An ant termite polyolefin cable sheath material and a preparation method thereof
By using a microencapsulated termite repellent and a secondary dispersion process with masterbatch, the problem of volatilization and decomposition of the termite repellent during high-temperature processing was solved. This achieved a balance between long-lasting slow release of the termite repellent and halogen-free flame retardant properties, thus improving the termite repellency and mechanical properties of cable sheathing materials.
Patent Information
- Application Number
- CN202611605617.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-16
- Publication Date
- 2026-11-24
AI Technical Summary
Existing anti-termite cable materials are prone to volatile decomposition of anti-termite agents during high-temperature processing, and their migration rate is fast during service life. Furthermore, the anti-termite agents in halogen-free flame retardant systems have poor dispersibility, making it difficult to balance anti-termite effect with mechanical properties.
The process employs a microencapsulated ant repellent and a masterbatch secondary dispersion process. The core is made by combining pyrethroids with natural plant extracts. The polymer capsule wall isolates the ant repellent at high temperatures, and the process achieves low-loss processing and long-lasting sustained release of the ant repellent in a halogen-free flame-retardant polyolefin system.
It effectively reduces the toxicity load of termite repellents, improves the retention rate and service life of termite repellents, enhances termite repellency, and balances halogen-free flame retardant properties with mechanical properties.
Smart Images

Figure CN123152199A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of wire and cable materials technology, specifically to an anti-ant polyolefin cable sheath material, its preparation method, and its application. Background Technology
[0002] With the acceleration of urbanization, power and communication lines are increasingly being laid underground. In areas with high termite infestations, faults caused by termite damage to cable sheaths are frequent and persistent, making termite-resistant cable materials an important functional material in the wire and cable industry.
[0003] Chemical termite control is currently the mainstream technical approach. Early organochlorine insecticides such as chlordane, lindane, and methyl parathion were banned due to their high toxicity and long residual period. Subsequently, low-toxicity termite repellents, represented by pyrethroids, were developed. However, existing technologies still have the following shortcomings: First, most methods directly incorporate termite repellents into the matrix in a free state. At extrusion processing temperatures around 180℃, the active ingredients of pyrethroids are prone to volatilization and decomposition, resulting in a low actual retention rate. Second, free-state termite repellents migrate rapidly during their service life, leading to a short termite-repellent effectiveness. Third, the polyvinyl chloride (PVC) system does not conform to the trend of halogen-free development, and in existing halogen-free flame-retardant polyolefin systems, the termite repellent exhibits poor dispersibility and interfacial compatibility when blended with a large amount of inorganic flame-retardant fillers, making it difficult to simultaneously achieve both mechanical and termite-repellent performance. Fourth, while simply increasing the amount of pyrethroids can enhance short-term efficacy, it contradicts environmental friendliness goals. Therefore, it is of great significance to develop a polyolefin sheath material that is low in toxicity and environmentally friendly, has stable processing, is long-lasting in terms of termite prevention, and also has halogen-free flame retardant properties. Summary of the Invention
[0004] To address the aforementioned shortcomings of existing technologies, the present invention aims to provide an anti-termite polyolefin cable sheath material and its preparation method. By combining the microencapsulation of the anti-termite agent with a secondary dispersion process of the masterbatch, the anti-termite agent achieves low-loss processing and long-term sustained release in a halogen-free flame-retardant polyolefin system.
[0005] According to one aspect of the present invention, an anti-termite polyolefin cable sheath material is provided, comprising the following components by weight: 100 parts of polyolefin base material, wherein the polyolefin base material is at least two selected from high-density polyethylene, linear low-density polyethylene, ethylene-vinyl acetate copolymer, and ethylene-octene copolymer; 2-8 parts of microencapsulated anti-termite agent, wherein the microencapsulated anti-termite agent has a core of a compound of pyrethroids and natural plant extracts and a wall polymer; 40-80 parts of halogen-free flame retardant, wherein the halogen-free flame retardant is a mixture of surface-treated aluminum hydroxide and magnesium hydroxide, wherein the mass ratio of aluminum hydroxide to magnesium hydroxide is 2:1 to 1:2; 3-8 parts of synergistic flame retardant; 4-12 parts of compatibilizer; 0.3-1.0 parts of antioxidant; 0.5-2.0 parts of lubricant; and 0.2-0.8 parts of light stabilizer.
