Low-smoke halogen-free flame-retardant crosslinked polyethylene insulation material and preparation method thereof

By introducing maleic anhydride-grafted POE and bifunctional modified mesoporous metal hydroxide into polyethylene materials, and combining zinc borate with vinyl MQ silicone resin to form a ceramic barrier layer, the problems of low flame retardant efficiency and high smoke density of halogen-free flame-retardant polyethylene materials are solved, achieving efficient flame retardant and smoke suppression effects.

CN123152196APending Publication Date: 2026-11-24GUANGDONG CABLE WORKS CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202611483855.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-22
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing halogen-free flame-retardant polyethylene materials suffer from low flame-retardant efficiency and high smoke density during flaming combustion.

Method used

Low-smoke, halogen-free, flame-retardant cross-linked polyethylene insulation material is used. Maleic anhydride-grafted POE is used as a compatibilizer to combine with bifunctional modified mesoporous metal hydroxide to form an interfacial bond. During the pyrolysis stage, a ceramic barrier layer is formed through the mesoporous structure and the synergistic effect of zinc borate and vinyl MQ silicone resin, thereby improving the flame retardant and smoke suppression performance.

Benefits of technology

While meeting the mechanical and electrical insulation properties of cable materials, the flame retardant and low-smoke properties of the materials are significantly improved, the smoke density during the flaming combustion stage is reduced, and the mechanical strength and electrical insulation properties of the materials are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

This application relates to the technical field of polymer composite material preparation, specifically disclosing a low-smoke halogen-free flame-retardant cross-linked polyethylene insulating material and its preparation method. The low-smoke halogen-free flame-retardant cross-linked polyethylene insulating material is prepared from the following raw materials in parts by weight: 100 parts polyethylene resin, 5-12 parts maleic anhydride-grafted POE, 80-120 parts bifunctional modified mesoporous metal hydroxide, 5-15 parts zinc borate, 3-8 parts vinyl MQ silicone resin, 1.5-2.5 parts cross-linking agent, 0.5-1.5 parts co-cross-linking agent, 0.6-1.2 parts antioxidant, and 0.5-1.5 parts lubricant. The cross-linked polyethylene insulating material obtained by this application has the advantages of low smoke density, excellent flame retardant properties, and good mechanical properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the technical field of polymer composite material preparation, and more specifically, it relates to a low-smoke, halogen-free, flame-retardant cross-linked polyethylene insulating material and its preparation method. Background Technology

[0002] With increasingly stringent fire safety requirements for critical infrastructure such as high-rise buildings, subways, tunnels, and nuclear power plants, the demand for low-smoke halogen-free flame-retardant cable materials continues to grow. Polyethylene (PE) materials, due to their lightweight, non-toxicity, excellent electrical insulation properties, chemical corrosion resistance, and good processing performance, have become one of the preferred base materials for cable insulation and sheathing. However, pure polyethylene matrix itself does not possess flame-retardant properties, is highly flammable, and easily produces molten droplets during combustion. Therefore, it is necessary to add a halogen-free flame-retardant system to achieve flame-retardant functionality.

[0003] Currently, the industry commonly uses inorganic flame retardant systems such as aluminum hydroxide and magnesium hydroxide. While these systems can achieve halogen-free, low-toxicity, and smoke-suppressing effects, they rely on endothermic dehydration and residue coverage to function, resulting in low flame retardant efficiency per unit mass. A large filler content is required to achieve the same flame retardant rating. High filler content significantly reduces the tensile strength and elongation at break of the material, transforming it from tough to brittle and impairing its electrical insulation properties. Furthermore, the strong polarity of inorganic fillers leads to poor compatibility with the non-polar polyethylene matrix, making them prone to agglomeration and internal defects, further deteriorating the material's mechanical and electrical properties.

[0004] Patent application CN121449993A discloses a low-smoke, halogen-free flame-retardant polyethylene material comprising the following components in parts by weight: 10-20 parts polyethylene, 10-20 parts polyolefin thermoplastic elastomer, 30-50 parts inorganic flame retardant, and 5-10 parts synergistic flame retardant; wherein the inorganic flame retardant is a non-expandable layered inorganic filler powder with a D50 particle size of 1-5 μm; the synergistic flame retardant is an expandable layered inorganic filler powder with a D50 particle size ≤30 μm; the non-expandable layered inorganic filler powder is selected from at least one of kaolin, brucite, talc, or mica; and the expandable layered inorganic filler powder is at least one of montmorillonite, layered sepiolite, or hydrotalcite.

[0005] In this scheme, a barrier layer is formed by the physical stacking of non-expanding layered inorganic filler powder to delay heat and oxygen transfer, thereby achieving excellent mechanical properties and low flameless smoke density. However, this physical barrier layer is prone to cracking or powder particle detachment under the high temperature erosion of continuous flaming combustion. This not only weakens the barrier effect, but the detached particles also disperse in the flue gas, leading to an increase in smoke density and a decrease in flame retardant efficiency during the flaming combustion stage. Summary of the Invention

[0006] To address the shortcomings of existing halogen-free flame-retardant polyethylene materials, such as low flame-retardant efficiency and high smoke density during flaming combustion, this application provides a low-smoke halogen-free flame-retardant cross-linked polyethylene insulation material and its preparation method.

[0007] This application provides a low-smoke, halogen-free, flame-retardant cross-linked polyethylene insulation material, employing the following technical solution: A low-smoke, halogen-free, flame-retardant cross-linked polyethylene insulation material is prepared from the following raw materials in parts by weight: 100 parts polyethylene resin, 5-12 parts maleic anhydride grafted POE, 80-120 parts bifunctional modified mesoporous metal hydroxide, 5-15 parts zinc borate, 3-8 parts vinyl MQ silicone resin, 1.5-2.5 parts crosslinking agent, 0.5-1.5 parts co-crosslinking agent, 0.6-1.2 parts antioxidant, and 0.5-1.5 parts lubricant; The bifunctional modified mesoporous metal hydroxide is prepared by using magnesium hydroxide micro powder, aluminum hydroxide micro powder and pore-forming agent as raw materials to obtain mesoporous metal hydroxide powder, or by using magnesium salt, aluminum salt and template agent as raw materials to obtain mesoporous metal hydroxide powder, and then by stepwise grafting modification with vinyl silane coupling agent and amino silane coupling agent.

