Thermoplastic elastomer composition, method for its manufacture and use thereof
A thermoplastic elastomer composition composed of ethylene-α-olefin copolymer and propylene polymers has solved the problem of poor crackability of automotive interior materials under tear-free processing, and has achieved molded parts with low high-speed surface impact energy and excellent crackability, thereby improving production efficiency and mechanical properties.
Patent Information
- Application Number
- CN202610677934.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2025-05-23
- Filing Date
- 2026-05-18
- Publication Date
- 2026-11-24
AI Technical Summary
In existing technologies, the outer skin material of the airbag device in automotive interior materials is difficult to crack quickly without tear line processing, resulting in low production efficiency.
A thermoplastic elastomer composition consisting of ethylene-α-olefin copolymer and propylene polymers, with ethylene structural units accounting for 55-80% and the product of monomer reactivity ratios r1r2≤1.8, is prepared by melt mixing with mineral oil, crosslinking agent and inorganic filler.
This technology enables high-speed surface impact of molded parts with low energy and excellent crack resistance under tear-free processing, thereby improving production efficiency and mechanical properties.
Smart Images

Figure FT_1 
Figure SMS_2 
Figure SMS_4
Abstract
Description
Technical Field
[0001] This invention relates to thermoplastic elastomer compositions. Background Technology
[0002] Thermoplastic elastomers are used in a variety of applications, primarily in vehicle parts, such as automotive parts, and in automotive interior materials, such as the outer skin material of the airbag cover (dashboard) (see, for example, Patent Document 1).
[0003] The back side of the aforementioned skin material is usually processed with tear lines to assist the deployment of the airbag (a process of forming a cut for deploying the airbag). However, in order to reduce production time and optimize production, a skin material with excellent crackability that can be easily cracked even without tear line processing is required.
[0004] Existing technical documents
[0005] Patent documents
[0006] Patent Document 1: International Publication No. 2021 / 200928 A1 (Single Volume) Summary of the Invention
[0007] The problem that the invention aims to solve
[0008] In this context, the problem to be solved by the present invention is to provide a thermoplastic elastomer composition capable of forming a molded body with low high-speed surface impact energy and excellent crack resistance.
[0009] means for solving problems
[0010] Given this background, the inventors conducted in-depth research and, as a result, completed this invention.
[0011] That is, the present invention relates to: [1] A thermoplastic elastomer composition comprising 100 parts by weight of (A) an ethylene-α-olefin copolymer and 20 to 90 parts by weight of (B) a propylene polymer, wherein, The percentage of ethylene-derived structural units in all structural units of (A) ethylene-α-olefin copolymer is greater than or equal to 55% by mass and less than 80% by mass. (A) The product of the monomer reactivity ratios r1 and r2 of the ethylene-α-olefin copolymer is less than 1.8.
[0012] Hereinafter, [2] to
[12] are each preferred embodiments or implementations of the present invention.
[0013] [2] According to the thermoplastic elastomer composition of [1], wherein the molar fraction AA of the α-olefin-α-olefin chain of the ethylene-α-olefin copolymer is 8.5 mol% or less (wherein the total of the peak area AA of the portion of monomer units bonded in the order of α-olefin unit-α-olefin unit, the peak area AE of the portion of monomer units bonded in the order of α-olefin unit-ethylene unit and the peak area EE of the portion of monomer units bonded in the order of ethylene unit-ethylene unit is set to 100 mol).
[0014] [3] The thermoplastic elastomer composition according to [1] or [2], wherein (A) the ethylene-α-olefin copolymer has structural units derived from non-conjugated dienes.
[0015] [4] The thermoplastic elastomer composition according to any one of [1] to [3], wherein the thermoplastic elastomer composition further contains (C) mineral oil.
[0016] [5] The thermoplastic elastomer composition according to any one of [1] to [4], wherein the thermoplastic elastomer composition further comprises (D) a crosslinking agent.
[0017] [6] The thermoplastic elastomer composition according to any one of [1] to [5], wherein the thermoplastic elastomer composition further contains (E) inorganic filler.
[0018] [7] The thermoplastic elastomer composition according to any one of [1] to [6], wherein the thermoplastic elastomer composition further contains an ethylene resin in which the ratio of (F) structural units derived from ethylene is 80% by mass or more.
[0019] [8] According to the thermoplastic elastomer composition of [7], wherein the density of (F) vinyl resin is 950 kg / m³. 3 above.
[0020] A method for manufacturing a thermoplastic elastomer composition according to any one of [9] [1] to [8], wherein the method comprises a step of melt-blending (A) an ethylene-α-olefin copolymer and (B) a propylene polymer in the presence of (D) a crosslinking agent.
[0021]
[10] The method for manufacturing a thermoplastic elastomer composition according to [9], wherein the method comprises: adding (F) an ethylene resin to a melt blend obtained in the presence of a (D) crosslinking agent in the presence of a (A) ethylene-α-olefin copolymer and a (B) propylene polymer and further performing a melt blend.
[0022]
[11] A molded body comprising any one of [1] to [8], wherein the compression set of the molded body is 36% to 70% under the conditions of a compression ratio of 25%, a test temperature of 70°C and a test time of 22 hours according to JIS K6262.
[0023]
[12] An interior trim for a vehicle, wherein the interior trim for a vehicle contains any one of the thermoplastic elastomer compositions described in [1] to [8].
[0024] Invention Effects
[0025] According to the present invention, a thermoplastic elastomer composition capable of forming molded articles with low high-speed surface impact energy and excellent crack resistance can be provided. Attached Figure Description
[0026] Figure 1 This is an embodiment of the ethylene-α-olefin copolymer used in this invention. 13 C-NMR spectrum.
[0027] Label Explanation
[0028] 1: Tββ
[0029] 2: Tβδ
[0030] 3: Tδδ
[0031] 4: Sβδ
[0032] 5: Sδδ
[0033] 6:Sγδ Detailed Implementation
[0034] This invention relates to a thermoplastic elastomer composition comprising 100 parts by weight of (A) an ethylene-α-olefin copolymer and 20 to 90 parts by weight of (B) a propylene polymer, wherein... The percentage of ethylene-derived structural units in all structural units of (A) ethylene-α-olefin copolymer is greater than or equal to 55% by mass and less than 80% by mass. (A) The product of the monomer reactivity ratios r1 and r2 of the ethylene-α-olefin copolymer is less than 1.8.
[0035] That is, the thermoplastic elastomer composition of the present invention contains the above-mentioned component (A) and component (B), and the above-mentioned component (A) has a product of a specified monomer composition and a monomer reactivity ratio.
[0036] The thermoplastic elastomer composition of the present invention is formed by containing the above-mentioned component (A) and component (B), thereby possessing the formability and rubber elasticity derived from thermoplasticity.
[0037] The thermoplastic elastomer composition of the present invention may consist only of the above-mentioned components (A) and (B) as essential components. In addition, it may contain optional components other than components (A) and (B), such as mineral oil (C), crosslinking agent, inorganic filler and / or vinyl resin (described later).
[0038] The following is a description of the essential and optional components mentioned above.
[0039] (A) Ethylene-α-olefin copolymer
[0040] The (A) ethylene-α-olefin copolymer constituting the thermoplastic elastomer composition of the present invention is a copolymer having structural units derived from ethylene and structural units derived from at least one monomer selected from the group consisting of α-olefins having 3 or more and 10 or fewer carbon atoms.
[0041] The percentage of ethylene-derived structural units in all structural units of (A) ethylene-α-olefin copolymer is greater than or equal to 55% by mass and less than 80% by mass.
[0042] The proportion of structural units derived from ethylene is 55% by mass or more, therefore (A) ethylene-α-olefin copolymer is a crosslinkable polymer, suitable for forming island phases of island structures in thermoplastic elastomer compositions through dynamic crosslinking.
[0043] The proportion of structural units derived from ethylene is less than 80% by mass, resulting in good softness and rubber elasticity.
[0044] (A) The ethylene-α-olefin copolymer is preferably a random copolymer.
[0045] (A) An ethylene-α-olefin copolymer may consist only of structural units derived from ethylene and structural units derived from at least one monomer in the group consisting of α-olefins having 3 or more and 10 or fewer carbon atoms, or may have other structural units.
[0046] Examples of α-olefins having 3 or more but less than 10 carbon atoms include cyclic olefins such as propylene, 1-butene, 2-methylpropylene, 1-pentene, 3-methyl-1-butene, 1-hexene, 3-methyl-1-pentene, 4-methyl-1-pentene, 1-heptene, 1-octene, 1-nonene, 1-decene, and vinylcyclohexane. In the preparation of (A) ethylene-α-olefin copolymers, α-olefins having 3 or more but less than 10 carbon atoms can be used alone or in combination with two or more. Preferably, structural units derived from at least one monomer selected from the group consisting of α-olefins having 3 or more but less than 10 carbon atoms include structural units derived from propylene, structural units derived from 1-butene, structural units derived from 4-methyl-1-pentene, structural units derived from 1-hexene, or structural units derived from 1-octene.
[0047] The proportion of ethylene-derived structural units in the (A) ethylene-α-olefin copolymer is greater than or equal to 55% by mass and less than 80% by mass, preferably 58% by mass and less than 78% by mass, more preferably 60% by mass and less than 75% by mass, and particularly preferably 62% by mass and less than 73% by mass (wherein the total amount of all structural units of the (A) ethylene-α-olefin copolymer is set to 100% by mass). The proportion of structural units in the (A) ethylene-α-olefin copolymer derived from at least one monomer selected from the group consisting of α-olefins with 3 or more and 10 or less carbon atoms is 10% by mass and more, preferably 15% by mass and less than 45% by mass, more preferably 20% by mass and less than 37% by mass, and particularly preferably 24% by mass and less than 33% by mass (wherein the total amount of all structural units of the (A) ethylene-α-olefin copolymer is set to 100% by mass).
[0048] By combining the fact that the ratio of ethylene-derived structural units in the (A) ethylene-α-olefin copolymer is 55% by mass or more, with the other necessary conditions of the present invention also being met, the thermoplastic elastomer composition of the present invention can achieve the technical effect of forming molded articles with low high-speed surface impact energy and excellent cracking resistance, as well as the technical effect of improving mechanical properties and flexibility.
[0049] (A) The ratio of structural units derived from ethylene to structural units derived from at least one monomer in the group consisting of α-olefins with 3 to 10 carbon atoms in (A) ethylene-α-olefin copolymers can be determined by infrared spectroscopy. Specifically, the infrared absorption spectrum of (A) ethylene-α-olefin copolymers can be measured using an infrared spectrophotometer, and the ratio of structural units derived from ethylene to structural units derived from at least one monomer in the group consisting of α-olefins with 3 to 10 carbon atoms in (A) ethylene-α-olefin copolymers can be calculated according to the methods described in "Characterization of Polyethylene Based on Infrared Absorption Spectra (by Takayama, Usami et al.)" or "Die Makromolekulare Chemie, 177, 461 (1976) (by Mc Rae, MA, Madam S, WF et al.)". The ratios of ethylene-derived structural units in components (A-1) and (A-2) described later, and the ratios of structural units derived from at least one monomer in the group consisting of α-olefins with 3 or more and 10 or fewer carbon atoms, can also be calculated in the same way.
