In-situ modified reinforced composite ultra-high pressure seal ring material and preparation method thereof

By performing surface activation and in-situ grafting treatment on aramid and polyester fibers, the interfacial bonding between the reinforcing fibers and the rubber matrix was improved, solving the problems of permanent deformation and leakage in ultra-high pressure sealing ring materials and enhancing sealing performance.

CN123152191APending Publication Date: 2026-11-24GUANGZHOU WONDERFUL SEALS TECH CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202611565029.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-10
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing ultra-high pressure sealing ring materials suffer from permanent compression deformation and cyclic residual deformation during long-term use due to fiber surface inertness, insufficient interfacial bonding, and filler agglomeration or uneven cross-linking. This, in turn, affects the sealing contact pressure and causes leakage problems.

Method used

By employing differentiated surface activation and in-situ grafting technology of aramid and polyester fibers, covalent bonds are formed through the ring-opening reaction of fiber surface active groups and epoxy groups, which improves the interfacial bonding between reinforcing fibers and rubber matrix, and reduces compression set and cyclic residual deformation.

Benefits of technology

It improves the sealing performance of sealing materials under ultra-high pressure, reduces the risk of sealing contact stress attenuation and leakage, and enhances the material's resistance to extrusion and crack bridging.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123152191A_ABST
    Figure CN123152191A_ABST
Patent Text Reader

Abstract

This invention belongs to the field of synthetic polymer sealing materials technology, specifically relating to an in-situ modified and reinforced composite ultra-high pressure sealing ring material and its preparation method. The invention involves sequentially cleaning aramid fibers with acetone, sodium dodecyl sulfonate, and mild alkali activation, and cleaning polyester fibers with acetone and ultraviolet-ozone photo-oxidation. Both types of activated fibers are then in-situ grafted onto the surface of the fibers with glycidyl methacrylate under nitrogen protection. Hydrogenated nitrile rubber, dicumyl peroxide, silane-modified nano-silica, and triallyl isocyanurate are then added, followed by compression molding and vulcanization. The resulting sealing ring material exhibits low compression set under ultra-high pressure conditions.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of synthetic polymer sealing materials technology, specifically relating to an in-situ modified and enhanced composite ultra-high pressure sealing ring material and its preparation method. Background Technology

[0002] Elastic seals in oil and gas extraction, ultra-high pressure hydraulic equipment, and high-pressure valves are subjected to high contact stress, temperature fluctuations, media swelling, and repeated pressure increases and decreases. Under long-term compression and cyclic shearing, the sealing material undergoes molecular chain slippage, packing network rearrangement, and interfacial debonding. After unloading, it cannot fully recover its original cross-section, exhibiting permanent compression deformation and cyclic residual deformation. Residual deformation reduces contact pressure and can form extrusion lips, cracks, or leakage channels at the sealing gap. Simply increasing hardness or adding rigid packing can suppress extrusion in the short term, but it increases heat generation, embrittlement, and processing difficulties, and may not reduce long-term permanent deformation.

[0003] Publication No. CN1715319A discloses a composite material of hydrogenated nitrile butadiene rubber and para-aramid fiber, using 100 parts by weight of hydrogenated nitrile butadiene rubber, 30-80 parts by weight of nano-silica, 5-30 parts by weight of para-aramid fiber, and 3-8 parts by weight of silane coupling agent, with KH-570 optional. The aramid pulp treatment route involves mixing silica, aramid, and acetone-diluted silane coupling agent, followed by drying and high-temperature baking. This scheme improves high-temperature strength and is used in oilfield packer sleeves, but it does not disclose the synergistic reinforcement of polyester staple fibers, differentiated surface activation of aramid and polyester, or GMA / BPO surface grafting.

[0004] Publication number CN103396591A discloses an ultra-high pressure acid-resistant rubber sealing material for oilfield acid pipelines with pressures of 100–140 MPa. This material uses a combination of hydrogenated nitrile butadiene rubber (NBR) and NBR, along with nano-carbon black, silica, peroxide curing agents, and co-curing agents. This patent recognizes the need for ultra-high pressure materials to balance high hardness, low compression set, and extrusion resistance, and points out that excessive filler can degrade compression set and processing performance; however, it does not employ surface-grafted dual fibers.

[0005] In summary, there is an urgent need for a new type of sealing ring material and its preparation method that can effectively solve the problem of permanent deformation of sealing rings under ultra-high pressure. Summary of the Invention

[0006] This invention provides an in-situ modified and reinforced composite ultra-high pressure sealing ring material and its preparation method. The sealing ring material belongs to the category of synthetic polymer sealing materials based on hydrogenated nitrile rubber. This invention addresses the problems of existing ultra-high pressure sealing materials, which suffer from significant compression set and cyclic residual deformation due to fiber surface inertness, insufficient interfacial bonding, and filler agglomeration or uneven cross-linking. This leads to attenuation of sealing contact pressure, extrusion damage at gaps, and leakage. By differentially activating aramid fibers and polyester fibers and performing separate in-situ grafting, the interfacial bonding between the reinforcing components and the rubber matrix is ​​improved, thereby enhancing the ultra-high pressure sealing performance of the material.

[0007] The specific technical solution is as follows: A method for preparing an in-situ modified and reinforced composite ultra-high pressure sealing ring material is as follows: S1: Fiber pretreatment and surface activation.

[0008] S11: Place the aramid fiber in acetone, sonicate, wash, then place it in an aqueous solution of sodium dodecyl sulfonate, sonicate, wash, and dry to obtain pretreated aramid fiber.

[0009] S12: The pretreated aramid fiber prepared in S11 is placed in a 0.5 mol / L sodium hydroxide aqueous solution, stirred, removed, washed, and dried to constant weight to obtain modified aramid fiber.

[0010] S13: Place polyester fibers in acetone, sonicate, wash, dry, UV treat, wash, and dry to constant weight to obtain modified polyester fibers.

[0011] S2: In situ grafting.

[0012] S21: The modified aramid fiber prepared in S12 is added to toluene, then glycidyl methacrylate, tetrabutylammonium bromide and phenothiazine are added, stirred, heated and stirred under nitrogen protection, cooled, washed and dried to constant weight to obtain in-situ grafted aramid fiber.

[0013] S22: The modified polyester fiber prepared in S13 is added to toluene, followed by the addition of glycidyl methacrylate, tetrabutylammonium bromide, and phenothiazine. The mixture is stirred and heated under nitrogen protection. After cooling, washing, and drying to constant weight, in-situ grafted polyester fiber is obtained.

