Electrically conductive wear-resistant ultrahigh molecular weight polyethylene composite and method of making same
By constructing a composite structure in UHMWPE consisting of irradiated crosslinked carrier particles, sheet-like MoS₂, and Y₂O₃-supported antimony-doped SnO₂ conductive phase, the problems of structural stability and electrostatic dissipation in the conductive and wear-resistant modification processes of UHMWPE were solved, thereby improving the wear resistance and electrostatic dissipation performance of the material.
Patent Information
- Application Number
- CN202611574417.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-12
- Publication Date
- 2026-11-24
AI Technical Summary
Existing UHMWPEs struggle to balance structural stability, processability, and long-term performance during conductive and wear-resistant modifications, especially in electrostatically sensitive environments where electrostatic dissipation and wear resistance are difficult to achieve simultaneously.
Composite functional particles were constructed by using irradiated crosslinked UHMWPE carrier particles, sheet-like MoS₂ and Y₂O₃ supported antimony-doped SnO₂ conductive phases. Through γ-ray irradiation, oxygen plasma treatment and mechanical composite, a stable conductive network was formed, which reduced frictional resistance and provided a charge transport path.
This achieves a balance between improved wear resistance and electrostatic dissipation performance in electrostatically sensitive environments, ensuring the structural stability and long-term performance of the composite material.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] This invention relates to the field of polymer composite materials technology, specifically to a conductive and wear-resistant ultra-high molecular weight polyethylene composite material and its preparation method. Background Technology
[0002] Ultra-high molecular weight polyethylene (UHMWPE) possesses high impact resistance, abrasion resistance, self-lubrication, and chemical corrosion resistance, making it well-suited for applications in guide rails, sliders, rollers, supports, and other engineering components with relative motion or frictional contact. However, UHMWPE is an electrically insulating material, prone to charge accumulation during friction, sliding, or continuous contact. When applied to electrostatically sensitive working environments, relying solely on the material's inherent properties makes it difficult to simultaneously meet both abrasion resistance and electrostatic dissipation requirements.
[0003] Current antistatic modification of UHMWPE typically involves adding conductive fillers such as carbon black, carbon nanomaterials, metals, or conductive ceramics to the polymer, forming charge transport paths through the contact between the fillers. However, UHMWPE melt viscosity is high, and fillers are prone to uneven dispersion or local agglomeration during processing. When the amount of conductive filler added is too low, it is difficult to establish effective contact between adjacent conductive particles, while excessive addition may adversely affect the mechanical properties, tribological properties, and processability of the matrix material. Furthermore, under long-term friction conditions, functional particles may migrate, detach, or redistribute, leading to a decrease in the stability of conductivity and wear resistance.
[0004] To improve the tribological properties of UHMWPE, layered solid lubricants such as MoS2 can be added to reduce frictional resistance, while radiation crosslinking can enhance the material's structural stability and wear resistance. To meet electrostatic dissipation requirements, conductive fillers are typically introduced. While the addition of different functional components can improve their respective properties, their dispersion state, interfacial bonding, and stability during use directly affect the overall performance of the composite material. Therefore, current technologies still need to further address the challenge of simultaneously achieving structural stability, processability, and long-term performance in the conductive and wear-resistant modification of UHMWPE. Summary of the Invention
[0005] The technical problem to be solved: This invention addresses the difficulty in simultaneously achieving structural stability, processability, and long-term performance during the conductive and wear-resistant modification of UHMWPE. It utilizes irradiated crosslinked UHMWPE carrier particles, sheet-like MoS2, and Y2O3-loaded antimony-doped SnO2 conductive phase to construct composite functional particles, which are then mixed with UHMWPE powder and pressed and sintered. This reduces frictional resistance and triboelectric tendency while providing pathways for charge transport and dissipation, improving the dispersion and interfacial stability of the functional phases, thereby enhancing both wear resistance and electrostatic dissipation performance.
[0006] Technical solution: A conductive and wear-resistant ultra-high molecular weight polyethylene composite material, comprising a continuous matrix formed of ultra-high molecular weight polyethylene and composite functional particles dispersed in the continuous matrix; the composite functional particles include irradiated cross-linked ultra-high molecular weight polyethylene carrier particles, sheet-like MoS2 and conductive ceramic particles, wherein the conductive ceramic particles include Y2O3 particles and an antimony-doped SnO2 conductive phase formed on the surface of the Y2O3 particles.
