Marine floating photovoltaic dual-component halogen-free flame-retardant cable material and preparation method thereof
By modifying the composite halogen-free flame retardant with a double-layer surface and using a stepwise silane grafting process, the prepared marine floating photovoltaic two-component halogen-free flame retardant cable material exhibits excellent hydrolysis resistance, corrosion resistance, weather resistance, and mildew resistance in marine environments. This solves the problem of insufficient stability of existing cable materials in marine service and achieves long-term stability and reliability.
Patent Information
- Application Number
- CN202611198230.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-07
- Publication Date
- 2026-11-24
AI Technical Summary
Existing photovoltaic cable materials, when used in floating photovoltaic power plants at sea, suffer from insufficient resistance to hydrolysis, corrosion, weathering, mechanical properties, electrical stability, and mildew and anti-adhesion properties, leading to decreased insulation performance and material aging, making it difficult to use stably for a long time in complex marine environments.
A double-layer surface modification was performed using a dried composite halogen-free flame retardant, and a two-component halogen-free flame retardant cable material for marine floating photovoltaics was prepared through a step-by-step silane grafting process. This process included modification with vinylalkoxysilane hydrolysate and fatty acid treatment solution, combined with step-by-step treatment of the polyolefin composite matrix and separate packaging of the crosslinking catalyst, to form a stable crosslinking network structure.
It improves the environmental tolerance and long-term service stability of cable materials under seawater immersion, salt spray and ultraviolet humid heat environments, and enhances flame retardancy, weather resistance, mildew and anti-adhesion properties and electrical stability, so as to meet the long-term service requirements of complex marine environments.
Smart Images

Figure CN123152192A_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of cable material technology, and more specifically, to a marine floating photovoltaic two-component halogen-free flame-retardant cable material and its preparation method. Background Technology
[0002] With the development of photovoltaic power generation technology, offshore floating photovoltaic power stations have gradually become an important form of marine new energy utilization. As an important component for power transmission and equipment connection, the material properties of photovoltaic cables directly affect the operational safety and long-term service reliability of the power station.
[0003] Existing terrestrial photovoltaic cable materials typically employ a halogen-free, low-smoke flame-retardant system composed of silane cross-linked polyolefins. These materials possess good insulation, flame-retardant, and processing properties, meeting the general requirements of terrestrial photovoltaic power plants. However, offshore floating photovoltaic cables operate under complex environments characterized by long-term seawater immersion, salt spray corrosion, strong ultraviolet radiation, alternating high temperature and humidity, dynamic bending from wind and waves, and the attachment of marine microorganisms. Their service conditions are significantly more demanding than those of terrestrial photovoltaic systems. Therefore, higher requirements are placed on the cable materials' resistance to hydrolysis, corrosion, weathering, mechanical properties, electrical stability, and surface anti-mildew and anti-adhesion properties.
[0004] In the aforementioned marine environment, existing silane cross-linked halogen-free cable materials are prone to problems such as water absorption, interface degradation, decreased insulation performance, material pulverization, cracking, and mechanical property attenuation, which in turn affect the cable's ability to resist long-term salt spray aging and repeated bending by wind and waves. Furthermore, under conditions of high humidity, high salinity, and alternating temperatures, the surface of the cable insulation or sheath layer is susceptible to mold growth, initial attachment of marine microorganisms and algae, and biofilm formation, exacerbating surface contamination, localized interface degradation, and long-term performance degradation. Simultaneously, existing weather-resistant systems, flame-retardant filling systems, and cross-linking systems lack sufficient stability under the combined effects of strong ultraviolet radiation, high-humidity salt spray, and biofilm attachment, making it difficult to simultaneously maintain flame retardancy, low smoke performance, corrosion resistance, weather resistance, anti-mold and anti-adhesion properties, mechanical properties, and electrical stability during long-term service. Summary of the Invention
[0005] The purpose of this application is to provide a marine floating photovoltaic two-component halogen-free flame-retardant cable material and its preparation method, so as to solve the problem of insufficient environmental tolerance and long-term service stability of existing photovoltaic cable materials under seawater immersion, salt spray and ultraviolet humid heat environments.
[0006] Other features and advantages of this application will become apparent from the following detailed description, or may be learned in part from practice of this application.
[0007] According to one aspect of this application, a method for preparing a marine floating photovoltaic two-component halogen-free flame-retardant cable material is provided. The cable material comprises a separately packaged main component and a crosslinking catalytic component. The preparation method includes the following steps: S1. The dried composite halogen-free flame retardant is subjected to first surface modification with vinylalkoxysilane hydrolysate and second surface modification with fatty acid treatment solution to obtain a double-layer modified halogen-free flame retardant. S2. The polyolefin composite matrix is divided into a first matrix and a second matrix. The first matrix is melt-grafted with a silane grafting system and extruded and granulated to obtain a silane grafting masterbatch. S3. Plasticize the second matrix to obtain a plasticized matrix. Then, perform a first intensive mixing of the plasticized matrix, the double-layer modified halogen-free flame retardant, and the functional additives to obtain a flame-retardant, weather-resistant, and anti-adhesion mixture. S4. Add the silane grafted masterbatch to the flame-retardant, weather-resistant and anti-adhesion mixture, and perform a second internal mixing to obtain the main material premix. Then, the main material premix is extruded, granulated, dried and sealed in packaging to obtain the main material component. S5. The crosslinking catalyst is mixed with the polyolefin support resin and extruded and granulated to obtain the crosslinking catalyst masterbatch, and the crosslinking catalyst masterbatch is sealed and packaged to obtain the crosslinking catalyst component.
[0008] According to one aspect of this application, this application also provides a marine floating photovoltaic two-component halogen-free flame-retardant cable material, the cable material comprising a main component and a crosslinking catalyst component, the main component being prepared from the following raw materials in parts by weight: based on 100 parts by weight of polyolefin composite matrix, 100 parts of polyolefin composite matrix, 80-120 parts of double-layer modified halogen-free flame retardant, 1.5-3.0 parts of silane graft monomer, 0.12-0.40 parts of initiator, 2.0-5.0 parts of corrosion and weather resistance additive, 2.0-6.0 parts of compatibility processing aid, and 0.5-3.0 parts of mildew and anti-adhesion additive; The crosslinking catalytic component includes a crosslinking catalyst and a polyolefin support resin. Based on 100 parts by weight of the polyolefin composite matrix in the main component, the amount of the polyolefin support resin is 2.0 to 10.0 parts, and the amount of the crosslinking catalyst is 0.05 to 0.25 parts. The polyolefin composite matrix includes high-density polyethylene, linear low-density polyethylene and ethylene-octene copolymer elastomer, and the weight ratio of high-density polyethylene, linear low-density polyethylene and ethylene-octene copolymer elastomer is 4-5:2:1; The polyolefin carrier resin is selected from at least one of high-density polyethylene, linear low-density polyethylene, and ethylene-octene copolymer elastomer; The double-layer modified halogen-free flame retardant is a flame retardant obtained by sequentially modifying a composite halogen-free flame retardant with a vinylalkoxysilane hydrolysate and a fatty acid treatment solution. The crosslinking catalyst is selected from at least one of tetrazirconium tetra(acetylacetone), diisopropoxybis(acetylacetone) titanium, and zirconium lactate ammonium; The corrosion-resistant and weather-resistant additive is selected from at least one of pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], tris(2,4-di-tert-butylphenyl) phosphite, bis(2,2,6,6-tetramethyl-4-piperidinyl) sebacate, and nano zinc oxide; The compatible processing aid is selected from at least one of maleic anhydride-grafted polyethylene, oxidized polyethylene wax, and polydimethylsiloxane. The anti-mildew and anti-adhesion additive includes at least one of quaternary ammonium salt modified nano silica, N-vanillyl nonylamide, and nano copper oxide.
[0009] As can be seen from the above technical solutions, the marine floating photovoltaic two-component halogen-free flame-retardant cable material and its preparation method in the exemplary embodiments of this application have at least the following advantages and positive effects: In some embodiments of this application, the technical solutions provided, on the one hand, overcome the problems of insufficient interfacial bonding, easy water absorption and poor dispersion stability of existing inorganic flame retardants in polyolefin matrix by using a double-layer surface modification technique of sequentially passing the dried composite halogen-free flame retardant through silane coupling agent hydrolysis solution and stearic acid treatment solution, thereby achieving the technical effect of improving the interfacial stability and marine environment tolerance of flame retardants.
[0010] On the other hand, by dividing the polyolefin compound matrix into a first matrix and a second matrix, a silane grafting masterbatch is first prepared, and then the second matrix, the double-layer modified halogen-free flame retardant and functional additives are subjected to a first internal mixing. After the first internal mixing, the silane grafting masterbatch is added for a second internal mixing. This overcomes the problems of mutual interference between grafting reaction, flame retardant dispersion and additive mixing in the existing one-time mixing, and achieves the technical effect of improving mixing uniformity and processing stability.
[0011] In addition, by preparing the main component and the crosslinking catalyst component separately and sealing them in packaging, the problems of premature crosslinking and subsequent decrease in melt flowability during the storage of single-component silane crosslinked cable materials are overcome, and the technical effects of improving storage stability, extrusion processing adaptability and crosslinking controllability are achieved.
[0012] In summary, this technical solution improves the environmental tolerance and long-term service stability of marine floating photovoltaic two-component halogen-free flame-retardant cable material under seawater immersion, salt spray and ultraviolet humid heat environments through the synergistic effect of double-layer surface modification with composite halogen-free flame retardant and stepwise silane grafting process of polyolefin matrix.