[0014] S3: Mixing. Preheat HNBR rubber, pass through a thin plasticizer, increase the roller gap to 3mm, add N-isopropyl-N′-phenyl-p-phenylenediamine and dioctyl phthalate, mix, add in-situ grafted aramid fiber prepared in S21 and in-situ grafted polyester fiber prepared in S22 in batches, continue mixing after each batch, add nano-silica modified with KH-570, mix, add dicumyl peroxide and triallyl isocyanurate, pass through a thin plasticizer, and sheet to obtain HNBR compounded rubber sheet.

[0015] S4: Compression vulcanization molding, the HNBR compound rubber sheet prepared in S3 is molded, pressure vulcanized, cooled and depressurized, and demolded to obtain the sealing ring material.

[0016] Furthermore, the aramid fiber described in S11 has a fiber diameter of 10-15 μm, a length of 3-10 mm, and a mass-to-volume ratio of aramid fiber to acetone of 1:50-1:100 g / mL.

[0017] The ultrasonic treatment described in S11 has the following parameter settings: ultrasonic frequency 40–80 kHz, ultrasonic power density 0.3–0.6 W / cm². 2 The ultrasound duration is 20–60 minutes.

[0018] The sodium dodecyl sulfonate aqueous solution described in S11 has a mass concentration of 2%, and the mass-volume ratio of aramid fiber to it is 1:50 g / mL.

[0019] The drying process described in S11 has the following parameters: temperature 70–90°C, duration 4–8 hours.

[0020] The pretreated aramid fiber described in S12 has a mass-to-volume ratio of 1:30 to 1:60 g / mL with sodium hydroxide aqueous solution.

[0021] The stirring described in S12 has the following parameters: temperature 50-70℃, speed 100-300rpm, and duration 1-3h.

[0022] The polyester fiber described in S13 has a fiber diameter of 10-20 μm, a length of 3-10 mm, and a mass-to-volume ratio of 1:50 to 1:100 g / mL with acetone.

[0023] The ultrasonic treatment described in S13 has the following parameter settings: ultrasonic frequency 40–80 kHz, ultrasonic power density 0.3–0.6 W / cm². 2 The ultrasound duration is 20–60 minutes.

[0024] The ultraviolet treatment described in S13 has the following parameters: wavelength 185nm and 254nm, ozone concentration 10-100ppm, and duration 10-50min.

[0025] Furthermore, the modified aramid fiber described in S21 has a mass-to-volume ratio of 1:50 g / mL to toluene.

[0026] The glycidyl methacrylate described in S21 is added in an amount of 10% to 30% of the mass of the modified aramid fiber.

[0027] The tetrabutylammonium bromide mentioned in S21 is added at an amount of 0.05% of the mass of the modified aramid fiber.

[0028] The phenothiazine described in S21 is added at an amount of 0.02% of the mass of the modified aramid fiber.

[0029] The heating and stirring reaction described in S21 has the following parameters: temperature 70-90℃, duration 4-8h.

[0030] The modified polyester fiber described in S22 has a mass-to-volume ratio of 1:50 g / mL to toluene.

[0031] The glycidyl methacrylate described in S22 is added at an amount of 10% to 30% of the mass of the modified polyester fiber.

[0032] The tetrabutylammonium bromide mentioned in S22 is added at an amount of 0.05% of the mass of the modified polyester fiber.

[0033] The phenothiazine described in S22 is added at an amount of 0.02% of the mass of the modified polyester fiber.

[0034] The heating and stirring reaction described in S22 has the following parameters: temperature 70-90℃, duration 4-8h.

[0035] Furthermore, the preheating described in S3 has the following parameter settings: temperature 50-70℃, duration 3-5min.

[0036] The thin-pass plasticizing process described in S3 has the following parameter settings: temperature 50-70℃, roller gap 0.5-1.5mm, and number of passes 5-15.

[0037] The HNBR compound sheet described in S3, based on 100 parts by weight of HNBR rubber, has the following composition of raw materials: 1-2 parts of N-isopropyl-N′-phenyl-p-phenylenediamine, 5-15 parts of dioctyl phthalate, 10-20 parts of in-situ grafted aramid fiber, 10-20 parts of in-situ grafted polyester fiber, 20-40 parts of KH-570 modified nano silica, 2-4 parts of dicumyl peroxide, and 1-2 parts of triallyl isocyanurate.

[0038] Furthermore, the pressure vulcanization described in S4 has the following parameter settings: pressure 10-20 MPa, temperature 150-170°C, and duration 20-40 min.

[0039] Compared with the prior art, the present invention has the following beneficial effects: 1. This invention employs aramid fibers and polyester fibers to synergistically reinforce a hydrogenated nitrile rubber matrix. The aramid fibers provide resistance to extrusion and crack bridging, while the polyester fibers disperse localized shear loads. Together, they reduce load concentration and improve the deformation and damage behavior of the sealing material under compression and differential pressure.

[0040] 2. This invention involves surface activation of aramid fibers and polyester fibers, followed by in-situ grafting of glycidyl methacrylate onto their surfaces. Covalent bonds are formed through the ring-opening reaction between the active groups on the fiber surface and the epoxy groups, thereby improving the interfacial bonding between the reinforcing fibers and the rubber matrix, reducing compression set and cyclic residual deformation, minimizing the attenuation of sealing contact stress, and improving the sealing performance of the synthesized polymer sealing material. Attached Figure Description

[0041] Figure 1 The diagram shows the pressure difference-gap data of the sealing ring materials prepared in Example 1 and Comparative Examples 1-3, where H1 represents Example 1 and C1-C3 represent Comparative Examples 1-3.

[0042] Figure 2 The diagram shows the critical sealing failure pressure differential distribution of the sealing ring materials prepared in Example 1 and Comparative Examples 1-3, where H1 represents Example 1 and C1-C3 represent Comparative Examples 1-3.

[0043] Figure 3 These are internal damage morphology images of the sealing ring materials prepared in Example 1 and Comparative Examples 1-3, where H1 represents Example 1 and C1-C3 represent Comparative Examples 1-3. Detailed Implementation

[0044] The following embodiments further explain and illustrate the technical solutions of the present invention. It should be specifically noted that each specific embodiment is a concretization and explanation of the technical solution and should not be considered as a limitation on the scope of protection of the present invention. Those skilled in the art still have the right to modify the technical solutions of these embodiments and make equivalent substitutions for some or all of the technical features, and these modifications or substitutions do not change the essence of the corresponding technical solutions, nor do they cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions described in the present invention.

[0045] This invention proposes an in-situ modified and reinforced composite ultra-high pressure sealing ring material and its preparation method, the detailed technical solution of which is as follows: 1. Fiber pretreatment and surface activation Aramid fibers were placed in acetone, sonicated, washed, and then placed in an aqueous solution of sodium dodecyl sulfonate, sonicated, washed, and dried to obtain pretreated aramid fibers.