[0007] The preparation method of the above-mentioned conductive and wear-resistant ultra-high molecular weight polyethylene composite material includes the following steps: S1. The ultra-high molecular weight polyethylene powder is sprayed with the irradiation sensitizer while stirring. After mixing evenly, the mixture is vacuum sealed and then treated with γ-ray irradiation. The irradiated ultra-high molecular weight polyethylene powder is then vacuum annealed to obtain irradiated cross-linked ultra-high molecular weight polyethylene carrier particles. S2. The irradiated cross-linked ultra-high molecular weight polyethylene carrier particles are subjected to oxygen plasma treatment, followed by a first stirring treatment with sheet-like MoS2, and then conductive ceramic particles are added for a second stirring treatment to obtain composite functional particles. S3. Mix the composite functional particles with ultra-high molecular weight polyethylene powder at low speed to obtain composite powder; S4. The composite powder is pressed and sintered to form a continuous matrix of ultra-high molecular weight polyethylene powder, thereby obtaining a conductive and wear-resistant ultra-high molecular weight polyethylene composite material.
[0008] Preferably, in step S1, the irradiation sensitizer is one or more of trimethylolpropane trimethacrylate, trimethylolpropane triacrylate, or triallyl isocyanurate, the amount of irradiation sensitizer added is 1-8% of the mass of ultra-high molecular weight polyethylene powder, the irradiated absorbed dose is 10-50 kGy, and the temperature of the vacuum annealing treatment is 80-120°C, and the time is 2-8 h.
[0009] Preferably, in step S2, the oxygen plasma treatment power is 100~200W, the time is 40~90s, the first stirring speed is 2500~4500 r / min, the second stirring speed is 1000~2000 r / min, and the mass ratio of the irradiated crosslinked ultra-high molecular weight polyethylene carrier particles, MoS2 and conductive ceramic particles is 100:(2~10):(20~50).
[0010] Preferably, in step S3, based on the total mass of the composite powder, the mass fraction of the composite functional particles is 30-40 parts, the mass fraction of the ultra-high molecular weight polyethylene powder is 60-80 parts, the speed of the low-speed stirring is 50-200 r / min, and the mixing time is 10-30 min.
[0011] Preferably, the pressing and sintering process in step S4 involves pre-pressing the composite powder at room temperature with a pressure of 5-10 MPa for 5-15 minutes, then heating it to 190-210°C and sintering it at a pressure of 8-15 MPa for 30-60 minutes. After sintering, the pressure is maintained and the temperature is cooled to below 80°C before demolding.
[0012] The preparation method of the above-mentioned conductive ceramic particles includes the following steps: S11. Disperse Y2O3 particles in water to obtain a Y2O3 aqueous dispersion with a mass fraction of 1~5wt%; S12. Under stirring conditions, tin-containing precursors and antimony-containing precursors are added to the Y2O3 aqueous dispersion, and ammonia is added to adjust the pH so that the hydrolysis products of tin and antimony co-precipitate on the Y2O3 surface to obtain the surface deposition precursor. S13. The surface deposition precursor is aged, separated into solid and liquid, washed, dried and calcined to convert the hydrolysis products of tin and antimony deposited on the Y2O3 surface into an antimony-doped SnO2 conductive phase, thus obtaining conductive ceramic particles.
[0013] Preferably, in step S12, the molar ratio of Sb in the antimony-containing precursor to Sn in the tin-containing precursor is 1:10 to 1:20, the tin-containing precursor is SnCl4·5H2O, the antimony-containing precursor is SbCl3 and / or SbCl5, the ammonia concentration is 5 to 15 wt%, the pH is adjusted to 8.0 to 9.0, and the co-precipitation temperature is 60 to 80°C.
[0014] Preferably, in step S13, the aging time is 1~4 h, the calcination temperature is 450~600℃, and the calcination time is 1~3 h.
[0015] Beneficial effects: The conductive and wear-resistant ultra-high molecular weight polyethylene composite material of the present invention has the following advantages: This invention first composites sheet-like MoS2 onto the surface of irradiated crosslinked UHMWPE carrier particles, then forms Y2O3 conductive ceramic particles with an antimony-doped SnO2 conductive phase on the composite surface. The sheet-like MoS2, with its layered and easily slipping properties, helps reduce frictional resistance and triboelectric tendency during material friction. The antimony-doped SnO2 conductive phase provides an electron transport path, conducting and dissipating the charge generated during friction. This invention works by simultaneously reducing static electricity generation and promoting static discharge, thus improving the electrostatic dissipation stability of the composite material.
[0016] This invention incorporates an irradiation sensitizer during the irradiation of UHMWPE carrier particles to enhance the effective cross-linking efficiency of macromolecular free radicals under gamma-ray irradiation. Gamma rays induce free radicals in the UHMWPE molecular chains, which further recombine to form a cross-linked structure. Vacuum annealing promotes further reaction of residual free radicals and reduces the influence of oxidation side reactions, thereby forming a more stable cross-linked network and improving the hardness, deformation resistance, and wear resistance of the carrier particles. The flake-like MoS2 further enhances friction reduction and lubrication. Oxygen plasma treatment improves the surface activity of the carrier particles, and a two-stage mechanical composite process sequentially bonds MoS2 and conductive ceramic particles to the surface of the carrier particles. This enhances the bonding stability between the functional phase and the carrier particles, reducing the tendency for functional particles to agglomerate, migrate, or detach during subsequent mixing, sintering, and friction use, thus helping to maintain the long-term wear resistance and conductivity of the composite material.