[0006] In some embodiments, the natural plant extract is at least one of azadirachtin, matrine, pyrethrin, and eugenol; the pyrethroid is at least one of bifenthrin, permethrin, and lambda-cyhalothrin; and the mass ratio of the two is 1:5 to 1:1.
[0007] In some embodiments, the wall material polymer is melamine resin, urea-formaldehyde resin, or chitosan-gelatin composite; the microencapsulated ant repellent has a particle size of 1 μm to 20 μm and a core-to-wall mass ratio of 1:0.5 to 1:2.
[0008] In some embodiments, the halogen-free flame retardant is surface-treated with a silane coupling agent or stearic acid; the synergistic flame retardant is at least one of zinc borate and microencapsulated red phosphorus.
[0009] In some embodiments, the sheath material further includes 5 to 15 parts of hollow glass microspheres, the surface of which is treated with a silane coupling agent.
[0010] In some embodiments, the polyolefin base material is composed of 30-50 parts of high-density polyethylene, 25-45 parts of linear low-density polyethylene, and 10-25 parts of ethylene-vinyl acetate copolymer; the compatibilizer is maleic anhydride-grafted polyethylene and / or maleic anhydride-grafted ethylene-vinyl acetate copolymer.
[0011] According to another aspect of the present invention, a method for preparing the above-mentioned environmentally friendly anti-termite polyolefin cable sheath material is also provided, comprising the following steps: S1. Core material compounding: Pyrethroids and natural plant extracts are mixed in a certain proportion to obtain a composite core material; S2. Microencapsulation: When the wall material polymer is melamine resin or urea-formaldehyde resin, an in-situ polymerization method is used: water is used as the continuous phase, an emulsifier is added to emulsify and disperse the composite core material, then the wall material prepolymer is added, and the temperature is raised to 60℃~85℃ for 1 h~4 h to cure. After filtration, washing, and drying, a microencapsulated termite repellent is obtained. When the wall material polymer is a chitosan-gelatin complex, a coagulation method is used: the emulsified core material emulsion is mixed with a gelatin aqueous solution, a chitosan aqueous solution is added, and the pH of the system is adjusted to 5.0~6.0 to allow the chitosan and gelatin to coagulate and coat the core material. After cross-linking curing, filtration, washing, and drying, a microencapsulated termite repellent is obtained. S3. Masterbatch preparation: Microencapsulated ant repellent, carrier resin, dispersant and antioxidant are mixed at high speed, and then melt-extruded and granulated by a twin-screw extruder to obtain ant repellent masterbatch; the carrier resin is linear low-density polyethylene and / or ethylene-vinyl acetate copolymer; S4. Co-extrusion: The termite-resistant masterbatch is mixed with polyolefin base material, halogen-free flame retardant, synergistic flame retardant, compatibilizer, antioxidant, lubricant and light stabilizer, and then added to a twin-screw extruder for melt blending and granulation to obtain the environmentally friendly termite-resistant polyolefin cable sheath material; the barrel temperature of the twin-screw extruder is 140℃~190℃.
[0012] Preferably, the emulsifier in step S2 is sodium dodecyl sulfate or alkylphenol polyoxyethylene ether; the high-speed mixing in step S3 is performed at a speed of 500 r / min to 700 r / min, a temperature of 75℃ to 85℃, and a time of 8 min to 12 min.
[0013] This invention also protects the use of the above-mentioned termite-resistant polyolefin cable sheath material in the preparation of termite-resistant cable sheaths.