[0046] The pretreated aramid fibers were placed in an aqueous sodium hydroxide solution, stirred, removed, washed, and dried to constant weight to obtain modified aramid fibers.

[0047] Polyester fibers (PET) are placed in acetone, ultrasonically treated, washed, dried, UV treated, washed, and dried to constant weight to obtain modified polyester fibers.

[0048] Acetone is a highly polar organic solvent that can effectively dissolve organic contaminants on the fiber surface. When ultrasound propagates in a liquid, it generates a cavitation effect. When the cavitation bubbles collapse, they produce localized high temperatures and pressures and intense microjets, which can effectively peel off contaminants adhering to the fiber surface. At the same time, ultrasonic oscillation promotes the diffusion and penetration of solvent molecules into the fiber surface, improving cleaning efficiency.

[0049] In aqueous solution, sodium dodecyl sulfonate molecules are oriented at the fiber / water interface with hydrophobic groups facing the fiber surface and hydrophilic groups facing the aqueous phase, reducing the interfacial tension between the fiber and water and improving the wettability of the fiber in water. After treatment with sodium dodecyl sulfonate, the surface of aramid fibers changes from hydrophobic to hydrophilic, and the OH- in the NaOH aqueous solution... - Ions attack the amide bonds in the aramid molecular chain, causing some of these bonds to hydrolyze and break, leading to the degradation and shedding of macromolecular chains on the fiber surface. This results in nanoscale to microscale indentations, etching pits, and rough structures on the fiber surface. Simultaneously, the hydrolysis of the amide bonds generates new polar functional groups such as carboxyl and amino groups on the fiber surface. These polar groups, on the one hand, increase the surface energy and wettability of the fiber, reducing the water contact angle; on the other hand, they provide chemically active sites for subsequent in-situ grafting reactions.

[0050] Ultraviolet light with a wavelength of 254 nm has high photon energy, which can directly break the C-C and CH bonds in the PET molecular chain, generating large molecular free radicals on the fiber surface. Ultraviolet light with a wavelength of 185 nm can photolyze oxygen molecules into reactive oxygen atoms. These oxygen atoms combine with oxygen molecules to form ozone, a strong oxidant that can be further decomposed into even more reactive oxygen free radicals under ultraviolet light irradiation. These reactive oxygen species attack the ester bonds and methylene groups in the PET molecular chain, causing oxidative breakage of the C-C and CH bonds. This introduces oxygen-containing polar groups such as carboxyl and hydroxyl groups onto the fiber surface. The introduced polar oxygen-containing groups increase the surface energy of the PET fiber, reduce the water contact angle, improve the fiber's wettability and interfacial compatibility with polar matrices, and generate nanoscale roughness on the surface.

[0051] 2. In-situ grafting Modified aramid fibers were added to toluene, followed by the addition of glycidyl methacrylate (GMA), tetrabutylammonium bromide (TBAB), and phenothiazine. The mixture was stirred and heated under nitrogen protection. After cooling, washing, and drying to constant weight, in-situ grafted aramid fibers were obtained.

[0052] Modified polyester fibers were added to toluene, followed by glycidyl methacrylate, tetrabutylammonium bromide, and phenothiazine. The mixture was stirred and heated under nitrogen protection. After cooling, washing, and drying to constant weight, in-situ grafted polyester fibers were obtained.

[0053] After treatment with an activated alkali, modified aramid fibers develop polar groups such as carboxyl groups on their surface. Under TBAB catalysis, amino groups act as nucleophiles, attacking the epoxy groups of GMA and undergoing ring-opening addition reactions to generate CN bonds and hydroxyl groups, thus chemically linking GMA molecules to the fiber surface. After UV treatment, modified polyester fibers introduce oxygen-containing groups such as carboxyl, hydroxyl, and carbonyl groups onto their surface. Under TBAB catalysis, carboxyl groups can undergo ring-opening esterification reactions with the epoxy groups of GMA to form ester bonds. Simultaneously, free radical precursors formed by partial molecular chain breakage are generated in the amorphous regions of the fiber surface.

[0054] 3. Mixing HNBR rubber is preheated, thin-pass plasticized, and the roller gap is increased to 3mm. N-isopropyl-N′-phenyl-p-phenylenediamine and dioctyl phthalate are added and mixed. In-situ grafted aramid fibers and in-situ grafted polyester fibers are added in batches, and mixing is continued after each batch. Nano-silica modified with KH-570 is added and mixed. Dicumyl peroxide (DCP) and triallyl isocyanurate (TAIC) are added, thin-pass plasticized, and sheeted to obtain HNBR compounded rubber sheet.

[0055] Through thin-pass plasticizing, the rubber macromolecular chains undergo mechanical degradation under shear stress, resulting in a decrease in molecular weight and Mooney viscosity, thereby improving the processing fluidity of the rubber compound. After in-situ grafting modification, the fibers exhibit good compatibility with HNBR, improving the interfacial wettability between the fibers and the rubber matrix. Under the shear force of the open mill, the fibers are forcibly dispersed into the rubber matrix, promoting the wetting and encapsulation of the fiber surface by the rubber molecular chains.

[0056] 4. Compression molding and vulcanization The HNBR compounded rubber sheet is molded, pressurized and vulcanized, cooled and depressurized, and then demolded to obtain the sealing ring material.

[0057] Under heating conditions, the peroxide bonds in the DCP molecule undergo homolytic cleavage, generating two cumeneoxy radicals. The HNBR molecular chain retains a certain number of unsaturated carbon-carbon double bonds and contains a large number of saturated methylene structures. The cumeneoxy radicals, on the one hand, abstract α-active hydrogens from the methylene groups in the HNBR molecular chain, generating large alkyl radicals on the HNBR molecular chain. When two large alkyl radicals meet, they undergo a coupling reaction to form a C-C crosslink. On the other hand, the cumeneoxy radicals directly add to the remaining unsaturated double bonds in the HNBR molecular chain, generating large radicals at the double bond positions, which initiate crosslinking reactions. The TAIC molecule contains three allyl groups. Initiated by the radicals generated from the decomposition of DCP, the allyl double bonds on the TAIC molecule are opened, forming TAIC radicals. These TAIC radicals can either undergo addition reactions with the large radicals on the HNBR molecular chain, connecting the TAIC molecule as a "bridge" between two HNBR molecular chains; or they can first self-polymerize to form oligomers and then react with the HNBR molecular chain. Each TAIC molecule contains three allyl groups, which can react with multiple HNBR molecular chains simultaneously to form multifunctional cross-linking nodes, effectively increasing the cross-linking density.

[0058] Example 1 A method for preparing an in-situ modified and reinforced composite ultra-high pressure sealing ring material is as follows: Table 1 Main Raw Materials

[0059] S1: Fiber pretreatment and surface activation.