[0050] (A) Ethylene-α-olefin copolymers may have structural units derived from monomers other than ethylene and at least one monomer selected from the group consisting of α-olefins having 3 or more and 10 or fewer carbon atoms. Examples of such other monomers include: chain-like non-conjugated dienes, such as 1,4-hexadiene, 1,6-octadiene, 2-methyl-1,5-hexadiene, 6-methyl-1,5-heptadiene, and 7-methyl-1,6-octadiene; and cyclic non-conjugated dienes, such as 1,5-cyclooctadiene, cyclohexadiene, cyclopentadiene, dimercyclopentadiene, methyltetrahydroindene, 5-vinyl-2-norbornene, 5-ethoxy-2-norbornene, 5-methylene-2-norbornene, and 5-isopropylidene-2-norbornene. The copolymer may contain 6-chloromethyl-5-isopropenyl-2-norbornene; trienes, such as 2,3-diisopropylidene-5-norbornene, 2-ethimide-3-isopropylidene-5-norbornene, 2-propenyl-2,2-norbornediene, and 4-ethimide-8-methyl-1,7-nonadiene; vinyl carboxylic acids, such as vinyl acetate; unsaturated carboxylic acids, such as methyl acrylate, ethyl acrylate, butyl acrylate, methyl methacrylate, and ethyl methacrylate; and unsaturated carboxylic acids, such as acrylic acid and methacrylic acid. (A) The ethylene-α-olefin copolymer may contain two or more structural units derived from the other monomer. From the viewpoint of crosslinking, the other monomer is preferably a non-conjugated diene having 5 or more and 15 or less carbon atoms, more preferably 5-ethimide-2-norbornene, dimercyclopentadiene, 5-vinyl-2-norbornene, or combinations thereof.
[0051] When the (A) ethylene-α-olefin copolymer has structural units derived from monomers other than ethylene and at least one monomer selected from the group consisting of α-olefins having 3 or more and 10 or less carbon atoms, the ratio of structural units derived from these other monomers is preferably 2% by mass or more and 15% by mass or less, more preferably 3% by mass or more and 8% by mass or less (wherein the total amount of the (A) ethylene-α-olefin copolymer is set to 100% by mass). The ratio of structural units derived from these other monomers can be determined by the aforementioned infrared spectroscopy method. The ratio of structural units derived from these other monomers in components (A-1) and (A-2) described later can also be determined in the same way.
[0052] Examples of (A) ethylene-α-olefin copolymers include: ethylene-propylene copolymers, ethylene-1-butene copolymers, ethylene-1-hexene copolymers, ethylene-4-methyl-1-pentene copolymers, ethylene-1-octene copolymers, ethylene-propylene-1-butene copolymers, ethylene-propylene-1-hexene copolymers, and ethylene-propylene-1-octene copolymers. From the viewpoint of crosslinking, ethylene-α-olefin-non-conjugated diene copolymers are preferred. Examples include: ethylene-propylene-5-ethimide-2-norbornene copolymers, ethylene-propylene-dicyclopentadiene copolymers, ethylene-propylene-1,4-hexadiene copolymers, ethylene-propylene-5-vinyl-2-norbornene copolymers, ethylene-1-butene-5-ethimide-2-norbornene copolymers, ethylene-1-butene-dicyclopentadiene copolymers, ethylene-1-butene-1,4-hexadiene copolymers, and ethylene-1-butene-5-vinyl-2-norbornene copolymers. It can also be an olefin block copolymer comprising polymeric blocks of ethylene and copolymeric blocks of ethylene-α-olefin. The ethylene-α-olefin copolymer as component (A) can be used alone or in combination with two or more components. As component (A), ethylene-propylene-5-ethylidene-2-norbornene copolymer is preferably used. In this embodiment, the ethylene-α-olefin copolymer is preferably an ethylene-α-olefin copolymer with a hardness of 85 or less according to JIS K6253.
[0053] The product of the monomer reactivity ratios r1 and r2 of (A) ethylene-α-olefin copolymer, which is a component of the thermoplastic elastomer composition of the present invention, is 1.8 or less.
[0054] By using an (A) ethylene-α-olefin copolymer with a monomer reactivity ratio product r1r2 of 1.8 or less, combined with other technical features of the present invention, the thermoplastic elastomer composition of the present invention can achieve a significant technical effect that overcomes the limitations of the prior art, such as the ability to form molded articles with low high-speed surface impact energy and excellent cracking resistance.
[0055] The product of monomer reactivity ratios, r1 and r2, is derived from the ethylene-α-olefin copolymer under the following conditions. 13 The peak areas AA, AE, and EE in the C-NMR spectrum are obtained from the following equation (2).
[0056] r1r2=EE{AA / (AE / 2) 2 Equation (2)
[0057] (In equation (2), the total of the peak areas AA, AE, and EE of the monomer units bonded in the order of α-olefin unit-α-olefin unit, which are derived from the monomer units bonded in the order of α-olefin unit-ethylene unit, is set to 100 mol%.)
[0058] The product of the monomer reactivity ratios can be calculated as follows. For example, using the AvanceNEO 600 (10mm low-temperature probe) manufactured by Bruker, under the following conditions: solvent: 1,2-dichlorobenzene / 1,1,2,2-tetrachloroethane-d2 (85 / 15 volume ratio), measurement temperature: 135℃, measurement method: Powergate proton decoupling method, pulse width: 45 degrees, pulse repetition time: 4 seconds, number of accumulations: 256, chemical shift value reference: tetramethylsilane, the reaction of (A) ethylene-α-olefin copolymer was carried out. 13 Determination of C-NMR spectra.
[0059] The measured [substance] can be identified based on the methods described in Kakugo et al., Macromolecules, 15, 1150 (1982); Cheng, Macromolecules, 17, 1950 (1984); Cheng, Macromolecules, 24, 4813 (1991); Wang et al., Macromol. Chem. Phys., 200, 2146 (1999); and Lee et al., Polymer Journal, 28, 696 (1996). 13 The peaks in the C-NMR spectrum are determined by equation (2) above. For example, in the case where the α-olefin is propylene, such as Figure 1 The structure of the formula described in the examples identifies the origin of each carbon atom. 13 The peaks of C-NMR were calculated using the following formula: the peak area PP, the peak area PE, and the peak area EE of the monomer units bonded in the order of propylene-propylene unit to ethylene unit. The peak areas were then normalized to a total of 100 mol% for PP, EE, and PE.
[0060] PP=Tββ+1 / 2Tβδ
[0061] EE = 1 / 2(Sβδ + Sδδ) + 1 / 4Sγδ
[0062] PE=Tβδ+2Tδδ
[0063] The product of the monomer reactivity ratios (r1 of ethylene and r2 of propylene) of the ethylene-α-olefin copolymer is calculated using the following formula (3).
[0064] r1r2=EE{PP / (PE / 2) 2 Equation (3)
[0065] In cases where the α-olefin is other than propylene, where there are two or more α-olefins, or where there is a structural unit derived from a monomer other than ethylene and at least one monomer selected from the group consisting of α-olefins with 3 or more and 10 or less carbon atoms, r1r2 can also be obtained from the above formula (2) based on the method described above, reflecting the different types of α-olefin units and structural units derived from monomers other than ethylene and at least one monomer selected from the group consisting of α-olefins with 3 or more and 10 or less carbon atoms.
[0066] The mechanism by which the high-speed surface impact energy of thermoplastic elastomer compositions is reduced by using (A) ethylene-α-olefin copolymers with a monomer reactivity product r1r2 of 1.8 or less is not necessarily clear. However, as mentioned above, the monomer reactivity product r1r2 is an indicator of the degree of α-olefin chains in (A) ethylene-α-olefin copolymers. More specifically, a small r1r2 indicates fewer α-olefin chains, and a large r1r2 indicates more α-olefin chains. It is presumed that r1r2 below a specified value and α-olefin chains below a specified ratio affect the semi-crystallization of the island phase and the higher-order structure such as the crystal grain size distribution of the (A) ethylene-α-olefin copolymer as the main component. Through these factors, the high-speed surface impact energy of thermoplastic elastomer compositions may be affected and have some correlation.
[0067] From the viewpoint of further reducing high-speed surface impact energy and improving flexibility, the product of monomer reactivity ratios r1r2 is preferably 1.7 or less, more preferably 1.4 or less, even more preferably 1.0 or less, and particularly preferably 0.7 or less.
[0068] From the viewpoint of achieving practically preferred impact resistance, increasing molecular weight during polymerization, and improving mechanical properties, the product of monomer reactivity ratios r1r2 is preferably 0.01 or more, more preferably 0.4 or more, and particularly preferably 0.6 or more.
[0069] The monomer reactivity product r1r2 of (A) ethylene-α-olefin copolymers can be adjusted by appropriately regulating the manufacturing conditions of (A) ethylene-α-olefin copolymers, such as polymerization temperature, catalyst, solvent, monomer dispersion in the polymerization tank, and / or hydrogen as a molecular weight regulator. As an example, when a Ziegler-Natta type catalyst (described later) is selected as the catalyst, the monomer reactivity product r1r2 of the resulting ethylene-α-olefin copolymer tends to be smaller.
[0070] Furthermore, as mentioned above, a smaller r1r2 indicates fewer α-olefin chains, while a larger r1r2 indicates more α-olefin chains. Highly random ethylene-α-olefin copolymers tend to have smaller r1r2, while highly block copolymers tend to have larger r1r2. In the field of ethylene-α-olefin copolymer manufacturing, manufacturing techniques for random copolymers and block copolymers have been established. Those skilled in the art have accumulated extensive insights into the conditions for manufacturing highly random copolymers and highly block copolymers. Therefore, by applying these insights, those skilled in the art can also manufacture ethylene-α-olefin copolymers with the desired monomer reactivity ratio product r1r2 without being forced to conduct excessive repeated experiments, and use them as (A) ethylene-α-olefin copolymers.
[0071] (A) The product of the monomer reactivity ratios r1 and r2 of the ethylene-α-olefin copolymer, as described above, can be obtained through... 13 The techniques established in this field, such as C-NMR determination, separation and area calculation of the obtained NMR peaks, and structural analysis based thereon, enable those skilled in the art to determine the monomer reactivity product r1r2 of obtainable ethylene-α-olefin copolymers, such as various commercially available products, without being forced to conduct excessive repeated experiments, select ethylene-α-olefin copolymers having the desired monomer reactivity product r1r2, and use them as (A) ethylene-α-olefin copolymer.
[0072] Furthermore, as mentioned above, ethylene-α-olefin copolymers with high randomness tend to have small r1r2, while ethylene-α-olefin copolymers with high blockiness tend to have large r1r2. Therefore, this can be taken into account to select ethylene-α-olefin copolymers with a high probability of having the desired r1r2 from the available ethylene-α-olefin copolymers with a certain degree of precision, thereby significantly reducing the need for practical determination of r1r2. Therefore, from this point of view, those skilled in the art can also select ethylene-α-olefin copolymers with the desired monomer reactivity ratio product r1r2 without being forced to conduct excessive repeated experiments, and use them as (A) ethylene-α-olefin copolymers.
