A method for polybutene bulk melt crystallization to form entirely directly a crystal form III stable at room temperature

By blending polybutene, antioxidants, and nucleating agent N,N′-dicyclohexyl-2,6-naphthalenediamide, combined with melt crystallization and room temperature cold pressing, the stability problem of crystal form III in polybutene melt processing was solved, and the dimensional and mechanical properties of the product were stabilized.

CN123152218APending Publication Date: 2026-11-24王友健
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611401282.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2026-07-24
Filing Date
2026-09-02
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing technologies make it difficult to directly form stable crystal form III at room temperature during the melt processing of polybutene, resulting in unstable molding dimensions and processing difficulties.

Method used

By blending polybutene, antioxidants, and nucleating agent N,N′-dicyclohexyl-2,6-naphthalenediamide, chain stereodefects are controlled, and melt crystallization is carried out at a specific temperature. The nucleating agent promotes the formation of crystal form III, and the room temperature cold pressing avoids crystal form changes caused by slow cooling.

Benefits of technology

It enables the direct formation of room-temperature stable crystal form III from polybutene bulk, which is suitable for injection molding and extrusion molding, and improves the dimensional stability and mechanical properties of the products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123152218A_ABST
    Figure CN123152218A_ABST
Patent Text Reader

Abstract

This invention discloses a method for directly forming polybutene (PB) into a stable room-temperature crystalline form III through bulk melt crystallization. By introducing amide-based small molecule compounds into PB, which has a certain degree of chain stereochemical defects, and under melt cooling conditions controlled according to typical polymer melt processing, the method achieves the technical effect of directly forming crystalline form III through PB melt crystallization. The method of this invention is simple to operate and can directly form a stable room-temperature crystalline form III through PB melt crystallization.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of semi-crystalline polymorph polymer crystal form control technology. More specifically, it relates to a method for directly melting and crystallizing polybutene (PB) bulk melt to obtain crystal form III. Through this method, crystal form III, which can be stably formed at room temperature, can be easily and directly melt-crystallized from PB melt. Background Technology

[0002] Polybutene (PB) is a semi-crystalline polycrystalline polymer material obtained by catalytic polymerization of 1-butene as a raw material, with or without the addition of small amounts of comonomers such as ethylene or propylene, under the action of a specific catalyst system. When the obtained PB chains have a certain degree of stereoregularity, such as a high degree of stereoisodality in its chain structure, it can usually exhibit semi-crystalline properties and can form different crystal forms such as I, I', II, and III under different crystallization conditions, thus exhibiting typical polycrystalline polymer behavior. However, when the PB chain structure has certain stereodefects, its crystallization behavior will be greatly affected.

[0003] PB crystal form I is a thermodynamically stable hexagonal crystal structure with a 3 / 1 helical chain conformation and a melting point typically around 125°C. It is generally derived from crystal form II via a II-I transformation. Direct crystallization of PB to form crystal form I under specific conditions is often very difficult. PB crystal form I' has the same 3 / 1 helical chain conformation as crystal form I and is also a hexagonal crystal structure. Therefore, its wide-angle X-ray scattering information is the same as crystal form I, except that its melting point is lower, typically around 95°C. Crystal form I' can be obtained by crystallization from PB solution or by limiting specific crystallization conditions after copolymerization. Under certain conditions, PB can partially or completely crystallize directly to crystal form I'. PB crystal form II is a thermodynamically metastable tetragonal crystal structure with an 11 / 3 helical chain conformation and a melting point around 115°C. During the melting and crystallization process of PB, kinetically, it preferentially crystallizes to crystal form II, which then undergoes a II-I transformation to obtain crystal form I. Therefore, in PB melt processing applications, the resulting products are often in crystal form II, requiring a certain time, such as about a week, to transform into thermodynamically stable crystal form I. PB crystal form III is an orthorhombic unit cell structure with a 4 / 1 helical chain conformation and a melting point around 95–98°C. Crystal form III can usually be obtained under solution conditions, often forming simultaneously with crystal form I from solution; PB can also produce crystal form III through epigenetic crystallization at certain interfaces; and under PB melt crystallization conditions, small amounts of crystal form III can also be formed through the introduction of additive components or the introduction of long-chain branched structures in PB.