[0017] This invention first constructs a functional structure on the surface of irradiated cross-linked ultra-high molecular weight polyethylene carrier particles, comprising a composite distribution of MoS2 and conductive ceramic particles. Then, the resulting composite functional particles are dispersed in a continuous matrix. Y2O3 serves as the inorganic carrier for the antimony-doped SnO2 conductive phase, causing the conductive phase to concentrate on the surface of the ceramic particles. This structure helps reduce the disordered agglomeration of fine functional particles, improves the effective utilization of the conductive phase in the composite material, and increases the possibility of establishing conductive contacts between adjacent conductive ceramic particles, thereby balancing material structural uniformity, wear resistance, and electrostatic dissipation performance. Detailed Implementation
[0018] The present invention will be further described below with reference to embodiments. These embodiments are illustrative of the present invention, but the present invention is not limited to these embodiments: The ultra-high molecular weight polyethylene powder used in the embodiments and comparative examples of this invention is UHMWPE-M400 powder produced by Lianhong New Material Technology Co., Ltd., with a molecular weight of approximately 4.0 × 10⁻⁶. 6g / mol; Y2O3 particles are Y2O3-500 type yttrium oxide powder produced by Bohuas Nanotechnology Co., Ltd., with an average particle size of 500~600 nm; plate-like MoS2 is MoS2-WO5 type molybdenum disulfide powder produced by Bohuas Nanotechnology Co., Ltd., with an average particle size of about 5 μm.
[0019] Example 1
[0020] A method for preparing a conductive and wear-resistant ultra-high molecular weight polyethylene composite material includes the following steps: S1. 10g of Y2O3 particles were ultrasonically dispersed in water to obtain a Y2O3 aqueous dispersion with a mass fraction of 1wt%. S2. Under stirring conditions, 4.65 g SnCl4·5H2O and 0.3 g SbCl3 were added to the Y2O3 aqueous dispersion, and 5 wt% ammonia was added to adjust the pH to 8.0. The reaction was carried out at 60 °C for 2 h to allow the hydrolysis products of tin and antimony to co-precipitate on the Y2O3 surface, thus obtaining the surface deposition precursor. S3. The surface deposition precursor is aged for 1 hour, then solid-liquid separation, washing, drying at 100℃ for 6 hours, and finally calcined at 450℃ for 1 hour to convert the hydrolysis products of tin and antimony deposited on the Y2O3 surface into antimony-doped SnO2 conductive phase, thus obtaining conductive ceramic particles. S4. Take 1000g of UHMWPE powder and place it in a high-speed mixer. Add 10g of trimethylolpropane trimethacrylate by spraying while stirring. After mixing evenly, vacuum seal the mixture and irradiate it with Co-60 γ-rays at a dose rate of 0.5 kGy / h for 20h. The total absorbed dose is 10kGy. After irradiation, anneal the powder in a vacuum oven at 80℃ for 2h to obtain irradiated crosslinked UHMWPE carrier particles. S5. The irradiated crosslinked UHMWPE carrier particles were subjected to oxygen plasma treatment at a power of 100W for 40s. Then, 100 parts by mass of the treated carrier particles and 2 parts by mass of MoS2 were taken and stirred at 2500 r / min for 15min. Subsequently, 20 parts by mass of conductive ceramic particles were added and stirred at 1000 r / min for 5min to obtain composite functional particles. S6. Take 30 parts by weight of composite functional particles and 70 parts by weight of UHMWPE powder and mix them at low speed of 50 r / min for 10 min to obtain composite powder. S7. Place the composite powder into a mold, pre-press it at 5 MPa for 5 minutes at room temperature, then heat it to 190°C and sinter it at 8 MPa for 30 minutes. After sintering, keep the pressure and cool it to below 80°C before demolding to obtain a conductive and wear-resistant ultra-high molecular weight polyethylene composite material.