[0013] It should be understood that the above general description and the following detailed description are exemplary and explanatory only, and are not intended to limit this application. Attached Figure Description
[0014] The accompanying drawings, which are incorporated in and form part of this specification, illustrate embodiments consistent with this application and, together with the description, serve to explain the principles of this application. It is obvious that the drawings described below are merely some embodiments of this application, and those skilled in the art can obtain other drawings based on these drawings without any inventive effort. In the drawings: Figure 1 This is a schematic diagram of the overall process for preparing a marine floating photovoltaic two-component halogen-free flame-retardant cable material in one embodiment; Figure 2 This is a flowchart of step S1 of a method for preparing a marine floating photovoltaic two-component halogen-free flame-retardant cable material in one embodiment; Figure 3 This is a flowchart of step S2 in a method for preparing a marine floating photovoltaic two-component halogen-free flame-retardant cable material in one embodiment; Figure 4 This is a flowchart of step S3 in a method for preparing a marine floating photovoltaic two-component halogen-free flame-retardant cable material in one embodiment; Figure 5 This is a flowchart of step S4 in a method for preparing a marine floating photovoltaic two-component halogen-free flame-retardant cable material in one embodiment; Figure 6 This is a flowchart of step S5 in a method for preparing a marine floating photovoltaic two-component halogen-free flame-retardant cable material in one embodiment. Detailed Implementation
[0015] Exemplary embodiments will now be described more fully with reference to the accompanying drawings. However, these exemplary embodiments can be implemented in many forms and should not be construed as limited to the examples set forth herein; rather, these embodiments are provided to make this application more comprehensive and complete, and to fully convey the concept of the exemplary embodiments to those skilled in the art.
[0016] Furthermore, the described features or characteristics may be combined in any suitable manner in one or more embodiments. Numerous specific details are provided in the following description to give a full understanding of embodiments of this application. However, those skilled in the art will recognize that the technical solutions of this application may be practiced without one or more of the specific details, or other methods may be employed. In other instances, well-known methods, implementations, or operations are not shown or described in detail to avoid obscuring various aspects of this application.
[0017] This application is intended to cover any variations, uses, or adaptations of this application that follow the general principles of this application and include common knowledge or customary techniques in the art not disclosed in this application. The specification and embodiments are to be considered exemplary only, and the true scope and spirit of this application are indicated by the following claims.
[0018] It should be understood that this application is not limited to the precise structure described above and shown in the accompanying drawings, and various modifications and changes can be made without departing from its scope. The scope of this application is limited only by the appended claims.
[0019] like Figure 1 As shown, this application provides a method for preparing a marine floating photovoltaic two-component halogen-free flame-retardant cable material, the cable material comprising a main component and a crosslinking catalytic component, and the preparation method comprising steps S1 to S5.
[0020] S1. The dried composite halogen-free flame retardant is subjected to first surface modification with vinylalkoxysilane hydrolysate and second surface modification with fatty acid treatment solution to obtain a double-layer modified halogen-free flame retardant. S2. The polyolefin composite matrix is divided into a first matrix and a second matrix. The first matrix is melt-grafted with a silane grafting system and extruded and granulated to obtain a silane grafting masterbatch. S3. Plasticize the second matrix to obtain a plasticized matrix. Then, perform a first intensive mixing of the plasticized matrix, the double-layer modified halogen-free flame retardant, and the functional additives to obtain a flame-retardant, weather-resistant, and anti-adhesion mixture. S4. Add the silane grafted masterbatch to the flame-retardant, weather-resistant and anti-adhesion mixture, and perform a second internal mixing to obtain the main material premix. Then, the main material premix is extruded, granulated, dried and sealed in packaging to obtain the main material component. S5. The crosslinking catalyst is mixed with the polyolefin support resin and extruded and granulated to obtain the crosslinking catalyst masterbatch, and the crosslinking catalyst masterbatch is sealed and packaged to obtain the crosslinking catalyst component.
[0021] like Figure 2 As shown, step S1 includes drying the composite halogen-free flame retardant, preparing the vinylalkoxysilane hydrolysate, first surface modification, preparing the fatty acid treatment solution, second surface modification, and drying and sieving steps.
[0022] Step S1 includes the following sub-steps: S1.1 Mix magnesium-containing inorganic flame retardant, aluminum-containing inorganic flame retardant and borate flame retardant synergist, and dry in a vacuum oven at 90-100℃ for 3-4 hours to obtain the dried composite halogen-free flame retardant.
[0023] The magnesium-containing inorganic flame retardant is selected from at least one of magnesium hydroxide, basic magnesium carbonate, and magnesium carbonate. The aluminum-containing inorganic flame retardant is selected from at least one of aluminum hydroxide and boehmite. The borate flame retardant synergist is selected from at least one of zinc borate, calcium borate, and magnesium borate. The weight ratio of the magnesium-containing inorganic flame retardant, the aluminum-containing inorganic flame retardant, and the borate flame retardant synergist is 60–75:20–35:3–8.
[0024] Vacuum drying of the composite halogen-free flame retardant can reduce the surface water content of the inorganic flame retardant, thereby reducing agglomeration and uncontrolled hydrolysis caused by excessive moisture during subsequent silane hydrolysis treatment. This improves the uniformity of surface modification of the composite halogen-free flame retardant. The synergistic use of magnesium-containing inorganic flame retardants, aluminum-containing inorganic flame retardants, and borate flame retardant synergists can address the needs of flame retardancy, charring synergy, and processing dispersion, thus improving the basic halogen-free flame retardant properties of cable materials.
[0025] S1.2. Mix ethanol and deionized water in a mass ratio of 70:30 to 95:5 to obtain ethanol-water mixed solvent A; Vinylalkoxysilane was added to the ethanol-water mixed solvent A to obtain a silane mixture. The pH of the silane mixture was adjusted to 4.0-5.0 with acetic acid, and the mixture was stirred and pre-hydrolyzed at 20-40°C for 20-60 min to obtain a vinylalkoxysilane hydrolysate.
[0026] The vinylalkoxysilane is selected from at least one of vinyltriethoxysilane and vinyltrimethoxysilane. The mass of the vinylalkoxysilane is 0.5% to 2.0% of the mass of the composite halogen-free flame retardant.
[0027] Using ethanol and deionized water as a mixed solvent can improve the dispersibility of vinylalkoxysilanes in the system and provide a suitable moisture environment for silane pre-hydrolysis. Maintaining the pH at 4.0–5.0 with acetic acid and pre-hydrolyzing at 20–40°C for 20–60 min can promote the formation of reactive hydrolysis products from vinylalkoxysilanes, thus facilitating subsequent bonding with the surface of the composite halogen-free flame retardant and improving the stability of the first surface modification.
[0028] S1.3. Take ethanol and deionized water and mix them in a mass ratio of 70:30 to 95:5 to obtain ethanol-water mixed solvent B; disperse the dried composite halogen-free flame retardant in the ethanol-water mixed solvent B, add the vinylalkoxysilane hydrolysate under stirring conditions of 500 to 1500 r / min, and continue to react at 50 to 80 °C for 1 to 3 h to obtain the first surface-modified slurry.
[0029] The dried composite halogen-free flame retardant was first dispersed in an ethanol-water mixed solvent B, and then a vinylalkoxysilane hydrolysate was added under stirring to allow the hydrolyzed silane components to gradually contact the surface of the composite halogen-free flame retardant. The reaction temperature was controlled at 50–80℃, and the reaction time was controlled at 1–3 h.
[0030] By adding vinylalkoxysilane hydrolysate under stirring conditions of 500–1500 r / min, the local agglomeration of the composite halogen-free flame retardant can be reduced, resulting in a more uniform distribution of silane hydrolysis products on the surface of the composite halogen-free flame retardant. Through this first surface modification, an organic reaction or compatible transition layer can be introduced between the composite halogen-free flame retardant and the polyolefin matrix, thereby improving the interfacial bonding and dispersion stability of the inorganic flame retardant in the polyolefin system.
[0031] S1.4 Add stearic acid to anhydrous ethanol and stir to dissolve or disperse at 60-75°C to obtain fatty acid treatment solution.
[0032] The mass of stearic acid is 0.3% to 1.5% of the mass of the composite halogen-free flame retardant. After adding stearic acid to anhydrous ethanol, the mixture is stirred at 60 to 75°C to dissolve or uniformly disperse the stearic acid in the anhydrous ethanol, forming a fatty acid treatment solution.
[0033] By preparing a fatty acid treatment solution, stearic acid can act more uniformly on the surface of the composite halogen-free flame retardant in the first surface modification slurry during the subsequent second surface modification process. This is beneficial for the formation of the outer fatty acid modified layer, reducing the surface polarity of the inorganic flame retardant, and improving its compatibility with the polyolefin composite matrix.
[0034] S1.5. Add the fatty acid treatment solution to the first surface-modified slurry, heat to 70-90°C, and continue the reaction for 30-90 minutes under stirring conditions of 500-1500 r / min to obtain a wet double-layer modified halogen-free flame retardant.
[0035] A fatty acid treatment solution was added to the first surface-modified slurry, and the reaction system was heated to 70-90°C. The reaction was continued for 30-90 minutes under stirring conditions of 500-1500 r / min, so that the fatty acid treatment solution acted on the surface of the first surface-modified composite halogen-free flame retardant.
[0036] By further treating with fatty acids after the first surface modification, a fatty acid modified layer can be formed on the outside of the vinylalkoxysilane modified layer, thereby obtaining a wet-state bilayer modified halogen-free flame retardant. This bilayer modified structure helps to reduce the surface hydrophilicity of the inorganic flame retardant, improve its wetting and dispersion state in the polyolefin matrix, thereby reducing interface defects and improving the water resistance, salt spray resistance and mechanical retention properties of the cable material.
[0037] S1.6. The wet double-layer modified halogen-free flame retardant is placed in a vacuum drying oven and dried for 3 to 8 hours at 80 to 110°C and a gauge pressure of -0.095 to -0.060 MPa. The dried flame retardant is then sieved through a 100 to 500 mesh screen to obtain the double-layer modified halogen-free flame retardant.
[0038] The wet double-layer modified halogen-free flame retardant was vacuum dried to remove ethanol, water and other volatile components from the system; after drying, it was sieved through a 100-500 mesh sieve to obtain a double-layer modified halogen-free flame retardant with a relatively uniform particle size distribution.
[0039] Vacuum drying reduces residual solvents and moisture in the double-layer modified halogen-free flame retardant, minimizing bubbles, voids, and interface defects during subsequent melt processing. Sieving removes larger agglomerates, making the double-layer modified halogen-free flame retardant more suitable for subsequent internal mixing and dispersion, thereby improving the processing stability and performance uniformity of the cable material.
[0040] like Figure 3 As shown, step S2 includes the following steps: dispensing of polyolefin compound matrix, preparation of grafted premix, and melt grafting granulation.