[0004] Under certain conditions, different crystalline structures of polyphosphate (PB) can transform into each other. For example, crystalline forms I' and III, which can remain stable at room temperature for a long time, can often transform into crystalline form II after being heated to 95°C and heat-treated for a certain period of time. Subsequently, crystalline form II can further transform into crystalline form I. It can be seen that crystalline form I can be formed through different pathways, but due to the different thermal histories, the resulting crystalline structures will also have certain differences.

[0005] Given that PB crystal form I is a thermodynamically stable crystalline structure, compared to other crystal forms, crystal form I has the highest melting point, the densest helical chain packing, and the most stable crystalline structure. Therefore, PB in crystal form I exhibits superior mechanical advantages such as resistance to high-temperature creep and slow crack propagation. It can be widely used in pressure pipes, fittings, pressure vessels, and other products, and its service life is significantly longer than that of polyethylene or polypropylene, which are also polyolefin materials. However, current technology shows that during processing and molding, PB inevitably first forms a metastable crystal form II due to kinetic advantages, and then slowly transforms into the stable crystal form I. This transformation is accompanied by significant volume shrinkage, which has a certain impact on PB extrusion molded products, especially causing great difficulties in injection molding processes with high dimensional requirements. To address this, the Tianjin University research group, in collaboration with the applicant, proposed a Chinese invention patent, "Method for Regulating the Transition from Crystal Form II to Crystal Form I by Adding Liquid Additives to Match the Melt Processing of Isotactic Poly(1-Butene)", application number 2018110826035, application date September 17, 2018, and authorization announcement date August 2, 2022. This method uses dichloromethane for treatment to achieve a rapid transition from crystal form II to crystal form I. Crystal forms I' and III of PB are relatively stable crystal forms that can remain stable at room temperature for a long time and do not spontaneously undergo crystal form transformation near room temperature. Therefore, they can meet the requirements of melt processing methods such as extrusion molding, especially injection molding. However, directly obtaining a crystalline structure dominated by crystal form I' or crystal form III from the molten state of PB, for example, if the crystal content of these two forms accounts for more than 90% or 95% of the total crystalline portion, is not easy to achieve. Literature shows that PB obtained by copolymerizing approximately 10% ethylene monomers can be fully obtained in crystal form I' during melt crystallization, but there are certain limitations on the melting temperature, which is unfavorable for melt processing. Summary of the Invention

[0006] The purpose of this invention is to overcome the shortcomings of existing crystal form III preparation technologies and provide a technical method that can directly form room-temperature stable crystal form III from PB bulk through melt crystallization. This method leverages the room-temperature stability of crystal form III to adapt to processing applications such as PB injection molding where dimensional stability is required. The invention combines PB chain stereodefect control, small molecule nucleating agent selection, and processing temperature control, providing a feasible technical approach for directly crystallizing PB from the bulk melt to form crystal form III during melt processing.

[0007] The technical objective of this invention is achieved through the following technical solution:

[0008] A method for directly forming a stable crystal form III of polybutene by melt crystallization at room temperature involves uniformly mixing polybutene, an antioxidant, and a nucleating agent N,N′-dicyclohexyl-2,6-naphthalenediamide, heating and melting the mixture, and then molding it in a room-temperature apparatus to obtain polybutene that can be completely melt-crystallized to form crystal form III. The antioxidant is a combination of antioxidant 1010 and antioxidant 168 in equal mass ratios, and the polybutene is polybutene with chain stereodefects. In the polybutene, antioxidant, and nucleating agent N,N′-dicyclohexyl-2,6-naphthalenediamide, the antioxidant has a mass percentage of 0.5%, and the nucleating agent has a mass percentage of 0.1%-1%. The melting temperature is 150-230 degrees Celsius.

