A bamboo-plastic master batch based on a bamboo powder modified material, a preparation method and application thereof
By employing a three-step gradient surface polarity control technology involving glycerol pre-wetting, polyethylene wax/zinc stearate coating, and EVA interface bridging, combined with a multi-stage venting and moisture-proof closed-loop control process, the problems of poor interfacial compatibility between bamboo powder and plastic matrices such as polyethylene, as well as performance degradation under high bamboo powder filling amounts, have been solved, enabling the efficient preparation and widespread application of bamboo-plastic masterbatch.
Patent Information
- Application Number
- CN202611347396.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-02
- Publication Date
- 2026-11-24
AI Technical Summary
In existing technologies, bamboo powder has poor interfacial compatibility with plastic matrices such as polyethylene. High bamboo powder content leads to deterioration in mechanical and processing properties. Furthermore, existing modification methods are complex, costly, and lack process stability.
A three-step gradient surface polarity control technology, consisting of glycerol pre-wetting, polyethylene wax/zinc stearate coating, and EVA interface bridging, combined with a multi-stage venting and moisture-proof closed-loop control process, was used to prepare bamboo-plastic masterbatch, achieving a balance of material properties under high bamboo powder filling content.
It significantly improves the interfacial compatibility between bamboo powder and plastic, ensures the strength, toughness and processing performance of the material under high bamboo powder filling, reduces costs and improves resource utilization and environmental benefits, and is suitable for industrial production.
Smart Images

Figure CN123152194A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of polymer composite materials technology, specifically to a bamboo-plastic masterbatch based on bamboo powder modified material, its preparation method and application, and more specifically, to a bamboo-plastic masterbatch that maintains good mechanical and processing properties under high bamboo powder filling content by gradient surface polarity control of bamboo powder, its preparation method and its application in bamboo-plastic composite materials. Technical Background Bamboo has a short growth cycle and strong regenerative capacity, making it an ideal green and renewable resource. However, in current technologies, large quantities of bamboo are often discarded due to flowering and death, resulting in low resource utilization. At the same time, daily necessities and building materials made from traditional petrochemical-based plastics (such as polyethylene) have high carbon footprints, high costs, and insufficient environmental friendliness.
[0002] Bamboo powder, a byproduct of bamboo processing, is widely available and inexpensive. Using bamboo powder as a reinforcing filler in a plastic matrix to prepare bamboo-plastic composites can reduce the proportion of petrochemical plastics used, decrease carbon emissions, and improve the comprehensive utilization rate of bamboo resources. However, current technologies for bamboo powder-plastic composites still face many technical challenges.
[0003] Firstly, the interfacial compatibility is poor. Bamboo powder contains a large number of polar hydroxyl groups on its surface, exhibiting strong hydrophilicity, while non-polar plastic resins such as polyethylene are hydrophobic. The interfacial bonding between the two is weak, and direct mixing easily leads to delamination, separation, bubbles, and pores. Direct mixing results in a decrease in the material's mechanical properties, tensile strength, flexural strength, impact toughness, appearance quality, and processing performance, thus limiting the industrial application of bamboo-based composite materials.
[0004] Secondly, bamboo powder is hygroscopic. Fluctuations in the particle size, moisture content, and ash content of bamboo powder can significantly affect melt flowability and granulation stability. When the moisture content of bamboo powder is too high, moisture, silver streaks, hollow particles, and batch-to-batch performance fluctuations are likely to occur during extrusion.
[0005] Third, high filler content presents processing difficulties. As the bamboo powder filler ratio increases, the melt viscosity and screw torque of the system rise. This easily leads to insufficient plasticization, uneven dispersion, increased equipment load, and difficulties in continuous production, making it difficult to balance high bamboo powder content with good processability. In existing technologies, the bamboo powder filler content is typically below 20%, resulting in limited environmental benefits.
[0006] Fourth, existing modification methods are limited. Existing methods using a single lubricant or simple mechanical mixing cannot simultaneously achieve multiple effects such as drying and dehumidifying bamboo powder, surface wetting and coating, interfacial compatibilization, melt lubrication, and toughness maintenance. As a result, the finished product is prone to problems such as brittleness, uneven color, and poor dimensional stability.
[0007] Fifth, existing bamboo-plastic materials do not offer significant cost and environmental advantages when the bamboo powder content is low; however, when the bamboo powder content is too high, mechanical properties and processing fluidity are easily sacrificed, and there is a lack of formulation systems and process windows suitable for large-scale manufacturing on conventional plastic production lines.
[0008] To address the aforementioned issues, various attempts have been made in existing research. Chinese patent CN110003678A discloses a technology for enhancing the interfacial compatibility of bamboo powder / recycled polyvinyl chloride based on octadecyl dopamine biomimetic modification. However, the aforementioned existing technologies still have the following shortcomings: firstly, the modification process is complex and costly; secondly, the bamboo powder filling amount is still relatively low; thirdly, there is a lack of precise control over the surface polarity gradient; and fourthly, the process stability is insufficient. Summary of the Invention
[0009] This invention addresses the technical problems of poor interfacial compatibility between bamboo powder and plastic matrices such as polyethylene, and the deterioration of mechanical and processing properties under high bamboo powder filling amounts in existing technologies. It provides a bamboo-plastic masterbatch based on bamboo powder-modified materials, its preparation method, and its applications. This invention achieves a good balance between the mechanical and processing properties of materials with high bamboo powder filling amounts through a three-step gradient surface polarity control technology of "glycerol pre-wetting → polyethylene wax / zinc stearate coating → EVA interface bridging," combined with a multi-stage venting and moisture-proof closed-loop control process.
[0010] The technical solution of this invention: A bamboo-plastic masterbatch based on bamboo powder modified material comprises the following raw material components in parts by weight: Bamboo powder 33-37 parts; preferably moso bamboo powder, which has advantages such as high fiber strength and toughness, high hardness and wear resistance.