[0021] Example 2
[0022] A method for preparing a conductive and wear-resistant ultra-high molecular weight polyethylene composite material includes the following steps: S1. 10g of Y2O3 particles were ultrasonically dispersed in water to obtain a Y2O3 aqueous dispersion with a mass fraction of 5wt%. S2. Under stirring conditions, 4.65 g SnCl4·5H2O and 0.2 g SbCl3 were added to the Y2O3 aqueous dispersion, and 15 wt% ammonia was added to adjust the pH to 9.0. The reaction was carried out at 80 °C for 2 h to allow the hydrolysis products of tin and antimony to co-precipitate on the Y2O3 surface, thus obtaining the surface deposition precursor. S3. The surface-deposited precursor was aged for 4 hours, then solid-liquid separation, washing, drying at 100℃ for 6 hours, and finally calcined at 600℃ for 3 hours to convert the hydrolysis products of tin and antimony deposited on the Y2O3 surface into antimony-doped SnO2 conductive phase, thus obtaining conductive ceramic particles. S4. Take 1000g of UHMWPE powder and place it in a high-speed mixer. Add 80g of trimethylolpropane trimethacrylate by spraying while stirring. After mixing evenly, vacuum seal the mixture and irradiate it with Co-60 γ-rays at a dose rate of 0.5 kGy / h for 80h. The total absorbed dose is 40kGy. After irradiation, anneal the powder in a vacuum oven at 120℃ for 8h to obtain irradiated crosslinked UHMWPE carrier particles. S5. The irradiated crosslinked UHMWPE carrier particles were subjected to oxygen plasma treatment at a power of 200W for 90s. Then, 100 parts by mass of the treated carrier particles and 10 parts by mass of MoS2 were mixed and stirred at 4500 r / min for 30min. Subsequently, 50 parts by mass of conductive ceramic particles were added and stirred at 2000 r / min for 20min to obtain composite functional particles. S6. Take 40 parts by weight of composite functional particles and 60 parts by weight of UHMWPE powder and mix them at low speed of 200 r / min for 30 min to obtain composite powder; S7. Place the composite powder into a mold, pre-press it at 10 MPa for 15 minutes at room temperature, then heat it to 210°C and sinter it at 15 MPa for 60 minutes. After sintering, keep the pressure and cool it to below 80°C before demolding to obtain a conductive and wear-resistant ultra-high molecular weight polyethylene composite material.
[0023] Example 3
[0024] A method for preparing a conductive and wear-resistant ultra-high molecular weight polyethylene composite material includes the following steps: S1. 10g of Y2O3 particles were ultrasonically dispersed in water to obtain a Y2O3 aqueous dispersion with a mass fraction of 3wt%. S2. Under stirring conditions, 4.65 g SnCl4·5H2O and 0.20 g SbCl3 were added to the Y2O3 aqueous dispersion, and 10 wt% ammonia was added to adjust the pH to 8.5. The reaction was carried out at 70 °C for 2 h to allow the hydrolysis products of tin and antimony to co-precipitate on the Y2O3 surface, thus obtaining the surface deposition precursor. S3. The surface deposition precursor is aged for 2 hours, then solid-liquid separation, washing, drying at 100℃ for 6 hours, and finally calcined at 550℃ for 2 hours to convert the hydrolysis products of tin and antimony deposited on the Y2O3 surface into antimony-doped SnO2 conductive phase, thus obtaining conductive ceramic particles. S4. Take 1000g of UHMWPE powder and place it in a high-speed mixer. Add 30g of trimethylolpropane trimethacrylate by spraying while stirring. After mixing evenly, vacuum seal the mixture and irradiate it with Co-60 γ-rays at a dose rate of 0.5 kGy / h for 60h. The total absorbed dose is 30kGy. After irradiation, anneal the powder in a vacuum oven at 100℃ for 4h to obtain irradiated crosslinked UHMWPE carrier particles. S5. The irradiated crosslinked UHMWPE carrier particles were subjected to oxygen plasma treatment at a power of 150W for 60s. Then, 100 parts by mass of the treated carrier particles and 5 parts by mass of MoS2 were mixed and stirred at 3500 r / min for 20min. Subsequently, 30 parts by mass of conductive ceramic particles were added and stirred at 1500 r / min for 10min to obtain composite functional particles. S6. Take 35 parts by weight of composite functional particles and 65 parts by weight of UHMWPE powder and mix them at low speed of 100 r / min for 20 min to obtain composite powder. S7. Place the composite powder into a mold, pre-press it at 8MPa for 10 minutes at room temperature, then heat it to 200℃ and sinter it at 10MPa for 45 minutes. After sintering, keep the pressure and cool it to below 80℃ before demolding to obtain a conductive and wear-resistant ultra-high molecular weight polyethylene composite material.