[0009] In the above technical solution, the mass percentage of the nucleating agent in polybutene, antioxidant and nucleating agent N,N′-dicyclohexyl-2,6-naphthalenediamide is 0.5%-1%.

[0010] In the above technical solution, the isotacticity of polybutene is lower than that of homopolymer polybutene (98%).

[0011] In the above technical solution, polybutene is a copolymer of ethylene and 1-butene. In the preparation, PB with chain stereodefects is obtained by copolymerizing ethylene monomer with 1-butene monomer to reduce isotacticity.

[0012] In the above technical solution, the polybutene is polybutene copolymerized with 4% ethylene. The copolymerization of ethylene and 1-butene is selected, wherein the mass of ethylene is 4% of the sum of the masses of the two monomers, and the isotacticity is reduced to 93-95%.

[0013] In the above technical solution, the melting temperature is 180-200 degrees Celsius.

[0014] In the above technical solutions, the material is heated and melted and then molded in a room temperature apparatus, using an extrusion granulation apparatus, an extrusion molding apparatus, or an injection molding apparatus.

[0015] The technical method provided by this invention involves melting and blending PB, antioxidants, and amide small molecules, then heating and melting them at existing melting temperatures. The mixture is then shaped in a room-temperature apparatus, such as an extrusion granulation apparatus or an injection molding apparatus. Due to the large temperature difference between the melt and the apparatus, the room-temperature apparatus acts as a continuous room-temperature cold-pressing force on the melt during the shaping process, effectively creating a faster cooling condition. This avoids the crystal form changes (i.e., reducing the proportion of crystal form III in the crystal structure, forming a crystal structure where crystal form III and part of crystal form II coexist) caused by slow cooling or holding the temperature during cooling.

[0016] The technical method provided by this invention applies to PB containing a certain amount of copolymer units, such as ethylene copolymer units, which has a certain amount of chain stereochemical defects. Normally, PB requires solution crystallization under certain conditions to obtain all of crystal form III, or solution crystallization or melt crystallization to obtain a small amount of crystal form III coexisting with other crystal forms, such as crystal form I' or crystal form II. The characteristic advantage of the technical method provided by this invention is that crystal form III can be obtained directly from the PB body containing a certain amount of chain stereochemical defects through melt crystallization. The technical solution of this invention is applicable to conventional PB melt processing molding methods, such as injection molding and extrusion molding. Especially when used for injection molding, it is beneficial to obtain products with stable dimensions and mechanical properties at room temperature. Attached Figure Description

[0017] Figure 1 This is the first DSC melting curve (heating rate of 10℃ / min) of PB / TMB5 samples containing 4% ethylene copolymer (TMB5 mass percentages of 0.1%, 0.5%, and 0, respectively) in the embodiments of the present invention.

[0018] Figure 2 This is a DSC cooling crystallization curve (cooling rate of 10℃ / min) of PB / TMB5 samples containing 4% ethylene copolymer (TMB5 mass percentages of 0.1%, 0.5%, and 0, respectively) in the embodiments of the present invention.

[0019] Figure 3 This is the second DSC melting curve (heating rate: 10℃ / min) of the PB / TMB5 sample containing 4% ethylene copolymer (TMB5 mass percentages were 0.1%, 0.5%, and 0, respectively).

[0020] Figure 4 This corresponds to the embodiments of the present invention. Figure 1 The first time in China and Figure 3The WAXD plot of PB containing 0.1% TMB5 nucleating agent in the second DSC melting curve and after further cooling and crystallization at 10 °C / min and storage at room temperature for 2 weeks.

[0021] Figure 5 This corresponds to the embodiments of the present invention. Figure 1 The first time in China and Figure 3 The WAXD plot of PB containing 0.5% TMB5 nucleating agent in the second DSC melting curve and after further cooling and crystallization at 10 °C / min and storage at room temperature for 2 weeks.

[0022] Figure 6 This corresponds to the embodiments of the present invention. Figure 1 The first time in China and Figure 3 The PB curve of the second DSC melting curve and its WAXD plot after further cooling and crystallization at 10℃ / mm and storage at room temperature for 2 weeks.

