Aging-resistant modified polypropylene composite material and preparation method thereof

By leveraging the synergistic effect of EPDM-g-MAH and oxazoline compounds, a multi-level interfacial bonding network was constructed, which solved the problems of aging resistance and oil resistance of automotive floor mat materials in complex environments, and improved the mechanical properties and interlayer bonding strength of the materials.

CN123152209APending Publication Date: 2026-11-24GUANGZHOU CHEAN IND CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202611410627.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-11
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing car floor mat materials suffer from insufficient aging resistance, oil resistance, abrasion resistance, and long-term elasticity retention under complex environments such as high humidity, alternating high and low temperatures, ultraviolet radiation, oil stains, and repeated mechanical wear. In particular, the interfacial bonding and interlayer bonding of the TPV system are insufficient.

Method used

EPDM-g-MAH and oxazoline compounds are used for synergistic compatibilization. The PP segments of EPDM-g-MAH are physically entangled with the PP matrix, and the maleic anhydride groups react with the oxazoline ring to form covalent bonds and react with the carboxyl groups of XNBR to construct a multi-level interfacial bonding network between the PP matrix and NBR, thereby enhancing the interfacial bonding force.

Benefits of technology

It achieves strong interfacial bonding, improves the material's mechanical properties, oil resistance, and aging resistance, while maintaining good elasticity and interlayer bonding strength.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

This invention relates to an aging-resistant modified polypropylene composite material and its preparation method. It utilizes EPDM-g-MAH and an oxazoline compound for synergistic compatibilization. Through the physical entanglement of the PP segments of EPDM-g-MAH with the PP matrix, the maleic anhydride groups and the oxazoline rings can react to form covalent bonds. Simultaneously, the oxazoline rings react with the carboxyl groups of XNBR. A multi-level interfacial bonding network is constructed between the PP matrix and NBR through the synergistic effect of EPDM-g-MAH, oxazoline, and XNBR, improving the bonding force between the PP matrix and NBR, while also enhancing the bonding force between the surface and the underlying layers. This achieves strong interfacial bonding, improving mechanical properties, oil resistance, and aging resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of polymer composite materials technology, specifically relating to an aging-resistant modified polypropylene composite material for automotive floor mats and its preparation method. Background Technology

[0002] As an important component of vehicle interiors, car floor mats are subjected to complex service environments such as high humidity, alternating high and low temperatures, ultraviolet radiation, oil stains, and repeated mechanical wear. This places stringent requirements on the materials' aging resistance, oil resistance, abrasion resistance, and long-term elasticity retention. Traditional car floor mat materials mainly include polyvinyl chloride (PVC) mats, thermoplastic elastomer (TPE) mats, and ethylene propylene diene monomer (EPDM) rubber blends.

[0003] Polyvinyl chloride (PVC) car floor mats are widely used due to their low cost and ease of cleaning. However, they tend to harden and become brittle at low temperatures, release irritating odors at high temperatures, and have insufficient abrasion and oil resistance, resulting in significant performance degradation after long-term use. Chinese patent CN1286278A discloses an outdoor-specific polypropylene composite resistant to light and heat weathering, which improves the weather resistance of polypropylene by adding composite light stabilizers and mineral reinforcing agents. However, it mainly targets components such as outdoor appliance housings and car bumpers, and does not address the flexibility and elasticity issues required for car floor mat applications. US20130267141A1 proposes a multi-layered car floor mat with a thermoplastic polyurethane (TPU) surface layer for abrasion and oil resistance, and a cross-linked polyethylene foam bottom layer for cushioning. However, the layers rely on adhesive bonding, which is prone to peeling failure due to adhesive aging during long-term use.