[0041] Step S2 includes the following sub-steps: S2.1 The polyolefin composite matrix is divided into a first matrix and a second matrix, wherein the first matrix accounts for 40% to 60% of the total mass of the polyolefin composite matrix, and the second matrix is the remaining part of the polyolefin composite matrix excluding the first matrix.
[0042] Specifically, the polyolefin composite matrix includes high-density polyethylene, linear low-density polyethylene, and ethylene-octene copolymer elastomer, wherein the weight ratio of high-density polyethylene, linear low-density polyethylene, and ethylene-octene copolymer elastomer is 4-5:2:1.
[0043] By dividing the polyolefin compound matrix into a first matrix and a second matrix, a portion of the polyolefin compound matrix can be melt-grafted with a silane grafting system to form a silane grafting masterbatch; the other portion serves as the internal mixing matrix for subsequent mixing of bilayer modified halogen-free flame retardants and functional additives. This step-by-step processing method helps reduce the mutual interference between the silane grafting reaction and the dispersion process of highly filled flame retardants, thereby improving the stability of the grafting reaction and the subsequent internal mixing and dispersion effect.
[0044] S2.2. Mix the first matrix with the silane grafting system to obtain a grafted premix.
[0045] Specifically, the silane grafting system includes a silane grafting monomer and an initiator. The silane grafting monomer is selected from at least one of vinyltrimethoxysilane and vinyltriethoxysilane. The initiator is a composite peroxide initiator, comprising dicumyl peroxide and 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane, wherein the mass ratio of dicumyl peroxide to 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane is 1:0.5–2. Based on 100 parts by weight of the polyolefin composite matrix, the amount of the silane grafting monomer is 1.5–3.0 parts, and the amount of the initiator is 0.12–0.40 parts.
[0046] By premixing the first matrix with silane graft monomers and initiators, the uniformity of their distribution within the first matrix can be improved, thus providing a homogeneous reaction basis for subsequent melt grafting. The composite peroxide initiator can initiate the generation of grafting active sites on polyolefin segments at melt processing temperatures, thereby promoting the bonding of silane graft monomers with the polyolefin matrix and enhancing the reactivity and subsequent hydrolytic crosslinking ability of the silane graft masterbatch.
[0047] S2.3. The grafted premix is added to an extruder and melt-grafted at 150-190°C. After extrusion, cooling and pelletizing, silane grafted masterbatch is obtained.
[0048] The grafted premix is added to an extruder, where the first matrix, silane grafting monomer, and initiator are melted and mixed at 150–190°C and a grafting reaction occurs. The melt after the reaction is extruded, cooled, and pelletized to obtain silane grafted masterbatch.
[0049] By performing melt grafting of the grafted premix in an extruder, continuous mixing and reaction can be achieved, enhancing the grafting degree of silane graft monomers onto the polyolefin matrix. After the silane grafted product is made into a masterbatch, it can be used in a subsequent second internal mixing process to improve the dispersion uniformity of the silane grafted components and facilitate the subsequent formation of hydrolyzable crosslinkable mixtures.
[0050] like Figure 4 As shown, step S3 includes a second matrix plasticization and a first mixing step of the double-layer modified halogen-free flame retardant and functional additives.
[0051] Step S3 includes the following sub-steps: S3.1 Add the second matrix to a mixing apparatus and plasticize it at 110-150°C for 2-5 minutes to obtain a plasticized matrix.
[0052] The second matrix is added to a mixing apparatus and plasticized at 110–150°C for 2–5 minutes to soften the second matrix and form a plasticized matrix suitable for further mixing.
[0053] By first plasticizing the second matrix, the matrix's ability to coat the double-layer modified halogen-free flame retardant and functional additives can be improved, reducing uneven dispersion and local agglomeration caused by direct addition of powder, thereby improving the uniformity of the subsequent flame-retardant, weather-resistant, and anti-adhesion mixture.
[0054] S3.2 Add the double-layer modified halogen-free flame retardant and functional additives to the plasticized matrix, and perform a first mixing at 110-150°C for 5-15 minutes to obtain a flame-retardant, weather-resistant, and anti-adhesion mixture.
[0055] The functional additives include corrosion-resistant and weather-resistant additives, compatibility processing aids, and anti-mildew and anti-adhesion additives. Based on 100 parts by weight of the polyolefin compound matrix, the amount of the double-layer modified halogen-free flame retardant is 80-120 parts, the amount of the corrosion-resistant and weather-resistant additive is 2.0-5.0 parts, the amount of the compatibility processing aid is 2.0-6.0 parts, and the amount of the anti-mildew and anti-adhesion additive is 0.5-3.0 parts.
[0056] The corrosion-resistant and weather-resistant additive is selected from at least one of pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], tris(2,4-di-tert-butylphenyl)phosphite, bis(2,2,6,6-tetramethyl-4-piperidinyl)sebacate, and nano zinc oxide.
[0057] The compatible processing aid is selected from at least one of maleic anhydride-grafted polyethylene, oxidized polyethylene wax, and polydimethylsiloxane.
[0058] The anti-mildew and anti-adhesion additive is selected from at least one of quaternary ammonium salt modified nano silica, N-vanillylnonamide, and nano copper oxide. The quaternary ammonium salt modified nano silica is nano silica that has been surface modified with 3-(trimethoxysilyl)propyldimethyloctadecylammonium chloride.
[0059] By incorporating a double-layer modified halogen-free flame retardant into the plasticized matrix, the flame retardant can be fully dispersed in the polyolefin system, forming a flame-retardant filler network. Simultaneously adding corrosion-resistant and weather-resistant additives, compatibility processing aids, and anti-mildew and anti-adhesion additives can improve the material's resistance to heat, oxygen, ultraviolet radiation, salt spray, high humidity, and marine microbial adhesion environments. It also improves the interfacial bonding, processing flowability, and surface stability of the highly filled system, resulting in a flame-retardant, weather-resistant, and anti-adhesion compound that combines flame retardancy, weather resistance, anti-mildew and anti-adhesion properties, and processing stability.
[0060] like Figure 5 As shown, step S4 includes the addition of silane grafted masterbatch, a second internal mixing step, and the main component extrusion granulation, drying, and sealing packaging steps.
[0061] Step S4 includes the following sub-steps: S4.1 After the first internal mixing is completed, the silane grafting masterbatch is added to the flame-retardant, weather-resistant and anti-adhesion mixture, and the mixture is subjected to a second internal mixing at 100-140°C for 2-8 minutes to obtain the main material premix. After obtaining the flame-retardant, weather-resistant, and anti-adhesion mixture, the silane grafting masterbatch is added to it to further mix the silane grafting masterbatch with the mixture that has already dispersed the double-layer modified halogen-free flame retardant and functional additives evenly.
[0062] By adding silane grafted masterbatch after the first mixing, silane grafted components can be introduced after the double-layer modified halogen-free flame retardant and functional additives have been basically dispersed. This reduces the mutual interference between the silane grafted components and the dispersion process of the highly filled flame retardant, thereby improving the dispersion uniformity of the silane grafted components in the main components and the controllability of the subsequent crosslinking reaction.
[0063] S4.2 Add the main premixed material to an extruder, extrude it at 140-180°C, and then cool and pelletize it to obtain the main component granules.
[0064] Extrusion at 140–180°C allows for further melting and homogenization of the main premix, resulting in granular main components with relatively stable dimensions. Cooling and pelletizing facilitate subsequent storage, transportation, and use in cable processing.
[0065] S4.3. The main component granules are dried at 60-80°C for 2-6 hours and sealed in aluminum-plastic composite bags to obtain the main component of the marine floating photovoltaic dual-component halogen-free flame-retardant cable material.
[0066] The main component contains a polyolefin compound matrix, a double-layer modified halogen-free flame retardant, functional additives, and a silane grafting component. By drying and sealing the main component granules, the residual moisture in the granules and the influence of external moisture can be reduced, the risk of premature hydrolysis and condensation of the silane grafting component during storage can be reduced, and the storage stability and subsequent extrusion processing stability of the main component can be improved.
[0067] like Figure 6 As shown, step S5 includes the preparation of crosslinked catalyst masterbatch and the sealing and packaging of crosslinked catalyst components.
[0068] Step S5 includes the following sub-steps: S5.1. The crosslinking catalyst is mixed with the polyolefin carrier resin and extruded and granulated to obtain the crosslinking catalyst masterbatch. The crosslinking catalyst masterbatch is then sealed and packaged to obtain the crosslinking catalyst component of the marine floating photovoltaic two-component halogen-free flame-retardant cable material.
[0069] The polyolefin carrier resin is selected from at least one of high-density polyethylene, linear low-density polyethylene, and ethylene-octene copolymer elastomer.
[0070] The crosslinking catalyst is selected from at least one of tetrazirconium tetra(acetylacetone), diisopropoxybis(acetylacetone) titanium, and zirconium lactate ammonium.
[0071] Based on 100 parts by weight of the polyolefin composite matrix in the main component, the amount of the polyolefin carrier resin is 2.0 to 10.0 parts, and the amount of the crosslinking catalyst is 0.05 to 0.25 parts.
[0072] The polyolefin carrier resin is used to support and disperse the crosslinking catalyst to form a crosslinking catalyst masterbatch. Because the polyolefin carrier resin is compatible with the polyolefin matrix in the main component, the crosslinking catalyst component can be uniformly mixed with the main component before or during cable extrusion, thereby improving the dispersion uniformity of the crosslinking catalyst. By separately preparing the crosslinking catalyst into a crosslinking catalyst component and sealing it in packaging, the crosslinking catalyst can be prevented from prematurely entering the main component, reducing the risk of premature crosslinking and increased gel content during storage of the main component.
[0073] This application also provides the application of the above-mentioned marine floating photovoltaic two-component halogen-free flame-retardant cable material in marine floating photovoltaic cables.
[0074] In one embodiment, the main material components and crosslinking catalyst components are mixed before cable extrusion, or separately metered and added to the cable extrusion equipment and mixed during the cable extrusion process. The mixed material is melt-plasticized and extruded onto the outside of the conductor, insulated core, or cable core to form an insulation layer or sheath layer. Subsequently, the extruded insulation layer or sheath layer is subjected to hydrolytic crosslinking treatment to obtain a marine floating photovoltaic cable.