[0023] Figure 7 This is the first DSC melting curve of homopolymer PB with isotacticity of 98% and TMB5 content of 0.1% and 0.5% in the comparative example of this invention (heating rate: 10℃ / min).

[0024] Figure 8 This is a DSC cooling crystallization curve (cooling rate: 10℃ / min) of homopolymer PB with isotacticity of 98% and samples containing 0.1% and 0.5% TMB5, respectively, in the comparative example of this invention.

[0025] Figure 9 This is a second DSC melting curve (heating rate: 10℃ / min) of homopolymer PB with isotacticity of 98% and TMB5 content of 0.1% and 0.5% respectively in the comparative example of this invention.

[0026] Figure 10 The images shown are WAXD diagrams of PB copolymer containing 4% ethylene before melting, after melting at 180°C followed by cold pressing, natural cooling, cooling to 90°C and holding at that temperature for 24 hours to complete melting and crystallization, and after subsequent storage at room temperature for 2 weeks.

[0027] Figure 11 The images show the WAXD diagrams of PB containing 4% ethylene copolymer units with 0.1% nucleating agent TMB5 added in the embodiments of the present invention before melting, after melting at 180°C, followed by cold pressing, natural cooling, cooling down to 90°C and holding at that temperature for 24 hours to complete melting and crystallization, and after subsequent storage at room temperature for 2 weeks.

[0028] Figure 12The images show the WAXD diagrams of PB containing 4% ethylene copolymer units with 0.5% nucleating agent TMB5 added in the embodiments of the present invention before melting, after melting at 180°C, followed by cold pressing, natural cooling, cooling down to 90°C and holding at that temperature for 24 hours to complete melting and crystallization, and after subsequent storage at room temperature for 2 weeks.

[0029] Figure 13 The 1D-WAXD image of the sample obtained by molding PB / 0.1%TMB5 at 200°C and then cold-pressing it at 25°C is shown in the embodiment of the present invention.

[0030] Figure 14 This is a 1D-WAXD diagram of PB / 0.1%TMB5 obtained in an embodiment of the present invention as it is cooled from 180°C to room temperature at a rate of 10°C / min.

[0031] Figure 15 This is a 1D-WAXD image of PB / 0.1%TMB5 in an embodiment of the present invention after being cooled from 180°C to room temperature at a rate of 10°C / min and then placed at room temperature for 2 weeks.

[0032] Figure 16 This is the WAXS diagram of PB / 1%TMB5 before melting at 180°C in an embodiment of the present invention.

[0033] Figure 17 This is a WAXS diagram of PB / 1%TMB5 after melting at 180°C and then cold-pressing at 25°C in an embodiment of the present invention.

[0034] Figure 18 This is the WAXS diagram of PB / 1%TMB5 in the embodiment of the present invention after melting at 180°C and then naturally cooling to room temperature.

[0035] Figure 19 This is a WAXS diagram of PB / 1%TMB5 after melting at 180°C, naturally cooling to room temperature, and storing for 2 weeks in an embodiment of the present invention.

[0036] Figure 20 This is the WAXS diagram of PB / 1%TMB5 in the embodiment of the present invention after melting at 180°C, being naturally cooled to 90°C and stored for 24 hours, and then naturally cooled to room temperature. Detailed Implementation

[0037] The present invention will be further described in detail below with reference to specific embodiments.

[0038] PB copolymerized with 4% ethylene was purchased from Zhenhai Refining & Chemical Co., Ltd., with a number average molecular weight of 250,000-300,000. Ethylene and 1-butene were selected for copolymerization, with the ethylene mass being 4% of the sum of the masses of the two monomers. During preparation, ethylene monomers were doped into the PB obtained through polymerization, resulting in chain stereodefects, which to some extent reduced the isotacticity. The isotacticity of homopolymer PB is concentrated around 98%, and by using ethylene monomer doping, the isotacticity was reduced to 93-95%.