[0008] By employing the above technical solution, maleic anhydride-grafted POE serves as a compatibilizer. Its polar groups can form interfacial bonds with the amino groups on the surface of the bifunctional modified mesoporous metal hydroxide. The vinyl groups on the surface of the mesoporous metal hydroxide can participate in the cross-linking reaction during the subsequent peroxide cross-linking process, anchoring the inorganic filler within the polymer cross-linking network. This effectively improves the dispersion uniformity of the inorganic filler in the high-filling system and reduces internal porosity and agglomeration defects. Upon heating, the metal hydroxide undergoes multi-stage endothermic dehydration. In the early stage of pyrolysis, the mesoporous structure promotes the uniform dehydration reaction on the particle surface and within the particles, and the dehydration residue maintains a fine particle size and porous framework structure. This high specific surface area inorganic framework can physically trap and adsorb some of the smoke precursors generated by polyethylene pyrolysis during the pyrolysis stage, reducing the amount of diffusion into the gas phase flame zone. Simultaneously, zinc borate decomposes at high temperature to generate glassy boron oxide. This glassy component can penetrate and wet the porous inorganic residue under capillary action, synergistically combining with the silica framework generated by the high-temperature oxidation of vinyl MQ silicone resin. This binds the loose inorganic residue into a more continuous and dense ceramic barrier layer, enhancing its resistance to airflow erosion. This application utilizes a dual synergistic mechanism of capturing smoke precursors in the early stage of pyrolysis and constructing a dense ceramic barrier layer on the combustion surface to improve the flame retardant and low-smoke properties of the cable material while meeting its mechanical and electrical insulation performance requirements.

[0009] Preferably, the polyethylene resin is a blend of low-density polyethylene and metallocene polyethylene in a mass ratio of (70~75):(25~30).

[0010] By adopting the above technical solutions, low-density polyethylene has excellent processing fluidity, which can improve the melt plasticization and extrusion processing performance of high-filler systems; metallocene polyethylene has a narrow molecular weight distribution and uniform comonomer distribution, which can improve the toughness of the matrix and the interfacial compatibility with inorganic fillers. The combination of the two can balance the processing and molding performance and mechanical properties of high-filler flame-retardant systems.

[0011] Preferably, the grafting rate of maleic anhydride-grafted POE is 0.8~1.2wt%.

[0012] Preferably, the crosslinking agent is dicumyl peroxide, and the co-crosslinking agent is triallyl isocyanurate.

[0013] Preferably, the antioxidant includes antioxidant 1010 and antioxidant 168.

[0014] Preferably, the lubricant is zinc stearate or polyethylene wax.

[0015] Preferably, the vinyl MQ silicone resin has a vinyl mass fraction of 2.0~4.0 wt%.

[0016] Preferably, the preparation method of the bifunctional modified mesoporous metal hydroxide includes the following steps: S11: Disperse magnesium hydroxide micro powder and aluminum hydroxide micro powder in water, add pore-forming agent and mix well, adjust pH to 8.5~9.0, spray dry, extract, dry to obtain mesoporous metal hydroxide powder; S12: Add a 1.5%~2.5% (w / w) vinylsilane coupling agent alcohol solution to the reactor, adjust the pH to 4.0~5.0, and hydrolyze for 40~60 min to obtain pre-hydrolyzed solution A; S13: Add an aminosilane coupling agent alcohol solution with a mass fraction of 1.5%~2.5% to the reactor, adjust the pH to 8.5~9.5, and hydrolyze for 40~60 min to obtain pre-hydrolyzed solution B; S14: Pre-hydrolyzed solution A and pre-hydrolyzed solution B are sequentially and uniformly sprayed onto the surface of mesoporous metal hydroxide powder and dried to obtain bifunctional modified mesoporous metal hydroxide.

[0017] By adopting the above technical solution and using a wet adsorption site-occupying pore-forming process, a mesoporous structure can be formed on the surface of the particles and inside the agglomerates after the pore-forming agent is removed by extraction. The resulting powder maintains a micron-sized particle size after secondary dispersion. The mesoporous structure can increase the contact area between the filler and the matrix, provide physical anchoring points, and significantly improve interfacial compatibility with bifunctional modification. At the same time, in the early stage of pyrolysis, the porous framework can retain part of the smoke precursor, which helps to reduce the density of flaming combustion smoke.

[0018] Preferably, the mass-to-volume ratio of the mesoporous metal hydroxide powder, pre-hydrolyzed solution A, and pre-hydrolyzed solution B is 1 g : (0.7~1.2 mL) : (0.5~0.8 mL).

[0019] Preferably, the pore-forming agent is polyethylene glycol.

[0020] More preferably, the polyethylene glycol is polyethylene glycol 2000.

[0021] Preferably, the mass ratio of the magnesium hydroxide micro powder to the aluminum hydroxide micro powder is (1.5~3):1.

[0022] Preferably, the particle size distribution of the magnesium hydroxide micro powder and aluminum hydroxide micro powder is 1~5μm.

[0023] Preferably, the amount of the pore-forming agent is 15% to 25% of the total mass of magnesium hydroxide micro powder and aluminum hydroxide micro powder.

[0024] A further preferred embodiment of the method for preparing the bifunctional modified mesoporous metal hydroxide includes the following steps: S21: Add the template agent to water, heat to 60~70℃, and add magnesium salt, aluminum salt and alkaline solution at the same time. Adjust the pH to 9.5~9.7, react for 12~18h, cool, wash, extract to obtain mesoporous metal hydroxide powder. S22: Add a 1.5%~2.5% (w / w) vinylsilane coupling agent alcohol solution to the reactor, adjust the pH to 4.0~5.0, and hydrolyze for 40~60 min to obtain pre-hydrolyzed solution A; S23: Add an aminosilane coupling agent alcohol solution with a mass fraction of 1.5%~2.5% to the reactor, adjust the pH to 8.5~9.5, and hydrolyze for 40~60 min to obtain pre-hydrolyzed solution B; S24: Pre-hydrolyzed solution A and pre-hydrolyzed solution B are sequentially and uniformly sprayed onto the surface of mesoporous metal hydroxide powder and dried to obtain bifunctional modified mesoporous metal hydroxide. In the magnesium and aluminum salts, Mg 2+ And Al 3+ The molar ratio is (2~4):1.