[0060] S11: Place 40g of aramid fiber in 3L of acetone and sonicate (ultrasonic frequency 60kHz, ultrasonic power density 0.45W / cm³). 2 (Ultrasound duration 40 min), rinse repeatedly with distilled water until the washing solution has no acetone odor, then take 30 g and place it in 1.5 L of 2% sodium dodecyl sulfate aqueous solution, and sonicate again (ultrasound frequency 60 kHz, ultrasound power density 0.45 W / cm³). 2 The fibers were removed by ultrasonic treatment (40 min), rinsed repeatedly with distilled water until no foam was found in the washing solution, and then dried in a forced-air drying oven at 80°C for 6 h to obtain pretreated aramid fibers.

[0061] S12: Take 25g of the pretreated aramid fiber prepared in S11 and place it in 1125mL of 0.5mol / L sodium hydroxide aqueous solution. Stir at 200rpm for 2h at 60℃. Take it out and rinse it repeatedly with distilled water until the washing solution is neutral. Dry it at 80℃ to constant weight to obtain modified aramid fiber.

[0062] S13: Place 40g of polyester fiber in 3L of acetone and sonicate (ultrasonic frequency 60kHz, ultrasonic power density 0.45W / cm³). 2 The modified polyester fiber was obtained by repeatedly rinsing with distilled water (40 min ultrasonic treatment), rinsing repeatedly with distilled water until the washing solution had no acetone odor, drying at 80℃ for 6 h, ultraviolet treatment (wavelengths 185 nm and 254 nm, ozone concentration 50 ppm, duration 30 min), washing three times with distilled water, and drying at 80℃ to constant weight.

[0063] S2: In situ grafting.

[0064] S21: Take 20g of the modified aramid fiber prepared in S12 and add it to 1L of toluene. Then add 4g of glycidyl methacrylate, 10mg of tetrabutylammonium bromide, and 4mg of phenothiazine. Stir until homogeneous, heat to 80℃ under nitrogen protection and stir for 6h. Cool naturally to room temperature, wash repeatedly with acetone 5 times, stirring thoroughly for 5min each time. Dry at 80℃ to constant weight to obtain in-situ grafted aramid fiber (grafting rate calculation formula). M1 was obtained by Soxhlet extraction with acetone for 8 hours and drying to constant weight, with a grafting rate of 1.2%.

[0065] S22: Take 20g of the modified polyester fiber prepared in S13 and add it to 1L of toluene. Then add 4g of glycidyl methacrylate, 10mg of tetrabutylammonium bromide and 4mg of phenothiazine. Stir until uniform, heat to 80℃ under nitrogen protection and stir for 6h. Cool naturally to room temperature, wash repeatedly with acetone 5 times, stirring thoroughly for 5min each time. Dry at 80℃ to constant weight to obtain in-situ grafted polyester fiber (grafting rate 0.9%).

[0066] S3: Mixing. Preheat 100g of HNBR rubber on the open mill rollers (temperature 60℃, duration 4min), then perform thin-pass plasticizing (temperature 60℃, roller gap 1mm, 10 passes; after each pass, fold the rubber sheet and refeed it into the rollers). Increase the roller gap to 3mm, add 1.5g of N-isopropyl-N′-phenyl-p-phenylenediamine and 10g of dioctyl phthalate, mix for 5min, and then add the in-situ grafted aramid fiber prepared in S21 in 3 batches (5g per batch). The in-situ grafted polyester fiber (5g per batch, 15g total) prepared by S22 was added and mixed for 4 minutes after each batch was added. Then, 30g of nano-silica modified by KH-570 was added, the temperature was raised to 110℃ and mixed for 10 minutes, the temperature was lowered to 75℃, 3g of dicumyl peroxide and 1.5g of triallyl isocyanurate were added, and the mixture was passed through a thin sheet (roller gap 2mm, thin sheet 5 times). The roller gap was adjusted to 3mm and the sheet was extruded to obtain HNBR compounded film.

[0067] S4: Compression vulcanization molding. The HNBR compounded rubber sheet prepared in S3 is molded, and vulcanized under pressure (15MPa, 160℃, 30min). The temperature is then reduced to 90℃, the pressure is released, and the mold is demolded to obtain the sealing ring material.

[0068] Example 2 The composition and preparation process are the same as in Example 1, except that: In the preparation process S11, the mass-to-volume ratio of aramid fiber to acetone is 1:50 g / mL, and other components are the same.

[0069] The ultrasonic treatment parameters in step S11 of the preparation process are set as follows: ultrasonic frequency 40kHz, ultrasonic power density 0.3W / cm³. 2 The ultrasonic treatment lasted for 20 minutes, and the drying parameters were set as follows: temperature 70℃, duration 4 hours, and other steps were the same.

[0070] In the preparation process S12, the mass-to-volume ratio of pretreated aramid fiber to sodium hydroxide aqueous solution is 1:30 g / mL, and other components are the same.

[0071] The stirring parameters in step S12 of the preparation process are set as follows: temperature 50℃, rotation speed 100rpm, duration 1h, and other steps are the same.

[0072] In the preparation process S13, the mass-to-volume ratio of polyester fiber to acetone is 1:50 g / mL, and other components are the same.

[0073] The UV treatment parameters in step S13 of the preparation process are set as follows: wavelength 185nm and 254nm, ozone concentration 10ppm, duration 10min, and other steps are the same.

[0074] In the preparation process S21, the amount of glycidyl methacrylate added is 10% of the mass of the modified aramid fiber, and the other components are the same.

[0075] The temperature and stirring reaction parameters in step S21 of the preparation process are set as follows: temperature 70℃, duration 4h, and other steps are the same.

[0076] In the preparation process S22, the amount of glycidyl methacrylate added is 10% of the mass of the modified polyester fiber, and the other components are the same.

[0077] The temperature and stirring reaction parameters in step S22 of the preparation process are set as follows: temperature 70℃, duration 4h, and other steps are the same.

[0078] In the S3 step of the preparation process, the preheating parameters are set as follows: temperature 50℃, duration 3min. The thin-pass plasticizing parameters are set as follows: temperature 50℃, roller gap 0.5mm, number of passes 5. Other steps are the same.

[0079] In the preparation process S3, based on 100 parts by mass of HNBR rubber, the composition of each raw material is as follows: 1 part of N-isopropyl-N′-phenyl p-phenylenediamine, 5 parts of dioctyl phthalate, 10 parts of in-situ grafted aramid fiber, 10 parts of in-situ grafted polyester fiber, 20 parts of KH-570 modified nano silica, 2 parts of dicumyl peroxide, 1 part of triallyl isocyanurate, and the other components are the same.