[0073] The peak areas AA, AE, and EE of the monomer units bonded in the order of α-olefin unit-α-olefin unit are not particularly limited. However, from the viewpoint of more effectively achieving the effect of reducing high-speed surface impact energy, the peak area AA of the monomer units bonded in the order of α-olefin unit-α-olefin unit is preferably 8.5 mol% or less (wherein, the total of the peak areas AA, AE, and EE of the monomer units bonded in the order of α-olefin unit-α-olefin unit is set to 100 mol%).
[0074] (A) The mole fraction of the peak area AA of the portion of the monomer unit bonded in the order of α-olefin unit-α-olefin unit in the ethylene-α-olefin copolymer is more preferably 7.0 mol% or less, further preferably 5.5 mol% or less, and particularly preferably 4.0 mol% or less.
[0075] (A) The mole fraction of the peak area AA of the portion of the ethylene-α-olefin copolymer derived from the monomer units bonded in the order of α-olefin unit-α-olefin unit is preferably 1.0 mol% or more, more preferably 3.0 mol% or more.
[0076] The mole fraction of the peak area EE of the portion of the monomer units in the (A) ethylene-α-olefin copolymer that is bonded in the order of ethylene unit-ethylene unit can be appropriately adjusted in the same way as the method for adjusting the product r1r2 of the monomer reactivity ratio described above. Alternatively, it can also be appropriately adjusted by adjusting the ratio of ethylene-derived structural units in all structural units of the (A) ethylene-α-olefin copolymer.
[0077] As preferred examples of (A) ethylene-α-olefin copolymers, the following ethylene random copolymers (A-1) and (A-2) can be cited.
[0078] The ethylene random copolymer (A-1) (hereinafter sometimes referred to as component (A-1)) is an ethylene random copolymer having 55% by mass and less than 80% by mass of structural units derived from ethylene, and structural units derived from at least one monomer selected from the group consisting of α-olefins having 3 or more and 10 or fewer carbon atoms, and a gel fraction greater than 10% by mass (wherein the total amount of the ethylene random copolymer is set to 100% by mass). Component (A-1) may have structural units derived from monomers other than ethylene and at least one monomer selected from the group consisting of α-olefins having 3 or more and 10 or fewer carbon atoms. Specific examples of α-olefins having 3 or more and 10 or less carbon atoms in component (A-1), preferred ranges of the ratio of structural units derived from ethylene in component (A-1), preferred ranges of the ratio of structural units derived from at least one monomer selected from the group consisting of α-olefins having 3 or more and 10 or less carbon atoms, specific examples of structural units derived from monomers other than ethylene and at least one monomer selected from the group consisting of α-olefins having 3 or more and 10 or less carbon atoms, preferred ranges of the ratio of such other monomers, and specific examples of ethylene random copolymers are the same as those described above regarding (A) ethylene-α-olefin copolymers.
[0079] The more cross-linked structures an ethylene random copolymer has, the greater its gel fraction.
[0080] Component (A-1) can be obtained, for example, by crosslinking component (A-2) described later. The gel fraction of component (A-1) can be determined by the following method based on the following gel mass of the thermoplastic elastomer composition containing component (A-1) and the mass of component (A-2) contained in the raw material of the thermoplastic elastomer composition.
[0081] The gel fraction of component (A-1) was determined using a Soxhlet extractor with an extraction tube connected to the lower part of a reflux condenser and a flask connected to the lower part of the extraction tube, by the method described below. Approximately 1 g of the thermoplastic elastomer composition and an empty wire mesh cage (mesh size: 400 mesh) were weighed. The wire mesh cage containing the thermoplastic elastomer composition was introduced into the extraction tube. 300 ml of o-xylene was introduced into the flask. The flask was heated, and the o-xylene was refluxed for 24 hours for extraction. After extraction, the wire mesh cage containing the extraction residue was removed from the extraction tube and dried under reduced pressure at 100°C using a vacuum dryer. The dried wire mesh cage containing the extraction residue was weighed. The gel mass of the thermoplastic elastomer composition was calculated based on the difference in mass between the dried wire mesh cage containing the extraction residue and the empty wire mesh cage. The gel fraction (mass %) of component (A-1) was calculated based on the following formula.
[0082] The gel fraction of component (A-1) = (mass of gel in the thermoplastic elastomer composition / mass of component (A-2)) × 100
[0083] The gel fraction of component (A-1) is preferably 20% by mass or more, and more preferably 40% by mass or more.
[0084] The more cross-linked structures an ethylene random copolymer has, the greater the gel fraction of the thermoplastic elastomer composition.
[0085] The gel fraction of the thermoplastic elastomer composition can be calculated using the following formula, based on the gel mass of the thermoplastic elastomer composition obtained by the same method as described above.
[0086] The gel fraction of a thermoplastic elastomer composition = (mass of gel in the thermoplastic elastomer composition / mass of the thermoplastic elastomer composition) × 100
[0087] The gel fraction of the thermoplastic elastomer composition is preferably 10% by mass or more and 90% by mass or less, more preferably 15% by mass or more and 60% by mass or less, and even more preferably 18% by mass or more and 40% by mass or less.
[0088] Component (A-1) can be obtained by crosslinking component (A-2), which will be described later. One method of crosslinking is to melt-blend a composition containing component (A-2) and the crosslinking agent (D), which will be described later. Crosslinking can be performed simultaneously during the manufacture of the thermoplastic elastomer composition of the present invention. In this case, a thermoplastic elastomer composition containing components (A-1) and (B) propylene polymer can be manufactured by melt-blending a composition containing component (A-2), the propylene polymer (B), and the crosslinking agent (D), as detailed below.
[0089] The ethylene random copolymer (A-2) (hereinafter sometimes referred to as component (A-2)) is an ethylene random copolymer having 55% by mass and less than 80% by mass of structural units derived from ethylene, and structural units derived from at least one monomer selected from the group consisting of α-olefins having 3 or more and 10 or less carbon atoms, and a gel fraction of 10% by mass or less (wherein the total amount of the ethylene random copolymer is set to 100% by mass). Component (A-2) may have structural units derived from monomers other than ethylene and at least one monomer selected from the group consisting of α-olefins having 3 or more and 10 or less carbon atoms. Specific examples of α-olefins having 3 or more and 10 or less carbon atoms in component (A-2), preferred range of the ratio of structural units derived from ethylene in component (A-2), preferred range of the ratio of structural units derived from at least one monomer selected from the group consisting of α-olefins having 3 or more and 10 or less carbon atoms, specific examples of structural units derived from monomers other than ethylene and at least one monomer selected from the group consisting of α-olefins having 3 or more and 10 or less carbon atoms, preferred range of the ratio of such other monomers, and specific examples of ethylene random copolymers are the same as in the case of ethylene-α-olefin copolymers (A).
[0090] The gel fraction of component (A-2) is preferably 5% by mass or less, more preferably 1% by mass or less. Component (A-2) preferably does not have a substantially cross-linked structure.
[0091] Mooney viscosity (ML) of component (A-2) measured at 125°C 1+4 The Mooney viscosity (ML) is preferably 5 or more and 350 or less, more preferably 10 or more and 300 or less, and even more preferably 40 or more and 200 or less. It should be noted that this Mooney viscosity (ML) is... 1+ (4125℃) was measured according to JIS K6300, “ML 1+4 "125℃" means the following.
[0092] M: Mooney viscosity
[0093] L: Using a large rotor
[0094] 125℃: Measurement temperature
[0095] 1+4: The measured value after heating the sample for 1 minute and then rotating the rotor at 2 rpm for 4 minutes.
[0096] It should be noted that when component (A-2) and mineral oil (hereinafter sometimes referred to as component (C)) are premixed, the Mooney viscosity (ML) of the ethylene random copolymer is... 1+4 The temperature (125℃) can be calculated using the following formula (1).
[0097] log(ML1 / ML2)=0.0066(ΔPHR) (1)
[0098] ML1: Mooney viscosity of ethylene random copolymer
[0099] ML2: Mooney viscosity of a mixture of ethylene random copolymer and component (C).
[0100] ΔPHR: The ratio of component (C) to 100 parts by mass of the ethylene random copolymer.
[0101] Component (A-2) can be manufactured by known methods or using commercially available products. Examples of methods for manufacturing component (A-2) include copolymerizing ethylene with at least one monomer selected from the group consisting of α-olefins having 3 or more and 10 or fewer carbon atoms in the presence of a known complex catalyst, such as a Ziegler-Natta catalyst, a metallocene complex, or a non-metallocene complex. It may also contain structural units derived from monomers other than ethylene and at least one monomer selected from the group consisting of α-olefins having 3 or more and 10 or fewer carbon atoms, such as non-conjugated dienes.
[0102] Examples of polymerization methods include slurry polymerization, solution polymerization, bulk polymerization, and gas-phase polymerization. Preferred examples of inert hydrocarbon solvents used in solution polymerization and slurry polymerization include propane, butane, isobutane, pentane, hexane, heptane, and octane. Two or more of these polymerization methods can be combined, and they can be either batch or continuous.
[0103] (B) Propylene polymers
[0104] The thermoplastic elastomer composition of the present invention contains (B) propylene polymers.
[0105] The propylene polymer (hereinafter sometimes referred to as component (B)) contained in the thermoplastic elastomer composition of the present invention is a propylene (co)polymer having more than 50% by mass and less than or equal to 100% by mass of structural units derived from propylene. Component (B) may have structural units derived from monomers other than propylene.
[0106] Since component (B) contains more than 50% by mass of propylene-derived structural units, it is a non-crosslinking or decomposable polymer compared to component (A), making it suitable for constituting the marine phase of the island structure of the thermoplastic elastomer composition of the present invention.
[0107] Other monomers besides propylene include ethylene and α-olefins with 4 or more carbon atoms, preferably ethylene and α-olefins with 4 or more but less than 20 carbon atoms.
[0108] Examples of α-olefins with 4 to 20 carbon atoms include: 1-butene, 1-pentene, 1-hexene, 1-heptene, 1-octene, 1-nonene, 1-decene, 1-undecene, 1-dodecene, 1-tetracene, 1-tetradecene, 1-pentadecaene, 1-hexadecene, 1-heptadecene, 1-octadecene, 1-nonadecaene, 1-eicosene, 3-methyl-1-butene, 3-methyl-1-pentene, 4-methyl-1-pentene, 2-ethyl-1-hexene, and 2,2,4-trimethyl-1-pentene. Monomers other than propylene can be used alone or in combination.
[0109] (B) The ratio of propylene-derived structural units, the ratio of ethylene-derived structural units, and the ratio of structural units derived from at least one monomer in the group consisting of α-olefins with 4 or more carbon atoms in propylene polymers can be determined by the same method as the ratio of each structural unit in (A) ethylene-α-olefin copolymers.
[0110] (B) The structure of the propylene polymer is not particularly limited. Examples include propylene homopolymers, propylene random copolymers, and multiphase propylene polymers. The thermoplastic elastomer compositions of the present invention may contain only one (B) propylene polymer or may contain two or more (B) propylene polymers.