[0075] The hydrolysis crosslinking treatment can be carried out by hot water crosslinking, steam crosslinking or constant temperature and humidity crosslinking, so that the hydrolyzable silane groups in the cable material undergo hydrolysis and condensation reaction under the action of crosslinking catalyst to form a crosslinked network structure.
[0076] This cross-linked network structure improves the dimensional stability, crack resistance, and electrical insulation performance retention of the insulation or sheath layer under conditions such as seawater immersion, salt spray corrosion, ultraviolet irradiation, humid and hot environments, and dynamic bending. Furthermore, the anti-mold and anti-adhesion additives reduce the risk of mold growth and initial adhesion of marine microorganisms, algae, or biofilms to the surface of the insulation or sheath layer in high-humidity and high-salt environments.
[0077] By using the two-component halogen-free flame-retardant cable material for marine floating photovoltaics of this application to prepare the insulation or sheath layer of marine floating photovoltaic cables, the resulting cable product can have halogen-free flame-retardant properties, water resistance, salt spray resistance, weather resistance, mildew and anti-adhesion properties, and extrusion processing stability, thus making it suitable for long-term service environments in marine floating photovoltaic power generation systems.
[0078] Example 1: Magnesium hydroxide was used as a magnesium-containing inorganic flame retardant, aluminum hydroxide as an aluminum-containing inorganic flame retardant, and zinc borate as a borate flame retardant synergist. The magnesium hydroxide, aluminum hydroxide, and zinc borate were mixed in a weight ratio of 65:30:5 to obtain a composite halogen-free flame retardant.
[0079] The composite halogen-free flame retardant was placed in a vacuum oven and dried at 95°C for 3.5 hours to obtain the dried composite halogen-free flame retardant.
[0080] Ethanol and deionized water were mixed at a mass ratio of 85:15 to obtain ethanol-water mixed solvent A. Based on the dry weight of 100 parts by weight of the composite halogen-free flame retardant, 1.2 parts by weight of vinyltriethoxysilane were added to the ethanol-water mixed solvent A to obtain a silane mixture. The pH of the silane mixture was adjusted to 4.5 using acetic acid, and the mixture was pre-hydrolyzed at 30°C for 40 min with stirring to obtain a vinylalkoxysilane hydrolysate.
[0081] Separately, ethanol and deionized water were mixed at a mass ratio of 85:15 to obtain an ethanol-water mixed solvent B. The dried composite halogen-free flame retardant was dispersed in the ethanol-water mixed solvent B, and the vinylalkoxysilane hydrolysate was added under stirring at 1000 r / min. The reaction was continued at 65 °C for 2 h to obtain the first surface-modified slurry.
[0082] Based on the dry basis of 100 parts by weight of composite halogen-free flame retardant, 0.8 parts by weight of stearic acid were added to anhydrous ethanol and stirred at 68°C to dissolve or disperse, thus obtaining a fatty acid treatment solution.
[0083] The fatty acid treatment solution was added to the first surface-modified slurry, the temperature was raised to 80°C, and the reaction was continued for 60 minutes under stirring at 1000 r / min to obtain a wet double-layer modified halogen-free flame retardant.
[0084] The wet double-layer modified halogen-free flame retardant was placed in a vacuum drying oven and dried for 5 hours at 95°C and a gauge pressure of -0.080 MPa. After drying, it was sieved through a 300-mesh sieve to obtain double-layer modified halogen-free flame retardant A1.
[0085] A polyolefin composite matrix of 100 parts by weight is composed of 57.1 parts by weight of high-density polyethylene, 28.6 parts by weight of linear low-density polyethylene, and 14.3 parts by weight of ethylene-octene copolymer elastomer. The weight ratio of high-density polyethylene, linear low-density polyethylene, and ethylene-octene copolymer elastomer is 4:2:1.
[0086] The polyolefin composite matrix is divided into a first matrix and a second matrix, wherein the first matrix is 50 parts by weight and the second matrix is 50 parts by weight.
[0087] Based on 100 parts by weight of a polyolefin composite matrix, 2.2 parts by weight of vinyltrimethoxysilane and 0.25 parts by weight of a composite peroxidation initiator were added to the first matrix and mixed evenly to obtain a grafting premix. The composite peroxidation initiator was composed of dicumyl peroxide and 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane in a mass ratio of 1:1.
[0088] The grafted premix is added to an extruder and melt-grafted at 170°C. After extrusion, cooling and pelleting, silane grafted masterbatch is obtained.
[0089] The second matrix is added to a mixing apparatus and plasticized at 130°C for 3 minutes to obtain a plasticized matrix.
[0090] Based on 100 parts by weight of polyolefin compound matrix, 100 parts by weight of double-layer modified halogen-free flame retardant A1, 3.5 parts by weight of corrosion and weather resistance agent, 3.0 parts by weight of compatibility processing aid and 1.5 parts by weight of mildew and anti-adhesion agent are added to the plasticized matrix. The mixture is then subjected to a first internal mixing at 130°C for 10 minutes to obtain a flame-retardant, weather-resistant and anti-adhesion mixture.
[0091] The corrosion-resistant and weather-resistant additive is composed of 0.8 parts by weight of pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], 0.8 parts by weight of tris(2,4-di-tert-butylphenyl) phosphite, 1.0 part by weight of bis(2,2,6,6-tetramethyl-4-piperidinyl) sebacate and 0.9 parts by weight of nano zinc oxide.
[0092] The compatible processing aid consists of 1.5 parts by weight of maleic anhydride-grafted polyethylene, 1.0 parts by weight of oxidized polyethylene wax, and 0.5 parts by weight of polydimethylsiloxane.
[0093] The anti-mildew and anti-adhesion additive is composed of 1.0 parts by weight of quaternary ammonium salt modified nano silica and 0.5 parts by weight of N-vanillylnonamide; the quaternary ammonium salt modified nano silica is nano silica that has been surface modified with 3-(trimethoxysilyl)propyldimethyloctadecylammonium chloride.
[0094] After the first mixing, the silane grafted masterbatch is added to the flame-retardant, weather-resistant, and anti-adhesion mixture, and a second mixing is carried out at 120°C for 5 minutes to obtain the main material premix.
[0095] The main premixed material is added to an extruder, extruded at 160°C, and then cooled and pelletized to obtain the main component granules.
[0096] The obtained main component granules were dried at 70°C for 4 hours and then sealed in aluminum-plastic composite bags to obtain the main component of the marine floating photovoltaic bicomponent halogen-free flame-retardant cable material of Example 1.
[0097] Another 5.0 parts by weight of linear low-density polyethylene were used as the polyolefin carrier resin. 0.12 parts by weight of tetrazirconium tetra(acetylacetone) were mixed with the polyolefin carrier resin. After extrusion granulation, drying and sealing packaging, the crosslinking catalytic component of the marine floating photovoltaic bicomponent halogen-free flame-retardant cable material of Example 1 was obtained.
[0098] Example 2: Example 2 is based on Example 1, but the aluminum-containing inorganic flame retardant is replaced with boehmite instead of aluminum hydroxide, and the borate flame retardant synergist is replaced with calcium borate instead of zinc borate. The magnesium-containing inorganic flame retardant remains magnesium hydroxide. The composite halogen-free flame retardant is composed of magnesium hydroxide, boehmite, and calcium borate in a weight ratio of 60:35:5.
[0099] Based on the dry basis of 100 parts by weight of composite halogen-free flame retardant, the amount of vinyltriethoxysilane used in the vinylalkoxysilane hydrolysate is 0.5 parts by weight, and the amount of stearic acid is 0.3 parts by weight.
[0100] The composite halogen-free flame retardant was vacuum dried at 90℃ for 4 hours. The silane mixture had a pH of 4.0, a pre-hydrolysis temperature of 20℃, and a pre-hydrolysis time of 60 minutes. The first surface modification temperature was 50℃, and the reaction time was 3 hours. The second surface modification temperature was 70℃, and the reaction time was 90 minutes. After drying and sieving, a double-layer modified halogen-free flame retardant A2 was obtained.
[0101] The polyolefin composite matrix consists of 62.5 parts by weight of high-density polyethylene, 25 parts by weight of linear low-density polyethylene, and 12.5 parts by weight of ethylene-octene copolymer elastomer, totaling 100 parts by weight. The weight ratio of high-density polyethylene, linear low-density polyethylene, and ethylene-octene copolymer elastomer is 5:2:1.
[0102] The polyolefin composite matrix is divided into a first matrix and a second matrix, wherein the first matrix is 60 parts by weight and the second matrix is 40 parts by weight.
[0103] Based on 100 parts by weight of polyolefin composite matrix, the amount of vinyltriethoxysilane added is 1.5 parts by weight, and the amount of composite peroxidation initiator added is 0.12 parts by weight. The composite peroxidation initiator is composed of dicumyl peroxide and 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane in a mass ratio of 1:0.5.
[0104] The melt grafting temperature of the silane grafting masterbatch is 150℃.
[0105] Based on 100 parts by weight of polyolefin composite matrix, the amount of double-layer modified halogen-free flame retardant A2 is 80 parts by weight, the amount of corrosion and weather resistance additive is 2.0 parts by weight, the amount of compatibility processing aid is 2.0 parts by weight, and the amount of anti-mildew and anti-adhesion additive is 0.8 parts by weight. The composition of the corrosion and weather resistance additive and the compatibility processing aid is the same as that in Example 1, and each component is calculated according to the mass ratio of each component in the corresponding additive in Example 1. The anti-mildew and anti-adhesion additive is composed of 0.6 parts by weight of quaternary ammonium salt modified nano silica and 0.2 parts by weight of N-vanillylnonamide.
[0106] The plasticizing temperature of the second matrix is 110℃, and the plasticizing time is 5 min; the first mixing temperature is 110℃, and the mixing time is 15 min.
[0107] After the first mixing, silane grafted masterbatch is added for a second mixing. The temperature of the second mixing is 100℃ and the mixing time is 8 minutes.
[0108] The extrusion temperature of the main component was 140°C, the drying temperature of the main component granules was 60°C, and the drying time was 6 hours, thus obtaining the main component of Example 2.
[0109] In addition, 2.0 parts by weight of high-density polyethylene was used as the polyolefin carrier resin, and 0.05 parts by weight of diisopropoxybis(acetylacetone)titanium was mixed with the polyolefin carrier resin. After extrusion granulation, drying and sealing packaging, the crosslinking catalytic component of Example 2 was obtained.
