Tread rubber composition for new energy vehicle tire and preparation process thereof

By combining bio-based solution-polymerized styrene-butadiene rubber and rice husk ash, and through the synergistic effect of modified hydrocarbon resin and silane coupling agent, the problem of decreased wet grip and wear resistance of tire tread rubber for new energy vehicles has been solved, achieving the preparation of low-carbon and environmentally friendly tread rubber that meets the requirements for use in new energy vehicles.

CN123152190APending Publication Date: 2026-11-24QINGDAO UNIV OF SCI & TECH +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611508625.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-28
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

After using bio-based fillers and rubber to replace traditional materials, the tread rubber of new energy vehicle tires suffers from reduced wet grip and wear resistance. Moreover, the production process relies on fossil resources, resulting in high carbon emissions, which makes it difficult to meet the usage requirements of new energy vehicles.

Method used

By combining bio-based solution-polymerized styrene-butadiene rubber with rice husk ash, and using modified hydrocarbon resins and silane coupling agents, a specific preparation process is employed, including internal mixing, compounding, and rubber refining stages, to improve the processing fluidity and filler dispersibility of the rubber compound, enhance interfacial bonding, and avoid the use of petroleum-based processing oils.

Benefits of technology

It achieves low-carbon and environmentally friendly tread compound, maintains excellent wet grip and wear resistance, while reducing dependence on fossil resources and meeting the requirements of high wear resistance and low rolling resistance for new energy vehicles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123152190A_ABST
    Figure CN123152190A_ABST
Patent Text Reader

Abstract

This invention discloses a tread rubber composition for new energy vehicle tires and its preparation process. It uses bio-based solution-polymerized styrene-butadiene rubber (SBR) and SBR together to reduce the petroleum-based dependence of the rubber matrix. Rice husk ash is used as a bio-based reinforcing filler to replace traditional silica. At the same time, modified resin is introduced to replace petroleum-based processing oil to improve the processing fluidity and filler dispersibility of the rubber compound. A silane coupling agent is used to enhance the interfacial bonding force between rice husk ash and the rubber matrix. The synergistic effect of carbon black, protective wax, stearic acid, antioxidant, accelerator, zinc oxide and sulfur is also used. The low carbonization of the tread rubber is achieved without adding processing oil, while ensuring the wet grip and wear resistance of the tread rubber.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of tire technology, specifically to a tread rubber composition for a tire specifically designed for new energy vehicles and its preparation process. Background Technology

[0002] With the rapid development of the new energy vehicle industry, the curb weight of new energy vehicles is generally 20%-30% higher than that of comparable fuel vehicles. Furthermore, the high instantaneous torque output of the motor and rapid acceleration from a standstill place more stringent requirements on the wear resistance, wet grip, and rolling resistance of the tire tread compound. Currently, new energy vehicle tire tread compounds typically employ a system combining solution-polymerized styrene-butadiene rubber (SBR) and butadiene rubber (BR), using petroleum-based processing oil as a softening plasticizer and precipitated silica (silica) as a reinforcing filler. A silane coupling agent is used to achieve interfacial bonding between the filler and the rubber matrix.

[0003] However, in the aforementioned traditional methods, the production of petroleum-based processing oils and precipitated silica is highly dependent on fossil resources, resulting in large carbon emissions, which contradicts the goal of carbon reduction throughout the entire life cycle of new energy vehicles. When attempting to replace traditional silica with bio-based fillers (such as rice husk ash) and partially replace petroleum-based rubber with bio-based rubber, the surface activity and dispersibility of bio-based fillers differ from those of traditional silica. Furthermore, the reduced processing fluidity of the rubber compound after removing the processing oil leads to uneven dispersion of the fillers in the rubber matrix and insufficient interfacial bonding. Consequently, the wet grip and abrasion resistance of the tread rubber are significantly reduced, making it difficult to meet the requirements for use in new energy vehicle tires. Summary of the Invention

[0004] The present invention aims to provide a tread rubber composition for tires for new energy vehicles and its preparation process, which achieves low carbon and environmental protection of the tread rubber while maintaining excellent wet grip and wear resistance.