[0025] Preferably, the amount of the template agent is 10% to 20% of the total mass of magnesium salt and aluminum salt.

[0026] Preferably, the mass-to-volume ratio of the mesoporous metal hydroxide powder, pre-hydrolyzed solution A, and pre-hydrolyzed solution B is 1 g : (0.7~1.2 mL) : (0.5~0.8 mL).

[0027] By employing the above technical solutions, mesoporous metal hydroxides with uniform pore size and high specific surface area can be prepared using a co-precipitation combined with a soft template method. The template agent is removed by extraction, while the flame-retardant activity of the hydroxide is retained. Stepwise hydrolysis and grafting of bissilanes endow the powder surface with both cross-linking activity and polar compatibility sites. Combined with the physical anchoring effect of mesopores, this achieves a simultaneous improvement in the interfacial performance and flame-retardant and smoke-suppressing properties of the highly filled system.

[0028] Preferably, the alkaline solution is a mixed solution of sodium hydroxide and sodium carbonate.

[0029] Preferably, the template agent is hexadecyltrimethylammonium bromide.

[0030] Preferably, the zinc borate and low melting point glass powder are premixed at a mass ratio of (3~4):1 before use.

[0031] Preferably, the softening point of the low melting point glass powder is not higher than 400°C.

[0032] By adopting the above technical solution, zinc borate and low-melting-point glass powder are physically mixed. At high temperature, zinc borate generates B2O3 glass phase, and glass powder provides the framework. The two work together to form a continuous ceramic barrier layer.

[0033] More preferably, the mesoporous metal hydroxide powder undergoes the following pretreatment steps before silane modification: The mesoporous metal hydroxide powder was immersed in an aqueous solution containing ammonium molybdate and ferric nitrate for 2-4 hours, followed by solid-liquid separation, drying, and then set aside for use.

[0034] Preferably, in the aqueous solution containing ammonium molybdate and ferric nitrate, the mass fraction of ammonium molybdate is 1% to 2.0%, and the mass fraction of ferric nitrate is 1% to 2.0%.

[0035] By adopting the above technical solution, the precursor is transformed in situ into active sites of iron and molybdenum oxides during the material combustion process. With the participation of oxygen, it catalyzes the oxidation of carbon soot particles and adsorbed soot precursors, thereby further improving the low-smoke performance of the material.

[0036] This application also provides a method for preparing a low-smoke, halogen-free, flame-retardant cross-linked polyethylene insulating material, comprising the following steps: After adding polyethylene resin and maleic anhydride-grafted POE into a mixer, the temperature is raised to 140~150℃ and the mixture is mixed for 3~5 minutes. Then, bifunctional modified mesoporous metal hydroxide, zinc borate, vinyl MQ silicone resin, antioxidant and lubricant are added and mixed for 3~5 minutes. The temperature is lowered to 105~110℃, crosslinking agent and co-crosslinking agent are added and mixed for 3~5 minutes. The mixture is then extruded through an extruder, cooled, pelletized, and shaped. Finally, it is crosslinked in an inert atmosphere at 175~180℃ for 25~30 minutes to obtain a low-smoke halogen-free flame-retardant crosslinked polyethylene insulation material.

[0037] By adopting the above technical solution, the process design of first melting the matrix, then dispersing the filler, and finally adding the crosslinking system ensures that the material maintains good fluidity and processing stability during extrusion. At the same time, the stepwise feeding process facilitates the full melting and blending of maleic anhydride-grafted POE and polyethylene matrix to form a uniform and compatible system. This promotes the uniform dispersion and interfacial bonding of bifunctional modified mesoporous metal hydroxide, zinc borate, and vinyl MQ silicone resin in the matrix, reducing agglomeration defects. Thus, while ensuring the material's excellent low-smoke halogen-free flame retardant properties, it also improves the mechanical strength, aging resistance, and electrical insulation reliability of the insulating material.

[0038] In summary, this application has the following beneficial effects: This application uses bifunctional modified mesoporous metal hydroxide as the main flame-retardant filler. The amino groups on the filler surface are grafted with maleic anhydride to form an interfacial bond, and the vinyl groups on the filler surface participate in the construction of the cross-linking network. At the same time, the mesoporous channels provide physical anchoring points, improve the dispersibility of the high-filler, reduce internal defects in the material, and take into account both mechanical and electrical properties. This high specific surface area inorganic framework can physically intercept or adsorb some of the small molecule volatiles and carbon particle precursors generated by polyethylene pyrolysis during the pyrolysis stage, which helps to reduce the smoke density during the flaming combustion stage. During combustion, zinc borate and vinyl MQ silicone resin synergistically form an erosion-resistant ceramic barrier layer, achieving a synergistic effect of flame retardancy and smoke suppression. Detailed Implementation

[0039] The present application will be further described in detail below with reference to the embodiments.

[0040] Unless otherwise specified, the raw materials used in the embodiments and comparative examples of this application are all commercially available.

[0041] The particle size distribution of zinc borate is 1~10μm; The particle size of low melting point glass powder is 2~10μm, and the softening point is about 390℃; The grafting rate of maleic anhydride onto POE was 0.8~1.2 wt%. The melt flow rate of low-density polyethylene at 190℃ and 2.16kg is 1.0~3.0g / 10min, and that of metallocene polyethylene is 0.5~3.0g / 10min. The vinyl content of vinyl MQ silicone resin is 2.0~4.0 wt%, and the M / Q molar ratio is 0.6~0.9.