[0025] Example 4
[0026] A method for preparing a conductive and wear-resistant ultra-high molecular weight polyethylene composite material includes the following steps: S1. 10g of Y2O3 particles were ultrasonically dispersed in water to obtain a Y2O3 aqueous dispersion with a mass fraction of 2wt%. S2. Under stirring conditions, 4.65 g SnCl4·5H2O and 0.25 g SbCl3 were added to the Y2O3 aqueous dispersion, and 10 wt% ammonia was added to adjust the pH to 8.2. The reaction was carried out at 65 °C for 2 h to allow the hydrolysis products of tin and antimony to co-precipitate on the Y2O3 surface, thus obtaining the surface deposition precursor. S3. The surface deposition precursor is aged for 1.5 h, then solid-liquid separation, washing, drying at 100 °C for 6 h, and finally calcined at 500 °C for 1.5 h to convert the hydrolysis products of tin and antimony deposited on the Y2O3 surface into antimony-doped SnO2 conductive phase, thus obtaining conductive ceramic particles. S4. Take 1000g of UHMWPE powder and place it in a high-speed mixer. Add 50g of trimethylolpropane trimethacrylate by spraying while stirring. After mixing evenly, vacuum seal the mixture and irradiate it with Co-60 γ-rays at a dose rate of 1.0 kGy / h for 40h. The total absorbed dose is 40kGy. After irradiation, anneal the powder in a vacuum oven at 90℃ for 6h to obtain irradiated crosslinked UHMWPE carrier particles. S5. The irradiated crosslinked UHMWPE carrier particles were subjected to oxygen plasma treatment at a power of 120W for 50s. Then, 100 parts by mass of the treated carrier particles and 3 parts by mass of MoS2 were mixed and stirred at 3000 r / min for 20min. Subsequently, 25 parts by mass of conductive ceramic particles were added and stirred at 1200 r / min for 10min to obtain composite functional particles. S6. Take 32 parts by weight of composite functional particles and 68 parts by weight of UHMWPE powder and mix them at low speed of 80 r / min for 15 min to obtain composite powder. S7. Place the composite powder into a mold, pre-press it at 6MPa for 8 minutes at room temperature, then heat it to 195℃ and sinter it at 9MPa for 40 minutes. After sintering, keep the pressure and cool it to below 80℃ before demolding to obtain a conductive and wear-resistant ultra-high molecular weight polyethylene composite material.
[0027] Example 5
[0028] A method for preparing a conductive and wear-resistant ultra-high molecular weight polyethylene composite material includes the following steps: S1. 10g of Y2O3 particles were ultrasonically dispersed in water to obtain a Y2O3 aqueous dispersion with a mass fraction of 4wt%. S2. Under stirring conditions, 4.65 g SnCl4·5H2O and 0.17 g SbCl3 were added to the Y2O3 aqueous dispersion, and 12 wt% ammonia was added to adjust the pH to 8.8. The reaction was carried out at 75 °C for 2 h to allow the hydrolysis products of tin and antimony to co-precipitate on the Y2O3 surface, thus obtaining the surface deposition precursor. S3. The surface-deposited precursor is aged for 3 hours, then solid-liquid separation, washing, drying at 100℃ for 6 hours, and finally calcined at 580℃ for 2.5 hours to convert the hydrolysis products of tin and antimony deposited on the Y2O3 surface into antimony-doped SnO2 conductive phase, thus obtaining conductive ceramic particles. S4. Take 1000g of UHMWPE powder and place it in a high-speed mixer. Add 60g of trimethylolpropane trimethacrylate by spraying while stirring. After mixing evenly, vacuum seal the mixture and irradiate it with Co-60 γ-rays at a dose rate of 1.0 kGy / h for 45h. The total absorbed dose is 45kGy. After irradiation, anneal the powder in a vacuum oven at 110℃ for 7h to obtain irradiated crosslinked UHMWPE carrier particles. S5. The irradiated crosslinked UHMWPE carrier particles were subjected to oxygen plasma treatment at a power of 180W for 80s. Then, 100 parts by mass of the treated carrier particles and 8 parts by mass of MoS2 were mixed and stirred at 4000 r / min for 25min. Subsequently, 40 parts by mass of conductive ceramic particles were added and stirred at 1800 r / min for 15min to obtain composite functional particles. S6. Take 38 parts by weight of composite functional particles and 62 parts by weight of UHMWPE powder and mix them at low speed of 150 r / min for 25 min to obtain composite powder. S7. Place the composite powder into a mold, pre-press it at 9 MPa for 12 minutes at room temperature, then heat it to 205°C and sinter it at 12 MPa for 50 minutes. After sintering, keep the pressure and cool it to below 80°C before demolding to obtain a conductive and wear-resistant ultra-high molecular weight polyethylene composite material.
[0029] Comparative Example 1 The difference between Comparative Example 1 and Example 3 is that hydroxymethylpropane trimethacrylate is not added in step S4, that is, the amount of irradiation sensitizer added is 0, and the remaining steps are the same as in Example 3.