[0080] The pressure vulcanization parameters in step S4 of the preparation process are set as follows: pressure 10 MPa, temperature 150 °C, duration 20 min, and other steps are the same.

[0081] Example 3 The composition and preparation process are the same as in Example 1, except that: In the preparation process S11, the mass-to-volume ratio of aramid fiber to acetone is 1:100 g / mL, and other components are the same.

[0082] The ultrasonic treatment parameters in step S11 of the preparation process are set as follows: ultrasonic frequency 80kHz, ultrasonic power density 0.6W / cm³. 2 The ultrasonic treatment lasted for 60 minutes, and the drying parameters were set as follows: temperature 90℃, duration 8 hours, and other steps were the same.

[0083] In the preparation process S12, the mass-to-volume ratio of pretreated aramid fiber to sodium hydroxide aqueous solution is 1:60 g / mL, and other components are the same.

[0084] The stirring parameters in step S12 of the preparation process are set as follows: temperature 70℃, rotation speed 300rpm, duration 3h, and other steps are the same.

[0085] In the preparation process S13, the mass-to-volume ratio of polyester fiber to acetone is 1:100 g / mL, and other components are the same.

[0086] The UV treatment parameters in step S13 of the preparation process are set as follows: wavelength 185nm and 254nm, ozone concentration 100ppm, duration 50min, and other steps are the same.

[0087] In the preparation process S21, the amount of glycidyl methacrylate added is 30% of the mass of the modified aramid fiber, and the other components are the same.

[0088] The temperature and stirring reaction parameters in step S21 of the preparation process are set as follows: temperature 90℃, duration 8h, and other steps are the same.

[0089] In the preparation process S22, the amount of glycidyl methacrylate added is 30% of the mass of the modified polyester fiber, and the other components are the same.

[0090] The temperature and stirring reaction parameters in step S22 of the preparation process are set as follows: temperature 90℃, duration 8h, and other steps are the same.

[0091] In the S3 step of the preparation process, the preheating parameters are set as follows: temperature 70℃, duration 5min. The thin-pass plasticizing parameters are set as follows: temperature 70℃, roller gap 1.5mm, number of passes 15. Other steps are the same.

[0092] In the preparation process S3, based on 100 parts by mass of HNBR rubber, the composition of each raw material is as follows: 2 parts of N-isopropyl-N′-phenyl p-phenylenediamine, 15 parts of dioctyl phthalate, 20 parts of in-situ grafted aramid fiber, 20 parts of in-situ grafted polyester fiber, 40 parts of KH-570 modified nano silica, 4 parts of dicumyl peroxide, 2 parts of triallyl isocyanurate, and the other components are the same.

[0093] The pressure vulcanization parameters in step S4 of the preparation process are set as follows: pressure 20 MPa, temperature 170 °C, duration 40 min, and other steps are the same.

[0094] Example 4 The composition and preparation process are the same as in Example 1, except that: In the preparation process S11, the mass-to-volume ratio of aramid fiber to acetone is 1:60 g / mL, and other components are the same.

[0095] The ultrasonic treatment parameters in step S11 of the preparation process are set as follows: ultrasonic frequency 50kHz, ultrasonic power density 0.4W / cm³. 2 The ultrasonic treatment lasted for 30 minutes, and the drying parameters were set as follows: temperature 75℃, duration 5 hours, and other steps were the same.

[0096] In the preparation process S12, the mass-to-volume ratio of pretreated aramid fiber to sodium hydroxide aqueous solution is 1:40 g / mL, and other components are the same.

[0097] The stirring parameters in step S12 of the preparation process are set as follows: temperature 55℃, rotation speed 150rpm, duration 2.5h, and other steps are the same.

[0098] In the preparation process S13, the mass-to-volume ratio of polyester fiber to acetone is 1:60 g / mL, and other components are the same.

[0099] The UV treatment parameters in step S13 of the preparation process are set as follows: wavelength 185nm and 254nm, ozone concentration 25ppm, duration 20min, and other steps are the same.

[0100] In the preparation process S21, the amount of glycidyl methacrylate added is 15% of the mass of the modified aramid fiber, and the other components are the same.

[0101] The temperature and stirring reaction parameters in step S21 of the preparation process are set as follows: temperature 75℃, duration 5h, and other steps are the same.

[0102] In the preparation process S22, the amount of glycidyl methacrylate added is 25% of the mass of the modified polyester fiber, and the other components are the same.

[0103] The temperature and stirring reaction parameters in step S22 of the preparation process are set as follows: temperature 75℃, duration 5h, and other steps are the same.

[0104] In the S3 step of the preparation process, the preheating parameters are set as follows: temperature 55℃, duration 3.5min. The thin-pass plasticizing parameters are set as follows: temperature 55℃, roller gap 1.3mm, number of passes 7. Other steps are the same.

[0105] In the preparation process S3, based on 100 parts by mass of HNBR rubber, the composition of each raw material is as follows: 1.3 parts of N-isopropyl-N′-phenyl-p-phenylenediamine, 7 parts of dioctyl phthalate, 12.5 parts of in-situ grafted aramid fiber, 12.5 parts of in-situ grafted polyester fiber, 25 parts of KH-570 modified nano silica, 2.5 parts of dicumyl peroxide, and 1.7 parts of triallyl isocyanurate. The other components are the same.

[0106] The pressure vulcanization parameters in step S4 of the preparation process are set as follows: pressure 12MPa, temperature 155℃, duration 25min, and other steps are the same.

[0107] Example 5 The composition and preparation process are the same as in Example 1, except that: In the preparation process S11, the mass-to-volume ratio of aramid fiber to acetone is 1:80 g / mL, and other components are the same.

[0108] The ultrasonic treatment parameters in step S11 of the preparation process are set as follows: ultrasonic frequency 70kHz, ultrasonic power density 0.5W / cm³. 2 The ultrasonic treatment lasted for 50 minutes, and the drying parameters were set as follows: temperature 85℃, duration 7 hours, and other steps were the same.

[0109] In the preparation process S12, the mass-to-volume ratio of pretreated aramid fiber to sodium hydroxide aqueous solution is 1:40 g / mL, and other components are the same.

[0110] The stirring parameters in step S12 of the preparation process are set as follows: temperature 65℃, rotation speed 250rpm, duration 1.5h, and other steps are the same.

[0111] In the preparation process S13, the mass-to-volume ratio of polyester fiber to acetone is 1:90 g / mL, and other components are the same.

[0112] The UV treatment parameters in step S13 of the preparation process are set as follows: wavelength 185nm and 254nm, ozone concentration 75ppm, duration 45min, and other steps are the same.

[0113] In the preparation process S21, the amount of glycidyl methacrylate added is 25% of the mass of the modified aramid fiber, and the other components are the same.