[0110] Apart from the differences mentioned above, the types of raw materials, feeding order, dispersion method, stirring conditions, drying and sieving method, mixing method and packaging method are all the same as in Example 1, resulting in the marine floating photovoltaic two-component halogen-free flame-retardant cable material of Example 2.
[0111] Example 3: Example 3 is based on Example 1, but the borate flame retardant synergist is replaced by magnesium borate instead of zinc borate; the magnesium-containing inorganic flame retardant remains magnesium hydroxide, and the aluminum-containing inorganic flame retardant remains aluminum hydroxide. The composite halogen-free flame retardant is composed of magnesium hydroxide, aluminum hydroxide, and magnesium borate in a weight ratio of 75:20:5.
[0112] Based on the dry basis of 100 parts by weight of the composite halogen-free flame retardant, the vinylalkoxysilane in the vinylalkoxysilane hydrolysate is composed of vinyltriethoxysilane and vinyltrimethoxysilane in a mass ratio of 1:1, with a total amount of 2.0 parts by weight, and the amount of stearic acid is 1.5 parts by weight.
[0113] The composite halogen-free flame retardant was vacuum dried at 100℃ for 3 hours. The silane mixture had a pH of 5.0, a pre-hydrolysis temperature of 40℃, and a pre-hydrolysis time of 20 minutes. The first surface modification temperature was 80℃, and the reaction time was 1 hour. The second surface modification temperature was 90℃, and the reaction time was 30 minutes. After drying and sieving, a double-layer modified halogen-free flame retardant A3 was obtained.
[0114] A polyolefin composite matrix consisting of 60 parts by weight of high-density polyethylene, 26.7 parts by weight of linear low-density polyethylene, and 13.3 parts by weight of ethylene-octene copolymer elastomer is used. The weight ratio of high-density polyethylene, linear low-density polyethylene, and ethylene-octene copolymer elastomer is approximately 4.5:2:1.
[0115] The polyolefin composite matrix is divided into a first matrix and a second matrix, wherein the first matrix is 40 parts by weight and the second matrix is 60 parts by weight.
[0116] Based on 100 parts by weight of polyolefin composite matrix, the amount of vinyltrimethoxysilane added is 3.0 parts by weight, and the amount of composite peroxidation initiator added is 0.40 parts by weight. The composite peroxidation initiator is composed of dicumyl peroxide and 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane in a mass ratio of 1:2.
[0117] The melting grafting temperature of the silane grafting masterbatch is 190℃.
[0118] Based on 100 parts by weight of polyolefin composite matrix, the amount of double-layer modified halogen-free flame retardant A3 is 120 parts by weight, the amount of corrosion and weather resistance additive is 5.0 parts by weight, the amount of compatibility processing aid is 6.0 parts by weight, and the amount of mildew and anti-adhesion additive is 2.5 parts by weight. The composition of the corrosion and weather resistance additive and the compatibility processing aid is the same as that in Example 1, and each component is calculated according to the mass ratio of each component in the corresponding additive in Example 1. The mildew and anti-adhesion additive is composed of 1.8 parts by weight of quaternary ammonium salt modified nano silica and 0.7 parts by weight of N-vanillylnonamide.
[0119] The plasticizing temperature of the second matrix is 150℃, the plasticizing time is 2min, the first mixing temperature is 150℃, and the mixing time is 5min.
[0120] After the first mixing, silane grafted masterbatch is added for a second mixing. The temperature of the second mixing is 140℃ and the mixing time is 2 minutes.
[0121] The extrusion temperature of the main component was 180°C, the drying temperature of the main component granules was 80°C, and the drying time was 2 hours, thus obtaining the main component of Example 3.
[0122] Another 10.0 parts by weight of ethylene-octene copolymer elastomer were used as the polyolefin carrier resin. 0.25 parts by weight of zirconium lactate were mixed with the polyolefin carrier resin. After extrusion granulation, drying and sealing packaging, the crosslinking catalytic component of Example 3 was obtained.
[0123] Apart from the differences mentioned above, the types of raw materials, feeding order, dispersion method, stirring conditions, drying and sieving method, mixing method and packaging method are all the same as in Example 1, resulting in the marine floating photovoltaic two-component halogen-free flame-retardant cable material of Example 3.
[0124] Application Example 1: The main material components and crosslinking catalyst components obtained in Example 1 are mixed before cable extrusion, or separately metered and added to the cable extrusion equipment and mixed during the cable extrusion process. The mixed material is melt-plasticized and then extruded onto the outside of the conductor, insulated core, or cable core to form an insulation layer or sheath layer. Subsequently, the extruded insulation layer or sheath layer undergoes a constant temperature and humidity crosslinking treatment at a temperature of 85°C, a relative humidity of 90%, and a treatment time of 6 hours to obtain a marine floating photovoltaic cable.
[0125] Through the above treatment, the hydrolyzable silane groups in the cable material can undergo hydrolysis and condensation reactions under the action of crosslinking catalysts to form a crosslinked network structure, thereby improving the performance retention of the insulation layer or sheath layer under seawater immersion, salt spray corrosion, ultraviolet humid heat and dynamic bending environments; at the same time, the anti-mold and anti-adhesion additives can reduce the risk of mold growth and initial adhesion of marine microorganisms, algae or biofilms on the surface of the insulation layer or sheath layer in high humidity and high salt environments.
[0126] Comparative Example 1: Comparative Example 1 is based on Example 1, but the first and second surface modification steps of the composite halogen-free flame retardant are omitted.
[0127] Specifically, magnesium hydroxide, aluminum hydroxide, and zinc borate were mixed in a weight ratio of 65:30:5 and vacuum dried at 95°C for 3.5 hours to obtain the dried composite halogen-free flame retardant B1.
[0128] 100 parts by weight of B1 were used instead of 100 parts by weight of the bilayer modified halogen-free flame retardant A1 in Example 1.
[0129] Except for the differences mentioned above, the composition of the polyolefin compound matrix, the silane grafting system, the composition of the functional additives, the preparation conditions of the main components, the composition and preparation conditions of the crosslinking catalyst components are all the same as in Example 1, resulting in the cable material of Comparative Example 1.
[0130] Comparative Example 2: Comparative Example 2, based on Example 1, only retains the first surface modification step of the composite halogen-free flame retardant, and omits the step of using fatty acid treatment liquid for the second surface modification.
[0131] Specifically, after preparing the first surface-modified slurry according to the method of Example 1, fatty acid treatment liquid is no longer added. Instead, the first surface-modified slurry is directly subjected to solid-liquid separation, washing, vacuum drying and sieving to obtain monolayer silane-modified halogen-free flame retardant B2.
[0132] 100 parts by weight of B2 were used instead of 100 parts by weight of the bilayer modified halogen-free flame retardant A1 in Example 1.
[0133] Except for the differences mentioned above, the composition of the polyolefin compound matrix, the silane grafting system, the composition of the functional additives, the preparation conditions of the main components, the composition and preparation conditions of the crosslinking catalyst components are all the same as those in Example 1, resulting in the cable material of Comparative Example 2.
[0134] Comparative Example 3: Comparative Example 3, based on Example 1, eliminates the stepwise processing of the first and second substrates and the pre-processing step of the silane grafting masterbatch.
[0135] Specifically, 100 parts by weight of polyolefin composite matrix are composed of 57.1 parts by weight of high-density polyethylene, 28.6 parts by weight of linear low-density polyethylene and 14.3 parts by weight of ethylene-octene copolymer elastomer.
[0136] Based on 100 parts by weight of polyolefin compound matrix, the polyolefin compound matrix, 2.2 parts by weight of vinyltrimethoxysilane, 0.25 parts by weight of composite peroxide initiator, 100 parts by weight of double-layer modified halogen-free flame retardant A1, 3.5 parts by weight of corrosion and weather resistance additive, 3.0 parts by weight of compatibility processing aid and 1.5 parts by weight of mildew and anti-adhesion additive are added into a mixing equipment at one time, and the mixture is mixed at 130°C for 10 minutes, and then mixed at 120°C for another 5 minutes to obtain the mixture.
[0137] The resulting mixture was processed under the same conditions as the main ingredient components of Example 1, including extrusion granulation, drying, and sealing packaging, to obtain the main ingredient components of Comparative Example 3.
[0138] The crosslinking catalytic components and preparation conditions of Comparative Example 3 were the same as those of Example 1.
[0139] Apart from the differences mentioned above, the types and amounts of other raw materials and post-processing conditions were the same as in Example 1, resulting in the cable material of Comparative Example 3.
[0140] Comparative Example 4: Comparative Example 4, based on Example 1, eliminates the separate preparation and packaging of the main component and the crosslinking catalyst component, and directly adds the crosslinking catalyst to the main component system.
[0141] Specifically, after the first mixing, the silane graft masterbatch and 0.12 parts by weight of tetrazirconium tetraacetylacetonate are added to the flame-retardant, weather-resistant and anti-adhesion mixture, and the mixture is mixed for a second time at 120°C for 5 minutes to obtain a hydrolyzable crosslinkable mixture containing a crosslinking catalyst.
[0142] The hydrolyzable crosslinkable mixture containing the crosslinking catalyst was processed according to the extrusion granulation, drying, and sealing packaging conditions of Example 1 to obtain the single-component cable material of Comparative Example 4.
[0143] Except that the crosslinking catalyst was not separately prepared as a crosslinking catalyst component and packaged separately, the other raw material composition, dosage, mixing conditions, extrusion granulation conditions and drying and packaging conditions were the same as in Example 1.
[0144] Comparative Example 5: Comparative Example 5 is based on Example 1, but the anti-mildew and anti-adhesion additives are omitted.
[0145] Specifically, in the first mixing step, 1.5 parts by weight of anti-mildew and anti-adhesion additive was not added. Except for the above differences, the surface modification method of the composite halogen-free flame retardant, the composition of the polyolefin composite matrix, the silane grafting system, the preparation conditions of the main component, and the composition and preparation conditions of the crosslinking catalyst were all the same as in Example 1, resulting in the cable material of Comparative Example 5.
[0146] Comparative Example 6: Comparative Example 6 is a conventional terrestrial photovoltaic silane cross-linked halogen-free cable material.