[0042] Preparation Examples 1-8: Bifunctional Modified Mesoporous Metal Hydroxides Preparation Example 1 The preparation method of the bifunctional modified mesoporous metal hydroxide in this example includes the following steps: S11: Add 360g of magnesium hydroxide micro powder with a particle size distribution of 1~5μm and 240g of aluminum hydroxide micro powder with a particle size distribution of 1~5μm to water, with a solid-liquid ratio of 1g:5mL. Add 3g of sodium hexametaphosphate and transfer to an ultrasonic device. Disperse the mixture at 200W and 30kHz for 25min. Add 90g of polyethylene glycol 2000 and stir at 300r / min for 10min. Adjust the pH to 8.5 with 10% ammonia water. Continue stirring at 300r / min for 30min to make the pH uniform and stable. Spray dry the mixture at an inlet temperature of 135℃ and an outlet temperature of 80℃. Extract twice with ethanol. After dispersion, dry at 60℃ and disperse again to obtain mesoporous metal hydroxide powder with a particle size distribution of 1~10μm. S12: Add a 1.5% (w / w) vinyltrimethoxysilane ethanol aqueous solution (wherein the volume fraction of the ethanol aqueous solution is 90%) to the reactor, adjust the pH to 5.0 with 5% (w / w) acetic acid, and hydrolyze for 40 min to obtain pre-hydrolyzed solution A. S13: Add a 1.5% (w / w) γ-aminopropyltriethoxysilane ethanol aqueous solution (wherein the volume fraction of the ethanol aqueous solution is 90%) to the reactor, adjust the pH to 8.5 with 5% (w / w) ammonia water, and hydrolyze for 40 min to obtain pre-hydrolyzed solution B. S14: Pre-hydrolyzed solution A and pre-hydrolyzed solution B are sequentially and uniformly sprayed onto the surface of mesoporous metal hydroxide powder, and dried at 110°C to constant weight to obtain bifunctional modified mesoporous metal hydroxide.

[0043] The mass-volume ratio of the mesoporous metal hydroxide powder, pre-hydrolyzed solution A, and pre-hydrolyzed solution B is 1 g: 0.7 mL: 0.5 mL.

[0044] Preparation Example 2 The preparation method of the bifunctional modified mesoporous metal hydroxide in this example includes the following steps: S11: Add 420g of magnesium hydroxide micro powder with a particle size distribution of 1~5μm and 180g of aluminum hydroxide micro powder with a particle size distribution of 1~5μm to water, with a solid-liquid ratio of 1g:5mL. Add 3g of sodium hexametaphosphate and transfer to an ultrasonic device. Disperse the mixture at 200W and 30kHz for 25min. Add 120g of polyethylene glycol 2000 and stir at 300r / min for 10min. Adjust the pH to 9.0 with 10% ammonia water. Continue stirring at 300r / min for 30min to make the pH uniform and stable. Spray dry the mixture at an inlet temperature of 135℃ and an outlet temperature of 80℃. Extract twice with ethanol. After dispersion, dry at 60℃ and disperse again to obtain mesoporous metal hydroxide powder with a particle size distribution of 1~10μm. S12: Add a 2% (w / w) vinyltrimethoxysilane ethanol aqueous solution (wherein the volume fraction of the ethanol aqueous solution is 90%) to the reactor, adjust the pH to 4.5 with 5% (w / w) acetic acid, and hydrolyze for 50 min to obtain pre-hydrolyzed solution A. S13: Add a 2% (w / w) γ-aminopropyltriethoxysilane ethanol aqueous solution (wherein the volume fraction of the ethanol aqueous solution is 90%) to the reactor, adjust the pH to 9.0 with 5% (w / w) ammonia water, and hydrolyze for 50 min to obtain pre-hydrolyzed solution B. S14: Pre-hydrolyzed solution A and pre-hydrolyzed solution B are sequentially and uniformly sprayed onto the surface of mesoporous metal hydroxide powder, and dried at 110°C to constant weight to obtain bifunctional modified mesoporous metal hydroxide.

[0045] The mass-volume ratio of the mesoporous metal hydroxide powder, pre-hydrolyzed solution A, and pre-hydrolyzed solution B is 1 g: 1 mL: 0.6 mL.

[0046] Preparation Example 3 The preparation method of the bifunctional modified mesoporous metal hydroxide in this example includes the following steps: S11: Add 450g of magnesium hydroxide micro powder with a particle size distribution of 1~5μm and 150g of aluminum hydroxide micro powder with a particle size distribution of 1~5μm to water, with a solid-liquid ratio of 1g:5mL. Add 3g of sodium hexametaphosphate and transfer to an ultrasonic device. Disperse the mixture at 200W and 30kHz for 25min. Add 150g of polyethylene glycol 2000 and stir at 300r / min for 10min. Adjust the pH to 9.0 with 10% ammonia water. Continue stirring at 300r / min for 30min to make the pH uniform and stable. Spray dry the mixture at an inlet temperature of 135℃ and an outlet temperature of 80℃. Extract twice with ethanol. After dispersion, dry at 60℃ and disperse again to obtain mesoporous metal hydroxide powder with a particle size distribution of 1~10μm. S12: Add a 2.5% (w / w) vinyltrimethoxysilane ethanol aqueous solution (wherein the volume fraction of the ethanol aqueous solution is 90%) to the reactor, adjust the pH to 4.0 with 5% (w / w) acetic acid, and hydrolyze for 60 min to obtain pre-hydrolyzed solution A. S13: Add a 2.5% (w / w) γ-aminopropyltriethoxysilane ethanol aqueous solution (wherein the volume fraction of the ethanol aqueous solution is 90%) to the reactor, adjust the pH to 9.5 with 5% (w / w) ammonia water, and hydrolyze for 60 min to obtain pre-hydrolyzed solution B. S14: Pre-hydrolyzed solution A and pre-hydrolyzed solution B are sequentially and uniformly sprayed onto the surface of mesoporous metal hydroxide powder, and dried at 110°C to constant weight to obtain bifunctional modified mesoporous metal hydroxide.

[0047] The mass-volume ratio of the mesoporous metal hydroxide powder, pre-hydrolyzed solution A, and pre-hydrolyzed solution B is 1 g: 1.2 mL: 0.8 mL.