[0011] 50-60 parts of polyethylene matrix; 3-8 parts of EVA resin; Polyethylene wax 1.0~2.5 parts; 0.5 to 1.2 parts of zinc stearate; Glycerin 0.3~0.8 parts; Antioxidant 0.1~0.5 parts; The bamboo powder has a particle size of 120-150 mesh, a moisture content of ≤1.0%, and an ash content of <1%; the EVA resin has a VA content of 18%-28%. The bamboo-plastic masterbatch is prepared by the following steps: (1) Bamboo powder pretreatment: The bamboo powder is sieved to 120-150 mesh and dried until the moisture content is ≤1.0% and the ash content is <1%; (2) Gradient surface modification: Add the bamboo powder obtained in step (1) into a high-speed mixer, heat it to 95℃~105℃ under stirring, and keep stirring for 5~10 minutes to remove moisture; then add glycerin, polyethylene wax and zinc stearate, EVA resin and antioxidant in sequence, and continue stirring for 2~5 minutes so that each additive can sequentially regulate the gradient polarity of the bamboo powder surface to obtain modified bamboo powder; (3) Melt blending: The modified bamboo powder obtained in step (2) and the polyethylene matrix are fed into a twin-screw extruder for melt blending. Vacuum exhaust is turned on during the extrusion process. (4) Extrusion granulation: The melt-blended material is cooled by air-cooled conveying and granulated to obtain bamboo-plastic masterbatch.
[0012] The following are the materials provided in the disclosure: In this invention, the following problems are solved through pretreatment: removing hydroxyl groups on the surface of bamboo powder to improve the interfacial compatibility between bamboo powder and plastic resin; solving the problem of insufficient material processing performance; and improving the key properties of the material such as strength and toughness to meet application standards.
[0013] Furthermore, the bamboo powder content in the bamboo-plastic masterbatch is 33%~37%, and the moisture content of the bamboo-plastic masterbatch is ≤0.5%.
[0014] Furthermore, it also includes 0.5 to 4 parts by weight of maleic anhydride-grafted polyethylene; the grafting rate of the maleic anhydride-grafted polyethylene is 0.5% to 2.0%.
[0015] Furthermore, the polyethylene matrix is selected from at least one of high-density polyethylene, low-density polyethylene, linear low-density polyethylene, or screened recycled polyethylene; the melt index of the polyethylene matrix is 1.5~5.0 g / 10 min.
[0016] In this invention, the amount of each component is expressed in parts by weight, and the preferred range is determined based on the following (the relative proportions between the components are adjusted accordingly when bamboo powder is 35 parts): 1. Bamboo powder, as a renewable reinforcing filler, directly affects the mechanical properties, cost, and processing fluidity of composite materials. In this invention, when the content is below 33 parts: the bamboo powder content is too low. Although the processing fluidity is good, the reinforcing effect as a renewable resource is not significant, and it cannot effectively reduce the amount of petrochemical-based polyethylene used. The cost and environmental advantages are not obvious, and the bamboo powder content of the finished material (after subsequent dilution) is difficult to reach the target range of 26%~28%. When the content is above 37 parts: the bamboo powder has a large specific surface area and the friction between particles increases sharply, resulting in a non-linear increase in the melt viscosity and screw torque of the system. At the same time, bamboo powder is prone to agglomeration in the matrix resin, resulting in deteriorated dispersibility and insufficient plasticization, which leads to a significant decrease in tensile strength and impact toughness. Therefore, the content is limited to 35±2 parts by weight (i.e., 33~37 parts), which can ensure the cost and environmental advantages brought by high filling while ensuring that the additives fully coat the surface of the bamboo powder.
[0017] 2. Polyethylene, as the continuous phase matrix resin, provides the melt flowability and basic mechanical framework of the composite material. It can be selected from HDPE, LDPE, or recycled polyethylene after screening. In this invention, when the content is less than 50 parts: the matrix resin cannot completely coat the bamboo powder particles, voids and interface defects are easily generated inside the masterbatch, resulting in poor granulation properties during extrusion granulation and easy powder shedding. When the content is more than 60 parts: although the processability is better, it will significantly dilute the effective bamboo powder content in the masterbatch. Therefore, it is limited to 50-60 parts. Since this invention adopts a "two-step dilution method", if the bamboo powder content in the masterbatch is less than 33%, the bamboo powder content in the finished product cannot be stably controlled above 26%, which weakens the significance of replacing petrochemical raw materials.
[0018] 3. EVA is the core "interface bridging" component for achieving gradient polarity control in this invention. Its molecular chain contains polar vinyl acetate (VA) segments and non-polar ethylene segments. In this invention, when the content is less than 3 parts: the EVA coverage of the polar surface of bamboo powder is discontinuous, and a complete polar gradient transition layer cannot be formed between bamboo powder and polyethylene. The interfacial stress concentration phenomenon is still serious, and the toughening and bridging effects are weak. When the content is more than 8 parts: excessive EVA (especially when the VA content is high) will self-aggregate due to the hydrogen bonding between its own polar groups, resulting in a significant increase in the melt viscosity of the system. At the same time, the high cost of EVA will drive up the material cost, and too much EVA will reduce the flexural modulus and heat resistance of the composite material. Therefore, limiting the EVA resin content to 3-8 parts can improve flexibility and interfacial wetting, and reduce the brittleness of the highly filled system. This invention preferably has a VA content of 18%-28%. Within this range, EVA can form good hydrogen bonding with the surface of bamboo powder and is fully compatible with the polyethylene matrix.
[0019] 4. In this invention, polyethylene wax, as a processing aid with both internal and external lubrication functions, improves flowability and forms a uniform coating layer on the surface of bamboo powder. When the content is less than 1.0 part: wetting and lubrication are insufficient, a dense non-polar coating layer cannot form on the surface of the bamboo powder, friction between the bamboo powder and resin increases, screw torque is too high, and burrs are easily generated in the pellets during pelleting. When the content is more than 2.5 parts: excessive polyethylene wax will precipitate onto the screw and barrel surfaces during extrusion, causing slippage, feeding difficulties, and wax mist on the surface of the product, reducing interlayer bonding and appearance quality. Therefore, the content is limited to 1.0~2.5 parts. 5. In this invention, zinc stearate is used as a dispersant and external lubricant in conjunction with polyethylene wax to reduce screw torque and decrease particle adhesion. When the dosage is less than 0.5 parts, it is difficult to effectively reduce the internal friction between bamboo powder particles, the additive is not evenly dispersed in the high-speed mixer, and white spots (undispersed bamboo powder agglomerates) easily appear on the cross-section of the masterbatch. When the dosage is greater than 1.2 parts, excessive zinc stearate will excessively reduce the melt strength, resulting in soft extrudate, severe particle adhesion during pelleting, and the stearic acid produced by the decomposition of zinc stearate will affect the odor and heat resistance of the material; therefore, the dosage is limited to 0.5~1.2 parts.