[0014] The beneficial effects of this invention are as follows: (1) The core is made of a combination of pyrethroids and natural plant extracts: Natural plant extracts (such as azadirachtin) have both repellent and feeding interference physiological activities, which synergize with pyrethroids. This can maintain the anti-ant effect while reducing the amount of pyrethroids used and reduce the toxicity load. (2) Microencapsulation solves the problem of processing loss: the capsule wall isolates the termite repellent from the high-temperature matrix during the melt processing stage, avoiding the loss of the termite repellent due to volatilization and decomposition at a processing temperature of about 180°C; during the service stage, the termite repellent is released slowly through the capsule wall, extending the shelf life; (3) Secondary dispersion process of masterbatch: First, the microencapsulated ant repellent is pre-dispersed in the carrier resin at a high concentration to obtain the masterbatch, and then it is mixed with the base material to avoid the ant repellent being subjected to high temperature shear for a long time in the main mixing process, while taking into account both the dispersion uniformity and the component retention rate. (4) Halogen-free flame retardant and termite prevention dual function integration: hydrated metal oxides with surface treatment are used as flame retardants, and zinc borate and other substances are used as synergists. The system burns with low smoke and no halogen. Surface treatment improves the interfacial compatibility between inorganic fillers and resin, and alleviates the decline in mechanical properties caused by a large amount of fillers. Attached Figure Description
[0015] Figure 1 This is a flowchart illustrating the preparation process of the anti-ant polyolefin sheath material according to an embodiment of the present invention. Detailed Implementation
[0016] The present invention will be further described below with reference to the accompanying drawings and embodiments. The following embodiments are only used to explain the present invention and are not intended to limit the scope of protection of the present invention.
[0017] The additives in each embodiment of the present invention can be selected in accordance with conventional methods in the art: the antioxidant can be selected from antioxidant 1010, antioxidant 1076, antioxidant 168 and their compound formulations; the light stabilizer can be selected from at least one of UV-327, UV-531, and light stabilizer 622; the lubricant can be selected from at least one of polyethylene wax, calcium stearate, and zinc stearate; the dispersant can be selected from polyethylene wax and stearate dispersants; the silane coupling agent can be selected from at least one of KH-550, KH-560, and KH-570. The specific selection of the above additives does not affect the implementation of the technical solution of the present invention.
[0018] Example 1 By weight, the components of the sheath material are: 40 parts high-density polyethylene, 35 parts linear low-density polyethylene, and 25 parts ethylene-vinyl acetate copolymer, totaling 100 parts polyolefin base material; 4 parts microencapsulated ant repellent; 40 parts aluminum hydroxide and 30 parts magnesium hydroxide (mass ratio 4:3) surface-treated with silane coupling agent KH-550; 5 parts zinc borate; 8 parts maleic anhydride-grafted polyethylene; 0.6 parts antioxidant 1010 and antioxidant 168 compound (mass ratio 1:1); 1.2 parts polyethylene wax; and 0.4 parts light stabilizer UV-327.
[0019] Preparation of microencapsulated ant repellent: Bifenthrin and azadirachtin were compounded at a mass ratio of 4:1 to obtain a composite core material; the composite core material was emulsified and dispersed using water as the continuous phase and sodium dodecyl sulfate as the emulsifier, melamine resin prepolymer was added, and the mixture was heated to 75℃ and cured for 2 h. After filtration, washing, and drying, microencapsulated ant repellent with a particle size of 3 μm to 10 μm was obtained (the mass ratio of core to wall was 1:1).
[0020] Preparation of anti-ant masterbatch: 40 parts of microencapsulated anti-ant agent, 52 parts of linear low-density polyethylene, 6 parts of ethylene-vinyl acetate copolymer, 1.6 parts of polyethylene wax dispersant, and 0.4 parts of antioxidant were mixed at high speed (600 r / min, 80℃, and 10 min), melt-extruded and granulated by a twin-screw extruder to obtain anti-ant masterbatch, in which the content of microencapsulated anti-ant agent was about 40 wt%.
[0021] Preparation of sheath material: The above-mentioned anti-ant masterbatch is mixed with polyolefin base material, halogen-free flame retardant, synergistic flame retardant, compatibilizer, antioxidant, lubricant and light stabilizer in the above proportions according to the amount of 4 parts of microencapsulated anti-ant agent (i.e., about 10 parts of anti-ant masterbatch). The mixture is added to a twin-screw extruder at a barrel temperature of 150℃~185℃, melt-blended and granulated to obtain environmentally friendly anti-ant polyolefin cable sheath material.