[0048] Preparation Example 4 The difference between this preparation example and Preparation Example 1 is as follows: S21: Add 266.39 g of hexadecyltrimethylammonium bromide to 0.9 L of deionized water, heat to 60 °C, slowly add 9 L of mixed salt solution with a molar concentration of 1 mol / L, and simultaneously slowly add alkaline solution with a molar concentration of 2 mol / L, adjust the pH to 9.7, maintain 60 °C, react for 12 h, cool, filter, wash with deionized water until the filtrate is neutral, then extract twice with anhydrous ethanol under reflux, wash with ethanol until no silver halide precipitate is found in the filtrate after testing with silver nitrate solution, disperse, dry at 60 °C, and disperse a second time to obtain mesoporous metal hydroxide powder with a particle size distribution of 1~5 μm; The mixed salt solution was prepared using magnesium nitrate hexahydrate, aluminum nitrate nonahydrate, and deionized water. The molar ratio of magnesium nitrate hexahydrate to aluminum nitrate nonahydrate was 2:1. The molar mass of magnesium nitrate hexahydrate was 256.41 g / mol, and the total amount used was 1538.46 g. The molar mass of aluminum nitrate nonahydrate was 375.13 g / mol, and the total amount used was 1125.39 g. The alkaline solution was prepared using sodium hydroxide, sodium carbonate, and deionized water. The molar ratio of sodium hydroxide to sodium carbonate was 3:1.

[0049] Steps S22 to S24 are the same as steps S12 to S14.

[0050] The preparation process is the same as in Example 1.

[0051] Preparation Example 5 The difference between this preparation example and preparation example 2 is as follows: S21: Add 386.22 g of hexadecyltrimethylammonium bromide to 1.2 L of deionized water, heat to 65 °C, slowly add 9 L of mixed salt solution with a molar concentration of 1 mol / L, and simultaneously slowly add alkaline solution with a molar concentration of 2 mol / L, adjust the pH to 9.5, maintain 65 °C, react for 18 h, cool, filter, wash with deionized water until the filtrate is neutral, then reflux extract twice with anhydrous ethanol, wash with ethanol until no silver halide precipitate is found in the filtrate when tested with silver nitrate solution, disperse, dry at 60 °C, and disperse a second time to obtain mesoporous metal hydroxide powder with a particle size distribution of 1~5 μm; The mixed salt solution was prepared using magnesium nitrate hexahydrate, aluminum nitrate nonahydrate, and deionized water. The molar ratio of magnesium nitrate hexahydrate to aluminum nitrate nonahydrate was 3:1. The molar mass of magnesium nitrate hexahydrate was 256.41 g / mol, and the total amount used was 1730.77 g. The molar mass of aluminum nitrate nonahydrate was 375.13 g / mol, and the total amount used was 844.04 g. The alkaline solution was prepared using sodium hydroxide, sodium carbonate, and deionized water. The molar ratio of sodium hydroxide to sodium carbonate was 3:1.

[0052] Steps S22 to S24 are the same as steps S12 to S14.

[0053] The preparation process is the same as in Example 2.

[0054] Preparation Example 6 The difference between this preparation example and preparation example 3 is as follows: S21: Add 504.28 g of hexadecyltrimethylammonium bromide to 0.9 L of deionized water, heat to 70 °C, slowly add 9 L of mixed salt solution with a molar concentration of 1 mol / L, and simultaneously slowly add alkaline solution with a molar concentration of 2 mol / L, adjust the pH to 9.5, maintain 70 °C, react for 18 h, cool, filter, wash with deionized water until the filtrate is neutral, then reflux extract twice with anhydrous ethanol, wash with ethanol until no silver halide precipitate is found in the filtrate after testing with silver nitrate solution, disperse, dry at 60 °C, and disperse again to obtain mesoporous metal hydroxide powder with a particle size distribution of 1~5 μm; The mixed salt solution was prepared using magnesium nitrate hexahydrate, aluminum nitrate nonahydrate, and deionized water. The molar ratio of magnesium nitrate hexahydrate to aluminum nitrate nonahydrate was 4:1. The molar mass of magnesium nitrate hexahydrate was 256.41 g / mol, and the total amount used was 1846.15 g. The molar mass of aluminum nitrate nonahydrate was 375.13 g / mol, and the total amount used was 675.23 g. The alkaline solution was prepared using sodium hydroxide, sodium carbonate, and deionized water. The molar ratio of sodium hydroxide to sodium carbonate was 3:1.

[0055] Steps S22 to S24 are the same as steps S12 to S14.

[0056] The preparation process is the same as in Example 3.

[0057] Preparation Example 7 The difference between this preparation example and preparation example 4 is as follows: Before silane modification, mesoporous metal hydroxide powders undergo the following pretreatment steps: Mesoporous metal hydroxide powder was added to an aqueous solution containing ammonium molybdate and ferric nitrate at a solid-liquid ratio of 1 g: 5 mL. The mixture was stirred and dispersed at 800 r / min for 30 min, and then stirred at 300 r / min for 2 h. The mixture was then filtered, washed with a small amount of deionized water, and dried at 60 °C to constant weight. The mixture was then dispersed a second time to control the particle size distribution of the powder to be 1~5 μm. The powder was then set aside for later use.

[0058] In the aqueous solution containing ammonium molybdate and ferric nitrate, the mass fraction of ammonium molybdate is 1%, the mass fraction of ferric nitrate is 1%, and the remainder is water.

[0059] The preparation process is the same as in Example 4.

[0060] Preparation Example 8 The difference between this preparation example and preparation example 4 is as follows: Before silane modification, mesoporous metal hydroxide powders undergo the following pretreatment steps: Mesoporous metal hydroxide powder was added to an aqueous solution containing ammonium molybdate and ferric nitrate at a solid-liquid ratio of 1 g: 5 mL. The mixture was stirred and dispersed at 800 r / min for 30 min, and then stirred at 300 r / min for 4 h. The mixture was then filtered, washed with a small amount of deionized water, and dried at 60 °C to constant weight. The mixture was then dispersed a second time to control the particle size distribution of the powder to be 1~5 μm. The powder was then set aside for later use.