[0147] The matrix consists of 70 parts by weight of low-density polyethylene and 30 parts by weight of ethylene-octene copolymer elastomer, comprising 100 parts by weight of ordinary polyolefin matrix.
[0148] Based on 100 parts by weight of a common polyolefin matrix, 90 parts by weight of an unmodified magnesium hydroxide and aluminum hydroxide composite flame retardant, 2.0 parts by weight of vinyltrimethoxysilane, 0.25 parts by weight of dicumyl peroxide, 0.15 parts by weight of dibutyltin dilaurate, and 1.5 parts by weight of a conventional weathering agent were added. The conventional weathering agent was a mixture of pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] and bis(2,2,6,6-tetramethyl-4-piperidinyl) sebacate, with a mass ratio of 1:1.
[0149] The above raw materials were added to a mixing equipment and mixed in one go. Then, they were extruded and granulated to obtain the conventional terrestrial photovoltaic silane crosslinked halogen-free cable material of Comparative Example 6. In the subsequent test sample preparation, Comparative Example 6 was subjected to hydrolysis crosslinking under the same crosslinking treatment conditions as the Example.
[0150] Unless otherwise stated, before preparing test samples, the main component and crosslinking catalyst component of the marine floating photovoltaic two-component halogen-free flame-retardant cable material obtained in the examples are mixed according to the dosage relationship in the corresponding examples, or separately metered and added to the molding equipment and mixed during the melt plasticizing process; the samples obtained in the comparative examples are prepared according to the component form and processing method corresponding to each comparative example.
[0151] Unless otherwise stated, the test samples obtained in the examples and comparative examples were conditioned for 24 hours at a temperature of 23℃±2℃ and a relative humidity of 50%±5% before testing. Except for the rating evaluation items and the condition observation items, all numerical performance tests were conducted in parallel using samples from the same batch, and the arithmetic mean of the valid test results was taken.
[0152] The tensile properties of the cable material were tested according to GB / T 1040.3-2006: Specifically, the cable materials obtained in the examples and comparative examples were respectively made into thin sheets with a thickness of 0.5 mm using a flat plate pressing device. Then, the thin sheets were placed in a constant temperature and humidity environment of 85°C and 90% relative humidity for 6 hours to allow the test pieces to undergo hydrolytic cross-linking.
[0153] After crosslinking treatment, the specimens were conditioned for 24 hours at a temperature of 23℃±2℃ and a relative humidity of 50%±5%, and then tensile specimens were prepared. The tensile speed was 200 mm / min, and each test group had no less than 5 valid parallel specimens. The tensile strength and elongation at break were measured and the arithmetic mean was taken.
[0154] The oxygen index was tested according to GB / T 2406.2-2009: Specifically, the cable materials obtained in the examples and comparative examples were pressed into samples that met the requirements of the standard, and the samples were placed in a constant temperature and humidity environment of 85°C and 90% relative humidity for 6 hours to induce hydrolytic crosslinking. Each group of samples was tested in triplicate, and the arithmetic mean of the oxygen index test results was taken. The test results are expressed as the oxygen index (LOI) in percentage form.
[0155] Vertical burning performance was tested according to GB / T 2408-2021: Specifically, the cable materials obtained in the examples and comparative examples were pressed into test pieces with dimensions of 125mm × 13mm × 0.5mm, and the test pieces were placed in a constant temperature and humidity environment of 85℃ and 90% relative humidity for 6 hours to allow the test pieces to undergo hydrolytic cross-linking. Five samples were tested in each group.
[0156] During the test, the afterflame time, afterglow time, total afterflame time, whether burning drips occurred and whether the drips ignited the indicator cotton were recorded after the first and second flame application of each sample. The vertical burning level was evaluated based on the test results, and the test results were recorded as V-0, V-1, V-2 or not reaching the corresponding level.
[0157] Gel content was tested using solvent extraction. Specifically, the sample after hydrolysis and cross-linking treatment was weighed and its initial mass m0 was recorded; the sample was placed in xylene for heating and extraction to fully dissolve the uncross-linked portion; after extraction, the residual sample was taken out, dried to constant weight, and its mass m1 was recorded. Each group of samples was tested in parallel three times, and the arithmetic mean was taken.
[0158] The gel content is calculated using the following formula: Gel content / % = m1 ÷ m0 × 100%.
[0159] Where m0 is the mass of the sample before extraction, and m1 is the mass of the residual sample after extraction and drying.
[0160] The results are used to characterize the insoluble content of cable materials after hydrolysis and crosslinking treatment, and serve as an auxiliary evaluation index for the formation of crosslinked networks.
[0161] Smoke density was tested according to the method specified in GB / T 8323.2: Specifically, the cable materials obtained in the examples and comparative examples were prepared into samples that met the testing requirements, and after hydrolysis crosslinking treatment, combustion smoke density tests were conducted. During the test, the maximum smoke density D corresponding to the smoke generated during the combustion of the sample was recorded. s Each sample group was tested in triplicate, and the arithmetic mean was taken.
[0162] The seawater absorption rate was tested using an artificial seawater immersion method. The artificial seawater is artificial seawater with a salinity of 3.5%, and its main salts include sodium chloride, magnesium chloride, sodium sulfate, calcium chloride, and potassium chloride.
[0163] Specifically, the cable materials obtained in the examples and comparative examples were made into cross-linked test pieces, and the sample mass m2 before immersion was recorded. The samples were then completely immersed in artificial seawater and soaked at room temperature for 1000 hours. After immersion, the samples were removed, surface moisture was wiped off with filter paper, and the mass m3 after immersion was measured within 5 minutes. Each group of samples was tested in triplicate, and the arithmetic mean was taken.
[0164] The water absorption rate after 1000 hours of seawater immersion is calculated using the following formula: Water absorption rate / % = (m 3- m2)÷m2×100%.
[0165] Where m2 is the mass of the sample before immersion, and m3 is the mass of the sample after immersion in seawater for 1000 hours.
[0166] The volume resistivity retention rate after seawater immersion was tested using the following method: Specifically, the cable materials obtained in the examples and comparative examples were made into cross-linked test pieces, and the volume resistivity ρ0 before seawater immersion was tested according to the method specified in GB / T 1410. The samples were then completely immersed in artificial seawater for 1000 hours at room temperature. After immersion, the samples were removed, surface moisture was wiped off, and the volume resistivity ρ1 after seawater immersion was tested under the same test conditions. Each group of samples was tested in triplicate, and the arithmetic mean was taken.
[0167] The volume resistivity retention rate after immersion in seawater for 1000 hours is calculated using the following formula: Volume resistivity retention rate / % = ρ1 ÷ ρ0 × 100%.
[0168] Wherein, ρ0 is the volume resistivity before seawater immersion, and ρ1 is the volume resistivity after seawater immersion for 1000 hours.
[0169] Neutral salt spray aging was tested according to the method specified in GB / T 10125: Specifically, the cable materials obtained in the examples and comparative examples were made into cross-linked test pieces and placed in a neutral salt spray test chamber for 1000 hours. After salt spray aging, the samples were removed, rinsed with deionized water to remove residual salt, dried, and then conditioned in an environment with a temperature of 23℃±2℃ and a relative humidity of 50%±5% for 24 hours. The tensile strength after aging was then tested according to GB / T 1040.3-2006. Each group of samples had no less than 5 valid parallel samples, and the arithmetic mean was taken.
[0170] The tensile strength retention rate after 1000 hours of neutral salt spray is calculated using the following formula: Tensile strength retention rate / % = T1 ÷ T0 × 100%.
[0171] Where T0 is the tensile strength before salt spray aging, and T1 is the tensile strength after 1000 hours of neutral salt spray.
[0172] UV-heat coupled aging is carried out using alternating UV irradiation and heat cycling: Specifically, each cycle includes an ultraviolet (UV) irradiation stage and a damp heat stage. The UV irradiation stage uses a 340nm UV light source and is performed at 60°C for 8 hours. The damp heat stage is performed at 50°C and 95% relative humidity for 4 hours, with a total cycle time of 5000 hours.
[0173] The cable materials obtained in the examples and comparative examples were made into cross-linked test pieces and placed in an ultraviolet-humid heat coupled aging device under the conditions described above. After aging, the samples were removed and conditioned for 24 hours in an environment with a temperature of 23℃±2℃ and a relative humidity of 50%±5%. Then, the elongation at break after aging was tested according to GB / T 1040.3-2006. Each group of samples had no less than 5 valid parallel samples, and the arithmetic mean was taken.
[0174] The elongation at break retention rate after 5000 hours of UV-humid heat coupled aging is calculated using the following formula: Elongation at break retention rate / % = E1 ÷ E0 × 100%.
[0175] Where E0 is the elongation at break before UV-induced humid heat coupling aging, and E1 is the elongation at break after 5000 hours of UV-induced humid heat coupling aging.
[0176] Dynamic bending performance was evaluated using repeated bending tests. Specifically, the cable materials obtained in the examples and comparative examples were extruded and coated onto the outside of the conductor, insulated core, or cable core to form an insulation layer or sheath layer. After being treated at a constant temperature and humidity of 85°C and 90% relative humidity for 6 hours, test samples were obtained. The test samples were fixed in a dynamic bending test device and repeatedly bent under the conditions of a bending angle of ±90°, a bending frequency of 30 times / min, and a bending radius of 6 times the outer diameter of the sample, for a total of 100,000 bending cycles.
[0177] After the test, observe whether cracks, splits, powdering, peeling or sheath damage appear on the sample surface, and record the test results as "no cracks, no peeling", "micro-cracks appear", "slight cracking", "local cracking" or "local cracking, sheath peeling".
[0178] Storage stability and extrusion processing suitability were evaluated using the following methods: Specifically, the cable materials obtained in the examples and comparative examples were sealed and packaged according to their respective packaging methods, and then placed in an environment with a temperature of 40°C and a relative humidity of 75% for 30 days. After storage, the main components and crosslinking catalyst components of the example samples were mixed according to their respective application ratios, and samples of the comparative examples samples were taken according to their corresponding component forms, and then added to extrusion equipment for melt extrusion.