[0114] The temperature and stirring reaction parameters in step S21 of the preparation process are set as follows: temperature 85℃, duration 7h, and other steps are the same.

[0115] In the preparation process S22, the amount of glycidyl methacrylate added is 15% of the mass of the modified polyester fiber, and the other components are the same.

[0116] The temperature and stirring reaction parameters in step S22 of the preparation process were set as follows: temperature 85℃, duration 7h, and other steps were the same.

[0117] In the S3 step of the preparation process, the preheating parameters are set as follows: temperature 65℃, duration 4.5min. The thin-pass plasticizing parameters are set as follows: temperature 65℃, roller gap 0.7mm, number of passes 13. Other steps are the same.

[0118] In the preparation process S3, based on 100 parts by mass of HNBR rubber, the composition of each raw material is as follows: 1.6 parts of N-isopropyl-N′-phenyl-p-phenylenediamine, 13 parts of dioctyl phthalate, 17 parts of in-situ grafted aramid fiber, 14 parts of in-situ grafted polyester fiber, 35 parts of KH-570 modified nano silica, 3.5 parts of dicumyl peroxide, and 1.4 parts of triallyl isocyanurate. The other components are the same.

[0119] The pressure vulcanization parameters in step S4 of the preparation process are set as follows: pressure 17 MPa, temperature 165℃, duration 35 min, and other steps are the same.

[0120] Comparative Example 1 The composition and preparation process are the same as in Example 1, except that: In processes S1 and S2 of the preparation process, no fiber treatment is performed; the fibers are directly mixed. Based on 100 parts by weight of HNBR rubber, the composition of each raw material is as follows: 1.5 parts of N-isopropyl-N′-phenyl-p-phenylenediamine, 10 parts of dioctyl phthalate, 15 parts of aramid fiber, 15 parts of polyester fiber, 30 parts of KH-570 modified nano-silica, 3 parts of dicumyl peroxide, and 1.5 parts of triallyl isocyanurate.

[0121] Comparative Example 2 The composition and preparation process are the same as in Example 1, except that: In process S1, only the aramid fiber is modified, while the polyester fiber is not modified. Based on 100 parts by weight of HNBR rubber, the composition of each raw material is as follows: 1.5 parts of N-isopropyl-N′-phenyl-p-phenylenediamine, 10 parts of dioctyl phthalate, 15 parts of in-situ grafted aramid fiber, 15 parts of polyester fiber, 30 parts of KH-570 modified nano silica, 3 parts of dicumyl peroxide, and 1.5 parts of triallyl isocyanurate.

[0122] Comparative Example 3 The composition and preparation process are the same as in Example 1, except that: In the preparation process S1, aramid fibers and polyester fibers are pretreated, but in S2, in-situ grafting is not performed. Instead, the modified fibers are directly put into the compound. Based on 100 parts by weight of HNBR rubber, the composition of each raw material is as follows: 1.5 parts of N-isopropyl-N′-phenyl-p-phenylenediamine, 10 parts of dioctyl phthalate, 15 parts of modified aramid fiber, 15 parts of modified polyester fiber, 30 parts of KH-570 modified nano silica, 3 parts of dicumyl peroxide, and 1.5 parts of triallyl isocyanurate.

[0123] Samples of the sealing ring materials prepared in Example 1 and Comparative Examples 1-3 were taken and prepared into cylindrical specimens (section diameter 5.33 mm). Compression (25% compression rate) was applied, and an ultra-high pressure sealing center boundary test was conducted (target temperature 150℃, pressure difference 0–160 MPa, gap 0–0.30 mm). Figure 1 As shown, H1 is Example 1, and C1-C3 are Comparative Examples 1-3. Within the radial gap range shown, the sealing boundary pressure difference of each group of materials decreases as the radial gap increases; under the same radial gap, the boundary pressure difference corresponding to Example 1 is higher than that of each comparative example.

[0124] Samples of the sealing ring materials prepared in Example 1 and Comparative Examples 1-3 were taken and prepared into cylindrical specimens (section diameter 5.33 mm). Compression (25% compression rate) was applied, and a critical sealing pressure difference test was conducted (the pressure was increased at 1 MPa / min after heating to 150°C, with a gap of 0.25 mm). Figure 2 As shown, H1 is Example 1, and C1-C3 are Comparative Examples 1-3. H1 is obviously shifted to the right, and from left to right, they are C1, C2, C3, and H1. When the failure probability is 50%, the critical seal failure pressure difference of H1 is 135.5 MPa, C1 is 39.5 MPa, C2 is 58.8 MPa, and C3 is 75.3 MPa. However, at 140 MPa, the failure probability of H1 is about 67.9%, indicating that H1 increases the center failure pressure difference, but 140 MPa is already higher than 135.5 MPa under the condition of 0.25 mm.

[0125] Samples of the sealing ring materials prepared in Example 1 and Comparative Examples 1-3 were taken and prepared into cylindrical specimens (section diameter 5.33 mm). Compression (25% compression rate) was applied, and three-dimensional morphology tests were performed (voltage 90 kV, current 100 μA, high-pressure side pressure 0–200 MPa, tests were conducted after decompression). Figure 3 As shown, H1 is Example 1, and C1-C3 are Comparative Examples 1-3. In H1, the cross-section is basically continuous. In C3, there are a few short, non-connected cracks. In C2, there are longer interface cracks. In C1, a highly connected crack network that extends to the surface is formed.

[0126] Combining Examples 1-5 and Comparative Examples 1-3, samples of the finally prepared sealing ring material were taken for compression set testing: The samples were prepared as cylindrical specimens (29 mm in diameter, 12.5 mm in height), placed at 23°C for 24 hours, and the initial height of the center of each specimen was measured using a thickness gauge with an accuracy of ±0.01 mm. Then, the specimens and height limiters were placed between two compression plates, and compression (25% compression rate) was applied. The specimens were then aged in an oven at 150°C for 72 hours, cooled for 30 minutes, and the clamps were released. The specimens were then placed on a plane at standard laboratory temperature (23°C, 50% relative humidity) and allowed to recover in a free state for 30 minutes. The final height of the center of the specimen was measured again, and the results were calculated. Where C is the permanent compression deformation, h0 is the original height of the sample, h1 is the height after compression, and h2 is the final height of the sample after recovery. Five sets of measurements were taken, and the average value was taken.