[0061] In the aqueous solution containing ammonium molybdate and ferric nitrate, the mass fraction of ammonium molybdate is 2%, the mass fraction of ferric nitrate is 2%, and the remainder is water.

[0062] The preparation process is the same as in Example 4.

[0063] Example 1 The preparation method of the low-smoke halogen-free flame-retardant cross-linked polyethylene insulation material in this embodiment includes the following steps: 500g of polyethylene resin and 25g of maleic anhydride-grafted POE were added to a mixer, heated to 140°C, and mixed for 3 minutes. Then, 400g of bifunctional modified mesoporous metal hydroxide, 25g of zinc borate, 15g of vinyl MQ silicone resin, 1.5g of antioxidant 1010, 1.5g of antioxidant 168, and 2.5g of zinc stearate from Preparation Example 1 were added and mixed for 3 minutes. The mixture was then cooled to 110°C, and 7.5g of dicumyl peroxide and 2.5g of triallyl isocyanurate were added and mixed for 3 minutes. The mixture was then extruded through an extruder, water-cooled at 30°C, and the surface moisture was dried by an air knife. Finally, the mixture was pelletized to obtain crosslinkable granules. The polyethylene resin is made by mixing low-density polyethylene and metallocene polyethylene, with a mass ratio of 75:25.

[0064] Extruder temperature settings: Zone 1 is 105℃, Zone 2 is 110℃, Zone 3 is 120℃, Zone 4 is 125℃, and the die head is 120℃.

[0065] Before performance testing: Under a nitrogen atmosphere, the prepared crosslinkable granules are preheated and melted on a flat vulcanizing machine, then pressurized to 12MPa, heated to 180℃, crosslinked for 25min, cooled and demolded, which is the low-smoke halogen-free flame-retardant crosslinked polyethylene insulation material. Standard samples are cut for performance testing.

[0066] Example 2 The difference between this embodiment and Embodiment 1 is that: The preparation method of the low-smoke halogen-free flame-retardant cross-linked polyethylene insulation material in this embodiment includes the following steps: 500g of polyethylene resin and 45g of maleic anhydride-grafted POE were added to a mixer, heated to 145°C, and mixed for 4 minutes. Then, 500g of bifunctional modified mesoporous metal hydroxide, 50g of zinc borate, 25g of vinyl MQ silicone resin, 2g of antioxidant 1010, 2g of antioxidant 168, and 5g of zinc stearate from Preparation Example 2 were added and mixed for 4 minutes. The mixture was then cooled to 105°C, and 10g of dicumyl peroxide and 5g of triallyl isocyanurate were added and mixed for 4 minutes. The mixture was then extruded through an extruder, water-cooled at 30°C, and the surface moisture was dried by an air knife. Finally, the mixture was pelletized to obtain crosslinkable granules.

[0067] The polyethylene resin is made by mixing low-density polyethylene and metallocene polyethylene, with a mass ratio of 70:30.

[0068] Before performance testing: Under a nitrogen atmosphere, the prepared crosslinkable granules are preheated and melted on a flat vulcanizing machine, then pressurized to 12MPa, heated to 175℃, crosslinked for 30min, cooled and demolded, which is the low-smoke halogen-free flame-retardant crosslinked polyethylene insulation material. Standard samples are cut for performance testing.

[0069] Everything else is the same as in Example 1.

[0070] Example 3 The difference between this embodiment and Embodiment 1 is that: The preparation method of the low-smoke halogen-free flame-retardant cross-linked polyethylene insulation material in this embodiment includes the following steps: 500g of polyethylene resin and 60g of maleic anhydride-grafted POE were added to a mixer, heated to 150°C, and mixed for 5 minutes. Then, 600g of bifunctional modified mesoporous metal hydroxide, 75g of zinc borate and low-melting-point glass powder premix, 40g of vinyl MQ silicone resin, 3g of antioxidant 1010, 3g of antioxidant 168, and 7.5g of zinc stearate were added and mixed for 5 minutes. The mixture was then cooled to 105°C, and 12.5g of dicumyl peroxide and 7.5g of triallyl isocyanurate were added and mixed for 5 minutes. The mixture was then extruded through an extruder, water-cooled at 30°C, and the surface moisture was dried by an air knife. Finally, the mixture was pelletized to obtain crosslinkable granules.

[0071] The polyethylene resin is made by mixing low-density polyethylene and metallocene polyethylene, with a mass ratio of 75:25.

[0072] The premix of zinc borate and low-melting-point glass powder is prepared by mixing zinc borate and low-melting-point glass powder at a mass ratio of 4:1 at high speed for 5 minutes.

[0073] Everything else is the same as in Example 1.

[0074] Example 4 The preparation method of the low-smoke halogen-free flame-retardant cross-linked polyethylene insulation material in this embodiment includes the following steps: 500g of polyethylene resin and 45g of maleic anhydride-grafted POE were added to a mixer, heated to 145°C, and mixed for 4 minutes. Then, 500g of the bifunctional modified mesoporous metal hydroxide, 50g of the premix of zinc borate and low-melting-point glass powder, 25g of vinyl MQ silicone resin, 2g of antioxidant 1010, 2g of antioxidant 168, and 5g of zinc stearate were added and mixed for 4 minutes. The mixture was then cooled to 105°C, 10g of dicumyl peroxide and 5g of triallyl isocyanurate were added, and the mixture was mixed for 4 minutes. The mixture was then extruded through an extruder, water-cooled at 30°C, and the surface moisture was dried by an air knife. Finally, the mixture was pelletized to obtain crosslinkable granules.

[0075] The polyethylene resin is made by mixing low-density polyethylene and metallocene polyethylene, with a mass ratio of 75:25.

[0076] Extruder temperature settings: Zone 1 is 105℃, Zone 2 is 110℃, Zone 3 is 120℃, Zone 4 is 125℃, and the die head is 120℃.

[0077] The premix of zinc borate and low melting point glass powder is prepared by mixing zinc borate and low melting point glass powder at a mass ratio of 3:1 at high speed for 5 minutes.