[0179] During extrusion, observe whether the material can be extruded continuously and stably, and record whether the surface of the extrudate shows roughness, charred particles, gel particles, broken strips, or obvious uneven melting. After storage, the gel content of the sample is determined by solvent extraction.
[0180] The samples used for the post-storage gel content test were samples that had been stored and had not undergone further hydrolytic crosslinking treatment. The lower the post-storage gel content and the smoother the extrudate surface, the better the storage stability and extrusion processing adaptability of the cable material.
[0181] The anti-mildew performance was tested according to the method specified in GB / T 24128-2018: Specifically, the cable materials obtained in the examples and comparative examples were made into cross-linked test pieces. The test pieces were placed in petri dishes, and the surface of the test pieces was covered with agar medium containing mold spores. They were then cultured for 28 days in an environment with a temperature of 28℃±2℃ and a relative humidity of not less than 90%. After the culture period, the growth of mold on the sample surface was observed, and the mold resistance level was evaluated according to the 0-4 level evaluation rules specified in GB / T 24128-2018. The lower the mold resistance level, the less mold growth on the sample surface and the better the mold resistance performance. The higher the mold resistance level, the more obvious the mold growth on the sample surface and the worse the mold resistance performance.
[0182] The resistance to initial attachment of marine organisms was evaluated using an artificial seawater biofilm attachment test. Specifically, the cable materials obtained in the examples and comparative examples were made into cross-linked test pieces and immersed in artificial seawater containing a marine microbial nutrient system, and cultured at 25℃±2℃ for 14 days. After the culture was completed, the samples were removed, the surface of any loosely attached material was gently rinsed off, and after drying, the surface of the samples was photographed, and the biofilm coverage area was counted using image analysis methods.
[0183] Biofilm coverage is calculated using the following formula: Biofilm coverage rate / % = Biofilm coverage area ÷ Sample test area × 100%.
[0184] The lower the biofilm coverage, the better the inhibition effect of the sample surface on the initial attachment of marine microorganisms.
[0185] In all the above tests, the sample preparation conditions, crosslinking treatment conditions, aging treatment conditions, and performance testing conditions used in the examples and comparative examples were kept consistent. For items requiring comparison of retention rates, samples before and after aging were prepared using the same batch of materials and tested according to the same method to ensure the comparability of test results between the examples and comparative examples.
[0186] The experimental data are shown in Tables 1, 2 and 3.
[0187] Table 1: Table 2: Table 3: As shown in Tables 1, 2, and 3, the marine floating photovoltaic bicomponent halogen-free flame-retardant cable materials obtained in Examples 1-3 all possess excellent comprehensive performance. Specifically, Example 1 exhibits a tensile strength of 18.6 MPa, an elongation at break of 305%, an oxygen index of 34.5%, a vertical flammability rating of V-0, a gel content of 87.8%, a water absorption rate of only 0.35% after 1000 hours of seawater immersion, and a volume resistivity retention rate of 91.2%. This demonstrates that the cable material of this application possesses good mechanical properties, flame-retardant properties, cross-linking stability, seawater resistance, and electrical insulation performance retention.
[0188] Meanwhile, as shown in Table 1, the maximum smoke density D in Examples 1-3 is... s The values were 118, 126, and 110, respectively, all lower than those of Comparative Examples 1–4, and significantly lower than the 238 of Comparative Example 6. These results indicate that using a double-layer modified halogen-free flame retardant combined with functional additives can improve the dispersion of the inorganic flame retardant in the polyolefin composite matrix, reduce smoke release caused by interface defects and localized uneven combustion during combustion, thereby lowering the maximum smoke density during material combustion and resulting in cable materials with better low-smoke performance.
[0189] In Example 2, the dosage of the double-layer modified halogen-free flame retardant and functional additives was relatively low, yet the tensile strength and elongation at break were high, indicating that the material still possessed good mechanical properties under low filler conditions. In Example 3, the dosage of the double-layer modified halogen-free flame retardant was higher, resulting in an oxygen index of 36.2%, further improving the flame retardant performance. However, the elongation at break was slightly lower than in Examples 1 and 2, suggesting that increasing the amount of flame retardant is beneficial for improving flame retardant performance but may have some impact on the material's flexibility.
[0190] Compared to Example 1, Comparative Example 1, which did not undergo double-layer surface modification of the composite halogen-free flame retardant, showed a decrease in tensile strength from 18.6 MPa to 13.2 MPa, a decrease in elongation at break from 305% to 205%, an increase in water absorption rate after 1000 hours of seawater immersion from 0.35% to 1.62%, and a decrease in volume resistivity retention rate after 1000 hours of seawater immersion from 91.2% to 64.8%. This indicates that without double-layer surface modification, the composite halogen-free flame retardant exhibits poor interfacial compatibility with the polyolefin matrix, easily leading to interfacial defects and water absorption channels, thereby resulting in a decrease in the retention rate of the material's mechanical properties, water resistance, and electrical insulation properties.
[0191] Compared to Example 1, Comparative Example 2 only underwent a first surface modification with vinylalkoxysilane and did not undergo a second surface modification with fatty acids. Its water absorption rate after 1000 hours of seawater immersion was 0.86%, and its volume resistivity retention rate after 1000 hours of seawater immersion was 78.6%, both significantly weaker than Example 1. This indicates that the second surface modification layer formed by the fatty acid treatment solution can further reduce the surface polarity of the composite halogen-free flame retardant and improve its dispersibility and water resistance in the polyolefin composite matrix.
[0192] Compared to Example 1, Comparative Example 3 did not employ a stepwise treatment method involving the first and second matrices, nor did it pre-prepare a silane grafting masterbatch. Its gel content was only 72.8%, and it exhibited localized cracking after 100,000 dynamic bends. This result indicates that dividing the polyolefin composite matrix into a first and second matrix, and pre-preparing a silane grafting masterbatch, helps reduce the mutual interference between the silane grafting reaction and the dispersion process of the highly filled flame retardant, thereby improving crosslinking uniformity and bending durability.
[0193] As shown in Table 3, after 30 days of storage at 40°C and 75% relative humidity, the gel contents of Examples 1-3 were 4.8%, 4.2%, and 5.5%, respectively. They were still able to be continuously and stably extruded after storage, and the extrudate surface was smooth. In contrast, Comparative Example 4 eliminated the separate preparation and packaging of the main component and the crosslinking catalyst, directly adding the crosslinking catalyst to the main component system. After 30 days of storage, the gel content increased to 38.5%, and uneven melting, gel particles, and broken strips appeared during extrusion. These results indicate that the separate preparation and sealed packaging of the main component and the crosslinking catalyst in this application can prevent premature hydrolysis and crosslinking of the main component during storage due to the early presence of the crosslinking catalyst, thereby improving the storage stability and extrusion processing adaptability of the cable material.
[0194] Table 3 also shows that the anti-mold rating of Examples 1-3 is all 0, with biofilm coverage rates of 6.8%, 9.5%, and 5.2%, respectively, significantly lower than 38.2% for Comparative Example 5 and 45.6% for Comparative Example 6. Comparative Example 5 did not contain any anti-mold and anti-adhesion additives. Although its mechanical properties, flame retardant properties, water resistance, and extrusion state after storage were similar to Example 1, its anti-mold rating decreased to 2, and its biofilm coverage rate significantly increased. These results indicate that anti-mold and anti-adhesion additives can effectively inhibit the growth of mold on the surface of cable materials under high humidity and high salinity environments and reduce the initial adhesion of marine microorganisms or biofilms to the cable material surface.
[0195] Comparative Example 6 is a conventional terrestrial photovoltaic silane cross-linked halogen-free cable material. Its water absorption rate after 1000 hours of seawater immersion reached 1.85%, and its volume resistivity retention rate after 1000 hours of seawater immersion was only 60.3%. Its tensile strength retention rate after 1000 hours of neutral salt spray was 65.0%, and it showed localized cracking and sheath detachment after 100,000 dynamic bending cycles. Furthermore, after 30 days of storage, its gel content reached 42.0%, its mildew resistance level was 3, and its biofilm coverage rate was 45.6%. Compared to Comparative Example 6, Example 1 showed significant improvements in seawater resistance, salt spray resistance, UV damp heat resistance, dynamic bending, storage stability, mildew resistance, and resistance to initial marine organism adhesion, indicating that the cable material obtained in this application is more suitable for the long-term service environment of floating photovoltaic cables at sea.
[0196] In summary, as shown in Comparative Examples 1-5, the double-layer surface modification of the composite halogen-free flame retardant, the stepwise preparation of the silane grafted masterbatch, the separate preparation and packaging of the main component and the crosslinking catalytic component, and the introduction of anti-mildew and anti-adhesion additives all contribute to the comprehensive performance of the material. Comparative Example 6 shows that the cable material of this application is more suitable for the long-term service environment of floating photovoltaic systems at sea compared to conventional terrestrial photovoltaic silane crosslinked halogen-free cable materials. The two-component halogen-free flame-retardant cable material for floating photovoltaic systems obtained in this application achieves a good balance between flame retardant performance, low smoke performance, mechanical properties, water resistance, salt spray resistance, UV damp heat resistance, dynamic bending performance, storage stability, anti-mildew performance, and resistance to initial adhesion of marine organisms.
Claims
1. A method for preparing a two-component halogen-free flame-retardant cable material for marine floating photovoltaic applications, characterized in that, The cable material comprises a main component and a crosslinking catalytic component, and the preparation method includes the following steps: S1. The dried composite halogen-free flame retardant is subjected to first surface modification with vinylalkoxysilane hydrolysate and second surface modification with fatty acid treatment solution to obtain a double-layer modified halogen-free flame retardant. S2. The polyolefin composite matrix is divided into a first matrix and a second matrix. The first matrix is melt-grafted with a silane grafting system and extruded and granulated to obtain a silane grafting masterbatch. S3. Plasticize the second matrix to obtain a plasticized matrix. Then, perform a first intensive mixing of the plasticized matrix, the double-layer modified halogen-free flame retardant, and the functional additives to obtain a flame-retardant, weather-resistant, and anti-adhesion mixture. S4. Add the silane grafted masterbatch to the flame-retardant, weather-resistant and anti-adhesion mixture, and perform a second internal mixing to obtain the main material premix. Then, the main material premix is extruded, granulated, dried and sealed in packaging to obtain the main material component. S5. The crosslinking catalyst is mixed with the polyolefin support resin and extruded and granulated to obtain the crosslinking catalyst masterbatch, and the crosslinking catalyst masterbatch is sealed and packaged to obtain the crosslinking catalyst component.