[0022] It should be noted that the carrier resin introduced into the termite-repellent masterbatch is a polyolefin base material. After taking into account all the components introduced into the termite-repellent masterbatch, the total amount of polyolefin base material is calculated as 100 parts; those skilled in the art can also make minor adjustments to the amount of each component in the base material during formulation (such as correspondingly reducing the amount of linear low-density polyethylene and ethylene-vinyl acetate copolymer) to ensure that the total amount of polyolefin base material is 100 parts.
[0023] Example 2 The difference from Example 1 is that: the final product dosage of the microencapsulated ant repellent is 6 parts (the ant repellent masterbatch is added at a dosage equivalent to 6 parts of the microencapsulated ant repellent); the core is changed to a mixture of high-efficiency cyhalothrin and matrine at a mass ratio of 3:1; the capsule wall is a chitosan-gelatin complex, prepared by the complex coagulation method, and the mass ratio of the core to the capsule wall is 1:1.
[0024] The specific preparation method of the chitosan-gelatin composite capsule wall is as follows: Prepare 1%–2% (w / w) chitosan aqueous solution (dissolved in 1% acetic acid) and gelatin aqueous solution (dissolved in a water bath at 40℃–50℃); add the emulsified core material emulsion to the gelatin aqueous solution and mix thoroughly; slowly add the chitosan solution dropwise, and adjust the pH of the system to 5.0–6.0 with acetic acid to allow the chitosan and gelatin to re-coagulate and coat the core material; then cool the system to below 10℃ to solidify the wall layer; add glutaraldehyde for crosslinking for 1–2 hours; filter, wash, and dry to obtain the microencapsulated ant repellent. The remaining components and preparation process are the same as in Example 1, and the method for calculating the amount of masterbatch is the same as in Example 1.
[0025] Example 3 The difference from Example 1 is that 10 parts of hollow glass microspheres treated with silane coupling agent (based on 100 parts of polyolefin base material) were added, and the amount of aluminum hydroxide was reduced to 32 parts and the amount of magnesium hydroxide was reduced to 22 parts, in order to increase the hardness of the sheath and reduce the density, so as to form a synergistic effect with the chemical control mechanism of the termite repellent. The rest is the same as in Example 1.
[0026] Comparative Example Comparative Example 1: The ant repellent was not microencapsulated. Bifenthrin and azadirachtin were directly compounded in a mass ratio of 4:1 and then incorporated into the sheath material of the same formulation in a free state. The remaining components and preparation process were the same as in Example 1.
[0027] Comparative Example 2: The microencapsulated ant repellent was replaced with a single bifenthrin core (without azadirachtin, and the amount of bifenthrin was equivalent to the pyrethrin component in Example 1). The same masterbatch process and sheath material formulation as in Example 1 were used, and the rest was the same as in Example 1.
[0028] Comparative Example 3: The mass ratio of bifenthrin to azadirachtin in the capsule core was changed to 6:1, that is, the mass ratio of natural plant extract to pyrethroid was 1:6, which is outside the range of 1:5 to 1:1 of the present invention. The rest is the same as in Example 1.
[0029] Comparative Example 4: The microencapsulated ant repellent was not prepared by masterbatch preparation. It was directly added to a twin-screw extruder for blending and granulation at one time with polyolefin base material, halogen-free flame retardant, synergistic flame retardant, compatibilizer, antioxidant, lubricant and light stabilizer. That is, step S3 was omitted. The rest was the same as in Example 1.
[0030] Application examples The sheath material obtained in Examples 1 to 3 is extruded and coated onto the outside of the cable core to produce an environmentally friendly cable sheath with termite-proof function.
[0031] Performance verification Performance tests were conducted on the sheath materials obtained in Examples 1 to 3 and Comparative Examples 1 to 4. Microcapsule encapsulation rate was calculated as the core mass relative to the total microcapsule mass; termite repellent retention rate was calculated as the mass fraction of residual termite repellent after treatment at 180℃ for 5 min relative to the initial amount added; tensile properties were tested according to GB / T 1040.2; oxygen index was tested according to GB / T 2406.2; termite testing was conducted according to the experimental population method of JB / T 10696.9—2011, with the qualification criterion being the absence of termite borer marks on the surface and edges after 28 days, recorded as FY1; the knockdown KT50 was only used as a comparative screening reference for the drug release rate; long-lasting efficacy was evaluated primarily by retesting the experimental population method after heat aging at 70℃ for 168 h, supplemented by changes in the knockdown KT50. The test results are shown in Table 1.