[0004] Thermoplastic vulcanizates (TPVs) are blends prepared using dynamic vulcanization technology. They possess the high elasticity of rubber at room temperature and can be melt-plasticized at high temperatures, combining the advantages of both rubber and thermoplastics. While traditional EPDM / PP type TPVs exhibit good weather resistance, their surface oil resistance is insufficient. Car floor mats are frequently exposed to oily contaminants such as engine oil and lubricating oil during use. Oil molecules penetrating the TPV system can cause the rubber phase to swell, disrupting interfacial bonding and reducing mechanical properties. Chinese patent CN110229421B reports a technical solution to improve the heat aging resistance of polypropylene materials by adding composite photothermal stabilizers, but it does not solve the problems of oil resistance and interlayer bonding in the TPV system. Chinese patent CN110667219A proposes a multilayer TPE composite material floor mat structure, but the interfacial bonding between the functional layers is insufficient, making interlayer separation prone to occur during long-term service.

[0005] Therefore, it is of great significance to develop a modified polypropylene composite material that simultaneously improves mechanical properties, oil resistance, and aging resistance. Summary of the Invention

[0006] The purpose of this invention is to provide an aging-resistant modified polypropylene composite material and its preparation method. The method utilizes EPDM-g-MAH and an oxazoline compound for synergistic compatibilization. Through the physical entanglement of the PP segments of EPDM-g-MAH with the PP matrix, the maleic anhydride groups and the oxazoline ring can react to form a covalent bond. Simultaneously, the oxazoline ring reacts with the carboxyl groups of XNBR. A multi-level interfacial bonding network is constructed between the PP matrix and NBR through the synergistic effect of EPDM-g-MAH, oxazoline, and XNBR, improving the bonding force between the PP matrix and NBR, while also enhancing the bonding force between the surface and the underlying layers. This achieves strong interfacial bonding and improves mechanical properties, oil resistance, and aging resistance.

[0007] To achieve the above objectives, the present invention provides the following technical solution: An aging-resistant modified polypropylene composite material is prepared by bilayer co-extrusion molding of a surface layer and a bottom layer. The surface layer is prepared by dynamic vulcanization of the following raw materials in parts by weight: NBR 45-55 parts, XNBR 5-25 parts, PP 65-75 parts, EPDM-g-MAH 5-10 parts, POE 8-12 parts, oxazoline compound 1.0-5.0 parts, vulcanizing agent 0.8-1.2 parts, and co-vulcanizing agent 0.8-1.2 parts. The bottom layer is prepared by dynamic vulcanization of the following raw materials in parts by weight: EPDM 65-75 parts, PP 55-65 parts, NBR-POE premix 15-25 parts, EPDM-g-MAH 5-10 parts, vulcanizing agent 1.0-1.5 parts, and co-vulcanizing agent 1.0-1.5 parts.

[0008] Preferably, the oxazoline compound is selected from one or more of 2,2'-bis(2-oxazoline) (BOZ), phenylene-bisoxazoline, and polymeric oxazoline.

[0009] The oxazoline compound is selected from one or more of 2,2'-bis(2-oxazoline), 1,3-phenylene-bis(2-oxazoline), 1,4-phenylene-bis(2-oxazoline), polyether-type oxazoline, polyester-type oxazoline, and polycarbonate-type oxazoline.

[0010] Preferably, the polymeric oxazoline is a terminal bisoxazoline oligomer obtained by ring-opening addition polymerization of a bisoxazoline compound and a dicarboxylic acid.

[0011] Preferably, the dicarboxylic acid is one or more of adipic acid, sebacic acid, carboxyl-terminated polyether, carboxyl-terminated polyester, and carboxyl-terminated polycarbonate.

[0012] Preferably, the polymeric oxazoline has a number-average molecular weight Mn≈1000-20000, more preferably Mn≈1000-15000, even more preferably Mn≈1000-9000, even more preferably Mn≈1000-8000, even more preferably Mn≈1000-5000, and even more preferably Mn≈1000-3000.

[0013] Preferably, the polymeric oxazoline contains about 1-100 mmol / g of oxazoline groups, more preferably about 1-80 mmol / g of oxazoline groups, even more preferably about 1-50 mmol / g of oxazoline groups, even more preferably about 1-30 mmol / g of oxazoline groups, even more preferably about 1-10 mmol / g of oxazoline groups, and even more preferably about 1-5 mmol / g of oxazoline groups.