2. The preparation method of a marine floating photovoltaic two-component halogen-free flame-retardant cable material according to claim 1, characterized in that, Step S1 includes the following sub-steps: S1.1 Mix magnesium-containing inorganic flame retardant, aluminum-containing inorganic flame retardant and borate flame retardant synergist, and dry in a vacuum oven at 90-100℃ for 3-4 hours to obtain the dried composite halogen-free flame retardant; S1.
2. Mix ethanol and deionized water in a mass ratio of 70:30 to 95:5 to obtain ethanol-water mixed solvent A; Vinylalkoxysilane was added to the ethanol-water mixed solvent A to obtain a silane mixture. The pH of the silane mixture was adjusted to 4.0-5.0 with acetic acid, and the mixture was stirred and pre-hydrolyzed at 20-40°C for 20-60 min to obtain a vinylalkoxysilane hydrolysate. S1.
3. Take another ethanol and deionized water and mix them in a mass ratio of 70:30 to 95:5 to obtain ethanol-water mixed solvent B; The dried composite halogen-free flame retardant was dispersed in the ethanol-water mixed solvent B, and the vinylalkoxysilane hydrolysate was added under stirring conditions of 500-1500 r / min. The reaction was continued at 50-80°C for 1-3 h to obtain the first surface-modified slurry. S1.4 Add stearic acid to anhydrous ethanol and stir to dissolve or disperse at 60-75°C to obtain fatty acid treatment solution; S1.
5. Add the fatty acid treatment solution to the first surface-modified slurry, heat to 70-90°C, and continue to react for 30-90 minutes under stirring conditions of 500-1500 r / min to obtain a wet double-layer modified halogen-free flame retardant. S1.
6. The wet double-layer modified halogen-free flame retardant is placed in a vacuum drying oven and dried for 3 to 8 hours at 80 to 110°C and a gauge pressure of -0.095 to -0.060 MPa. The dried flame retardant is then sieved through a 100 to 500 mesh screen to obtain the double-layer modified halogen-free flame retardant.
3. The preparation method of a marine floating photovoltaic two-component halogen-free flame-retardant cable material according to claim 2, characterized in that, In step S1.1, the magnesium-containing inorganic flame retardant is selected from at least one of magnesium hydroxide, basic magnesium carbonate, and magnesium carbonate; The aluminum-containing inorganic flame retardant is selected from at least one of aluminum hydroxide and boehmite; The borate flame retardant synergist is selected from at least one of zinc borate, calcium borate, and magnesium borate; The weight ratio of the magnesium-containing inorganic flame retardant, the aluminum-containing inorganic flame retardant, and the borate flame retardant synergist is 60–75: 20–35: 3–8.
4. The preparation method of a marine floating photovoltaic two-component halogen-free flame-retardant cable material according to claim 2, characterized in that, The vinylalkoxysilane is selected from at least one of vinyltriethoxysilane and vinyltrimethoxysilane, and the mass of the vinylalkoxysilane is 0.5% to 2.0% of the mass of the composite halogen-free flame retardant. The mass of the stearic acid is 0.3% to 1.5% of the mass of the composite halogen-free flame retardant.
5. The preparation method of a marine floating photovoltaic two-component halogen-free flame-retardant cable material according to claim 1, characterized in that, Step S2 includes the following sub-steps: S2.1 The polyolefin composite matrix is divided into a first matrix and a second matrix, wherein the first matrix accounts for 40% to 60% of the total mass of the polyolefin composite matrix, and the second matrix is the remaining part of the polyolefin composite matrix excluding the first matrix; S2.
2. Mix the first matrix with the silane grafting system to obtain a grafted premix; S2.
3. The grafted premix is added to an extruder and melt-grafted at 150-190°C. After extrusion, cooling and pelletizing, silane grafted masterbatch is obtained.
6. The method for preparing a marine floating photovoltaic two-component halogen-free flame-retardant cable material according to claim 5, characterized in that, The polyolefin composite matrix includes high-density polyethylene, linear low-density polyethylene and ethylene-octene copolymer elastomer, and the weight ratio of high-density polyethylene, linear low-density polyethylene and ethylene-octene copolymer elastomer is 4-5:2:1; The silane grafting system includes silane grafting monomers and initiators; The silane graft monomer is selected from at least one of vinyltrimethoxysilane and vinyltriethoxysilane; The initiator is a composite peroxidation initiator, which includes dicumyl peroxide and 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane, wherein the mass ratio of dicumyl peroxide to 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane is 1:0.5-2. Based on 100 parts by weight of the polyolefin composite matrix, the amount of silane grafted monomer is 1.5 to 3.0 parts, and the amount of initiator is 0.12 to 0.40 parts.
7. The method for preparing a marine floating photovoltaic two-component halogen-free flame-retardant cable material according to claim 1, characterized in that, Step S3 includes the following sub-steps: S3.1 Add the second matrix to a mixing apparatus and plasticize it at 110-150°C for 2-5 minutes to obtain a plasticized matrix; S3.2 Add the double-layer modified halogen-free flame retardant and functional additives to the plasticized matrix, and perform a first internal mixing at 110-150°C for 5-15 minutes to obtain a flame-retardant, weather-resistant, and anti-adhesion mixture; The functional additives include corrosion and weather resistance additives, compatible processing aids, and anti-mildew and anti-adhesion additives; Based on 100 parts by weight of the polyolefin composite matrix, the amount of the double-layer modified halogen-free flame retardant is 80-120 parts, the amount of the corrosion and weather resistance additive is 2.0-5.0 parts, the amount of the compatibility processing aid is 2.0-6.0 parts, and the amount of the mildew and anti-adhesion additive is 0.5-3.0 parts. The corrosion-resistant and weather-resistant additive is selected from at least one of pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], tris(2,4-di-tert-butylphenyl) phosphite, bis(2,2,6,6-tetramethyl-4-piperidinyl) sebacate, and nano zinc oxide; The compatible processing aid is selected from at least one of maleic anhydride-grafted polyethylene, oxidized polyethylene wax, and polydimethylsiloxane. The anti-mildew and anti-adhesion additive includes at least one of quaternary ammonium salt modified nano silica, N-vanillylnonamide and nano copper oxide, wherein the quaternary ammonium salt modified nano silica is nano silica that has been surface modified with 3-(trimethoxysilyl)propyldimethyloctadecylammonium chloride.
8. The method for preparing a marine floating photovoltaic two-component halogen-free flame-retardant cable material according to claim 1, characterized in that, Step S4 includes the following sub-steps: S4.1 After the first internal mixing is completed, the silane grafting masterbatch is added to the flame-retardant, weather-resistant and anti-adhesion mixture, and the mixture is subjected to a second internal mixing at 100-140°C for 2-8 minutes to obtain the main material premix. S4.2 Add the main premix to an extruder, extrude at 140-180°C, and then cool and pelletize to obtain the main component granules; S4.
3. The main material component granules are dried at 60-80°C for 2-6 hours and then sealed in aluminum-plastic composite bags to obtain the main material component.
9. The method for preparing a marine floating photovoltaic two-component halogen-free flame-retardant cable material according to claim 1, characterized in that, Step S5 includes the following sub-steps: S5.
1. The crosslinking catalyst is mixed with a polyolefin support resin and extruded and granulated to obtain a crosslinking catalyst masterbatch, and the crosslinking catalyst masterbatch is sealed and packaged to obtain the crosslinking catalyst component; The polyolefin carrier resin is selected from at least one of high-density polyethylene, linear low-density polyethylene, and ethylene-octene copolymer elastomer; The crosslinking catalyst is selected from at least one of tetrazirconium tetra(acetylacetone), diisopropoxybis(acetylacetone) titanium, and zirconium lactate ammonium; Based on 100 parts by weight of the polyolefin composite matrix in the main component, the amount of the polyolefin carrier resin is 2.0 to 10.0 parts, and the amount of the crosslinking catalyst is 0.05 to 0.25 parts.
10. A type of marine floating photovoltaic two-component halogen-free flame-retardant cable material, characterized in that, It includes a main component and a crosslinking catalyst component. The main component is prepared from the following raw materials in parts by weight: 100 parts of polyolefin composite matrix, 80-120 parts of bilayer modified halogen-free flame retardant, 1.5-3.0 parts of silane grafted monomer, 0.12-0.40 parts of initiator, 2.0-5.0 parts of corrosion and weather resistance additive, 2.0-6.0 parts of compatibility processing aid, and 0.5-3.0 parts of mildew and anti-adhesion additive; The crosslinking catalytic component includes a crosslinking catalyst and a polyolefin support resin. Based on 100 parts by weight of the polyolefin composite matrix in the main component, the amount of the polyolefin support resin is 2.0 to 10.0 parts, and the amount of the crosslinking catalyst is 0.05 to 0.25 parts. The polyolefin composite matrix includes high-density polyethylene, linear low-density polyethylene and ethylene-octene copolymer elastomer, and the weight ratio of high-density polyethylene, linear low-density polyethylene and ethylene-octene copolymer elastomer is 4-5:2:1; The polyolefin carrier resin is selected from at least one of high-density polyethylene, linear low-density polyethylene, and ethylene-octene copolymer elastomer; The double-layer modified halogen-free flame retardant is a flame retardant obtained by sequentially modifying a composite halogen-free flame retardant with a vinylalkoxysilane hydrolysate and a fatty acid treatment solution. The crosslinking catalyst is selected from at least one of tetrazirconium tetra(acetylacetone), diisopropoxybis(acetylacetone) titanium, and zirconium lactate ammonium; The corrosion-resistant and weather-resistant additive is selected from at least one of pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], tris(2,4-di-tert-butylphenyl) phosphite, bis(2,2,6,6-tetramethyl-4-piperidinyl) sebacate, and nano zinc oxide; The compatible processing aid is selected from at least one of maleic anhydride-grafted polyethylene, oxidized polyethylene wax, and polydimethylsiloxane. The anti-mildew and anti-adhesion additive includes at least one of quaternary ammonium salt modified nano silica, N-vanillyl nonylamide, and nano copper oxide.