[0005] To achieve the above objectives, the technical solution adopted by the present invention is as follows: a tread rubber composition for a special tire for new energy vehicles, wherein, by weight, the raw materials for preparing the tread rubber composition include: 75-85 parts of bio-based solution-polymerized styrene-butadiene rubber, 18.75-31.25 parts of solution-polymerized styrene-butadiene rubber, 73-83 parts of rice husk ash, 3 parts of carbon black, 1.5-2 parts of protective wax, 5.84-6.64 parts of silane coupling agent, 1.5-2.5 parts of stearic acid, 1.8-2.5 parts of antioxidant, 3.0-4.0 parts of accelerator, 1.5-3 parts of zinc oxide, 40-52 parts of modified resin, and 1.0-1.5 parts of sulfur.

[0006] Preferably, the bio-based solution-polymerized styrene-butadiene rubber has a styrene content of 15% and a vinyl content of 30%. The rice husk ash has a nitrogen adsorption specific surface area of ​​160 m² / g. The modified resin is a modified hydrocarbon resin with a softening point of 100-106℃, a number-average molecular weight Mn=480, and a weight-average molecular weight Mw=720. The accelerator is a mixture of accelerator DPG and accelerator CZ, wherein the accelerator DPG is 1-1.5 parts and the accelerator CZ is 2.0-2.5 parts.

[0007] On the other hand, the present invention proposes a preparation process for preparing the above-mentioned tread rubber composition, the preparation process including a mixing stage, a compounding stage and a rubber mixing stage; The mixing stage is as follows: bio-based solution polystyrene-butadiene rubber, solution polystyrene-butadiene rubber, rice husk ash, carbon black, stearic acid, and protective wax are put into a mixing machine, and a silane coupling agent is injected at the same time. The mixture is mixed at a speed of 50-55 rpm for 30-60 seconds to obtain a mixture. The mixing stage is as follows: add modified resin to the mixture, mix for 1 minute, then reduce the speed and pressure while opening the internal mixer to add antioxidant and zinc oxide and mix for 1 minute. Then, mix at a constant temperature between 138℃ and 142℃ for 1 minute. Finally, discharge the glue at a temperature of 155℃ to obtain the masterbatch. The rubber mixing stage is as follows: using a one-step rubber mixing process, the masterbatch is discharged into the open mill and then mixed in a thin pass with a cooling and supplementary mixing at a speed of 10-50 rpm and a roll gap of 2-4 mm for 1-5 minutes. Then, accelerators and sulfur are added and the mixture is transferred to a secondary open mill, where it is mixed again at a speed of 10-50 rpm and a roll gap of 2-4 mm for 8-15 minutes. Finally, it is transferred to a two-roll sheeting mill to obtain the tread rubber composition.

[0008] Preferably, during the mixing stage, the rotation speed is 55 revolutions per minute and the mixing time is 50 seconds.

[0009] Preferably, during the mixing stage, the temperature for constant temperature mixing is 140°C.

[0010] Preferably, during the rubber mixing stage, the time for cooling and remixing in the thin mill is 3 minutes, and the mixing time in the secondary open mill is 10-12 minutes.

[0011] Preferably, during the rubber refining stage, before adding accelerators and sulfur, the masterbatch is tapped and refined 2-4 times.

[0012] Compared with the prior art, the beneficial effects of the present invention are as follows: This invention employs a combination of bio-based solution-polymerized styrene-butadiene rubber (SBR) and solution-polymerized SBR to reduce the petroleum-based dependence of the rubber matrix. Rice husk ash is used as a bio-based reinforcing filler to replace traditional silica. Modified resin is introduced to replace petroleum-based processing oil to improve the processing fluidity and filler dispersibility of the rubber compound. A silane coupling agent is used to enhance the interfacial bonding between rice husk ash and the rubber matrix. The synergistic effects of carbon black, protective wax, stearic acid, antioxidants, accelerators, zinc oxide, and sulfur are also incorporated. This invention achieves low-carbon tread rubber without adding processing oil, while ensuring the wet grip and abrasion resistance of the tread rubber. Attached Figure Description

[0013] Figure 1 This is a flowchart illustrating the preparation process of the tread rubber composition for the new energy vehicle tires of the present invention. Detailed Implementation

[0014] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only a part of the embodiments of the present invention, and not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.

[0015] It should be noted that if the embodiments of the present invention involve directional indicators (such as up, down, left, right, front, back, etc.), the directional indicators are only used to explain the relative positional relationship and movement of the components in a specific posture. If the specific posture changes, the directional indicators will also change accordingly.