[0014] Preferably, the molar ratio of carboxyl groups to α-azolinyl groups in the XNBR is 1.5:1-0.8:1.3, more preferably 1.3:1-0.8:1.2, more preferably 1.2:1-0.8:1.1, more preferably 1.1:1-0.8:1.2, and even more preferably 1:1-0.8:1.1.

[0015] Preferably, the vulcanizing agent is a peroxide vulcanizing agent.

[0016] Preferably, the vulcanizing agent is DCP and the vulcanizing co-agent is TAIC.

[0017] Preferably, the surface layer further includes 12-18 parts of carbon black, 6-10 parts of plasticizer, and 0.5-1.5 parts of antioxidant.

[0018] Preferably, the bottom layer further includes 15-25 parts carbon black, 12-18 parts paraffin oil, and 0.5-1.5 parts antioxidant.

[0019] Preferably, the thickness of the surface layer is 0.8-1.2 mm.

[0020] Preferably, the thickness of the bottom layer is 3.5-4.5 mm.

[0021] The method for preparing the NBR-POE premix is ​​as follows: NBR and POE are premixed in an internal mixer at a mass ratio of (2-3):1 at 160-180℃ for 8-15 min to obtain the premix.

[0022] The dynamic vulcanization process of the surface layer is as follows: First, PP is melt-plasticized in an internal mixer at 170-190℃. Then, NBR, XNBR, POE, EPDM-g-MAH, carbon black, plasticizer, antioxidant and oxazoline compound are added in sequence and mixed evenly. Then, DCP and TAIC are added and dynamically vulcanized for 3-10 minutes at 170-190℃ and rotor speed of 60-200 r / min. The material is then discharged and granulated.

[0023] The dynamic vulcanization process of the bottom layer is as follows: First, PP is melted and plasticized in an internal mixer at 170-190℃. Then, EPDM, NBR-POE premix, EPDM-g-MAH, carbon black, paraffin oil, and antioxidant are added in sequence and mixed evenly. Then, DCP and TAIC are added, and dynamic vulcanization is carried out for 3-10 minutes at 170-190℃ and rotor speed of 60-200 r / min. The material is then discharged and granulated.

[0024] The method for preparing the composite material is as follows: the surface granules and the bottom granules are respectively added to the two extruders of the double-layer co-extrusion machine, and after being melted and plasticized, they are compounded in the co-extrusion die. The die temperature is 180-200℃. After traction cooling and shaping, the composite material with a double-layer integrated structure is obtained.

[0025] Compared with the prior art, the present invention has achieved the following beneficial effects: 1) This invention employs EPDM-g-MAH and oxazoline compounds for synergistic compatibilization. Through the physical entanglement of the PP segments of EPDM-g-MAH with the PP matrix, the maleic anhydride groups and the oxazoline ring can react to form a covalent bond. At the same time, the oxazoline ring reacts with the carboxyl groups of XNBR. A multi-level interfacial bonding network is constructed between the PP matrix and NBR through the synergistic effect of EPDM-g-MAH, oxazoline and XNBR, which improves the bonding force between the PP matrix and NBR, and at the same time improves the bonding force between the surface and the bottom layer, thus achieving strong interfacial bonding and improving mechanical properties, oil resistance and aging resistance.

[0026] 2) This invention achieves a balance between oil resistance and elasticity retention by compounding NBR and XNBR. The XNBR molecular chain has a high carboxyl content, which can react with the oxazoline ring. A multi-level interfacial bonding network is constructed between the PP matrix and NBR through the synergistic effect of EPDM-g-MAH, oxazoline and XNBR, which not only achieves strong interfacial bonding, but also improves the elongation at break and compression set performance. Detailed Implementation

[0027] Various exemplary embodiments of the present invention are now described in detail. This detailed description should not be considered as a limitation of the present invention, but rather as a more detailed description of certain aspects, features, and embodiments of the present invention. It should be understood that the terminology used in this invention is merely for describing particular embodiments and is not intended to limit the present invention. It should be noted that any aspects not described in detail in this invention are conventional practices in the art and are not the focus of this invention.