[0111] (B) Propylene polymers can be manufactured by known methods or using commercially available products. Examples of methods for manufacturing propylene polymers include: polymerizing propylene (and other monomers as needed) in the presence of a Ziegler-Natta catalyst or a complex-type catalyst such as a metallocene complex or a non-metallocene complex. Examples of polymerization methods include: slurry polymerization, solution polymerization, bulk polymerization, and gas-phase polymerization. Preferred examples of inert hydrocarbon solvents used in solution polymerization and slurry polymerization include: propane, butane, isobutane, pentane, hexane, heptane, and octane. Two or more of these polymerization methods can be combined, and they can be either batch or continuous. Continuous gas-phase polymerization and bulk-gas-phase polymerization involving continuous bulk polymerization and gas-phase polymerization are preferred methods for manufacturing multiphase propylene polymer materials.
[0112] In this specification, the term "multiphase propylene polymeric material" refers to a mixture having the following structure: a copolymer (II) having dispersed structural units derived from ethylene, and structural units derived from propylene and structural units derived from at least one monomer selected from the group consisting of α-olefins having 4 or more carbon atoms, in a matrix of polymer (I) having more than 80% by mass and less than or equal to 100% by mass (wherein the total mass of the polymer is set to 100% by mass) (hereinafter sometimes simply referred to as "polymer (I)"), in a matrix of polymer (I) having more than 20% by mass and less than 90% by mass (wherein the total mass of the copolymer is set to 100% by mass) (hereinafter sometimes simply referred to as "copolymer (II)").
[0113] In component (B) of the multiphase propylene polymer material, when the total amount of the multiphase propylene polymer material is set to 100% by mass, the structural units derived from propylene are 50% by mass or more.
[0114] The amount of polymer (I) contained in the multiphase propylene polymer material is preferably 60% by mass or more and 90% by mass or less, more preferably 75% by mass or more and 85% by mass or less (wherein, the total amount of the multiphase propylene polymer material is set to 100% by mass). The amount of copolymer (II) contained in the multiphase propylene polymer material is preferably 10% by mass or more and 40% by mass or less, more preferably 15% by mass or more and 25% by mass or less (wherein, the total amount of the multiphase propylene polymer material is set to 100% by mass).
[0115] In copolymer (II), the α-olefin having 4 or more carbon atoms is preferably an α-olefin having 4 or more carbon atoms and 20 or fewer carbon atoms. Examples of α-olefins having 4 or more carbon atoms and 20 or fewer carbon atoms are the same as those of the monomers mentioned above, except for propylene. In copolymer (II), the α-olefin having 4 or more carbon atoms can be used alone or in combination of two or more.
[0116] The ratio of ethylene-derived structural units in copolymer (II) is preferably 22% by mass or more and 80% by mass or less, more preferably 25% by mass or more and 70% by mass or less, and even more preferably 27% by mass or more and 60% by mass or less (wherein the total amount of structural units derived from propylene and structural units derived from at least one monomer from the group consisting of α-olefins with 4 or more carbon atoms, and structural units derived from ethylene is set to 100% by mass). The ratio of propylene-derived structural units in copolymer (II) to structural units derived from at least one monomer from the group consisting of α-olefins with 4 or more carbon atoms is preferably 20% by mass or more and 78% by mass or less, more preferably 30% by mass or more and 75% by mass or less, and even more preferably 40% by mass or more and 73% by mass or less (wherein the total amount of structural units derived from propylene and structural units derived from at least one monomer from the group consisting of α-olefins with 4 or more carbon atoms, and structural units derived from ethylene is set to 100% by mass).
[0117] Preferred examples of copolymer (II) include: propylene-ethylene copolymer, ethylene-1-butene copolymer, ethylene-1-hexene copolymer, ethylene-1-octene copolymer, propylene-ethylene-1-butene copolymer, propylene-ethylene-1-hexene copolymer, and propylene-ethylene-1-octene copolymer, with propylene-ethylene copolymer being preferred. Copolymer (II) is generally a random copolymer.
[0118] From the viewpoint of moldability and mechanical properties, the melt flow rate (MFR) of the (B) propylene polymer, measured according to JIS K7210 at a temperature of 230°C and a load of 21.18 N, is preferably 0.3 g / 10 min or more and 200 g / 10 min or less. More preferably, the melt flow rate of the (B) propylene polymer is 2.5 g / 10 min or more and 105 g / 10 min or less.
[0119] (B) Intrinsic viscosity (hereinafter referred to as [η]) of the xylene insoluble portion of propylene polymers at 20°C (hereinafter referred to as the CXIS portion). cxis The concentration of dl / g is preferably 0.1 dl / g or more and 6.0 dl / g or less, more preferably 0.3 dl / g or more and 5.0 dl / g or less, and even more preferably 1.0 dl / g or more and 3.5 dl / g or less.
[0120] (B) Intrinsic viscosity of the xylene-soluble fraction (hereinafter referred to as CXS fraction) of propylene polymers at 20°C (hereinafter referred to as [η]). cxs The preferred concentration is 1.0 dl / g or higher and 6.0 dl / g or lower.
[0121] The intrinsic viscosity can be determined by following these steps: Measure the specific viscosity in tetrahydronaphthalene at 135°C using an Ubbelohde viscometer. Based on the obtained specific viscosity, calculate the intrinsic viscosity by extrapolation using the method described on page 491 of "Polymer Solutions, Polymer Experimentation 11" (Kyoritsu Publishing Co., Ltd., 1982).
[0122] Here, the CXS and CXIS fractions were obtained by the following method: Approximately 5 g of (B) propylene polymer was completely dissolved in 500 ml of boiling xylene. The resulting xylene solution was slowly cooled to 20°C and allowed to adjust at 20°C for at least 4 hours. The precipitate was then separated from the solution by filtration. This precipitate is the CXIS fraction. It should be noted that the substance obtained by removing the solvent from this solution is the xylene-soluble fraction (CXS fraction) at 20°C.
[0123] As (B) propylene polymers, propylene homopolymers, propylene-ethylene random copolymers, propylene-ethylene-1-butene random copolymers, or multiphase propylene polymers are preferred, propylene homopolymers or multiphase propylene polymers are more preferred, and propylene homopolymers are even more preferred.
[0124] (C) Mineral oil
[0125] The thermoplastic elastomer composition of the present invention may contain (C) mineral oil.
[0126] (C) mineral oil can be mixed with (A) ethylene-α-olefin copolymer, i.e. (A) ethylene-α-olefin copolymer can be filled with (C) mineral oil.
[0127] In this embodiment, the mineral oil (C) preferably used as a softener can be exemplified by high-boiling fractions of petroleum such as aromatic mineral oil, naphthenic mineral oil, and paraffinic mineral oil (average molecular weight 300-1500, pour point below 0°C). Among these, paraffinic mineral oil is preferred.
[0128] (C) Mineral oil is preferably added as a filler oil to (A) ethylene-α-olefin copolymer, and particularly preferably ethylene-α-olefin-nonconjugated diene copolymer. The method of addition can be a known method, for example: (1) a method of mechanically mixing the two using a mixing device such as a roller or a Banbury mixer; (2) a method of adding component (C) to a solution of component (A) prepared in solution form, and then desolvating it by means of stripping or the like.
[0129] When mineral oil (C) is used as the filler oil for the ethylene-α-olefin copolymer (A), the Mooney viscosity (ML) of the composition (oil-extended polymer) containing mineral oil (C) and ethylene-α-olefin copolymer (A) was measured at 125°C. 1+4The Mooney viscosity (ML) is preferably 5 or more and 300 or less, more preferably 10 or more and 250 or less, and even more preferably 40 or more and 200 or less. It should be noted that this Mooney viscosity (ML) 1+4 (125℃) was measured according to JIS K6300.
[0130] From the viewpoint of achieving the Mooney viscosity described above, the amount of mineral oil added (C) is preferably 20 to 90 parts by mass relative to 100 parts by mass of the total mass of (A) ethylene-α-olefin copolymer and (C) mineral oil, more preferably 25 to 80 parts by mass, and even more preferably 30 to 60 parts by mass.
[0131] (D) Crosslinking agent
[0132] In the thermoplastic elastomer composition of the present invention, it is preferable to form an island structure. Therefore, it is preferable to manufacture the thermoplastic elastomer composition by a process of melt-blending a mixture containing (A) an ethylene-α-olefin copolymer and (B) a propylene polymer in the presence of a (D) crosslinking agent.
[0133] As the preferred (D) crosslinking agent used in this embodiment, crosslinking agents commonly used for rubber crosslinking can be used, such as: organic peroxides, phenolic resins, sulfur, sulfur-containing compounds, p-benzoquinone, derivatives of p-benzoquinone dioxime, bismaleimide compounds, epoxy compounds, silane compounds, and amino resins. Among these, organic peroxides and phenolic resins are preferred.
[0134] Examples of organic peroxides include: ketone peroxides, diacyl peroxides, hydroperoxides, dialkyl peroxides, peroxyketals, alkyl peresters, percarbonates, peroxydicarbonates, and peroxide esters.
[0135] Specific examples of organic peroxides include: dicumyl peroxide, 2,5-dimethyl-2,5-di(tert-butylperoxide)hexane, 2,5-dimethyl-2,5-di(tert-butylperoxide)hexyne, 1,3-bis(tert-butylperoxide isopropyl)benzene, tert-butylcumyl peroxide, di-tert-butyl peroxide, 2,2,4-trimethylpentyl-2-hydroperoxide, diisopropylbenzene hydrogen peroxide, cumyl peroxide, tert-butyl peroxide, 1,1-di(tert-butylperoxide)-3,5,5-trimethylcyclohexane, 1,1-di-tert-butylperoxide cyclohexane, isobutyl peroxide, 2,4-dichlorobenzoyl peroxide, o-methylbenzoyl peroxide, bis(3,5,5-trimethylhexanoyl) peroxide, lauroyl peroxide, benzoyl peroxide, and p-chlorobenzoyl peroxide. Among them, 2,5-dimethyl-2,5-di(tert-butylperoxide)hexane and 2,5-dimethyl-2,5-di(tert-butylperoxide)hexyne are preferred.
[0136] Organic peroxides can be used alone or in combination with two or more.
[0137] The organic peroxide used in this embodiment can be in any form, including liquid, powder, and granules. Furthermore, to ensure good dispersibility, it is more preferable to dilute the organic peroxide with an inorganic filler, mineral diluent such as oil or solvent, which is inert to crosslinking reactions. Additionally, it is more preferable to add it in a liquid state. Among these, paraffin-based oils are preferred diluents, considering their operability and impact on the product.
[0138] To ensure a uniform and slow crosslinking reaction, organic peroxides and crosslinking aids can be used in combination. As crosslinking aids, multifunctional compounds such as sulfur compounds, methacrylates (salts), and maleimides can be used. Examples of crosslinking aids include: sulfur, p-benzoquinone dioxime, p,p'-dibenzoyl-p-benzoquinone dioxime, ethylene glycol dimethacrylate, diethylene glycol dimethacrylate, triethylene glycol dimethacrylate, tetraethylene glycol dimethacrylate, polyethylene glycol dimethacrylate, trimethylolpropane trimethacrylate, diallyl phthalate, tetraallyl propoxy ethane, triallyl isocyanurate, N,N'-m-phenylene bismaleimide, maleic anhydride, divinylbenzene, zinc diacrylate, and zinc dimethacrylate. Preferably, N,N'-m-phenylene bismaleimide, p,p'-dibenzoyl-p-benzoquinone dioxime, divinylbenzene, trimethylolpropane trimethacrylate, or triallyl isocyanurate are used. N,N'-m-phenylene bismaleimide can also be used alone as a crosslinking agent.