[0016] Furthermore, if the embodiments of this invention involve descriptions such as "first" or "second," these descriptions are for descriptive purposes only and should not be construed as indicating or implying their relative importance or implicitly specifying the number of technical features indicated. Thus, a feature defined with "first" or "second" may explicitly or implicitly include at least one of those features. Additionally, the use of "and / or" or "and / or" throughout the text includes three parallel solutions. For example, "A and / or B" includes solution A, solution B, or a solution where both A and B are satisfied simultaneously. Furthermore, the technical solutions of the various embodiments can be combined with each other, but this must be based on the ability of those skilled in the art to implement them. When the combination of technical solutions is contradictory or impossible to implement, it should be considered that such a combination of technical solutions does not exist and is not within the scope of protection claimed by this invention.

[0017] Example 1 Please see Figure 1This invention provides a tread rubber composition for tires specifically designed for new energy vehicles. The raw materials for preparing the tread rubber composition, by weight, include: The composition includes 75 parts of bio-based solution-polymerized styrene-butadiene rubber (SBR), 31.25 parts of solution-polymerized SBR, 73 parts of rice husk ash, 3 parts of carbon black, 1.5 parts of protective wax, 5.84 parts of silane coupling agent, 1.5 parts of stearic acid, 1.8 parts of antioxidant, 3.0 parts of accelerator, 1.5 parts of zinc oxide, 40 parts of modified resin, and 1.0 part of sulfur. The accelerator is a mixture of accelerator DPG and accelerator CZ, wherein accelerator DPG is 1 part and accelerator CZ is 2.0 parts.

[0018] Preferably, the bio-based solution-polymerized styrene-butadiene rubber has a styrene content of 15% and a vinyl content of 30%. The nitrogen adsorption specific surface area of ​​rice husk ash is 160 m² / g. The modified resin is a modified hydrocarbon resin, wherein the modified hydrocarbon resin has a softening point of 100-106℃, a number-average molecular weight Mn=480, and a weight-average molecular weight Mw=720.

[0019] By using rice husk ash with a nitrogen adsorption specific surface area of ​​160 m² / g as a bio-based reinforcing filler, and combining it with bio-based solution-polymerized styrene-butadiene rubber with a styrene content of 15% and a vinyl content of 30%, as well as modified hydrocarbon resin with a softening point of 100-106℃, the modified hydrocarbon resin effectively improved the processing fluidity and filler dispersibility of the rubber compound without the addition of processing oil. The rice husk ash and silane coupling agent worked together to enhance the interfacial bonding force between the filler and rubber, thus achieving a low-carbon and environmentally friendly tread compound while maintaining excellent wet grip and wear resistance.

[0020] The preparation process of the tread rubber composition for the above-mentioned new energy vehicle tires includes a mixing stage, a compounding stage, and a rubber mixing stage. The internal mixing stage involves adding bio-based solution-polymerized styrene-butadiene rubber, solution-polymerized styrene-butadiene rubber, rice husk ash, carbon black, stearic acid, and protective wax into an internal mixer, while simultaneously injecting a silane coupling agent. The mixture is then mixed at a speed of 50 rpm for 30 seconds to obtain the final product.

[0021] The mixing stage is as follows: the modified resin is added to the mixture, and after mixing for 1 minute, the speed and pressure are reduced while the internal mixer is opened to add the antioxidant and zinc oxide and mix for 1 minute. Then, the mixture is kept at a constant temperature of 138°C for 1 minute. Finally, the glue is discharged at a temperature of 155°C to obtain the masterbatch.

[0022] The rubber compounding stage is as follows: A one-step compounding process is used. After the masterbatch is fed into a two-roll mill, it undergoes thin-pass cooling and supplementary mixing at 10 rpm with a 2mm roll gap for 1 minute. Then, accelerators and sulfur are added and the mixture is transferred to a secondary two-roll mill, where it is mixed again at 10 rpm with a 2mm roll gap for 8 minutes. Finally, it is transferred to a two-roll sheeter to obtain the tread rubber composition. Preferably, the mixing time in the secondary two-roll mill is 10 minutes.

[0023] Furthermore, during the rubber refining stage, before adding accelerators and sulfur, the masterbatch is tapped and refined twice.