[0030] Comparative Example 2 The difference between Comparative Example 2 and Example 3 is that vacuum annealing is not performed after irradiation treatment in step S4, while the remaining steps are the same as in Example 3.
[0031] Comparative Example 3 The difference between Comparative Example 3 and Example 3 is that in step S5, the irradiated crosslinked UHMWPE carrier particles are not subjected to oxygen plasma treatment, and subsequent stirring is carried out directly. The remaining steps are the same as in Example 3.
[0032] Comparative Example 4 The difference between Comparative Example 4 and Example 3 is that: in step S5, no flake MoS2 is added, and only 100 parts by mass of carrier particles and 30 parts by mass of conductive ceramic particles are stirred to obtain composite functional particles. The remaining steps are the same as in Example 3.
[0033] Comparative Example 5 The difference between Comparative Example 5 and Example 3 is that conductive ceramic particles are not added in step S5. Instead, 100 parts by mass of carrier particles and 5 parts by mass of flake MoS2 are subjected to a first stirring treatment to obtain composite functional particles. The remaining steps are the same as in Example 3.
[0034] Comparative Example 6 The difference between Comparative Example 6 and Example 3 is that Y2O3 particles are not added, and pure antimony-doped SnO2 particles are directly prepared as conductive ceramic particles. The remaining steps are the same as in Example 3. The preparation method of pure antimony-doped SnO2 particles includes the following steps: S1. Take 4.65 g SnCl4·5H2O and 0.20 g SbCl3, dissolve them in 100 mL of deionized water, stir until completely dissolved, and add 10 wt% ammonia water dropwise to the mixed solution under stirring to adjust the pH of the system to 8.5. React at 70℃ for 2 h to obtain fine pure antimony-doped SnO2 particle precursor precipitate. S2. The obtained precipitate was aged for 2 h, then subjected to solid-liquid separation, washing, drying at 100℃ for 6 h, and finally calcined at 550℃ for 2 h to obtain a pure antimony-doped SnO2 conductive phase.
[0035] Comparative Example 7 The difference between Comparative Example 7 and Example 3 is that the UHMWPE powder is not irradiated in step S4, while the remaining steps are the same as in Example 3.
[0036] Comparative Example 8 The difference between Comparative Example 8 and Example 3 is that in step S6, 50 parts by mass of composite functional particles are mixed with 50 parts by mass of UHMWPE powder to obtain composite powder, and the remaining steps are the same as in Example 3.
[0037] Testing: Surface resistivity was measured according to GB / T 31838.3-2019 using a three-electrode system and a high-resistivity meter. The measuring electrode diameter was 50±0.1 mm, and the inner diameter of the annular electrode was 63.5±0.1 mm. A DC voltage of 100±5 V was applied, and a stable value was read after 60±5 s. Electrostatic decay performance was tested under the conditions of 23±3℃ and 12±3% RH. An initial voltage of +5000 V was applied to the sample, and the time required for the voltage to decay to 500 V was recorded as the electrostatic decay time. The sample was worn using a pin-disc friction and wear tester. Before the test, the composite material sample was polished to a surface roughness Ra of 0.5 μm. The test parameters were: normal load 5 N, sliding linear velocity 0.2 m / s, and test time 15 seconds. After the wear test, the mass loss Δm of the sample before and after wear was measured using an electronic balance with an accuracy of ±0.001mg. The wear volume V=Δm / ρ was converted according to the density ρ of the composite material. The specific wear rate was calculated according to the formula K=V / (F·S), where F is the normal load (N) and S is the total sliding distance (m). The surface resistivity was measured before and after wear, and the resistivity change rate ΔR=(R1-R0) / R0×100% was calculated. The tensile strength and elongation at break were measured on a universal testing machine using a type 1A dumbbell-shaped sample according to GB / T 1040.2-2022. The test speed was 50 mm / min and the test temperature was 23±2℃.
[0038] Table 1 Conductivity and Static Dissipation Properties
[0039] As can be seen from Table 1, the embodiments generally exhibit low surface resistivity, fast electrostatic decay rate, and small resistance change before and after wear. In this invention, the antimony-doped SnO2 conductive phase formed on the surface of Y2O3 particles can establish an electron transport pathway inside the composite material, enabling the charge generated by friction to be discharged in a timely manner. The lamellar MoS2 utilizes its layered slip properties to reduce frictional resistance and triboelectric tendency. At the same time, Y2O3, as a conductive phase carrier, helps to reduce the disordered agglomeration of fine conductive phases. The irradiated crosslinked UHMWPE carrier particles have good deformation resistance and wear resistance stability. Combined with oxygen plasma treatment and two-stage mechanical composite, the bonding between MoS2 and conductive ceramic particles and the carrier can be enhanced, so that the conductive structure can still be well maintained after friction.