[0032] Table 1. Performance Comparison of Examples and Comparative Examples
[0033] As can be seen from Table 1: Firstly, in the 28-day experimental group test, no termite tooth marks were observed on the surface and along the edges of each embodiment, meeting the FY1 qualification criterion; while Comparative Example 1 (free termite repellent), Comparative Example 2, and Comparative Example 4 all showed slight tooth marks along the edges, and Comparative Example 3 showed tooth marks on both the surface and along the edges, failing to meet the qualification criterion. This proves that microencapsulation, compound synergy, and secondary dispersion of masterbatch are all indispensable for maintaining long-lasting termite repellency.
[0034] Secondly, microencapsulation increased the retention rate of the ant repellent under processing conditions of 180℃×5 min from 63% in Comparative Example 1 to over 88% (88% to 92% measured in Examples 1 to 3), indicating that the capsule wall effectively inhibited volatilization and decomposition during processing.
[0035] Third, the KT50 of the knockdown method in the example was higher than that in the control sample, indicating that the capsule wall has a controlled release effect on the ant repellent. After heat aging at 70℃ for 168 h, the KT50 of Example 1 increased only from 38 min to 45 min, while that of Comparative Example 1 increased from 20 min to 74 min. The long-term effect of the example is significant (the KT50 of the knockdown method is only used as a reference for the release rate comparison and is not a basis for judging the product qualification).
[0036] Fourth, the surface-treated halogen-free flame retardant and compatibilizer, in combination, maintain a tensile strength of over 14 MPa, an elongation at break of not less than 430%, and an oxygen index of not less than 32% in the example. Both the mechanical properties and flame retardant properties meet the general requirements for cable sheath materials.
[0037] Fifth, in Comparative Example 2 (single bifenthrin capsule core, not combined with natural plant extracts), slight tooth marks were observed along the edge after 28 days in the experimental group method, while no tooth decay was observed in the Example. This indicates that the synergistic combination of pyrethroids and natural plant extracts is the key to maintaining long-lasting ant protection, and a single active ingredient is difficult to achieve both knockdown and food refusal.
[0038] Sixth, in Comparative Example 3, the mass ratio of natural plant extract to pyrethroid was 1:6, which is lower than the lower limit of 1:5 in this invention. On the one hand, the proportion of plant extract is too low, resulting in insufficient synergistic effect of antifeedant and knockdown with pyrethroid, thus reducing the termite-repellent effect. On the other hand, the emulsification and dispersion stability decreased after the core material polarity ratio was changed, the microcapsule encapsulation rate dropped to 72%, the 180℃ retention rate dropped to 78%, and the processing loss increased significantly. In the experimental group method, tooth marks were observed on the surface and along the edges after 28 days, proving that the compounding ratio range limited by this invention is a necessary condition to ensure long-term termite-repellent effect.
[0039] Seventh, in Comparative Example 4, the secondary dispersion step of the masterbatch was omitted, and the microencapsulated termite repellent was directly mixed with the base material. The retention rate at 180°C decreased from more than 88% in the example to 70%. After aging at 70°C, KT50 increased to 68 min. Slight tooth marks were observed along the edge in the experimental group method after 28 days, which proves that the secondary dispersion process of the masterbatch has an independent contribution to the uniform dispersion of microcapsules in the base material and processing protection.
[0040] The above description is merely a preferred embodiment of the present invention and is not intended to limit the invention. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.