[0127] Based on Examples 1-5 and Comparative Examples 1-3, samples of the finally prepared sealing ring material were taken and subjected to cyclic compression residual deformation tests: The samples were prepared into cylindrical specimens (diameter 29 mm, height 12.5 mm), placed at 23°C for 24 hours, and the initial height of the center of each specimen was measured using a thickness gauge with an accuracy of ±0.01 mm. Compression was applied using an electronic universal testing machine (25% compression rate, 1000 cycles, loading / unloading rate 10 mm / min). After completion, the specimens were allowed to recover for 30 minutes at standard laboratory temperature (temperature 23°C, relative humidity 50%), and the final height of the center of the specimens was measured again. The results were calculated... Where C is the residual deformation rate under cyclic compression, h0 is the original height of the specimen, and h2 is the final height of the specimen after recovery), 5 sets of measurements were taken and the average value was taken.

[0128] Combining Examples 1-5 and Comparative Examples 1-3, samples of the finally prepared sealing ring material were taken and subjected to tensile strength tests: the samples were prepared into dumbbell-shaped specimens (gauge length 25 mm), placed at 23°C for 24 h, the cross-sectional area of ​​the narrow part of the specimen was measured, and the test was performed using a universal testing machine (tensile rate 500 mm / min). The maximum force value during the fracture process was recorded, and the tensile strength was calculated. Where F is the maximum force and W is the cross-sectional area of ​​the narrow part of the sample, 5 sets were measured and the average value was taken.

[0129] Based on Examples 1-5 and Comparative Examples 1-3, samples of the finally prepared sealing ring material were taken for tear strength testing: The samples were prepared into uncut right-angled specimens and placed at 23°C for 24 hours. Using a thickness gauge with an accuracy of ±0.01 mm, the thickness of the torn edge (right-angled region) of the specimen was measured. Five sets of measurements were taken, and the average value was calculated. Then, a universal testing machine was used for testing (tensile rate 500 mm / min). The maximum force value during the tearing process was recorded, and the results were calculated. (where T is the tear strength, F is the maximum force, and d is the sample thickness), 5 sets were measured, and the average value was taken.

[0130] Based on Examples 1-5 and Comparative Examples 1-3, samples of the finally prepared sealing ring material were taken for sealing contact stress attenuation rate testing: The samples were prepared as cylindrical specimens (29 mm in diameter, 12.5 mm in height), placed at 23°C for 24 hours, and the initial height of the center of each specimen was measured using a thickness gauge with an accuracy of ±0.01 mm. Then, the specimens and height limiters were placed between two compression plates, and compression (25% compression rate) was applied. After stabilization, the initial compression force was recorded. The specimens were then aged in a 150°C oven for 168 hours, cooled for 30 minutes, and the residual compression force was recorded under compression. The stress attenuation rate was calculated. Where R is the sealing contact stress attenuation rate, F0 is the initial compressive force, and F T (The residual compressive force after the test) was measured in 5 groups, and the average value was taken.

[0131] Based on Examples 1-5 and Comparative Examples 1-3, samples of the finally prepared sealing ring material were taken and subjected to critical tear pressure tests: The sealing ring material was placed in a high-pressure sealing test fixture (gap 0.25 mm), heated to 150°C, and the pressure was increased (pressure increase rate 1 MPa / min). When the pressure gauge showed a sudden and unsustainable drop in system pressure, or when a large amount of test medium leaked from the seal, the peak pressure at the moment of failure was recorded, which is the critical tear pressure of the sample under the test conditions. Five sets of measurements were taken and the average value was taken.

[0132] Based on Examples 1-5 and Comparative Examples 1-3, samples of the finally prepared sealing ring material were taken for leakage rate testing: the sealing ring material was placed in a high-pressure sealing test fixture (gap 0.05mm), heated to 150℃, increased the pressure to 140MPa, maintained for 168h, and the flow meter was used to take readings. Five sets of measurements were taken and the average value was taken.

[0133] The specific test results are shown in Tables 2 and 3. Figure 1 , Figure 2 , Figure 3 As shown: Table 2 Comparison of core performance of Examples 1-5 and Comparative Examples 1-3

[0134] Table 3 Performance Comparison of Examples 1-5 and Comparative Examples 1-3

[0135] The comparison results above show that Example 1 exhibits the best overall performance. Deep cleaning and activation, along with simultaneous chemical grafting of two fibers, constructs a robust interfacial network, demonstrating that Example 1 successfully solves the problem of significant compression set and cyclic residual deformation in current ultra-high pressure materials caused by fiber surface inertness, insufficient interfacial bonding, and filler agglomeration or uneven cross-linking. Under compression set test conditions of 150℃, 72h, and 25% compression ratio, the material prepared in Example 1 exhibits a compression set of 9.3±0.8%. Under leakage test conditions of 150℃, 140MPa, a radial gap of 0.05mm, and a holding time of 168h, the leakage rate is less than 0.01mL / min. These results indicate that the dual-fiber surface modification of this invention... The composite scheme can improve the deformation recovery ability and ultra-high pressure sealing performance of the synthetic polymer sealing material; the overall performance of Examples 2 to 5 is slightly lower than that of Example 1 but still maintains a high level, which shows that excellent performance improvement effect is still achieved under a large range of parameter changes; Comparative Example 1 does not treat the fiber in any way and directly mixes it, and the fiber surface exhibits high chemical inertness; Comparative Example 2 only modifies the aramid fiber. Although the aramid is strengthened, the unmodified polyester fiber has extremely poor compatibility with HNBR during mixing and vulcanization, and the stress preferentially concentrates at the polyester interface and causes damage; Comparative Example 3 has pretreatment but no in-situ grafting. Under long-term thermo-oxidative conditions, the physical interlocking force will quickly fail due to rubber creep.

[0136] In summary, it is clear from the above embodiments and comparative examples that the in-situ modified and enhanced composite ultra-high pressure sealing ring material provided by the present invention significantly improves both compression set and cyclic residual deformation. This is attributed to the construction of deep cleaning and activation, and simultaneous chemical grafting of dual fibers, thereby solving the problems of large compression set, large cyclic residual deformation, and leakage caused by insufficient interfacial bonding and filler agglomeration in composite ultra-high pressure sealing ring materials under long-term static pressure, cyclic pressure rise and fall, and high-temperature media.

Claims

1. An in-situ modified and reinforced composite ultra-high pressure sealing ring material, characterized in that: The sealing ring material is a synthetic polymer sealing material with hydrogenated nitrile rubber as the matrix and in-situ grafted aramid fiber and in-situ grafted polyester fiber as reinforcing components. Based on 100 parts by weight of hydrogenated nitrile butadiene rubber, the following components are included by weight: 1-2 parts of N-isopropyl-N′-phenyl-p-phenylenediamine, 5-15 parts of dioctyl phthalate, 10-20 parts of in-situ grafted aramid fiber, 10-20 parts of in-situ grafted polyester fiber, 20-40 parts of KH-570 modified nano-silica, 2-4 parts of dicumyl peroxide, and 1-2 parts of triallyl isocyanurate.