[0040] Comparative Example 1, without the addition of an irradiation sensitizer, showed reduced effective cross-linking efficiency of UHMWPE free radicals under γ-ray irradiation, resulting in insufficient cross-linking structure and deformation resistance of the carrier particles. Therefore, although the initial conductive phase remained, the conductive network was more easily disturbed after friction, exhibiting poor conductivity stability. Comparative Example 2, omitting vacuum annealing, resulted in insufficient subsequent reaction and stabilization of residual free radicals after irradiation. The material was more susceptible to oxidation side reactions during subsequent processing and use, leading to decreased functional structure stability and more pronounced resistance changes after wear. Comparative Example 3, without oxygen plasma treatment, showed reduced efficiency of UHMWPE carrier particles. The surface activity of the bulk material is low, and the functional phase is more likely to detach, migrate, or redistribute during mechanical recombination and friction, resulting in a decrease in the continuity of the conductive pathway. Comparative Example 4, without the addition of MoS2, retains the antimony-doped SnO2 conductive phase, but loses the friction-reducing effect of MoS2 and its auxiliary support and anchoring effect on the conductive ceramic particles. This increases the tendency for triboelectric charging and functional particle rearrangement, thus reducing the stability of conductivity after wear. Comparative Example 5, without the addition of conductive ceramic particles, lacks the antimony-doped SnO2 as the main conductive phase, making it impossible to form an effective electron transport network. Therefore, the surface resistance increases significantly, and electrostatic decay energy decreases. The resistance was significantly weakened. Comparative Example 6 directly used pure antimony-doped SnO2 particles, and the initial conductivity remained at a good level. However, without Y2O3 as a relatively stable inorganic support, the conductive phase was more prone to agglomeration, migration, and local detachment, leading to a significant increase in resistance after friction. Comparative Example 7 did not perform irradiation crosslinking on the UHMWPE support. The support particles lacked a stable crosslinking network, making them more prone to deformation and structural rearrangement during sintering and friction. This caused changes in the positions of the MoS2 and conductive ceramic particles attached to its surface, thereby disrupting the original conductive contact relationship and reducing the initial electrostatic dissipation capacity and the resistance after wear. Electrical stability decreased significantly. In Comparative Example 8, increasing the content of composite functional particles increased the number of conductive phases, which further improved the initial conductivity and electrostatic decay performance. However, excessive functional particles weakened the integrity of the UHMWPE continuous matrix and increased particle agglomeration and interface defects, making the conductive network more easily destroyed during friction and reducing the resistance stability after wear. This indicates that the present invention does not rely solely on increasing the content of conductive filler to obtain performance, but rather achieves the coordination of electrostatic dissipation performance and long-term conductivity stability through irradiated crosslinking carrier, MoS2, Y2O3-loaded antimony-doped SnO2, and appropriate composite ratio.
[0041] Table 2 Wear and Mechanical Properties
[0042] As can be seen from Table 2, all embodiments exhibit good overall wear resistance, along with good tensile strength and elongation at break. The network structure formed by irradiation crosslinking in this invention is beneficial for improving the hardness and deformation resistance of the carrier particles. The plate-like MoS2 reduces frictional shear due to its easy interlayer slippage characteristics, while the Y2O3 carrier helps improve the dispersion stability of the conductive phase and reduce local agglomeration.
[0043] Comparative Example 1, lacking an irradiation sensitizer, suffered from reduced effective cross-linking and insufficient resistance to deformation of the carrier, resulting in decreased wear resistance. Comparative Example 2, without vacuum annealing, exhibited insufficient residual free radicals and cross-linked structural stability after irradiation, impacting wear and mechanical properties. Comparative Example 3, without oxygen plasma treatment, showed weak bonding between functional particles and the carrier, leading to easy detachment and interfacial failure. Comparative Example 4, without MoS2, lost its layered solid lubrication effect, significantly increasing friction, shear, and wear. Comparative Example 5, without conductive ceramics, retained cross-linked UHM... WPE and MoS2, therefore, still have good wear resistance and mechanical properties, but cannot take into account the function of electrostatic dissipation; Comparative Example 6 directly uses pure antimony-doped SnO2, and the fine particles are more likely to agglomerate and form stress concentration, resulting in a decrease in mechanical and wear resistance; Comparative Example 7 does not undergo radiation crosslinking, and although the molecular chain has greater mobility, the carrier hardness and resistance to plastic deformation are insufficient, thus aggravating wear; Comparative Example 8 has too high a content of functional particles, which weakens the integrity of the continuous UHMWPE matrix and increases agglomeration and interface defects, thereby reducing mechanical and wear resistance.