[0020] 6. In this invention, glycerol assists in wetting the surface of bamboo powder, improving the dispersion and processing stability of additives. Its highly polar polyhydroxy structure preferentially adsorbs onto the bamboo powder surface. When its dosage is less than 0.3 parts: it cannot effectively penetrate the capillary channels of bamboo powder, and its neutralization and shielding effect on free hydroxyl groups is insufficient, easily leading to "point-like exposure" during subsequent polyethylene wax coating, affecting the interfacial water resistance. When it is more than 0.8 parts: excessive glycerol cannot form chemical bonds with bamboo powder, and free glycerol migrates to the interface, acting as a plasticizer, reducing material rigidity and heat distortion temperature, and the masterbatch particles are prone to stickiness. Therefore, this invention selects 0.3~0.8 parts by weight of glycerol. 7. When the antioxidant used in this invention is less than 0.1 parts: it cannot effectively inhibit the thermo-oxidative degradation of lignin in bamboo powder during high-temperature extrusion, the masterbatch color easily turns yellow and chars, and the mechanical properties degrade rapidly after long-term storage. When the amount exceeds 0.5 parts, the antioxidant effect tends to saturate, which not only increases the cost, but also causes excess antioxidant to precipitate in the melt, affecting the surface gloss. Therefore, this invention limits the antioxidant to 0.1~0.5 parts by weight.
[0021] 8. Maleic anhydride-grafted polyethylene is preferably used at 0.5-4 parts by weight. PE-g-MAH acts as a chemical compatibilizer, and its anhydride groups can undergo esterification (chemical bonding) with the hydroxyl groups of bamboo powder. Below 0.5 parts: there are too few chemical bonding sites, which cannot reinforce the physical coating layer, resulting in insignificant compatibilization. Above 4 parts: the grafted material forms an excessively thick chemical layer at the interface, leading to increased interfacial brittleness. Furthermore, the cost of PE-g-MAH is much higher than that of ordinary polyethylene, significantly increasing raw material costs and making it uneconomical. The grafting rate is preferably controlled between 0.5% and 2.0%. Too low a grafting rate results in insufficient reactivity, while too high a grafting rate easily leads to cross-linking and gelation during processing; therefore, it is limited to 0.5-4 parts by weight.
[0022] This invention also incorporates antioxidant 1010 / 168 or a similar antioxidant system to reduce extrusion thermo-oxidative aging and maintain stable particle color and mechanical properties.
[0023] This invention also provides a method for preparing the above-mentioned bamboo-plastic masterbatch based on bamboo powder modified material, comprising the following steps: (1) Bamboo powder pretreatment: The bamboo powder is sieved to 120-150 mesh and dried until the moisture content is ≤1.0% and the ash content is <1%; (2) Gradient surface modification: Add the bamboo powder obtained in step (1) into a high-speed mixer, heat it to 95℃~105℃ under stirring, and keep stirring for 5~10 minutes to remove moisture; then add glycerin in sequence, stir, then add polyethylene wax and zinc stearate, continue stirring until the polyethylene wax is completely melted and evenly dispersed in the bamboo powder, then add EVA resin and antioxidant, continue stirring for 2~5 minutes, so that each additive sequentially modulates the gradient polarity of the bamboo powder surface to obtain modified bamboo powder; (3) Melt blending: The modified bamboo powder obtained in step (2) and the polyethylene matrix are put into a twin-screw extruder for melt blending. Vacuum exhaust is turned on during the extrusion process; the temperature control range of the extruder is 120℃~188℃. (4) Extrusion granulation: The melt-blended material is cooled by air-cooled conveying and granulated to obtain bamboo-plastic masterbatch.
[0024] Furthermore, in step (4), a special conveying process is adopted, namely, waterless multi-stage forced air-cooling conveying: the extruded strip is continuously introduced into a perforated air-cooled conveyor belt or a closed air-cooling device through a traction device. Filtered room temperature or dehumidified air is forced to blow air above and / or below the conveyor belt, and the air volume and conveying speed are adjusted by frequency conversion so that the strip reaches a state of non-stickiness and stable pelleting, and then it is cut into 3-4 mm particles, finally obtaining bamboo plastic masterbatch with a bamboo powder content of about 35%.
[0025] Furthermore, the drying in step (1) can be done at 90℃~105℃ for 2h~4h, or by heating and dehumidifying in a high-speed mixer. This can stabilize the particle size and moisture content, and reduce extrusion bubbles, silver streaks, and pores.
[0026] Furthermore, the stirring speed of the high-speed mixer in step (2) is 400~600 rpm.
[0027] Furthermore, in step (2), 0.5 to 4 parts by weight of maleic anhydride-grafted polyethylene are added simultaneously with the EVA resin.
[0028] Further, in step (2), a 200L high-speed mixer is preferred; after starting at low speed, the speed is increased to 500 rpm; the temperature is maintained at 100℃±5℃ for 8 minutes to remove moisture; glycerin, polyethylene wax, zinc stearate, EVA and optional compatibilizer are added in sequence, and mixing is continued for 2 to 5 minutes. This allows the additives to melt and uniformly coat the bamboo powder, reducing the exposure of free hydroxyl groups and improving interfacial compatibility.
[0029] Furthermore, the mechanism of gradient surface modification in step (2) is as follows: glycerol first penetrates into the surface of bamboo powder and neutralizes free hydroxyl groups, reducing the polarity of the bamboo powder surface; polyethylene wax and zinc stearate form a non-polar lubricating coating layer on the surface of bamboo powder; EVA resin utilizes the amphiphilic structure of polar vinyl acetate segments and non-polar ethylene segments in its molecular chain to form a polar gradient transition layer between the coating layer on the bamboo powder surface and the polyethylene matrix, thereby achieving gradient release of interfacial stress.
[0030] Furthermore, in steps (2) to (4), a multi-stage exhaust and moisture-proof closed-loop control is formed: the high-speed mixing stage removes free water from the surface of bamboo powder; the twin-screw extrusion stage removes volatiles and water vapor from the melt through vacuum exhaust and descaling; air-cooled conveying avoids secondary moisture absorption caused by water cooling; and the finished product is packaged in moisture-proof packaging using inner lining bags or aluminum-plastic composite bags.