[0024] Example 2 This invention provides a tread rubber composition for tires specifically designed for new energy vehicles. The raw materials for preparing the tread rubber composition, by weight, include: The composition includes 80 parts of bio-based solution-polymerized styrene-butadiene rubber (SBR), 25 parts of solution-polymerized SBR, 77 parts of rice husk ash, 3 parts of carbon black, 1.7 parts of protective wax, 6.16 parts of silane coupling agent, 2 parts of stearic acid, 2.2 parts of antioxidant, 3.5 parts of accelerator, 2 parts of zinc oxide, 45 parts of modified resin, and 1.2 parts of sulfur. The accelerator is a mixture of accelerator DPG and accelerator CZ, wherein 1.2 parts of accelerator DPG and 2.3 parts of accelerator CZ are present.

[0025] Preferably, the bio-based solution-polymerized styrene-butadiene rubber has a styrene content of 15% and a vinyl content of 30%. The nitrogen adsorption specific surface area of ​​rice husk ash is 160 m² / g.

[0026] The preparation process of the tread rubber composition for the above-mentioned new energy vehicle tires includes a mixing stage, a compounding stage, and a rubber mixing stage. The mixing stage involves adding bio-based solution-polymerized styrene-butadiene rubber, solution-polymerized styrene-butadiene rubber, rice husk ash, carbon black, stearic acid, and protective wax into a mixing mill, while simultaneously injecting a silane coupling agent. The mixture is then mixed at a speed of 53 rpm for 50 seconds to obtain the final product.

[0027] The mixing stage is as follows: the modified resin is added to the mixture, and after mixing for 1 minute, the speed and pressure are reduced while the internal mixer is opened to add the antioxidant and zinc oxide and mix for 1 minute. Then, the mixture is kept at a constant temperature of 140°C for 1 minute. Finally, the glue is discharged at a temperature of 155°C to obtain the masterbatch.

[0028] The rubber compounding stage is as follows: A one-step compounding process is used. After the masterbatch is fed into a two-roll mill, it undergoes thin-pass cooling and supplementary mixing at 30 rpm with a 3mm roll gap for 3 minutes. Then, accelerators and sulfur are added and the mixture is transferred to a secondary two-roll mill, where it is mixed again at 30 rpm with a 3mm roll gap for 10 minutes. Finally, it is transferred to a two-roll sheeter to obtain the tread rubber composition. Preferably, the mixing time in the secondary two-roll mill is 11 minutes.

[0029] Furthermore, during the rubber refining stage, before adding accelerators and sulfur, the masterbatch is tapped and refined three times.

[0030] Example 3 This invention provides a tread rubber composition for tires specifically designed for new energy vehicles. The raw materials for preparing the tread rubber composition, by weight, include: The composition includes 85 parts of bio-based solution-polymerized styrene-butadiene rubber (SBR), 18.75 parts of solution-polymerized SBR, 83 parts of rice husk ash, 3 parts of carbon black, 2 parts of protective wax, 6.64 parts of silane coupling agent, 2.5 parts of stearic acid, 2.5 parts of antioxidant, 4.0 parts of accelerator, 3 parts of zinc oxide, 52 parts of modified resin, and 1.5 parts of sulfur. The accelerator is a mixture of accelerator DPG and accelerator CZ, wherein 1.5 parts of accelerator DPG and 2.5 parts of accelerator CZ are used.

[0031] Preferably, the bio-based solution-polymerized styrene-butadiene rubber has a styrene content of 15% and a vinyl content of 30%. The nitrogen adsorption specific surface area of ​​rice husk ash is 160 m² / g.

[0032] The preparation process of the tread rubber composition for the above-mentioned new energy vehicle tires includes a mixing stage, a compounding stage, and a rubber mixing stage. The mixing stage involves adding bio-based solution-polymerized styrene-butadiene rubber, solution-polymerized styrene-butadiene rubber, rice husk ash, carbon black, stearic acid, and protective wax into a mixing mill, while simultaneously injecting a silane coupling agent. The mixture is then mixed at a speed of 55 rpm for 60 seconds to obtain the final product.

[0033] The mixing stage is as follows: the modified resin is added to the mixture, and after mixing for 1 minute, the speed and pressure are reduced while the internal mixer is opened to add the antioxidant and zinc oxide and mix for 1 minute. Then, the mixture is kept at a constant temperature of 142°C for 1 minute. Finally, the glue is discharged at a temperature of 155°C to obtain the masterbatch.