[0139] (D) There is no particular limitation on the amount of crosslinking agent added, and those skilled in the art can appropriately set the amount of (D) crosslinking agent added to be suitable for crosslinking (A) ethylene-α-olefin copolymer at the desired level.
[0140] (D) Crosslinking agents sometimes decompose in processes used for crosslinking (A) ethylene-α-olefin copolymers, such as melt blending. Therefore, the suitable amount of (D) crosslinking agent is not specified as the amount of (D) crosslinking agent remaining in the thermoplastic elastomer composition of the present invention, but is generally specified as the amount of (D) crosslinking agent before melt blending (A) ethylene-α-olefin copolymer and (B) propylene polymer in the presence of (D) crosslinking agent.
[0141] Relative to 100 parts by mass of the total amount of (A) ethylene-α-olefin copolymer and (B) propylene polymer, the amount of (D) crosslinking agent before melt mixing is preferably 0.001 parts by mass or more and 3.0 parts by mass or less, more preferably 0.01 parts by mass or more and 2.0 parts by mass or less, and even more preferably 0.3 parts by mass or more and 1.0 parts by mass or less.
[0142] When the crosslinking aid is used together with (D) crosslinking agent, the amount of crosslinking aid before melt mixing is preferably 0.01 parts by mass or more and 10 parts by mass or less, more preferably 0.5 parts by mass or more and 1.0 parts by mass or less, relative to 100 parts by mass of the total amount of (A) ethylene-α-olefin copolymer and (B) propylene polymer.
[0143] (E) Inorganic packing
[0144] The thermoplastic elastomer composition of the present invention may contain (E) inorganic fillers.
[0145] By including (E) inorganic fillers, the thermoplastic elastomer composition of this embodiment can possess excellent properties, such as mechanical strength and dimensional stability.
[0146] Examples of inorganic fillers include: talc, clay, calcium carbonate, barium carbonate, magnesium carbonate, zinc carbonate, calcium sulfate, barium sulfate, magnesium sulfate, zinc oxide, iron oxide, calcium oxide, magnesium oxide, aluminum oxide, titanium oxide, barium oxide, calcium silicate, calcined kaolin, glass fiber, hollow glass spheres, zeolite, silica, diatomaceous earth, asbestos, metal soap, titanium dioxide, mica, and potassium titanate fiber. Among these, calcium carbonate, talc, silica, or clay are preferred, with calcium carbonate being even more preferred. (E) Inorganic fillers can be used alone or in combination with two or more types.
[0147] (E) There is no particular limitation on the amount of inorganic filler used. For example, it can be used in an amount of 50 parts by mass or less, preferably 1 part by mass or more and 40 parts by mass or less, and particularly preferably 10 parts by mass or more and 20 parts by mass or less, relative to 100 parts by mass of the total mass of (A) ethylene-α-olefin copolymer and (B) propylene polymer.
[0148] (F) Ethylene resins
[0149] The thermoplastic elastomer composition of the present invention may contain an ethylene resin (hereinafter also referred to as "(F) component") with a ratio of (F) structural units derived from ethylene of 80% by mass or more.
[0150] By using an ethylene-based resin that also contains 80% or more of structural units derived from ethylene (F), the thermoplastic elastomer composition of this embodiment can possess excellent properties, such as high rigidity and durability.
[0151] When the thermoplastic elastomer composition of this embodiment is manufactured by a manufacturing method having a two-stage melt-blending process, the rigidity and flowability of the thermoplastic elastomer composition can be improved more effectively by adding component (F) in the second melt-blending process. In this case, it is preferable not to add crosslinking agent (D) in the second melt-blending process.
[0152] From the viewpoint of mechanical properties, (F) among ethylene resins in which the proportion of structural units derived from ethylene is 80% by mass or more, the proportion of structural units derived from ethylene is preferably 90% by mass or more, and more preferably 95% by mass or more.
[0153] (F) In addition to having structural units derived from ethylene, the component may also have structural units derived from at least one monomer selected from the group consisting of α-olefins having 3 or more and 10 or fewer carbon atoms. Examples of α-olefins having 3 or more and 10 or fewer carbon atoms include cyclic olefins such as propylene, 1-butene, 2-methylpropene, 1-pentene, 3-methyl-1-butene, 1-hexene, 3-methyl-1-pentene, 4-methyl-1-pentene, 1-heptene, 1-octene, 1-nonene, 1-decene, and vinylcyclohexane.
[0154] Component (F) may contain two or more structural units derived from α-olefins having 3 or more but less than 10 carbon atoms. The structural units derived from at least one monomer selected from the group consisting of α-olefins having 3 or more but less than 10 carbon atoms are preferably examples of: structural units derived from propylene, structural units derived from 1-butene, structural units derived from 4-methyl-1-pentene, structural units derived from 1-hexene, or structural units derived from 1-octene. Component (F) may have structural units derived from monomers other than ethylene and α-olefins having 3 or more but less than 10 carbon atoms.
[0155] (F) The density of component (F) is not particularly limited, but from the viewpoint of improving the mechanical properties and rigidity of the thermoplastic elastomer composition, 950 kg / m³ is preferred. 3 The above, more preferably 955 kg / m 3 The above is particularly preferred, with 960 kg / m³ being the optimal value. 3 above.
[0156] From a lightweight perspective, the density of component (F) is preferably 1000 kg / m³. 3 the following.
[0157] (F) The MFR of the component is not particularly limited. From the viewpoint of flowability, the MFR measured under the conditions of 190°C and 21.18N load is preferably 0.1g / 10min or more, more preferably 1g / 10min or more, and particularly preferably 10g / 10min or more.
[0158] From the viewpoint of surface smoothness of the molded article, the MFR of the (F) component measured under the conditions of 190°C and 21.18N load is preferably 100g / 10min or less, more preferably 50g / 10min or less, and particularly preferably 20g / 10min or less.
[0159] There is no particular limitation on the amount of component (F). From the viewpoint of rigidity and durability, the amount of component (F) is preferably 10 parts by mass or more, more preferably 30 parts by mass or more, and particularly preferably 60 parts by mass or more, relative to 100 parts by mass of (A) ethylene-α-olefin copolymer.
[0160] From the viewpoint of flexibility, the amount of component (F) used is preferably 200 parts by mass or less, more preferably 100 parts by mass or less, and particularly preferably 70 parts by mass or less, relative to 100 parts by mass of (A) ethylene-α-olefin copolymer.
[0161] Other ingredients
[0162] The thermoplastic elastomer composition of the present invention may contain various components and additives, except for (A) ethylene-α-olefin copolymer and (B) propylene polymer, which are essential components, and (C) mineral oil, (D) crosslinking agent, (E) inorganic filler and (F) ethylene resin, which are preferred components, in a ratio of 80% by mass or more.
[0163] As various ingredients and additives, it may contain polymers or oligomers other than those mentioned above (A), (B), and (F), lubricants, softeners other than mineral oil mentioned above (C), organic fillers (e.g., fibers, wood flour, cellulose powder, carbon fibers, graphite, and carbon black), antioxidants (e.g., phenolic antioxidants, sulfur-containing antioxidants, phosphorus-containing antioxidants, lactone antioxidants, and vitamin antioxidants), weather stabilizers, ultraviolet absorbers (e.g., benzotriazole ultraviolet absorbers, triazine ultraviolet absorbers, aniline ultraviolet absorbers, and benzophenone ultraviolet absorbers), heat stabilizers, and light stabilizers (e.g., hindered amine light stabilizers and benzoic acid). Ester light stabilizers), pigments (e.g., inorganic pigments, organic pigments, and pigment dispersants), nucleating agents, foaming agents, foaming nucleating agents, plasticizers, flame retardants, brightening agents, antibacterial agents, light diffusing agents, adsorbents, metal oxides (e.g., zinc oxide and magnesium oxide), wetting and dispersing agents, VOC / odor removal agents, water-retaining agents (e.g., aqueous media containing amphiphilic polymers), abrasion resistance enhancers, metal chlorides (e.g., ferric chloride and calcium chloride), hydrotalcite, lubricants (e.g., hydrocarbon lubricants, fatty acid lubricants, fatty acid amide lubricants, ester lubricants, alcohol lubricants, metal soap lubricants, organosilicon lubricants such as silicone oil, silicone rubber, and inorganic lubricants), and aluminates. These components and additives can be used alone or in combination of two or more.
[0164] Examples of resins other than components (A), (B), and (F) include: olefin resins (excluding substances equivalent to components (A), (B), and (F)), olefin elastomers (excluding substances equivalent to components (A), (B), and (F)), aromatic vinyl / conjugated diene copolymers (copolymers having structural units derived from aromatic vinyl compounds and structural units derived from conjugated diene compounds), polyphenylene ether resins, polyamide resins, polyester resins, polyoxymethylene resins, and polymethyl methacrylate resins.
[0165] Examples of aromatic vinyl / conjugated diene copolymers (copolymers having structural units derived from aromatic vinyl compounds and structural units derived from conjugated diene compounds) include: aromatic vinyl compound-conjugated diene compound polymers, aromatic vinyl compound-conjugated diene compound-aromatic vinyl compound polymers, and their hydrogenated products. The hydrogenated products of aromatic vinyl compound-conjugated diene compound-aromatic vinyl compound polymers are preferred.
[0166] Thermoplastic elastomer compositions
[0167] The thermoplastic elastomer composition of the present invention contains 100 parts by weight of (A) an ethylene-α-olefin copolymer and 20 to 90 parts by weight of (B) a propylene polymer.
[0168] By having the above-described proportions, the thermoplastic elastomer composition of the present invention readily forms an island structure in which an island phase mainly composed of (A) ethylene-α-olefin copolymer is dispersed in an ocean phase mainly composed of (B) propylene polymers. By having the physical properties of a thermoplastic elastomer composition, represented by thermoplasticity and rubber elasticity, and also possessing the other necessary conditions of the present invention, the effect of the present invention, which is to be able to manufacture molded articles with excellent crack resistance, can be achieved.
[0169] From the viewpoint of formability and mechanical properties, the thermoplastic elastomer composition of the present invention preferably contains 25 or more parts by mass of (B) propylene polymer relative to 100 parts by mass of (A) ethylene-α-olefin copolymer, and more preferably contains 30 or more parts by mass of (B) propylene polymer.
[0170] On the other hand, from the viewpoint of flexibility, the thermoplastic elastomer composition of the present invention preferably contains 70 or less parts by weight of (B) propylene polymer relative to 100 parts by weight of (A) ethylene-α-olefin copolymer, and more preferably contains 50 or less parts by weight of (B) propylene polymer.
[0171] The thermoplastic elastomer composition of the present invention can be a composition containing carbon-14 (14C) as a constituent element, or it can be a composition obtained by recycling materials (mechanical recycling).
[0172] The concentration of carbon-14 (14C) in the thermoplastic elastomer composition was determined as pMC (percentage of modern carbon, in %) by AMS (Accelerator mass spectrometry) as specified in ISO 16620-2:2019.