[0031] Furthermore, in step (3), the twin-screw extruder has a screw length-to-diameter ratio of 36:1 to 44:1 and a screw speed of 180 to 260 rpm; the vacuum exhaust pressure is -0.06 MPa to -0.08 MPa. The temperature control of each zone of the twin-screw extruder along the material conveying direction is as follows: Zone 1 115℃ to 125℃, Zone 2 140℃ to 150℃, Zone 3 155℃ to 165℃, Zone 4 165℃ to 175℃, Zone 5 175℃ to 185℃, Zone 6 182℃ to 192℃, and the die head 170℃ to 180℃. This achieves plasticization, mixing, exhaust, and dispersion, avoiding thermal degradation of bamboo powder and uneven melt dispersion.
[0032] Furthermore, in step (4), the air-cooled conveying process uses an air-cooled conveyor belt or air duct for cooling, and the length of the pellets after pelletizing is 3mm~4mm. This prevents secondary moisture absorption, pellet adhesion, and subsequent injection molding bubbling.
[0033] The present invention also provides the application of the above-mentioned bamboo-plastic masterbatch in the preparation of bamboo-plastic composite materials, wherein the bamboo-plastic masterbatch is mixed with polyethylene matrix at a weight ratio of 75~80:20~25, and the mixture is processed by molding to obtain bamboo-plastic composite material; the bamboo powder content in the bamboo-plastic composite material is 26%~28%.
[0034] In the above applications, the molding process is injection molding or extrusion molding, and the processing temperature is 150℃~190℃; the tensile strength of the bamboo-plastic composite material is 18MPa~24MPa, the flexural strength is 28MPa~38MPa, and the notched impact strength is 4kJ / m. 2 ~8kJ / m 2 24-hour water absorption rate ≤1.5%.
[0035] In the above applications, during molding and processing, 0.5-3 parts by weight of color masterbatch and / or 0.5-3 parts by weight of functional masterbatch are added; the functional masterbatch is selected from one or more of antioxidant masterbatch, antistatic masterbatch, UV absorption masterbatch, or light-stabilizing masterbatch. This step mainly involves adding different colored masterbatches (such as white, gray, yellow, red, green, blue, and black) according to customer needs, and the aforementioned functional additives can also be added.
[0036] The above-mentioned equipment is compatible with conventional plastic processing equipment, ensuring consistency in product color, size, and appearance.
[0037] One of the innovations of this invention lies in its bamboo powder surface modification technology, which solves the interfacial compatibility problem. The existing technology faces the challenge that bamboo powder contains a large number of hydroxyl groups on its surface, resulting in poor interfacial compatibility with non-polar plastic resins such as polyethylene. Direct mixing leads to low material strength, poor toughness, easy delamination, and poor flowability during processing, causing equipment blockage. This invention, however, utilizes a composite additive system of "glycerol + zinc stearate + polyethylene wax + EVA resin," combined with a specific high-speed mixing process, to modify the surface of bamboo powder. Glycerol and zinc stearate neutralize and coat the polar hydroxyl groups on the bamboo powder surface; polyethylene wax and EVA resin act as compatibilizers, building a "bridge" between the bamboo powder and the plastic matrix, significantly improving interfacial bonding. This fundamentally solves the compatibility problem between bamboo powder and plastic resins, laying the foundation for achieving high bamboo powder filling content.
[0038] The innovation of this invention lies in the process control of high bamboo powder filling content, achieving a balance between cost and performance: traditional bamboo-plastic materials have low bamboo powder filling content (usually <20%), resulting in limited environmental benefits and cost advantages; excessive filling content leads to a decrease in the material's mechanical properties and processing difficulties. This invention achieves high filling content through a two-step process control: first, bamboo-plastic masterbatch with a bamboo powder content as high as 35% is prepared; then, the masterbatch is mixed with a polyethylene matrix in a certain proportion, controlling the bamboo powder content of the finished product to approximately 27%. While ensuring the material's strength, toughness, and processing performance, the utilization rate of bamboo powder is significantly improved, and the proportion of petrochemical plastics used is significantly reduced, achieving a win-win situation of cost reduction and environmental benefits.
[0039] The innovation of this invention lies in its customized high-speed mixing and extrusion granulation process, ensuring industrial stability. Current technical problems include the bamboo powder's hygroscopic nature and uneven additive dispersion, leading to issues such as bubbles, adhesion, and performance fluctuations during extrusion granulation, thus affecting industrial production stability. This invention optimizes key mixing and granulation parameters: In the high-speed mixing stage, process parameters of 100℃ and 500 rpm are used to remove moisture from the bamboo powder during stirring, while simultaneously achieving uniform additive dispersion. In the extrusion granulation stage, segmented temperature control from 120-188℃, combined with a special conveying + air duct cooling + pelletizing process, prevents particle adhesion and moisture absorption, ensuring stable masterbatch quality. This solves the industrial production challenges of masterbatch with high bamboo powder content, and the process is compatible with conventional plastic equipment, allowing for direct large-scale promotion.
[0040] The innovation of this invention lies in the multi-dimensional value innovation of environmental protection, cost, and application scenarios: (1) Environmental value: Replacing some petrochemical plastics with renewable bamboo resources reduces carbon emissions and at the same time consumes a large amount of planted and easily discarded bamboo resources, realizing the efficient use of resources. (2) Cost value: The cost of bamboo powder raw materials is much lower than that of pure plastics, and the high filling amount directly reduces the material production cost and enhances the product's market competitiveness. (3) Application value: The modified material is compatible with color masterbatch and functional masterbatch, and is suitable for various processes such as extrusion and injection molding. It can be processed into daily necessities and building materials such as stools, chairs, and profiles, with a wide range of application scenarios.
[0041] This invention utilizes gradient surface polarity control, significantly improving interfacial compatibility. The invention proposes a three-step gradient surface polarity control technology: "glycerol pre-wetting → polyethylene wax / zinc stearate coating → EVA interface bridging." Glycerol first penetrates the bamboo powder surface and neutralizes free hydroxyl groups; polyethylene wax and zinc stearate form a non-polar lubricating coating layer; EVA resin utilizes its amphiphilic structure to form a polar gradient transition layer. Compared with existing technologies, this invention achieves a gradient transition from hydrophilic to hydrophobic on the bamboo powder surface, avoiding interfacial stress concentration.