[0044] Obviously, the above embodiments are merely illustrative examples for clear explanation and are not intended to limit the implementation. Those skilled in the art will recognize that other variations or modifications can be made based on the above description. It is neither necessary nor possible to exhaustively list all possible implementations here. However, obvious variations or modifications derived therefrom are still within the scope of protection of this invention.
Claims
1. A conductive and wear-resistant ultra-high molecular weight polyethylene composite material, characterized in that, The invention comprises a continuous matrix formed of ultra-high molecular weight polyethylene and composite functional particles dispersed in the continuous matrix; the composite functional particles include irradiated cross-linked ultra-high molecular weight polyethylene carrier particles, sheet-like MoS2 and conductive ceramic particles, wherein the conductive ceramic particles include Y2O3 particles and an antimony-doped SnO2 conductive phase formed on the surface of the Y2O3 particles.
2. The method for preparing the conductive and wear-resistant ultra-high molecular weight polyethylene composite material according to claim 1, characterized in that, Includes the following steps: S1. The ultra-high molecular weight polyethylene powder is sprayed with the irradiation sensitizer while stirring. After mixing evenly, the mixture is vacuum sealed and then treated with γ-ray irradiation. The irradiated ultra-high molecular weight polyethylene powder is then vacuum annealed to obtain irradiated cross-linked ultra-high molecular weight polyethylene carrier particles. S2. The irradiated cross-linked ultra-high molecular weight polyethylene carrier particles are subjected to oxygen plasma treatment, followed by a first stirring treatment with sheet-like MoS2, and then conductive ceramic particles are added for a second stirring treatment to obtain composite functional particles. S3. Mix the composite functional particles with ultra-high molecular weight polyethylene powder at low speed to obtain composite powder; S4. The composite powder is pressed and sintered to form a continuous matrix of ultra-high molecular weight polyethylene powder, thereby obtaining a conductive and wear-resistant ultra-high molecular weight polyethylene composite material.
3. The preparation method according to claim 2, characterized in that, In step S1, the irradiation sensitizer is one or more of trimethylolpropane trimethacrylate, trimethylolpropane triacrylate, or triallyl isocyanurate. The amount of irradiation sensitizer added is 1-8% of the mass of ultra-high molecular weight polyethylene powder, the irradiated absorbed dose is 10-50 kGy, and the vacuum annealing treatment is performed at a temperature of 80-120°C for 2-8 hours.
4. The preparation method according to claim 2, characterized in that, In step S2, the oxygen plasma treatment power is 100~200W and the time is 40~90s. The first stirring treatment speed is 2500~4500 r / min and the second stirring treatment speed is 1000~2000 r / min. The mass ratio of the irradiated crosslinked ultra-high molecular weight polyethylene carrier particles, MoS2 and conductive ceramic particles is 100:(2~10):(20~50).
5. The preparation method according to claim 2, characterized in that, In step S3, the composite functional particles have a mass fraction of 30-40 parts, the ultra-high molecular weight polyethylene powder has a mass fraction of 60-80 parts, the low-speed stirring speed is 50-200 r / min, and the mixing time is 10-30 min.
6. The preparation method according to claim 2, characterized in that, The pressing and sintering process in step S4 involves pre-pressing the composite powder at room temperature with a pressure of 5-10 MPa for 5-15 minutes, then heating it to 190-210°C and sintering it at a pressure of 8-15 MPa for 30-60 minutes. After sintering, the pressure is maintained and the temperature is cooled to below 80°C before demolding.
7. The preparation method according to claim 2, characterized in that, The method for preparing the conductive ceramic particles includes the following steps: S11. Disperse Y2O3 particles in water to obtain a Y2O3 aqueous dispersion with a mass fraction of 1~5wt%; S12. Under stirring conditions, tin-containing precursors and antimony-containing precursors are added to the Y2O3 aqueous dispersion, and ammonia is added to adjust the pH so that the hydrolysis products of tin and antimony co-precipitate on the Y2O3 surface to obtain the surface deposition precursor. S13. The surface deposition precursor is aged, separated into solid and liquid, washed, dried and calcined to convert the hydrolysis products of tin and antimony deposited on the Y2O3 surface into an antimony-doped SnO2 conductive phase, thus obtaining conductive ceramic particles.
8. The preparation method according to claim 7, characterized in that, In step S12, the molar ratio of Sb in the antimony-containing precursor to Sn in the tin-containing precursor is 1:10 to 1:
20. The tin-containing precursor is SnCl4·5H2O, and the antimony-containing precursor is SbCl3 and / or SbCl5. The ammonia concentration is 5 to 15 wt%, the pH is adjusted to 8.0 to 9.0, and the co-precipitation temperature is 60 to 80℃.
9. The preparation method according to claim 7, characterized in that, In step S13, the aging time is 1-4 h, the calcination temperature is 450-600℃, and the calcination time is 1-3 h.