[0173] It is known that carbon-14 (14C) is present in a certain proportion in carbon dioxide in the atmosphere, and therefore plants that grow by ingesting atmospheric carbon dioxide, such as corn and trees, contain 14C. Furthermore, it is known that petroleum or other fossil resources, which are believed to be stored underground for a long time, contain almost no carbon-14 (14C). Therefore, by using plant-derived substances in the raw materials of the monomers of component (A) ethylene-α-olefin copolymer, component (B) propylene polymer, and / or component (C) mineral oil used in thermoplastic elastomer compositions, it is possible to include carbon-14 (14C) in the constituent elements of the thermoplastic elastomer.
[0174] In the manufacture of ethylene resins in which the components (A) ethylene-α-olefin copolymers and / or components (B) propylene polymers, optional components (C) mineral oils and / or (F) ethylene-derived structural units are present in a ratio of 80% by mass or more, monomers derived from fossil resources (e.g., ethylene, propylene, 1-butene, 1-hexene), plant-derived monomers (e.g., ethylene, propylene, 1-butene, 1-hexene), and chemically recycled monomers (e.g., ethylene, propylene, 1-butene, 1-hexene) may be used, and two or more of them may be used in combination.
[0175] As specific combinations of monomers, examples include: ethylene derived from fossil resources / ethylene derived from plants / chemically recycled ethylene; propylene derived from fossil resources / propylene derived from plants / chemically recycled propylene; propylene derived from fossil resources / propylene derived from plants / chemically recycled propylene / ethylene derived from fossil resources / ethylene derived from plants / chemically recycled ethylene.
[0176] Monomers derived from fossil resources use carbon from underground resources such as petroleum, coal, and natural gas as their source and typically contain almost no carbon-14 (14C). Well-known methods for producing monomers derived from fossil resources include, for example, methods for producing olefins through the cracking of naphtha / ethane derived from petroleum and the dehydrogenation of ethane / propane.
[0177] Plant-derived monomers use carbon that cycles through the Earth's surface in the form of plants and animals as their source, and typically contain a certain proportion of carbon-14 (14C). Examples of methods for manufacturing plant-derived monomers include the cracking of bio-naphtha / vegetable oil / animal oil, the dehydrogenation of bio-propane, methods for separating alcohols from fermentation products such as sugars extracted from plant raw materials such as sugarcane or corn and then subjecting them to dehydration reactions (e.g., Japanese Patent Publication Nos. 2010-511634, 2011-506628, and 2013-503647), and methods for reacting ethylene obtained from plant-derived ethanol with n-butene via a metathesis reaction (e.g., WO2007 / 055361).
[0178] Chemically recycled monomers use carbon generated from the decomposition and combustion of waste as a source, and the amount of carbon-14 (14C) they contain varies depending on the waste. Known methods for manufacturing chemically recycled monomers include, for example, methods for thermally decomposing waste plastics (e.g., Japanese Patent Application Publication No. 2017-512246), methods for cracking waste vegetable oil / waste animal oil (e.g., Japanese Patent Application Publication No. 2018-522087), and methods for gasifying / alcoholizing / dehydrating waste such as kitchen waste / biomass waste / food waste / waste oil / waste wood / waste paper / and / or waste plastics (e.g., Japanese Patent Application Publication No. 2019-167424 and WO2021 / 006245).
[0179] When using two or more olefins derived from fossil resources, olefins derived from plants, and chemically recycled olefins, the olefins manufactured separately can be mixed in combinations such as olefins derived from fossil resources / olefins derived from plants, olefins derived from fossil resources / chemically recycled olefins, olefins derived from plants / chemically recycled olefins, and olefins derived from fossil resources / olefins derived from plants / chemically recycled olefins. Alternatively, a substance can be manufactured in the form of a mixture of the above-mentioned olefin combinations by using a mixture of compounds derived from fossil resources / compounds derived from plants, compounds derived from fossil resources / chemically recycled compounds, compounds derived from plants / chemically recycled compounds, and compounds derived from fossil resources / compounds derived from plants / chemically recycled compounds as a raw material / intermediate in the olefin manufacturing process.
[0180] As a component containing C14 (14C), the ethylene-α-olefin copolymer can be a commercially available ethylene copolymer or an ethylene polymer having more than 90% by mass of monomer units derived from ethylene. Examples include: the "I'M GREEN" series manufactured by Braskem, the "TRUCIRCLE" series manufactured by SABIC, and the "CirculenRenew" series manufactured by LyondellBasell.
[0181] As a component containing carbon-14 (14C), (B) propylene polymers can be commercially available propylene polymers. Examples include: the "Bornewables" series manufactured by Borealis, the "TRUCIRCLE" series manufactured by SABIC, and the "CirculenRenew" series manufactured by LyondellBasell.
[0182] From the viewpoint of reducing environmental impact, the C14 (14C) concentration of the thermoplastic elastomer composition is preferably 0.2 pMC% or more, more preferably 0.5 pMC% or more, even more preferably 1 pMC% or more, and even more preferably 5 pMC% or more, particularly preferably 10 pMC% or more. From the viewpoint of cost, it is preferably 99 pMC% or less, more preferably 95 pMC% or less, even more preferably 90 pMC% or less, even more preferably 70 pMC% or less, and particularly preferably 50 pMC% or less.
[0183] The carbon-14 (14C) concentration of a thermoplastic elastomer composition can be adjusted by changing the ratio of fossil-derived olefins, plant-derived olefins, and chemically recycled olefins used in the manufacture of the thermoplastic elastomer composition.
[0184] The method for manufacturing the thermoplastic elastomer composition of the present invention is not particularly limited, but it is preferably manufactured by a method including a step of blending (preferably melt blending) the (A) ethylene-α-olefin copolymer and (B) propylene polymer (and various additives represented by components (C) to (F) as needed) as raw materials. For example, blending can be carried out by conventional methods using a conventional extruder, Banbury mixer, roller, Brabender plastograph, or Kneader Brabender. It is preferred to manufacture by melt blending using an extruder, especially a twin-screw extruder. In addition, all the components to be blended can be melt blended together, or a portion of the components can be blended and then the remaining components added and melt blended, and one or more melt blending processes can be performed. The temperature during melt blending is preferably 150°C to 300°C, more preferably 180°C to 250°C. The time during melt blending is preferably 20 seconds to 30 minutes, more preferably 30 seconds to 20 minutes. The ingredients to be mixed can be added in any order, or at the same time.
[0185] In manufacturing the thermoplastic elastomer composition of the present invention, crosslinking may or may not be performed. From the viewpoint of controlling the island structure and melt viscosity, crosslinking is preferred.
[0186] In the preferred manufacturing method where crosslinking is performed, it is preferable to carry out the process of melt-blending (A) ethylene-α-olefin copolymer and (B) propylene polymer in the presence of (D) crosslinking agent.
[0187] When using (A) ethylene-α-olefin copolymer, the Mooney viscosity (ML) of (A) ethylene-α-olefin copolymer is preferred. 1+4The melt flow rate of (B) propylene polymers was 0.3 g / 10 min to 200 g / 10 min, measured at 230 °C and under a load of 21.18 N, with a value of 40 or higher at 125 °C.
[0188] When (A) ethylene-α-olefin copolymer is filled with (C) mineral oil, it is preferable to perform a process of melt-blending the oil-extended polymer containing (C) mineral oil and (A) ethylene-α-olefin copolymer with (B) propylene polymer in the presence of (D) crosslinking agent. The preferred Mooney viscosity (ML) of the oil-extended polymer is... 1+4 The melt flow rate of (B) propylene polymers was 0.3 g / 10 min to 200 g / 10 min, measured at 230 °C and under a load of 21.18 N, with a value of 30 or higher at 125 °C.
[0189] When performing more than two melt-blending operations, it is preferable to first melt-blend (A) ethylene-α-olefin copolymer and (B) propylene polymer in the presence of (D) crosslinking agent in a previous step, and then in a subsequent step, add (F) ethylene-derived structural units at a ratio of 80% by mass or more to the melt blend obtained in the previous step, and further melt-blend. By performing the subsequent step, the rigidity of the resulting thermoplastic elastomer composition is further improved.
[0190] The temperature during the subsequent melt-mixing process is preferably 150°C to 300°C, more preferably 180°C to 250°C. The melt-mixing time is not particularly limited, but is preferably 5 seconds to 30 minutes, more preferably 10 seconds to 10 minutes.
[0191] Subsequent processes are preferably carried out under conditions where (D) crosslinking agent is substantially absent.
[0192] The thermoplastic elastomer composition of the present invention achieves significant technical effects of high practical value, such as low high-speed surface impact energy and excellent crack resistance of the resulting molded article, by having the monomer reactivity ratio product r1r2 of the (A) ethylene-α-olefin copolymer, which is a component thereof, below a specified value, and simultaneously possessing all other necessary conditions of the present invention.
[0193] The high-speed surface impact energy of the thermoplastic elastomer composition of the present invention is not particularly limited. The high-speed surface impact energy of the puncture point obtained in the high-speed surface impact test of an injection molded body with a length of 150 mm, a width of 90 mm, and a thickness of 2.0 mm, obtained by injection molding of the thermoplastic elastomer composition at a molding temperature of 220°C and a mold temperature of 50°C, under the conditions of a 1 / 2-inch piercing pin diameter, a piercing pin speed of 2.8 m / s, and a test temperature of 23°C, is preferably 12.0 J or less, more preferably 10.9 J or less, further preferably 10.3 J or less, and particularly preferably 10.0 J or less.
[0194] When the high-speed surface impact energy is below the aforementioned upper limit, the molded body obtained from the thermoplastic elastomer composition has excellent cracking resistance. For example, in the case of a skin material for an automotive dashboard, it can be easily cracked when the airbag deploys, even without tear line processing.
[0195] From the perspectives of impact resistance, vacuum forming properties, and sag, the aforementioned high-speed surface impact energy is preferably 3.0J or more, more preferably 5.0J or more, and particularly preferably 9.0J or more.
[0196] The high-speed surface impact energy can be appropriately adjusted by regulating the product of the monomer reactivity ratios r1 and r2 of the (A) ethylene-α-olefin copolymer. For example, the high-speed surface impact energy can be reduced by decreasing r1 and r2.
[0197] The melt flow rate (MFR) of the thermoplastic elastomer composition of the present invention is not particularly limited. The MFR measured according to JIS K7210 at a temperature of 230°C and a load of 98.07 N is preferably 0.1 g / 10 min to 300 g / 10 min, more preferably 0.5 g / 10 min to 100 g / 10 min, and particularly preferably 5 g / 10 min to 90 g / 10 min.
[0198] From the viewpoint of ensuring fluidity for molding, it is preferable that the melt flow rate (MFR) of the thermoplastic elastomer composition is above the aforementioned lower limit value.
[0199] From the viewpoint of suppressing burrs during injection molding and ensuring uniform sheet thickness during extrusion molding, it is preferable that the melt flow rate (MFR) of the thermoplastic elastomer composition is below the aforementioned upper limit value.
[0200] The melt flow rate (MFR) of the thermoplastic elastomer composition of the present invention can be appropriately adjusted by selecting and adjusting the type, properties, compounding amount and manufacturing conditions of each component constituting the thermoplastic elastomer composition. For example, the MFR can be reduced by increasing (A) the amount of ethylene-α-olefin copolymer and (B) reducing the amount of propylene polymer.