[0042] This invention utilizes a synergistic compatibilization strategy combining physical coating and chemical bonding. The strategy primarily employs physical coating, supplemented by chemical bonding. The polyhydroxyl groups in the glycerol molecule form hydrogen bonds with the cellulose molecules on the bamboo powder surface, while the polar groups in the EVA molecular chain form hydrogen bonds with the residual hydroxyl groups on the bamboo powder surface. The results of the examples show that the tensile strength of the bamboo-plastic composite material of this invention can reach 19.8~23.8 MPa.
[0043] This invention employs a multi-stage closed-loop control system for exhaust and moisture prevention, resulting in excellent process stability. The invention proposes a multi-stage closed-loop control process for exhaust and moisture prevention, consisting of "high-speed mixing and dehumidification + vacuum exhaust and volatilization + air-cooled moisture-proof packaging," effectively solving the batch fluctuation problem caused by moisture absorption in industrial production.
[0044] This invention employs a two-step dilution method to achieve high bamboo powder filling. First, bamboo-plastic masterbatch with a bamboo powder content of approximately 35% is prepared, and then diluted to a finished product with a bamboo powder content of approximately 27%, thus achieving high bamboo powder filling while ensuring processing fluidity.
[0045] This invention provides a quantitative characterization of the process window, making it suitable for industrial scale-up. Through systematic experiments, this invention determines the optimal range of key process parameters, forming a complete process window and solving the problem of difficulty in scale-up in existing technologies.
[0046] Beneficial technical effects of the present invention: 1. Advantages in environmental protection and resource utilization (1) Efficient utilization of renewable resources: Bamboo has a short growth cycle and strong regeneration. A large number of bamboo flowers and dies and are easily discarded. This invention uses bamboo powder as the main filling material, which greatly improves the utilization rate of bamboo resources and reduces resource waste.
[0047] (2) Significantly reduce carbon emissions: Replacing some of the petrochemical plastics such as polyethylene with bamboo powder directly reduces the proportion of petrochemical products used, and reduces carbon emissions in the production and use of plastics, which is in line with the development trend of green, low-carbon and circular economy.
[0048] (3) Reduce white pollution: Bamboo-based materials can partially replace traditional plastic daily necessities and building materials, reducing the environmental pressure caused by plastic waste while ensuring performance.
[0049] 2. Cost and benefit advantages (1) Raw material costs are significantly reduced: The price of bamboo powder raw materials is much lower than that of petrochemical resins such as polyethylene. This invention achieves finished materials with a bamboo powder content of up to 27%, which directly reduces the unit cost of materials and significantly improves the profit margin of products.
[0050] (2) Strong process adaptability and low industrialization cost: The preparation process is compatible with conventional 200L high-speed mixers, twin-screw extruders, air-cooled conveying pelletizing lines and plastic molding equipment such as injection molding and extrusion. No new special reaction kettles or special molding equipment are required. Only process control such as dehumidification, vacuum exhaust, air-cooled conveying and moisture-proof packaging needs to be configured on the existing production line to achieve continuous and large-scale production, thereby reducing equipment modification investment, debugging cycle and industrialization implementation cost.
[0051] (3) Enhanced product added value: Modified bamboo-plastic materials combine the processing performance of plastics with the natural texture of bamboo. Customization can be achieved by adding color masterbatch and functional masterbatch, thereby enhancing the market competitiveness and added value of the products.
[0052] 3. Technical and performance advantages (1) Solved the compatibility problem between bamboo powder and plastic: Through a composite additive system composed of glycerol, zinc stearate, polyethylene wax, and EVA resin, combined with a specific surface modification process, the interfacial bonding force between bamboo powder and polyethylene matrix was effectively improved, solving the problems of easy delamination and poor mechanical properties of traditional bamboo-plastic materials. As a further preferred option, one or more of maleic anhydride-grafted polyethylene (PE-g-MAH / MAPE), maleic anhydride-grafted POE, silane coupling agent, titanate coupling agent, or aluminate coupling agent can be added; among them, the polar groups of the grafted polyolefin can form hydrogen bonds or esterification with the hydroxyl groups on the surface of bamboo powder, and the polyolefin segments are compatible with the polyethylene matrix, which can significantly improve the interfacial adhesion and dispersion stability. If necessary, POE, SEBS or SEBS-g-MAH and other elastomer toughening agents, as well as antioxidants, ultraviolet absorbers and light stabilizers can be added to further improve low-temperature impact, outdoor weather resistance and thermal processing stability.
[0053] (2) Stable performance under high bamboo powder filling: The present invention achieves a high filling ratio of 35% bamboo powder masterbatch content and about 27% bamboo powder content in finished material, while ensuring the strength, toughness and processing fluidity of the material, avoiding the defects of the material becoming brittle, easy to break and difficult to process under high filling.
[0054] To achieve a 35% bamboo powder masterbatch content while maintaining material stability, this invention employs the following combined measures: First, the bamboo powder is controlled at 120-150 mesh and pre-dried to a moisture content ≤1.0% to reduce moisture and agglomeration. Second, a composite compatibilizing and lubricating system of EVA + polyethylene wax + zinc stearate + optional PE-g-MAH is used to form a continuous coating layer on the bamboo powder surface. Third, a masterbatch with approximately 35% bamboo powder content is first prepared, and then diluted with the polyethylene matrix in proportion to a finished product with approximately 27% bamboo powder content, avoiding insufficient plasticization caused by direct high-proportion filling. Fourth, segmented temperature control, moderate shearing, and vacuum degassing are used in the twin-screw extruder, with the temperature controlled within the range of 120℃-188℃ to balance resin melting and bamboo powder thermal stability. Fifth, air-cooled conveying and pelletizing are used to avoid secondary moisture absorption of the masterbatch due to water cooling. Through the above material system and process window, good flowability, strength, toughness, and particle consistency can be maintained even with high bamboo powder content.
[0055] (3) Good process stability and high product consistency: The key parameters (temperature, speed, and cooling process) of high-speed mixing and extrusion granulation have been optimized, effectively solving problems such as bamboo powder moisture absorption, uneven dispersion of additives, and particle adhesion, thus ensuring the stability and consistency of product quality in industrial production. Process stability can be further achieved through the following methods: when raw materials are put into storage, the particle size, moisture content, ash content, and color of bamboo powder are tested; after drying, bamboo powder is transported in a closed system or temporarily stored in a moisture-proof manner; in the high-speed mixing stage, temperature, time, and torque changes are used as the endpoints for dehumidification and coating; in the extrusion stage, automatic metering feeding, melt pressure monitoring, and vacuum degassing are used to prevent feeding fluctuations and air bubbles; in the pelletizing stage, air-cooled conveying, online screening, and particle length control are used; before finished product packaging, the moisture content, melt index, particle appearance, and mechanical properties of injection molding samples are tested, and moisture-proof packaging is carried out using inner lining bags or aluminum-plastic composite bags, thereby ensuring the consistency of performance of different batches of masterbatch and products.