[0078] Before performance testing: Under a nitrogen atmosphere, the prepared crosslinkable granules are preheated and melted on a flat vulcanizing machine, then pressurized to 12MPa, heated to 180℃, crosslinked for 30min, cooled and demolded, which is the low-smoke halogen-free flame-retardant crosslinked polyethylene insulation material. Standard samples are cut for performance testing.

[0079] Example 5 The difference between this embodiment and embodiment 4 is that: The bifunctional modified mesoporous metal hydroxide was prepared from Example 5; The rest is the same as in Example 4.

[0080] Example 6 The difference between this embodiment and embodiment 4 is that: The bifunctional modified mesoporous metal hydroxide was prepared from Example 6; The rest is the same as in Example 4.

[0081] Example 7 The difference between this embodiment and embodiment 4 is that: The bifunctional modified mesoporous metal hydroxide was prepared from Example 7; The rest is the same as in Example 4.

[0082] Example 8 The difference between this embodiment and embodiment 4 is that: The bifunctional modified mesoporous metal hydroxide was prepared from Example 8; The rest is the same as in Example 4.

[0083] Comparative Example 1 The difference between this comparative example and Example 1 is as follows: A bifunctional modified metal hydroxide was used to replace the bifunctional modified mesoporous metal hydroxide by an equal mass. The preparation method of the bifunctional modified metal hydroxide in this comparative example includes the following steps: S11: Add 360g of magnesium hydroxide micro powder with a particle size distribution of 1~5μm and 240g of aluminum hydroxide micro powder with a particle size distribution of 1~5μm to water, with a solid-liquid ratio of 1g:5mL. Add 3g of sodium hexametaphosphate, transfer to an ultrasonic device, and ultrasonically disperse for 25min at 200W and 30kHz. Spray dry at an inlet temperature of 135℃ and an outlet temperature of 80℃. Wash twice with anhydrous ethanol. After dispersion, dry at 60℃ and disperse again to obtain metal hydroxide powder with a particle size distribution of 1~10μm. S12: Add a 1.5% (w / w) vinyltrimethoxysilane ethanol aqueous solution (wherein the volume fraction of the ethanol aqueous solution is 90%) to the reactor, adjust the pH to 5.0 with 5% (w / w) acetic acid, and hydrolyze for 40 min to obtain pre-hydrolyzed solution A. S13: Add a 1.5% (w / w) γ-aminopropyltriethoxysilane ethanol aqueous solution (wherein the volume fraction of the ethanol aqueous solution is 90%) to the reactor, adjust the pH to 8.5 with 5% (w / w) ammonia water, and hydrolyze for 40 min to obtain pre-hydrolyzed solution B. S14: Pre-hydrolyzed solution A and pre-hydrolyzed solution B are sequentially and uniformly sprayed onto the surface of the metal hydroxide powder, and dried at 110°C to constant weight to obtain bifunctional modified metal hydroxide.

[0084] Everything else is the same as in Example 1.

[0085] Comparative Example 2 The difference between this comparative example and Example 1 is as follows: No vinyl MQ silicone resin was added; Everything else is the same as in Example 1.

[0086] The low-smoke halogen-free flame-retardant cross-linked polyethylene insulation materials prepared in Examples 1-8 and Comparative Examples 1-2 were subjected to the following performance tests, and the specific test results are shown in Table 1.

[0087] Table 1. Performance test data of cross-linked polyethylene insulation materials prepared in Examples 1-8 and Comparative Examples 1-2

[0088] As can be seen from Table 1, the volume resistivity of all embodiments and comparative examples is ≥1.0×10⁻⁶. 14 Ω·cm, meeting the electrical performance requirements of cable insulation materials.

[0089] The comparison between Example 1 and Comparative Example 1 shows that the metal hydroxide composition, modification method and dosage are the same for both, and the only difference is the mesoporous structure. The introduction of the mesoporous structure provides a high specific surface area framework for adsorbing and capturing smoke precursors in the early stage of pyrolysis, and improves the interfacial bonding through physical anchoring of the pores, thus contributing to flame retardancy, smoke suppression and mechanical properties.

[0090] The comparison between Example 1 and Comparative Example 2 shows that the contribution of vinyl MQ silicone resin is mainly reflected in the combustion performance. Without its addition, the material's anti-dripping ability decreases, and the vertical burning rating and oxygen index decrease accordingly.

[0091] The comparison of Examples 1-3 shows that as the amount of difunctional modified mesoporous metal hydroxide increases, the flame retardant and smoke suppression properties of the material continuously improve, while the tensile strength and elongation at break decrease accordingly. Furthermore, compared to Comparative Example 1, Example 3 has a relatively higher filler content, but the elongation at break is similar, indicating that the synergistic effect of mesoporous channel anchoring and difunctional interfacial bonding effectively buffers the damage to toughness caused by high filler content.

[0092] A comparison of Examples 2 and 4 shows that, with comparable filler amounts, the co-precipitation combined with the soft template method, along with the premixing of zinc borate and low-melting-point glass powder, results in superior flame retardancy, smoke suppression, and mechanical properties. A comparison of Examples 4-6 shows that increasing the magnesium-aluminum ratio effectively reduces smoke density and improves light transmittance. The increased magnesium-aluminum ratio leads to greater dehydration of the hydroxyl groups in the layers, enhancing the heat absorption, cooling, and dilution effects; simultaneously, the increased proportion of magnesium oxide in the residue facilitates the formation of a high-temperature resistant ceramic skeleton.

[0093] A comparison of Examples 7-8 with Example 4 shows that after loading iron and molybdenum components into the mesoporous channels, the smoke density further decreased and the light transmittance further increased, with a more significant decrease in the density of flaming smoke. Meanwhile, the oxygen index and vertical combustion rating remained essentially unchanged. This indicates that the loaded iron and molybdenum components mainly contribute to smoke suppression by catalyzing the oxidation of soot and adsorbed smoke precursors in the presence of oxygen, with limited impact on the flame-retardant and self-extinguishing properties of the material. Mechanically, the tensile strength remained basically unchanged, while the elongation at break decreased slightly, and the effect was controllable under low loads.