[0201] The hardness of the thermoplastic elastomer composition of the present invention is not particularly limited, and the molded body made from the thermoplastic elastomer composition (for example, using a 25mm T-die with a width of 100mm) can be molded. The extruder melts and extrudes the material from a T-die under conditions of a barrel temperature of 220°C, a fully threaded screw, and a screw speed of 40 rpm. The extruded molten film is then air-cooled along a metal roller to form an extruded molded body (approximately 95 mm wide and 1.0 mm thick). Six such extruded bodies are stacked to produce a sample with a thickness of 6 mm. The Shore A hardness, measured using a hardness tester according to JIS K6253, is preferably 40–100, more preferably 50–95, and particularly preferably 60–90.
[0202] From the perspective of mechanical properties and formability, it is preferable that the Shore A hardness is above the lower limit value.
[0203] From the viewpoint of flexibility, it is preferable that the Shore A hardness is below the aforementioned upper limit value.
[0204] The Shore A hardness can be appropriately adjusted by selecting and regulating the types, properties, proportions, and manufacturing conditions of the components constituting the thermoplastic elastomer composition. For example, the Shore A hardness can be increased by reducing (A) the amount of ethylene-α-olefin copolymer and (B) increasing the amount of propylene polymer.
[0205] The compression set (C. Set) of the thermoplastic elastomer composition of the present invention is not particularly limited. The compression set of a molded article made from the thermoplastic elastomer composition (e.g., a molded article with a thickness of approximately 2.1 mm produced by preheating the thermoplastic elastomer composition at 180°C and a maximum pressure of 10 MPa for 3 minutes, pressing for 3 minutes, and then cooling and pressing for 3 minutes) under the conditions of a compression ratio of 25% as measured according to JIS K6262, a test temperature of 70°C, and a test time of 22 hours is preferably 36% or more to 70% or less. More preferably, the compression set is 60% or less; further preferably, 58% or less; and particularly preferably, 55% or less. More preferably, the compression set is 10% or more; further preferably, 20% or more; and particularly preferably 36% or more.
[0206] From the viewpoint of rubber elasticity, it is preferable that the compression set is below the aforementioned upper limit value.
[0207] From the perspective of mechanical properties and formability, it is preferable that the compression set is above or above the lower limit value.
[0208] The compression set (C. Set) of the thermoplastic elastomer composition of the present invention can be adjusted by selecting and adjusting the amount of oil, as well as the type, properties, proportions, and manufacturing conditions of each component constituting the thermoplastic elastomer composition. For example, compression set can be reduced by decreasing the amount of (B) propylene polymer, increasing the amount of (A) ethylene-α-olefin copolymer, and increasing the amount of (D) crosslinking agent. Furthermore, when using (C) mineral oil, the compression set can also be appropriately adjusted by adjusting the amount of (C) mineral oil.
[0209] The use of the thermoplastic elastomer compositions of the present invention is not particularly limited, but they are preferably used in various applications where thermoplastic elastomers have historically been suitable. They are particularly preferred for constituting part or all of various components or articles manufactured by injection molding or extrusion molding.
[0210] Injection-molded articles, which are preferred applications of the thermoplastic elastomer composition of the present invention, can be manufactured using the thermoplastic elastomer composition of the present invention, for example, using conventional injection molding or various molding methods as needed, such as gas injection molding, injection compression molding, or short-shot foaming molding. The molding conditions in the above-described injection molding are not particularly limited, and can be carried out under conditions of a molding temperature of typically 100°C to 300°C, preferably 180°C to 280°C, an injection pressure of 5 MPa to 100 MPa, preferably 10 MPa to 80 MPa, and a mold temperature of 20°C to 80°C, preferably 20°C to 60°C.
[0211] The thermoplastic elastomer composition of the present invention can be used for a variety of applications without particular limitation. It achieves significant technical effects of high practical value, such as low high-speed surface impact energy and excellent crack resistance in the resulting molded articles. Furthermore, it can impart various other properties derived from the thermoplastic elastomer composition, making it particularly suitable for use as a surface material for interior parts of various vehicles, such as dashboards and glove boxes, and automobiles. It is also suitable for various components of household appliances, residential equipment machinery, industrial components, and building materials, including various automotive interior and exterior parts, but the applications of the present invention are not limited to these.
[0212] Example
[0213] The present invention will now be described in more detail based on embodiments, but the present invention is not limited to these embodiments.
[0214] The physical properties and characteristics of the examples / comparative examples were evaluated using the following methods.
[0215] 1. The product of monomer reactivity ratios r1r2
[0216] The determination of ethylene-α-olefin copolymers was carried out under the following conditions. 13 C-NMR was used to determine the product of monomer reactivity ratios using the method described in Cheng, Macromolecules, 17, 1950 (1984).
[0217] • Equipment: AvanceNEO 600 (10mm cryogenic probe) manufactured by Bruker
[0218] • Solvent for determination: 1,2-dichlorobenzene / 1,1,2,2-tetrachloroethane-d2 (85 / 15 volume ratio)
[0219] • Measurement temperature: 135℃
[0220] • Measurement method: Powergate proton decoupling method
[0221] • Pulse width: 45 degrees
[0222] • Pulse repetition time: 4 seconds
[0223] • Total number of times: 256
[0224] • Chemical shift value standard: tetramethylsilane
[0225] The following example illustrates the method for determining the product of monomer reactivity ratios of the ethylene-α-olefin copolymer (A-2-i) used in Example 1. In the copolymer, S represents a secondary carbon atom, and T represents a tertiary carbon atom. They are classified using Greek letters chosen based on their distance from the nearest tertiary carbon atoms on either side, such as αα, αδ, βδ, δδ, and γδ. α, β, and γ represent the positions of the first, second, and third atoms in the molecular chain, respectively, starting from the nearest tertiary carbon atom. δ represents the position of the fourth and subsequent atoms in the molecular chain, starting from the nearest tertiary carbon atom. The following structure illustrates an example of the classification of secondary carbon atoms based on these symbols. This structure represents a portion of the copolymer's structure with hydrogen atoms omitted.
[0226]
[0227] like Figure 1 The identification shown originates from individual carbon atoms. 13 C-NMR peaks. Figure 1 The peak areas of the respective spectra are as follows.
[0228] Tββ: 0.8082
[0229] Tβδ: 2.8015
[0230] Tδδ: 7.2456
[0231] Sβδ: 14.126
[0232] Sδδ: 37.202
[0233] Sγδ: 12.993
[0234] The peak areas PP, PE, and EE derived from the monomer units bonded in a propylene-propylene-propylene sequence were calculated using the following formulas and normalized to a total of 100 mol%.
[0235] PP=Tββ+1 / 2Tβδ
[0236] EE = 1 / 2(Sβδ + Sδδ) + 1 / 4Sγδ
[0237] PE=Tβδ+2Tδδ
[0238] The product of the monomer reactivity ratios (r1 of ethylene and r2 of propylene) of the ethylene-α-olefin copolymer is calculated using the following formula (3).
[0239] r1r2=EE{PP / (PE / 2) 2 Equation (3)
[0240] 2. Melt Flow Rate (MFR, unit: g / 10 min)
[0241] The measurements were performed according to JIS K7210 under the conditions of 230℃ temperature, 98.07N load, and method B.
[0242] 3. Manufacturing method of extruded molded articles
[0243] The USV25mm die was manufactured by Union Plastics, which uses a T-die with a width of 100mm. The thermoplastic elastomer compositions of the examples and comparative examples were melt-extruded from a T-die under the conditions of a barrel temperature of 220°C, a fully threaded screw, and a screw speed of 40 rpm in an extruder. The extruded molten film was air-cooled along a metal roller to form an extruded molded body (approximately 95 mm wide and 1.0 mm thick).
[0244] 4. Hardness
[0245] Following JIS K 6253, six extruded bodies obtained by the method described in section 3 above were overlapped to produce a sample with a thickness of 6 mm. The instantaneous Shore A hardness was obtained using a hardness tester.
[0246] 5. Manufacturing method of compressed tablets
[0247] The thermoplastic elastomer compositions of the examples or comparative examples were heated and pressed for 5 minutes at a temperature of 200°C and a maximum pressure of 10 MPa using a compression molding machine F-37 manufactured by Shinto Metal Industries, Ltd., and then cooled and pressed for 5 minutes at a temperature of 23°C and a maximum pressure of 10 MPa to produce compressed sheets (150 mm in length, 150 mm in width, and 2.2 mm in thickness).
[0248] 6. Compression set
[0249] Large test pieces were prepared from the compressed sheet obtained by the method described in section 5 above, according to JIS K 6262. The compression set was measured under the conditions of a test temperature of 70°C, a compression ratio of 25%, and a test time of 22 hours.
[0250] 7. Manufacturing method of injection molded articles
[0251] Using an IS100EN-3A injection molding machine manufactured by Toshiba Machine Co., Ltd., the thermoplastic elastomer compositions manufactured in the examples and comparative examples were injection molded at a molding temperature of 220°C and a mold temperature of 50°C, thereby obtaining injection molded bodies with a length of 150 mm, a width of 90 mm, and a thickness of 2.0 mm.
[0252] 8. High-speed surface impact energy
[0253] High-speed surface impact tests were conducted on the injection-molded bodies manufactured in step 7 above using a Hydroshot HITS-P10 manufactured by Shimadzu Corporation under the conditions of a 1 / 2-inch firing pin diameter, a firing pin speed of 2.8 m / s, a test piece support platform diameter of 40 mm, and a test temperature of 23°C. The high-speed surface impact energy at the puncture point was measured.
[0254] 9. Evaluation of crackability
[0255] Based on the high-speed surface impact energy value obtained in section 8 above, the crackability was evaluated according to the following criteria.
[0256] A: The high-speed surface impact energy is below 10.3J, confirming very good crackability.
[0257] B: High-speed surface impact energy is greater than 10.3J and less than or equal to 10.9J, confirming good crackability.
[0258] C: High-speed surface impact energy greater than 10.9J and less than or equal to 12.0J confirms easy cracking.
[0259] D: High-speed surface impact energy is greater than 12.0J, and crackability has not been confirmed.
[0260] Details of the materials used in the examples / comparative examples are described below.
[0261] <Component (A)> Ethylene-α-olefin copolymer
[0262] (A-2-i)+(C): Oil-extended ethylene-propylene-5-ethylidene-2-norbornene copolymer (a mixture of 100 parts by weight of component (A-2-i) and 50 parts by weight of component (C))
[0263] Mooney viscosity (ML) of (A-2-i)+(C) 1+4 125℃) = 53
[0264] The Mooney viscosity (ML) of (A1-i) calculated from the above equation (1) 1+4 125℃) = 113
[0265] Composition of (A-2-i)
[0266] The percentage of structural units derived from ethylene is 63.2% by mass.
[0267] The percentage of structural units derived from propylene is 32.5% by mass.
[0268] The ratio of structural units derived from 5-ethimide-2-norbornene is 4.3% by mass.