[0056] 4. Application and Market Advantages: Modified bamboo-plastic materials are compatible with functional additives such as color masterbatch, antioxidant masterbatch, and antistatic masterbatch. They are suitable for various molding processes such as extrusion and injection molding, and can be processed into daily necessities and building materials such as stools, chairs, benches, tables, and outdoor profiles, with strong market adaptability. Attached Figure Description
[0057] Figure 1 This is a process flow diagram of the preparation method and application of bamboo-plastic masterbatch of the present invention.
[0058] Figure 2 This diagram illustrates the interface bonding before and after surface modification of bamboo powder, serving to explain the coating and interface compatibilization mechanism of composite additives.
[0059] Figure 3 These are SEM / micrographs of cross-sections of modified bamboo powder / HDPE and unmodified bamboo powder / HDPE according to the present invention; where a represents unmodified bamboo powder and b represents modified bamboo powder / HDPE.
[0060] Figure 4 This diagram illustrates the bamboo powder particle size distribution and the 120-150 mesh control range of the present invention. The purpose of this control is to remove coarse particles and agglomerates, control the proportion of excessively fine powder, ensure uniform dispersion of bamboo powder, stable moisture content, and consistent extrusion flowability and product appearance.
[0061] Figure 5 This is a schematic diagram of the morphology and cross-sectional dispersion of the bamboo-plastic masterbatch of the present invention, used to illustrate the particle length, appearance uniformity and cross-sectional dispersion state.
[0062] Figure 6 This diagram illustrates a comparison of the mechanical properties, processing fluidity, and water absorption of embodiments and comparative examples of the present invention. Relative index: Unmodified comparative example = 100. Detailed Implementation
[0063] To make the objectives, technical solutions, and beneficial effects of this invention clearer, the invention will be further described in detail below with reference to the accompanying drawings and specific embodiments. It should be understood that the specific embodiments described herein are merely illustrative and not intended to limit the invention. All reagents, solvents, compounds, etc., unless otherwise specified, are commercially available.
[0064] Example 1: A method for preparing bamboo-plastic masterbatch based on bamboo powder modified material I. Bamboo-plastic masterbatch formulation ; II. Preparation Method (1) Bamboo powder pretreatment: sieve the bamboo powder of moso bamboo, take the 120-150 mesh sieve portion, dry it at 100℃ for 3 hours until the moisture content is ≤1.0% and the ash content is <1%.
[0065] (2) Gradient surface modification: Add 35 parts by weight of dried bamboo powder to a 200L high-speed mixer, start from low speed and gradually increase to 500 rpm, while raising the temperature to 100℃; keep stirring at 100℃ and 500 rpm for 8 minutes to remove moisture. Then add in sequence: 0.5 parts by weight of glycerin, stir for 1 minute (pre-wetting stage); 1.5 parts by weight of polyethylene wax and 0.8 parts by weight of zinc stearate, stir until the wax is completely melted (coating stage); 5 parts by weight of EVA resin and 0.2 parts by weight of antioxidant 1010, stir for 2~3 minutes (interface bridging stage), and discharge.
[0066] (3) Melt blending and extrusion granulation: Modified bamboo powder and 57 parts by weight of HDPE were melt blended and extruded in a twin-screw extruder (length-to-diameter ratio 40:1, speed 220 rpm). Temperatures in each zone: Zone 1 120℃, Zone 2 145℃, Zone 3 160℃, Zone 4 170℃, Zone 5 178℃, Zone 6 185℃, and die head 175℃. Vacuum exhaust: -0.06MPa to -0.08MPa. The extrudate was cooled by an air-cooled conveyor belt and granulated (length 3mm to 4mm) to obtain bamboo-plastic masterbatch.
[0067] The air-cooled conveying adopts waterless multi-stage forced air-cooled conveying: the extruded strip is continuously fed into the perforated air-cooled conveyor belt or the closed air-cooling device through the traction device, and filtered room temperature or dehumidified air is forced to be supplied above and / or below the conveyor belt. The air volume and conveying speed are adjusted by frequency conversion so that the strip can be non-sticky and can be stably granulated.
[0068] (4) Preparation of bamboo-plastic composite material: Take 78 parts by weight of bamboo-plastic masterbatch and 22 parts by weight of HDPE, dry mix them, and injection mold (170℃~180℃). The bamboo powder content of the finished product is about 27.3%.
[0069] The moisture content of bamboo powder was tested according to GB / T 6284-2006 "General Method for Determination of Moisture in Chemical Products - Loss on Drying Method". The powder was dried to constant weight at 105±2℃, and the percentage of weight loss was calculated.
[0070] Example 2 The difference from Example 1 is that 2 parts by weight of PE-g-MAH were added to the bamboo-plastic masterbatch formulation, and HDPE was adjusted to 53 parts by weight, added simultaneously with EVA during the interface bridging stage of gradient surface modification. The rest is the same as in Example 1.
[0071] Example 3 The difference from Example 1 is as follows: the high-speed mixing speed is 600 rpm, the temperature is 105°C, and the dehumidification and stirring are performed for 6 minutes; the temperatures of each zone of the extruder are 125°C, 150°C, 165°C, 175°C, 185°C, 190°C, and 178°C, respectively, and the screw speed is 260 rpm. The rest is the same as in Example 1.
[0072] Example 4 The difference from Example 1 is that 75 parts by weight of bamboo-plastic masterbatch are mixed with 25 parts by weight of HDPE, resulting in a finished product with a bamboo powder content of approximately 26.25%. The rest is the same as in Example 1.
[0073] Example 5 The difference from Example 1 is that 80 parts by weight of bamboo-plastic masterbatch are mixed with 20 parts by weight of HDPE, resulting in a finished product with a bamboo powder content of approximately 28.00%. The rest is the same as in Example 1.