Claims

1. A low smoke, halogen-free, flame-retardant, crosslinked polyethylene insulation material, characterized in that, It is prepared from the following raw materials in parts by weight: 100 parts polyethylene resin, 5-12 parts maleic anhydride grafted POE, 80-120 parts bifunctional modified mesoporous metal hydroxide, 5-15 parts zinc borate, 3-8 parts vinyl MQ silicone resin, 1.5-2.5 parts crosslinking agent, 0.5-1.5 parts co-crosslinking agent, 0.6-1.2 parts antioxidant, and 0.5-1.5 parts lubricant; The bifunctional modified mesoporous metal hydroxide is prepared by using magnesium hydroxide micro powder, aluminum hydroxide micro powder and pore-forming agent as raw materials to obtain mesoporous metal hydroxide powder, or by using magnesium salt, aluminum salt and template agent as raw materials to obtain mesoporous metal hydroxide powder, and then by stepwise grafting modification with vinyl silane coupling agent and amino silane coupling agent.

2. The low smoke, zero halogen, flame retardant crosslinked polyethylene insulation of claim 1, wherein, The polyethylene resin is a blend of low-density polyethylene and metallocene polyethylene in a mass ratio of (70~75):(25~30).

3. The low smoke, zero halogen, flame retardant crosslinked polyethylene insulation of claim 2, wherein, The method for preparing the bifunctional modified mesoporous metal hydroxide includes the following steps: S11: Disperse magnesium hydroxide micro powder and aluminum hydroxide micro powder in water, add pore-forming agent and mix well, adjust pH to 8.5~9.0, spray dry, extract, dry to obtain mesoporous metal hydroxide powder; S12: Add a 1.5%~2.5% (w / w) vinylsilane coupling agent alcohol solution to the reactor, adjust the pH to 4.0~5.0, and hydrolyze for 40~60 min to obtain pre-hydrolyzed solution A; S13: Add an aminosilane coupling agent alcohol solution with a mass fraction of 1.5%~2.5% to the reactor, adjust the pH to 8.5~9.5, and hydrolyze for 40~60 min to obtain pre-hydrolyzed solution B; S14: Pre-hydrolyzed solution A and pre-hydrolyzed solution B are sequentially and uniformly sprayed onto the surface of mesoporous metal hydroxide powder and dried to obtain bifunctional modified mesoporous metal hydroxide.

4. The low-smoke halogen-free flame-retardant cross-linked polyethylene insulation material according to claim 3, characterized in that, The amount of the pore-forming agent is 15% to 25% of the total mass of magnesium hydroxide micro powder and aluminum hydroxide micro powder.

5. The low-smoke halogen-free flame-retardant cross-linked polyethylene insulation material according to claim 3, characterized in that, The mass ratio of magnesium hydroxide micro powder to aluminum hydroxide micro powder is (1.5~3):

1.

6. The low-smoke halogen-free flame-retardant cross-linked polyethylene insulation material according to claim 1, characterized in that, The method for preparing the bifunctional modified mesoporous metal hydroxide includes the following steps: S21: Add the template agent to water, heat to 60~70℃, and add magnesium salt, aluminum salt and alkaline solution at the same time. Adjust the pH to 9.5~9.7, react for 12~18h, cool, wash, extract to obtain mesoporous metal hydroxide powder. S22: Add a 1.5%~2.5% (w / w) vinylsilane coupling agent alcohol solution to the reactor, adjust the pH to 4.0~5.0, and hydrolyze for 40~60 min to obtain pre-hydrolyzed solution A; S23: Add an aminosilane coupling agent alcohol solution with a mass fraction of 1.5%~2.5% to the reactor, adjust the pH to 8.5~9.5, and hydrolyze for 40~60 min to obtain pre-hydrolyzed solution B; S24: Pre-hydrolyzed solution A and pre-hydrolyzed solution B are sequentially and uniformly sprayed onto the surface of mesoporous metal hydroxide powder and dried to obtain bifunctional modified mesoporous metal hydroxide. The molar ratio of Mg 2+ and Al 3+ in the magnesium salt and the aluminum salt is (2-4):

1.

7. The low-smoke halogen-free flame-retardant cross-linked polyethylene insulation material according to claim 6, characterized in that, Before undergoing silane modification, the mesoporous metal hydroxide powder undergoes the following pretreatment steps: The mesoporous metal hydroxide powder was immersed in an aqueous solution containing ammonium molybdate and ferric nitrate for 2-4 hours, followed by solid-liquid separation, drying, and then set aside for use.

8. The low-smoke halogen-free flame-retardant cross-linked polyethylene insulation material according to claim 7, characterized in that, In the aqueous solution containing ammonium molybdate and ferric nitrate, the mass fraction of ammonium molybdate is 1%~2.0% and the mass fraction of ferric nitrate is 1%~2.0%.

9. The low-smoke halogen-free flame-retardant cross-linked polyethylene insulation material according to claim 1, characterized in that, The zinc borate and low melting point glass powder are premixed at a mass ratio of (3~4):1 before use.

10. A method for preparing a low-smoke, halogen-free, flame-retardant cross-linked polyethylene insulating material as described in any one of claims 1 to 9, characterized in that, Includes the following steps: After adding polyethylene resin and maleic anhydride-grafted POE into a mixer, the temperature is raised to 140~150℃ and the mixture is mixed for 3~5 minutes. Then, bifunctional modified mesoporous metal hydroxide, zinc borate, vinyl MQ silicone resin, antioxidant and lubricant are added and mixed for 3~5 minutes. The temperature is lowered to 105~110℃, crosslinking agent and co-crosslinking agent are added and mixed for 3~5 minutes. The mixture is then extruded through an extruder, cooled, pelletized, and shaped. Finally, it is crosslinked in an inert atmosphere at 175~180℃ for 25~30 minutes to obtain a low-smoke halogen-free flame-retardant crosslinked polyethylene insulation material.

Citation Information

Patent Citations

  • Low-smoke halogen-free flame-retardant polyethylene material as well as preparation method and application thereof

    CN121449993A