Claims
1. A termite-resistant polyolefin cable sheath material, characterized in that, The following components are included in parts by weight: 100 parts of polyolefin base material, wherein the polyolefin base material is at least two of high-density polyethylene, linear low-density polyethylene, ethylene-vinyl acetate copolymer and ethylene-octene copolymer; 2-8 parts of microencapsulated ant repellent, wherein the microencapsulated ant repellent uses a compound of pyrethroids and natural plant extracts as the core and a polymer wall material as the wall. 40-80 parts of halogen-free flame retardant, wherein the halogen-free flame retardant is a mixture of surface-treated aluminum hydroxide and magnesium hydroxide, and the mass ratio of aluminum hydroxide to magnesium hydroxide is 2:1 to 1:2; Synergistic flame retardant 3-8 parts; compatibilizer 4-12 parts; antioxidant 0.3-1.0 parts; lubricant 0.5-2.0 parts; light stabilizer 0.2-0.8 parts.
2. The anti-termite polyolefin cable sheath material according to claim 1, characterized in that: The natural plant extract is at least one of azadirachtin, matrine, pyrethrin, and eugenol; the pyrethroid is at least one of bifenthrin, permethrin, and lambda-cyhalothrin; the mass ratio of the natural plant extract to the pyrethroid is 1:5 to 1:
1.
3. The anti-termite polyolefin cable sheath material according to claim 1, characterized in that: The wall material polymer is melamine resin, urea-formaldehyde resin, or chitosan-gelatin complex; the microencapsulated ant repellent has a particle size of 1-20 μm and a core-to-wall mass ratio of 1:0.5-1:
2.
4. The anti-termite polyolefin cable sheath material according to claim 1, characterized in that: The halogen-free flame retardant is surface-treated with a silane coupling agent or stearic acid; the synergistic flame retardant is at least one of zinc borate and microencapsulated red phosphorus.
5. The anti-termite polyolefin cable sheath material according to claim 1, characterized in that: It also includes 5 to 15 parts of hollow glass microspheres, the surface of which is treated with a silane coupling agent.
6. The anti-termite polyolefin cable sheath material according to claim 1, characterized in that: The polyolefin base material is composed of 30-50 parts of high-density polyethylene, 25-45 parts of linear low-density polyethylene, and 10-25 parts of ethylene-vinyl acetate copolymer; the compatibilizer is maleic anhydride-grafted polyethylene and / or maleic anhydride-grafted ethylene-vinyl acetate copolymer.
7. A method for preparing the anti-termite polyolefin cable sheath material as described in any one of claims 1 to 6, characterized in that, Includes the following steps: S1. Core material compounding: Pyrethroids and natural plant extracts are mixed in a certain proportion to obtain a composite core material; S2. Microencapsulation: When the wall material polymer is melamine resin or urea-formaldehyde resin, an in-situ polymerization method is used: water is used as the continuous phase, an emulsifier is added to emulsify and disperse the composite core material, then the wall material prepolymer is added, and the temperature is raised to 60℃~85℃ for 1 h~4 h to cure; when the wall material polymer is chitosan-gelatin composite, a coagulation method is used: the emulsified and dispersed composite core material is mixed with gelatin aqueous solution and chitosan aqueous solution, the pH value of the system is adjusted to 5.0~6.0, so that chitosan and gelatin undergo coagulation to coat the core material, and then crosslinking and curing are performed; both methods are filtered, washed and dried to obtain microencapsulated ant repellent; S3. Masterbatch preparation: Microencapsulated ant repellent, carrier resin, dispersant and antioxidant are mixed at high speed, and then melt-extruded and granulated by a twin-screw extruder to obtain ant repellent masterbatch; the carrier resin is linear low-density polyethylene and / or ethylene-vinyl acetate copolymer; S4. Co-extrusion: The termite-resistant masterbatch is mixed with polyolefin base material, halogen-free flame retardant, synergistic flame retardant, compatibilizer, antioxidant, lubricant and light stabilizer, and then added to a twin-screw extruder for melt blending and granulation to obtain the environmentally friendly termite-resistant polyolefin cable sheath material; the barrel temperature of the twin-screw extruder is 140℃~190℃.
8. The preparation method according to claim 7, characterized in that: In step S2, the emulsifier is sodium dodecyl sulfate or alkylphenol polyoxyethylene ether; in step S3, the high-speed mixing speed is 500 r / min to 700 r / min, the temperature is 75℃ to 85℃, and the time is 8 min to 12 min.
9. The use of the termite-resistant polyolefin cable sheath material as described in any one of claims 1 to 6 in the preparation of termite-resistant cable sheaths.