[0074] Example 6 The difference from Example 1 is that the final formulation uses 78 parts bamboo-plastic masterbatch, 19.5 parts HDPE, 1.5 parts gray masterbatch, and 1.0 part antioxidant masterbatch, totaling 100 parts; the theoretical bamboo powder mass fraction is 27.3%. The rest is the same as in Example 1. Comparative Example 1 (direct mixing of unmodified bamboo powder) 27.3 parts bamboo powder and 72.7 parts HDPE were directly mixed, totaling 100 parts. The bamboo powder particle size and drying conditions were the same as in Example 1. Glycerin, EVA, polyethylene wax, zinc stearate, and PE-g-MAH were not added. Samples were prepared under extrusion and injection molding conditions consistent with the final composite material. This comparative example was used to compare unmodified systems with the same bamboo powder content.
[0075] Comparative Example 2 (glycerol modification only) The mixture consists of 35 parts by weight of bamboo powder, 55 parts by weight of HDPE, 0.5 parts by weight of glycerin, and 0.2 parts by weight of antioxidant 1010. The preparation method is the same as in Example 1, but only glycerin is added in the gradient surface modification step; polyethylene wax, zinc stearate, and EVA are not added. The finished product contains approximately 27% bamboo powder.
[0076] Comparative Example 3 (without EVA) The mixture consists of 35 parts by weight of bamboo powder, 55 parts by weight of HDPE, 1.5 parts by weight of polyethylene wax, 0.8 parts by weight of zinc stearate, 0.5 parts by weight of glycerin, and 0.2 parts by weight of antioxidant 1010. The preparation method is the same as in Example 1, but EVA is not added in the gradient surface modification step. The finished product contains approximately 27% bamboo powder.
[0077] Performance Tests and Results: Tensile strength is tested according to GB / T 1040.2-2022 "Determination of tensile properties of plastics - Part 2: Test conditions for molded and extruded plastics". A type 1A dumbbell-shaped specimen is used, with a tensile speed of 50 mm / min.
[0078] Bending strength is tested according to GB / T 9341-2008 "Determination of bending properties of plastics". Specimen size: 80mm × 10mm × 4mm, span: 64mm, testing speed: 2 mm / min.
[0079] Notched impact strength GB / T 1043.1-2008 "Determination of impact properties of simply supported plastic beams - Part 1: Non-instrumental impact testing". Type A notch (notch depth 2mm), pendulum energy 2J or 4J (selected according to toughness).
[0080] Melt flow rate GB / T 3682.1-2018 "Determination of melt mass flow rate (MFR) and melt volumetric flow rate (MVR) of thermoplastics - Part 1: Standard method". Test temperature 190℃, load 2.16 kg (applicable to polyethylene).
[0081] Moisture content of granules / bamboo powder shall be determined according to GB / T 2677.2—2011 or by a validated equivalent oven drying method; if the masterbatch is dried using the 105±2℃ oven loss method, it shall be reported as “105℃ drying loss”, and it shall be stated that the value may include volatiles other than water.
[0082] The 24-hour water absorption rate of the finished product is determined according to GB / T 1034-2008 "Determination of Water Absorption of Plastics". Following Method 1 (immersion method), the sample is dried to constant weight at 50℃, then immersed in distilled water at 23±0.5℃ for 24 hours. After removing and wiping off surface moisture, the sample is weighed and the result is calculated.
[0083] Masterbatch granule appearance conforms to GB / T 2547-2008 "Sampling Methods for Plastics" and visual inspection method. Visually inspect the uniformity, color difference, charred black spots, and degree of adhesion of the granules, and measure the granule length (3mm~4mm) with vernier calipers.
[0084] Place the injection-molded standard sample (or actual product) under normal lighting conditions (illuminance of about 300~500 lux) and visually observe it from 30cm away. Record whether there are defects such as silver streaks, bubbles, delamination, cracks and color differences on the surface.
[0085] ; Results analysis: (1) Effect of gradient surface polarity control: The tensile strength of Example 1 was 21.5 MPa, while that of Comparative Example 1 was only 18 MPa, proving that the three-step gradient surface modification effectively improved the interfacial bonding.
[0086] (2) Synergistic effect of compatibilizer: Example 2 (with PE-g-MAH): tensile strength 23.8MPa, flexural strength 37.5MPa, impact strength 6.8kJ / m 2 The water absorption rate is only 0.9%, which is better than that of Example 1.
[0087] (3) Synergistic effect of additives: The tensile strength of Comparative Example 2 (glycerin only) was 17 MPa, and that of Comparative Example 3 (without EVA) was 18 MPa, both of which were much lower than the 21.5 MPa of Example 1, proving that each additive is indispensable in the three-step gradient modification.
[0088] (4) Processing fluidity: The melt flow rate of Examples 1-6 was 3.0-4.5 g / 10 min, while that of Comparative Example 1 was only 1.5 g / 10 min.
[0089] (5) Water resistance: The water absorption rate of Examples 1 to 6 is 0.9% to 1.3%, and that of Comparative Example 1 is 1.2%.
[0090] (6) Appearance of finished products: As shown in the table above, the injection-molded products of Examples 1-6 have a uniform and smooth surface, without obvious silver streaks, bubbles, delamination, or cracking. However, the product of Comparative Example 1 has a large number of silver streaks and visible bubbles, Comparative Example 2 has localized silver streaks, and Comparative Example 3 has slight silver streaks. This indicates that only under the synergistic effect of the complete "gradient surface polarity control" and "multi-stage exhaust and moisture-proofing" processes of this invention can the appearance defects of the high bamboo powder filler system during the injection molding process be eliminated, resulting in bamboo-plastic products that meet the appearance quality requirements of daily-use and building materials products. This verifies the effectiveness of this invention in solving the appearance problems caused by bamboo powder moisture absorption.
[0091] The table below provides a detailed comparison between the unmodified bamboo powder / polyethylene comparative example (Comparative Example 1) and Example 2: ; Industrial applicability The bamboo-plastic masterbatch, its preparation method, and its applications provided by this invention feature a clear process flow, simple operation, and conventional equipment, making it suitable for large-scale industrial production. The resulting bamboo-plastic composite material can be widely used in daily necessities (stools, chairs, benches, tables, etc.), building materials (outdoor profiles, flooring, railings, etc.), and packaging materials. This invention replaces some petrochemical plastics with renewable bamboo resources, reducing carbon emissions and white pollution, and has significant economic, social, and environmental benefits.