[0034] The rubber compounding stage is as follows: A one-step compounding process is used. After the masterbatch is fed into a two-roll mill, it undergoes thin-pass cooling and supplementary mixing at 50 rpm with a 4mm roll gap for 5 minutes. Then, accelerators and sulfur are added and the mixture is transferred to a secondary two-roll mill, where it is mixed again at 50 rpm with a 4mm roll gap for 15 minutes. Finally, it is transferred to a two-roll sheeter to obtain the tread rubber composition. Preferably, the mixing time in the secondary two-roll mill is 12 minutes.

[0035] Furthermore, during the rubber refining stage, before adding accelerators and sulfur, the masterbatch is tapped and refined four times.

[0036] The following comparison further illustrates the performance of the tread rubber composition for tires specifically designed for new energy vehicles: I. Proportion settings; Comparative Example 1 (Traditional Petroleum-Based Scheme): 100 parts solution-polymerized styrene-butadiene rubber, 80 parts precipitated silica, 3 parts carbon black, 15 parts processing oil, 1.7 parts protective wax, 6.4 parts silane coupling agent, 2 parts stearic acid, 2.2 parts antioxidant, 3.5 parts accelerator, 2 parts zinc oxide, 30 parts aromatic resin, and 1.2 parts sulfur.

[0037] Comparative Example 2 (using processing oil instead of modified resin): The only difference from Example 2 is that 15 parts of processing oil are used instead of 45 parts of modified resin, while the other components and amounts are exactly the same as in Example 2.

[0038] Comparative Example 3 (rice husk ash replaced with an equal amount of precipitated silica): The only difference from Example 2 is that 77 parts of precipitated silica are used instead of 77 parts of rice husk ash, while the other components and amounts are exactly the same as in Example 2.

[0039] II. Main physical performance tests; Tests were conducted according to standards such as GB / T 528-2009, GB / T 531.1-2008, GB / T 9867-2008, and GB / T 529-2008. The results are shown in the table below: Table 1 Main physical properties

[0040] The tensile strength, tear strength, and abrasion resistance of Examples 1-3 are all superior to or equivalent to Comparative Example 1 (traditional petroleum-based scheme). This indicates that, without the addition of processing oil, the synergistic effect of the modified resin and rice husk ash can effectively ensure the reinforcing effect and mechanical properties of the compound. In Comparative Example 2, after replacing the modified resin with processing oil, all mechanical properties and abrasion resistance showed significant deterioration, proving that the modified resin plays an irreplaceable role in improving filler dispersibility and enhancing interfacial bonding. In Comparative Example 3, precipitated silica replaced rice husk ash. Although the hardness increased slightly, the tensile strength and tear strength were lower than in Example 2, and the abrasion value also increased. This indicates that the specific specification of rice husk ash selected in this invention, with a nitrogen adsorption specific surface area of ​​160 m² / g, has a better reinforcing efficiency than ordinary precipitated silica.

[0041] III. Dynamic Mechanical Performance Test (DMA); The dynamic mechanical analyzer (DMA) was used for testing under the conditions of 1% strain, 10 Hz frequency, and a heating rate of 3℃ / min, with a temperature range of -60℃ to 80℃. The tanδ value at 0℃ represents wet grip (the higher the value, the better), and the tanδ value at 60℃ represents rolling resistance (the lower the value, the better). The results are shown in the table below. Table 2 Dynamic Mechanical Properties

[0042] The 0℃ tanδ values ​​of Examples 1-3 are all higher than those of all comparative examples, indicating that the tread compound of the present invention has superior wet grip. This is attributed to the good interaction between rice husk ash and bio-based solution-polymerized styrene-butadiene rubber (30% vinyl content), as well as the promoting effect of the modified resin on filler dispersion. Meanwhile, the 60℃ tanδ values ​​of Examples 1-3 are all lower than those of all comparative examples, indicating lower rolling resistance, which is beneficial for extending the driving range of new energy vehicles. Compared with Example 2, Comparative Example 2 uses processing oil instead of modified resin, resulting in decreased filler dispersion and insufficient interfacial bonding, leading to a decrease in 0℃ tanδ and an increase in 60℃ tanδ, thus simultaneously deteriorating both wet grip and rolling resistance performance. Comparative Example 3 uses precipitated silica instead of rice husk ash, and its 0℃ tanδ is lower than that of Example 2, while its 60℃ tanδ is higher, further verifying the necessity and superiority of using specific specifications of rice husk ash in the present invention.