2. The in-situ modified and reinforced composite ultra-high pressure sealing ring material according to claim 1, characterized in that: The in-situ grafted aramid fiber has a diameter of 10-15 μm and a length of 3-10 mm. After activation treatment, the amino and carboxyl groups on the surface of the aramid fiber form covalent bonds with the epoxy groups of glycidyl methacrylate through ring-opening addition, while retaining the carbon-carbon double bonds in glycidyl methacrylate.

3. The in-situ modified and reinforced composite ultra-high pressure sealing ring material according to claim 1, characterized in that: The in-situ grafted polyester fiber has a diameter of 10-20 μm and a length of 3-10 mm. After activation treatment, the carboxyl and hydroxyl groups on the surface of the polyester fiber form covalent bonds with the epoxy groups of glycidyl methacrylate through ring-opening addition, while retaining the carbon-carbon double bonds in glycidyl methacrylate.

4. A method for preparing an in-situ modified and reinforced composite ultra-high pressure sealing ring material according to any one of claims 1-3, characterized in that: S1: Fiber pretreatment and surface activation; S11: Place the aramid fiber in acetone, sonicate, wash, then place it in an aqueous solution of sodium dodecyl sulfonate, sonicate, wash, and dry to obtain pretreated aramid fiber. S12: The pretreated aramid fiber prepared in S11 was placed in a 0.5 mol / L sodium hydroxide aqueous solution, stirred, removed, washed, and dried to constant weight to obtain modified aramid fiber; S13: Polyester fibers are placed in acetone, ultrasonically treated, washed, dried, ultraviolet treated, washed, and dried to constant weight to obtain modified polyester fibers. S2: In-situ grafting; S21: The modified aramid fiber prepared in S12 was added to toluene, then glycidyl methacrylate, tetrabutylammonium bromide and phenothiazine were added, stirred, heated and stirred under nitrogen protection, cooled, washed and dried to constant weight to obtain in-situ grafted aramid fiber. S22: The modified polyester fiber prepared in S13 was added to toluene, then glycidyl methacrylate, tetrabutylammonium bromide and phenothiazine were added, stirred, heated and stirred under nitrogen protection, cooled, washed and dried to constant weight to obtain in-situ grafted polyester fiber. S3: Mixing. Preheat HNBR rubber, pass through a thin plasticizer, increase the roller gap to 3mm, add N-isopropyl-N′-phenyl-p-phenylenediamine and dioctyl phthalate, mix, add in-situ grafted aramid fiber prepared in S21 and in-situ grafted polyester fiber prepared in S22 in batches, continue mixing after each batch, add nano-silica modified with KH-570, mix, add dicumyl peroxide and triallyl isocyanurate, pass through a thin plasticizer, and sheet to obtain HNBR compounded rubber sheet; S4: Compression vulcanization molding, the HNBR compound rubber sheet prepared in S3 is molded, pressure vulcanized, cooled and depressurized, and demolded to obtain the sealing ring material.

5. The method for preparing an in-situ modified and reinforced composite ultra-high pressure sealing ring material according to claim 4, characterized in that: The aramid fiber described in S11 has a mass-to-volume ratio of 1:50 to 1:100 g / mL with acetone. The ultrasonic treatment described in S11 has the following parameter settings: ultrasonic frequency 40–80 kHz, ultrasonic power density 0.3–0.6 W / cm². 2 The ultrasound duration is 20–60 minutes. The sodium dodecyl sulfonate aqueous solution described in S11 has a mass concentration of 2%, and the mass-volume ratio of aramid fiber to it is 1:50 g / mL. The drying process described in S11 has the following parameters: temperature 70–90°C, duration 4–8 hours.

6. The method for preparing an in-situ modified and reinforced composite ultra-high pressure sealing ring material according to claim 4, characterized in that: The pretreated aramid fiber described in S12 has a mass-to-volume ratio of 1:30 to 1:60 g / mL with sodium hydroxide aqueous solution. The stirring described in S12 has the following parameters: temperature 50-70℃, speed 100-300rpm, and duration 1-3h.

7. The method for preparing an in-situ modified and reinforced composite ultra-high pressure sealing ring material according to claim 4, characterized in that: The polyester fiber described in S13 has a mass-to-volume ratio of acetone of 1:50 to 1:100 g / mL. The ultrasonic treatment described in S13 has the following parameter settings: ultrasonic frequency 40–80 kHz, ultrasonic power density 0.3–0.6 W / cm². 2 The ultrasound duration is 20–60 minutes. The ultraviolet treatment described in S13 has the following parameters: wavelength 185nm and 254nm, ozone concentration 10-100ppm, and duration 10-50min.

8. The method for preparing an in-situ modified and reinforced composite ultra-high pressure sealing ring material according to claim 4, characterized in that: The modified aramid fiber described in S21 has a mass-to-volume ratio of 1:50 g / mL to toluene. The glycidyl methacrylate described in S21 is added at an amount of 10% to 30% of the mass of the modified aramid fiber. The tetrabutylammonium bromide described in S21 is added at an amount of 0.05% of the mass of the modified aramid fiber. The phenothiazine described in S21 is added at an amount of 0.02% of the mass of the modified aramid fiber; The heating and stirring reaction described in S21 has the following parameters: temperature 70-90℃, duration 4-8h.

9. The method for preparing an in-situ modified and reinforced composite ultra-high pressure sealing ring material according to claim 4, characterized in that: The modified polyester fiber described in S22 has a mass-to-volume ratio of 1:50 g / mL to toluene. The glycidyl methacrylate described in S22 is added at an amount of 10% to 30% of the mass of the modified polyester fiber. The tetrabutylammonium bromide mentioned in S22 is added at an amount of 0.05% of the mass of the modified polyester fiber; The phenothiazine described in S22 is added at an amount of 0.02% of the mass of the modified polyester fiber. The heating and stirring reaction described in S22 has the following parameters: temperature 70-90℃, duration 4-8h.

10. The method for preparing an in-situ modified and reinforced composite ultra-high pressure sealing ring material according to claim 4, characterized in that: The preheating described in S3 has the following parameters: temperature 50-70℃, duration 3-5min; The thin-pass plasticizing process described in S3 has the following parameter settings: temperature 50-70℃, roller gap 0.5-1.5mm, and number of passes 5-15. The pressure vulcanization described in S4 has the following parameters: pressure 10-20 MPa, temperature 150-170°C, and duration 20-40 min.

Citation Information

Patent Citations

  • Oilfield ultrahigh-pressure acid-resistant rubber seal material and preparation method thereof

    CN103396591A

  • Hydrogenized nitrile butadiene rubber and para aromatic polyamide fibre composite material and its preparing method

    CN1715319A