[0269] EE = 59.7 mol%
[0270] PP = 4.6 mol%
[0271] PE = 35.7 mol%
[0272] r1r2=0.86
[0273] (A-2-ii): Ethylene-propylene-5-ethylidene-2-norbornene copolymer
[0274] Mooney viscosity (ML) of (A-2-ii) 1+4 125℃) = 64
[0275] Composition of (A-2-ii)
[0276] The proportion of structural units derived from ethylene is 64.7% by mass.
[0277] The proportion of structural units derived from propylene is 31.2% by mass.
[0278] The ratio of structural units derived from 5-ethimide-2-norbornene is 4.1% by mass.
[0279] EE = 61.7 mol%
[0280] PP = 3.3 mol%
[0281] PE = 35.0 mol%
[0282] r1r2=0.67
[0283] (A-2-iii)+(C): Oil-extended ethylene-propylene-5-ethylidene-2-norbornene copolymer (a mixture of 100 parts by weight of component (A-2-iii) and 100 parts by weight of component (C))
[0284] Mooney viscosity (ML) of (A-2-iii)+(C) 1+4 125℃) = 37
[0285] The Mooney viscosity (ML) of (A-2-iii) calculated from equation (1) above. 1+4 125℃) = 169
[0286] Composition of (A-2-iii)
[0287] The percentage of structural units derived from ethylene is 68.0% by mass.
[0288] The percentage of propylene-derived structural units = 29.0% by mass
[0289] The ratio of structural units derived from 5-ethimide-2-norbornene is 3.0% by mass.
[0290] EE = 64.0 mol%
[0291] PP = 5.0 mol%
[0292] PE = 31.0 mol%
[0293] r1r2=1.34
[0294] • (A-2-iv)+(C): Oil-extended ethylene-propylene-5-ethylidene-2-norbornene copolymer (a mixture of 100 parts by weight of component (A-2-iv) and 40 parts by weight of component (C))
[0295] Mooney viscosity (ML) of (A-2-iv)+(C) 1+4 125℃) = 54
[0296] The Mooney viscosity (ML) of (A-2-iv) calculated from the above equation (1) 1+4 125℃) = 99
[0297] Composition of (A-2-iv)
[0298] The percentage of structural units derived from ethylene is 64.7% by mass.
[0299] The percentage of structural units derived from propylene is 31.3% by mass.
[0300] The percentage of structural units derived from 5-ethimide-2-norbornene is 3.9% by mass.
[0301] EE = 61.6 mol%
[0302] PP = 6.7 mol%
[0303] PE = 31.7 mol%
[0304] r1r2=1.64
[0305] • (A-2-v)+(C): Oil-extended ethylene-propylene-5-ethylidene-2-norbornene copolymer (a mixture of 100 parts by weight of component (A-2-v) and 75 parts by weight of component (C))
[0306] Mooney viscosity (ML) of (A-2-v)+(C) 1+4 125℃) = 55
[0307] The Mooney viscosity (ML) of (A-2-v) calculated from the above equation (1) 1+4 125℃) = 172
[0308] Composition of (A-2-v)
[0309] The proportion of structural units derived from ethylene is 63.1% by mass.
[0310] The percentage of structural units derived from propylene is 33.5% by mass.
[0311] The percentage of structural units derived from 5-ethimide-2-norbornene is 3.4% by mass.
[0312] EE = 57.4 mol%
[0313] PP = 9.0 mol%
[0314] PE = 33.6 mol%
[0315] r1r2=1.83
[0316] <Ingredient (B)> Acrylic polymers
[0317] (Bi): Multiphase propylene polymer material, manufactured by Sumitomo Chemical Co., Ltd., trade name "Sumitomo NOBLEN AH561".
[0318] MFR (230℃, 21.2N) = 3g / 10 minutes, [η]cxis ] = 1.7 dl / g, [η cxs =3.8 dl / g, Amount of polymer (I) = 80% by mass, Ethylene-derived structural units contained in copolymer (II) = 37% by mass
[0319] (B-ii): Propylene homopolymer, manufactured by Sumitomo Chemical Co., Ltd., trade name "Sumitomo NOBLEN D101".
[0320] MFR (230℃, 21.2N) = 0.5g / 10 minutes, [η] cxis =3.0 dl / g
[0321] (B-iii): Propylene homopolymer, manufactured by Sumitomo Chemical Co., Ltd., trade name "Sumitomo NOBLEN Y501N"
[0322] MFR (230℃, 21.2N) = 13g / 10 minutes, [η] cxis =1.5dl / g
[0323] <Ingredient (C)> Mineral oil
[0324] (Ci): Paraffin-based mineral oil, manufactured by Idemitsu Kosan Co., Ltd., trade name "PW-100".
[0325] Pour point = -12.5℃
[0326] <Component (D)> Crosslinking agent
[0327] (Di) + (C): Manufactured by Kayaku Nouryon Co., Ltd., trade name "APO-10DL" (a mixture of 10% by mass of component (Di) and 90% by mass of component (C) (wherein, the total amount of (Di) and (C) is set to 100% by weight)).
[0328] (Di): 2,5-Dimethyl-2,5-di(tert-butylperoxide)hexane
[0329] <Composition (E)> Inorganic filler
[0330] (Ei): Manufactured by Sanfuku Kogyo Co., Ltd., trade name "MFP-CLLAR" (Masterbatch with 80% calcium carbonate content by mass).
[0331] <Component (F)> Ethylene resins
[0332] (Fi): Manufactured by Keiyo Polyethylene Co., Ltd., trade name "M6901"
[0333] MFR (190℃, 21.18N) = 13g / 10 minutes
[0334] Density = 962 kg / m³ 3
[0335] • The proportion of structural units derived from ethylene is greater than 90% by mass.
[0336] Crosslinking aid: Manufactured by Seiko Chemical Co., Ltd., trade name "Hi-Cross MS50" (a substance obtained by diluting trimethylolpropane trimethacrylate to 50% using silica).
[0337] Antioxidant: Manufactured by BASF Japan Co., Ltd., trade name "IRGANOX (registered trademark) 1010"
[0338] <Example 1>
[0339] A thermoplastic elastomer composition was obtained by melt-blending 45.0 parts by weight of oil-extended ethylene-propylene-5-ethylidene-2-norbornene copolymer ((A-2-i)+(C)), 14.0 parts by weight of multiphase propylene polymer (Bi), 15.0 parts by weight of (Ci) mineral oil, 1.8 parts by weight of crosslinking agent ((Di)+(C)), 0.4 parts by weight of crosslinking aid, and 0.1 parts by weight of antioxidant in the upstream process of a twin-screw extruder (TEX34αIII) manufactured by Nippon Steel Co., Ltd. at a barrel temperature of 200°C ± 20°C. Then, 6.0 parts by weight of inorganic filler (Ei) and 20.0 parts by weight of ethylene resin (Fi) were melt-blended in the downstream process of the twin-screw extruder at a barrel temperature of 200°C ± 20°C. The obtained thermoplastic elastomer composition was subjected to extrusion molding, compression molding, or injection molding using methods 3, 5, or 7 described above to obtain a molded article. The physical property test results of the molded article are shown in Table 1.
[0340] <Examples 2-6 and Comparative Example 1>
[0341] Except for changing the proportions of the raw materials as shown in Table 1, the same procedures as in Example 1 were followed to produce a thermoplastic elastomer composition and a molded body, which were then evaluated.
[0342] The results are shown in Table 1.
[0343] [Table 1]
[0344] Industrial practicality
[0345] The thermoplastic elastomer composition of the present invention can form molded articles with low high-speed surface impact energy and excellent crack resistance. In addition, it can impart various other properties derived from thermoplastic elastomer compositions. Therefore, it is suitable for use as a surface material for various automotive interior parts, such as dashboards and glove boxes, and has high application potential in various industrial fields such as transportation machinery industry, electrical and electronic industry, and construction industry.
Claims
1. A thermoplastic elastomer composition comprising 100 parts by weight of (A) an ethylene-α-olefin copolymer and 20 to 90 parts by weight of (B) a propylene polymer, wherein, The percentage of ethylene-derived structural units in all structural units of (A) ethylene-α-olefin copolymer is greater than or equal to 55% by mass and less than 80% by mass. (A) The product of the monomer reactivity ratios r1 and r2 of the ethylene-α-olefin copolymer is less than 1.
8.
2. The thermoplastic elastomer composition according to claim 1, wherein, (A) The molar fraction AA of the α-olefin-α-olefin chain in the ethylene-α-olefin copolymer is less than 8.5 mol% (wherein, the total of the peak area AA of the portion of the monomer unit bonded in the order of α-olefin unit-α-olefin unit, the peak area AE of the portion of the monomer unit bonded in the order of α-olefin unit-ethylene unit, and the peak area EE of the portion of the monomer unit bonded in the order of ethylene unit-ethylene unit is set as 100 mol%).
3. The thermoplastic elastomer composition according to claim 1 or 2, wherein, (A) Ethylene-α-olefin copolymers have structural units derived from non-conjugated dienes.
4. The thermoplastic elastomer composition according to claim 1 or 2, wherein, The thermoplastic elastomer composition also contains (C) mineral oil.
5. The thermoplastic elastomer composition according to claim 1 or 2, wherein, The thermoplastic elastomer composition also contains (D) a crosslinking agent.
6. The thermoplastic elastomer composition according to claim 1 or 2, wherein, The thermoplastic elastomer composition also contains (E) inorganic filler.
7. The thermoplastic elastomer composition according to claim 1 or 2, wherein, The thermoplastic elastomer composition further contains an ethylene resin in which the ratio of (F) ethylene-derived structural units is 80% by mass or more.
8. The thermoplastic elastomer composition according to claim 7, wherein, (F) the density of the ethylene-based resin is 950 kg / m 3 The above.
9. A method for manufacturing the thermoplastic elastomer composition according to claim 1 or 2, wherein, The manufacturing method includes a step of melt-blending (A) an ethylene-α-olefin copolymer and (B) a propylene polymer in the presence of (D) a crosslinking agent.
10. The method for manufacturing the thermoplastic elastomer composition according to claim 9, wherein, The manufacturing method includes: adding (F) an ethylene resin to a melt blend obtained in the step of melt blending (A) an ethylene-α-olefin copolymer and (B) a propylene polymer in the presence of (D) a crosslinking agent, and further melt blending the mixture.
11. A molded body, wherein, The molded body comprises the thermoplastic elastomer composition according to claim 1 or 2. According to JIS K6262, under the conditions of 25% compression ratio, 70°C test temperature, and 22 hours test time, the compression set of the molded body is 36% to 70%.
12. An interior panel for a vehicle, wherein, The interior trim of the vehicle contains the thermoplastic elastomer composition as described in claim 1 or 2.
Citation Information
Patent Citations
Methods for producing one or more olefins, olefins and polymers
JP2010511634A
Integrated method for the production of ethylene-butylene copolymer, ethylene-butylene copolymer and use of ethylene and 1-butylene as comonomers supplied from renewable natural raw materials.
JP2011506628A
Microorganisms and methods for producing n-propanol
JP2013503647A
How to convert mixed waste plastics (mwp) into valuable petrochemicals
JP2017512246A
Process for producing bio-hydrocarbons by thermally cracking a bio-renewable feedstock containing at least 65 wt% isoparaffins