[0043] The tire tread rubber composition for new energy vehicles provided by this invention achieves comprehensive optimization of key physical and dynamic mechanical properties through the synergistic effect of bio-based solution-polymerized styrene-butadiene rubber, rice husk ash with a specific nitrogen adsorption surface area, modified hydrocarbon resin, and silane coupling agent, without the addition of petroleum-based processing oil. The performance data of the three embodiments consistently fall within the formulation range defined in claim 1, satisfying the stringent requirements of new energy vehicle tires for high wear resistance, strong wet grip, and low rolling resistance, while significantly reducing the tread rubber's dependence on fossil resources and decreasing carbon emissions. This demonstrates good technical feasibility and low-carbon environmental benefits.

[0044] The above description is merely an exemplary embodiment of the present invention and does not limit the patent scope of the present invention. Any equivalent structural transformations made using the contents of the present invention's specification and drawings under the technical concept of the present invention, or direct / indirect applications in other related technical fields, are included within the patent protection scope of the present invention.

Claims

1. A tread rubber composition for a new energy vehicle tire, characterized by, The raw materials for preparing the tread rubber composition, by weight, include: Bio-based solution-polymerized styrene-butadiene rubber (SBR) 75-85 parts, solution-polymerized SBR 18.75-31.25 parts, rice husk ash 73-83 parts, carbon black 3 parts, protective wax 1.5-2 parts, silane coupling agent 5.84-6.64 parts, stearic acid 1.5-2.5 parts, antioxidant 1.8-2.5 parts, accelerator 3.0-4.0 parts, zinc oxide 1.5-3 parts, modified resin 40-52 parts, sulfur 1.0-1.5 parts.

2. The tread rubber composition for a tire for new energy vehicles according to claim 1, characterized by, The bio-based solution-polymerized styrene-butadiene rubber has a styrene content of 15% and a vinyl content of 30%.

3. The tread rubber composition for a tire for new energy vehicles according to claim 1, characterized by, The nitrogen adsorption specific surface area of ​​the rice husk ash is 160 m² / g.

4. The tread rubber composition for a tire for new energy vehicles according to claim 1, characterized by, The modified resin is a modified hydrocarbon resin, which has a softening point of 100-106℃, a number-average molecular weight Mn=480, and a weight-average molecular weight Mw=720.

5. The tread rubber composition for a tire for new energy vehicles according to claim 1, characterized by, The accelerator is a mixture of accelerator DPG and accelerator CZ, wherein the accelerator DPG is 1-1.5 parts and the accelerator CZ is 2.0-2.5 parts.

6. A manufacturing process characterized by, The preparation process for the tread rubber composition as described in any one of claims 1-5 includes a mixing stage, a compounding stage, and a rubber mixing stage. The mixing stage is as follows: bio-based solution polystyrene-butadiene rubber, solution polystyrene-butadiene rubber, rice husk ash, carbon black, stearic acid, and protective wax are put into a mixing machine, and a silane coupling agent is injected at the same time. The mixture is mixed at a speed of 50-55 rpm for 30-60 seconds to obtain a mixture. The mixing stage is as follows: add modified resin to the mixture, mix for 1 minute, then reduce the speed and pressure while opening the internal mixer to add antioxidant and zinc oxide and mix for 1 minute. Then, mix at a constant temperature between 138℃ and 142℃ for 1 minute. Finally, discharge the glue at a temperature of 155℃ to obtain the masterbatch. The rubber mixing stage is as follows: using a one-step rubber mixing process, the masterbatch is discharged into the open mill and then mixed in a thin pass with a cooling and supplementary mixing at a speed of 10-50 rpm and a roll gap of 2-4 mm for 1-5 minutes. Then, accelerators and sulfur are added and the mixture is transferred to a secondary open mill, where it is mixed again at a speed of 10-50 rpm and a roll gap of 2-4 mm for 8-15 minutes. Finally, it is transferred to a two-roll sheeting mill to obtain the tread rubber composition.

7. The preparation process according to claim 6, characterized in that, During the intensive mixing stage, the rotation speed is 55 revolutions per minute, and the mixing time is 50 seconds.

8. The preparation process according to claim 6, characterized in that, During the mixing stage, the constant temperature mixing temperature is 140℃.

9. The preparation process according to claim 6, characterized in that, During the rubber mixing stage, the time for cooling and remixing in the thin mill is 3 minutes, and the time for mixing in the secondary open mill is 10-12 minutes.

10. The preparation process according to claim 6, characterized in that, During the rubber refining stage, before adding accelerators and sulfur, the masterbatch is tapped and refined 2-4 times.