[0028] Furthermore, regarding numerical ranges in this invention, it should be understood that each intermediate value between the upper and lower limits of the range is also specifically disclosed. Any stated value or intermediate value within a stated range, as well as each smaller range between any other stated value or intermediate value within said range, are also included within this invention. The upper and lower limits of these smaller ranges may be independently included or excluded from the range. Unless otherwise stated, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art described herein. While only preferred methods and materials have been described herein, any methods and materials similar to or equivalent to those described herein may be used in the implementation or testing of this invention.

[0029] Example 1 An aging-resistant modified polypropylene composite material, Surface formulation (parts by weight): NBR (230S) 50, XNBR (Krynac231) 10, PP (PPH-M600X) 70, EPDM-g-MAH 8, POE (ENGAGE™ 7256) 10, 2,2'-bis(2-oxazoline) (BOZ) 1.5, DCP 1.0, TAIC 1.0, carbon black 15, plasticizer DOP 8, antioxidant RD1.

[0030] Base formulation (parts by weight): EPDM (Kumho 2380) 70, PP (PPH-M600X) 60, NBR-POE premix 20, EPDM-g-MAH 8, DCP 1.2, TAIC 1.2, carbon black 20, paraffin oil 15, antioxidant RD1.

[0031] The molar ratio of carboxyl groups to BOZ-α-zoline groups in the XNBR is 1.12:1.

[0032] Includes the following steps: Step 1, Dynamic vulcanization of the surface: First, melt and plasticize PP in an internal mixer at 170-190℃. Then, add NBR, XNBR, POE, EPDM-g-MAH, carbon black, plasticizer, antioxidant and oxazoline compound in sequence and mix evenly. Then, add DCP and TAIC and vulcanize dynamically for 5 min at 185℃ and rotor speed of 200 r / min. Then, discharge and granulate.

[0033] Step 2, Preparation of NBR-POE premix: NBR and POE are premixed in an internal mixer at 160℃ for 10 min at a mass ratio of 3:1 to obtain NBR-POE premix.

[0034] Step 3, dynamic vulcanization of the bottom layer: First, melt and plasticize PP in an internal mixer at 170-190℃, then add EPDM, NBR-POE premix, EPDM-g-MAH, carbon black, paraffin oil and antioxidant in sequence and mix evenly. Then add DCP and TAIC and vulcanize dynamically at 180℃ and rotor speed of 185r / min for 6 minutes, then discharge and granulate.

[0035] Step 4, preparation of composite material: The surface granules and the bottom granules are added to the two extruders of the double-layer co-extrusion machine, respectively. After being melted and plasticized, they are compounded in the co-extrusion die at a temperature of 180-200℃. After traction cooling and shaping, they are wound up to obtain a double-layer integrated composite material with a surface layer thickness of 1.0 mm and a bottom layer thickness of 4.0 mm.

[0036] Comparative Example 1 An aging-resistant modified polypropylene composite material was prepared according to the method of Example 1, the only difference being that BOZ was not added to the surface formulation, and the amount of EPDM-g-MAH was increased to 9.5 parts (i.e., EPDM-g-MAH was used to replace BOZ), while the rest remained unchanged.

[0037] Comparative Example 2 An aging-resistant modified polypropylene composite material was prepared according to the method of Example 1, except that EPDM-g-MAH was not added to the surface formulation, and the amount of BOZ was increased to 9.5 parts (i.e., BOZ was used to replace EPDM-g-MAH), while the rest remained unchanged.

[0038] Comparative Example 3 An aging-resistant modified polypropylene composite material was prepared according to the method of Example 1, except that all NBR in the surface formulation was replaced with XNBR (i.e., 0 parts NBR and 70 parts XNBR), while the rest remained unchanged.

[0039] Comparative Example 4 An aging-resistant modified polypropylene composite material was prepared according to the method of Example 1, except that all XNBR in the surface formulation was replaced with NBR (i.e., 0 parts XNBR and 70 parts NBR), while the rest remained unchanged.

[0040] Comparative Example 5 An aging-resistant modified polypropylene composite material was prepared according to the method of Example 1, except that step 2 was omitted and step 3 was completed by directly adding 15 parts by weight of NBR and 5 parts by weight of POE to replace 20 parts by weight of NBR-POE premix, with the rest remaining unchanged.

