant RD, and antioxidant 4010NA; the cold-resistant plasticizer is at least one of dioctyl sebacate and dioctyl adipate; and the peroxide crosslinking agent is at least one of dicumyl peroxide and 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane.

10. The high-strength, low-temperature resistant rubber material prepared by the method according to any one of claims 1 to 9.