[0092] The technical solution of the present invention will be further described below with reference to the accompanying drawings. It should be understood that the following embodiments are for illustrative purposes only and are not intended to limit the scope of protection of the present invention. Equivalent substitutions or modifications made by those skilled in the art without departing from the concept of the present invention should all fall within the scope of protection of the present invention.
Claims
1. A bamboo-plastic masterbatch based on bamboo powder modified material, characterized in that, The raw material components include the following parts by weight: Bamboo powder 33-37 parts; polyethylene matrix 50-60 parts; EVA resin 3-8 parts; polyethylene wax 1.0-2.5 parts; zinc stearate 0.5-1.2 parts; glycerin 0.3-0.8 parts; antioxidant 0.1-0.5 parts; the VA content of the EVA resin is 18%-28%; The bamboo-plastic masterbatch is prepared by the following steps: (1) Bamboo powder pretreatment: The bamboo powder is sieved to 120-150 mesh and dried until the moisture content is ≤1.0% and the ash content is <1%; (2) Gradient surface modification: Add the bamboo powder obtained in step (1) into a high-speed mixer, heat it to 95℃~105℃ under stirring, and keep stirring for 5~10 minutes to remove moisture; then add glycerin, polyethylene wax and zinc stearate, EVA resin and antioxidant in sequence, and continue stirring for 2~5 minutes so that each additive can sequentially regulate the gradient polarity of the bamboo powder surface to obtain modified bamboo powder; (3) Melt blending: The modified bamboo powder obtained in step (2) and the polyethylene matrix are fed into a twin-screw extruder for melt blending. Vacuum exhaust is turned on during the extrusion process. (4) Extrusion granulation: The melt-blended material is cooled by air-cooled conveying and granulated to obtain bamboo-plastic masterbatch.
2. The bamboo-plastic masterbatch based on bamboo powder modified material according to claim 1, characterized in that, The bamboo powder content in the bamboo-plastic masterbatch is 33%~37%, and the moisture content of the bamboo-plastic masterbatch is ≤0.5%.
3. The bamboo-plastic masterbatch based on bamboo powder modified material according to claim 1, characterized in that, It also includes 0.5 to 4 parts by weight of maleic anhydride-grafted polyethylene; the grafting rate of the maleic anhydride-grafted polyethylene is 0.5% to 2.0%.
4. The bamboo-plastic masterbatch based on bamboo powder modified material according to claim 1, characterized in that, The polyethylene matrix is selected from at least one of high-density polyethylene, low-density polyethylene, linear low-density polyethylene, or screened recycled polyethylene; the melt index of the polyethylene matrix is 1.5~5.0 g / 10 min; the antioxidant is selected from at least one of antioxidant 1010, antioxidant 168, and antioxidant 1076.
5. A method for preparing bamboo-plastic masterbatch based on bamboo powder modified material as described in any one of claims 1 to 4, characterized in that, Includes the following steps: (1) Bamboo powder pretreatment: The bamboo powder is sieved to 120-150 mesh and dried until the moisture content is ≤1.0% and the ash content is <1%; (2) Gradient surface modification: Add the bamboo powder obtained in step (1) into a high-speed mixer, heat it to 95℃~105℃ at a stirring speed of 400~600 rpm, and keep stirring for 5~10 minutes to remove moisture; then add glycerin, polyethylene wax and zinc stearate, EVA resin and antioxidant in sequence, and continue stirring for 2~5 minutes so that each additive can sequentially regulate the gradient polarity of the bamboo powder surface to obtain modified bamboo powder; (3) Melt blending: The modified bamboo powder obtained in step (2) and the polyethylene matrix are fed into a twin-screw extruder for melt blending. Vacuum exhaust is turned on during the extrusion process. The twin-screw extruder has a screw length-to-diameter ratio of 36:1 to 44:1 and a screw speed of 180 to 260 rpm. The vacuum exhaust pressure is -0.06 MPa to -0.08 MPa. (4) Extrusion granulation: The melt-blended material is cooled by air-cooled conveying and granulated to obtain bamboo-plastic masterbatch.
6. The method for preparing bamboo-plastic masterbatch based on bamboo powder modified material according to claim 5, characterized in that, In step (2), 0.5 to 4 parts by weight of maleic anhydride-grafted polyethylene are added simultaneously with the EVA resin.
7. The method for preparing bamboo-plastic masterbatch based on bamboo powder modified material according to claim 5, characterized in that, The mechanism of gradient surface modification in step (2) is as follows: glycerol first penetrates into the surface of bamboo powder and neutralizes free hydroxyl groups, reducing the polarity of the bamboo powder surface; polyethylene wax and zinc stearate form a non-polar lubricating coating layer on the surface of bamboo powder; EVA resin utilizes the amphiphilic structure of polar vinyl acetate segments and non-polar ethylene segments in its molecular chain to form a polar gradient transition layer between the coating layer on the bamboo powder surface and the polyethylene matrix, thereby achieving gradient release of interfacial stress.
8. The application of a bamboo-plastic masterbatch as described in any one of claims 1 to 4 or a bamboo-plastic masterbatch prepared by the preparation method as described in any one of claims 5 to 7 in the preparation of bamboo-plastic composite materials, characterized in that, The bamboo-plastic masterbatch is mixed with polyethylene matrix at a weight ratio of 75~80:20~25, and then processed to obtain bamboo-plastic composite material; the bamboo powder content in the bamboo-plastic composite material is 26%~28%.
9. The application of bamboo-plastic masterbatch based on bamboo powder modified material according to claim 8, characterized in that, The molding process is injection molding or extrusion molding, with a processing temperature of 150℃~190℃; the tensile strength of the bamboo-plastic composite material is 18MPa~24MPa, the flexural strength is 28MPa~38MPa, and the notched impact strength is 4kJ / m. 2 ~8kJ / m 2 24-hour water absorption rate ≤1.5%.
10. The application of bamboo-plastic masterbatch based on bamboo powder modified material according to claim 8, characterized in that, During molding and processing, 0.5-3 parts by weight of color masterbatch and / or 0.5-3 parts by weight of functional masterbatch are added; the functional masterbatch is selected from one or more of antioxidant masterbatch, antistatic masterbatch, ultraviolet absorption masterbatch or light-stabilized masterbatch.
Citation Information
Patent Citations
Bionic modified reinforced bamboo powder / recycled polyvinyl chloride interfacial compatibility technology based on octadecanoyl-based dopamine
CN110003678A