[0041] Performance testing The performance of the aging-resistant modified polypropylene composite materials obtained in Example 1 and Comparative Examples 1-5 was tested using the following methods: Elongation at break: The elongation at break was determined according to GB / T 528-2009.

[0042] Tear strength: Tear strength was determined according to GB / T 529-2008.

[0043] Compression set: The compression set was determined according to GB / T 7759.1-2015.

[0044] Interlayer peel strength: The interlayer peel strength was determined according to GB / T 8808-1988.

[0045] Oil resistance: Oil resistance was determined according to GB / T 1690-2010.

[0046] Hot air aging strength retention rate: The hot air aging strength retention rate was determined according to GB / T 3512-2014. The results are shown in Table 1.

[0047] Table 1. Performance of Aging-Resistant Modified Polypropylene Composites Comparing Example 1 with Comparative Examples 1 and 2, it can be seen that the aging-resistant modified polypropylene composite material of Example 1 exhibits superior performance in terms of elongation at break, tear strength, compression set, interlaminar peel strength, oil resistance rate of change in mass, and retention of strength under hot air aging. This indicates a significant synergistic compatibilizing effect between EPDM-g-MAH and the oxazoline compound. Although EPDM-g-MAH alone can generate some interfacial interaction with polar rubber through the maleic anhydride group, it lacks chemical bonding; when BOZ is used alone, the oxazoline ring can undergo a ring-opening reaction with the carboxyl group of XNBR to form chemical bonds, but it lacks physical entanglement anchors with the non-polar PP phase. When the two coexist, the PP segments of EPDM-g-MAH are physically entangled with the PP matrix, and the maleic anhydride groups can react with the oxazoline ring to form a covalent bond. At the same time, the oxazoline ring reacts with the carboxyl group of XNBR. Through the synergistic effect of EPDM-g-MAH, oxazoline and XNBR, a multi-level interfacial bonding network is constructed between the PP matrix and NBR, which improves the bonding force between the PP matrix and NBR, and at the same time improves the bonding force between the surface and the bottom layer. This achieves strong interfacial bonding and improves mechanical properties, oil resistance and aging resistance.

[0048] Comparing Example 1 with Comparative Examples 3 and 4, it can be seen that the oil resistance of Comparative Example 4 deteriorates sharply, and the interlayer peel strength also decreases significantly. This may be because although NBR has a certain degree of oil resistance, it lacks reactive functional groups and cannot form chemical bonds with oxazoline. Comparative Example 3 has the best oil resistance, but its elongation at break and compression set performance are worse. This is because the XNBR molecular chain has a high carboxyl content, a high crosslinking density, and strong polarity, resulting in reduced flexibility. In Example 1, the NBR and XNBR blend achieves a balance between oil resistance and elasticity retention. The carboxyl groups of XNBR can react with the oxazoline ring, constructing a multi-level interfacial bonding network between the PP matrix and NBR through the synergistic effect of EPDM-g-MAH, oxazoline, and XNBR, thus achieving strong interfacial bonding.

[0049] Comparing Example 1 and Comparative Example 5, it can be seen that the compression set of Example 1 is significantly better than that of the Comparative Example. This may be because the introduction of the NBR-POE premix gives the underlying EPDM / PP system a finer phase dispersion structure. As a highly efficient toughening component, POE can adjust the viscosity of the system during dynamic vulcanization, promote the fragmentation and refinement of the rubber phase, and at the same time, the flexible segments of POE endow the material with better elastic recovery ability, reducing compression set.

[0050] The above embodiments are merely illustrative examples and are not intended to limit the implementation. Those skilled in the art will recognize that other variations or modifications can be made based on the above description. It is neither necessary nor possible to exhaustively list all possible implementations. However, obvious variations or modifications derived therefrom are still within the scope of protection of this invention.

Claims

1. An aging-resistant modified polypropylene composite material, characterized in that, The material is prepared by double-layer co-extrusion molding of a surface layer and a bottom layer. The surface layer is prepared by dynamic vulcanization of the following raw materials in parts by weight: NBR 45-55 parts, XNBR 5-25 parts, PP 65-75 parts, EPDM-g-MAH 5-10 parts, POE 8-12 parts, oxazoline compound 1.0-5.0 parts, vulcanizing agent 0.8-1.2 parts, and co-vulcanizing agent 0.8-1.2 parts. The bottom layer is prepared by dynamic vulcanization of the following raw materials in parts by weight: EPDM 65-75 parts, PP 55-65 parts, NBR-POE premix 15-25 parts, EPDM-g-MAH 5-10 parts, vulcanizing agent 1.0-1.5 parts, and co-vulcanizing agent 1.0-1.5 parts.

2. The aging-resistant modified polypropylene composite material according to claim 1, characterized in that, The oxazoline compound is selected from one or more of 2,2'-bis(2-oxazoline), phenylene-bisoxazoline, and polymeric oxazoline.

3. The aging-resistant modified polypropylene composite material according to claim 1, characterized in that, The oxazoline compound is selected from one or more of 2,2'-bis(2-oxazoline), 1,3-phenylene-bis(2-oxazoline), 1,4-phenylene-bis(2-oxazoline), polyether-type oxazoline, polyester-type oxazoline, and polycarbonate-type oxazoline.

4. The aging-resistant modified polypropylene composite material according to claim 2, characterized in that, The molar ratio of carboxyl groups to α-azolinyl groups in the XNBR is 1.5:1 to 0.8:1.

3.

5. The aging-resistant modified polypropylene composite material according to claim 1, characterized in that, The vulcanizing agent is a peroxide-based vulcanizing agent.

6. The aging-resistant modified polypropylene composite material according to claim 1, characterized in that, The vulcanizing agent is DCP, and the vulcanizing co-agent is TAIC.

7. The aging-resistant modified polypropylene composite material according to claim 1, characterized in that, The surface layer also includes 12-18 parts of carbon black, 6-10 parts of plasticizer, and 0.5-1.5 parts of antioxidant, and the bottom layer also includes 15-25 parts of carbon black, 12-18 parts of plasticizer, and 0.5-1.5 parts of antioxidant.

8. The method for preparing the aging-resistant modified polypropylene composite material according to any of the preceding claims, characterized in that, Includes the following steps: Step 1, Dynamic vulcanization process of the surface layer: First, melt and plasticize PP in an internal mixer at 170-190℃, then add NBR, XNBR, POE, EPDM-g-MAH, carbon black, plasticizer, antioxidant and oxazoline compound in sequence and mix evenly. Then add DCP and TAIC, and dynamically vulcanize for 3-10 min at 170-190℃ and rotor speed of 60-200 r / min. Then discharge and granulate. Step 2, Dynamic vulcanization of the bottom layer: First, melt and plasticize PP in an internal mixer at 170-190℃. Then, add EPDM, NBR-POE premix, EPDM-g-MAH, carbon black, paraffin oil, and antioxidant in sequence and mix evenly. Then, add DCP and TAIC and dynamically vulcanize for 3-10 minutes at 170-190℃ and rotor speed of 60-200 r / min. Then, discharge and granulate. Step 3: Preparation of composite material: The surface granules and the bottom granules are added to the two extruders of the double-layer co-extrusion machine, respectively. After being melted and plasticized, they are compounded in the co-extrusion die at a temperature of 180-200℃. After traction cooling and shaping, the composite material with a double-layer integrated structure is obtained.

9. The preparation method according to claim 8, characterized in that, The preparation method of the NBR-POE premix in step two is as follows: NBR and POE are premixed in an internal mixer at 160-180℃ for 8-15 min at a mass ratio of (2-3):1 to obtain premix a.

Citation Information

Patent Citations

  • A high-temperature resistant injection-molded polypropylene material, its preparation method and application

    CN110229421B

  • Automobile foot mat TPE composite material and preparation method thereof

    CN110667219A

  • Outdoor-type polypropylene compound resisting against light radiation, high-temp, weather and ageing

    CN1286278A

  • Foot mat of automobile