[0039] Considering the melting temperature is between 150-230 degrees Celsius under melt processing conditions, antioxidants were added to the blend of ethylene and 1-butene. Antioxidant 1010 and antioxidant 168 were selected and used in a 1:1 mass ratio. Both were purchased from Tianjin Lianlong New Material Co., Ltd. Antioxidant 1010, specifically pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], has CAS number 6683-19-8 and molecular formula C1. 73 H 108 O 12 The structural formula is as follows:

[0040]

[0041] Antioxidant 168, namely tris[2,4-di-tert-butylphenyl]phosphite, CAS No. 31570-04-4, chemical formula C42H 63 O3P, the structural formula is as follows:

[0042]

[0043] The TMB5 used is named N,N′-Dicyclohexyl-2,6-naphthalenediamide in Chinese and N,N′-Dicyclohexyl-2,6-naphthalenediamide in English. Its structure is described as follows: There is a naphthalene ring in the middle (two benzene rings in parallel), and an amide bond (-CO-NH-) is attached to the 2nd and 6th positions of the naphthalene ring. A cyclohexyl group (a six-membered saturated carbon ring) is attached to the nitrogen atom of each amide bond.

[0044] Take PB (containing 4% ethylene copolymer), antioxidant, and TMB5 according to the following proportions: PB 994g, antioxidant 5g, and TMB5 1g. After initial homogenization at room temperature (20-25°C), extrude and granulate using a twin-screw extruder (TSE-35, Nanjing Ruilaibo Machinery Co., Ltd.) at 200°C. Allow to cool naturally to room temperature to obtain PB / 0.1%TMB5, where TMB5 mass percentage is 0.1%, and the TMB5 mass is calculated as: TMB5 mass / (sum of TMB5 + 4% ethylene copolymer PB + antioxidant mass) × 100%. Following the same steps and process parameters, adjust PB to 990g, antioxidant to 5g, and TMB5 to 5g, extrude and granulate, and allow to cool naturally to room temperature to obtain PB / 0.5%TMB5; adjust PB to 985g, antioxidant to 5g, and TMB5 to 10g, extrude and granulate, and allow to cool naturally to room temperature to obtain PB / 1%TMB5.

[0045] Take 34g of the PB / 0.1%TMB5, PB / 0.5%TMB5 and PB / 1%TMB5 granules obtained above, respectively, and mold them at a mold temperature of 200℃ and then cold press them at 25℃ to obtain test pieces with a thickness of 2mm (side length or diameter of 20cm), which are stored at room temperature; when performing DSC and WAXD tests, samples are taken from the test pieces to verify the formed crystal structure.

[0046] Taking PB / 0.1%TMB5 as an example, a 7mg sample was taken from a 2mm thick PB / 0.1%TMB5 specimen, placed in an aluminum crucible, and then placed in a DSC (LNP95, Linkam) instrument. The temperature was increased to 180℃ at 10℃ / min and held for 5min. The resulting first DSC melting curve was obtained. Similarly, the same test was performed on PB / 0.5%TMB5. The first heating process of the sample is mainly to eliminate the thermal history, such as... Figure 1 PB containing 0.1% and 0.5% TMB5 nucleating agent exhibits a melting peak at around 90℃ (corresponding to the melting peak of crystal form III), while PB without TMB5 nucleating agent exhibits a melting peak at 114℃.

[0047] After the initial heating to 180°C and melting for 5 minutes, the temperature was lowered to 30°C at a rate of 10°C / min. The resulting DSC cooling crystallization curve is shown below. Figure 2 During the cooling process, PB containing 0.1% and 0.5% TMB5 nucleating agent exhibited a crystallization-promoting effect due to the nucleating agent, resulting in a significantly higher crystallization temperature compared to PB without the nucleating agent. However, PB without TMB5 nucleating agent... Figure 2 The corresponding cooling crystallization curves show crystallization peaks below 40℃, while PB with added 0.1% and 0.5% TMB5 nucleating agent, respectively, exhibit crystallization peaks below 40℃. Figure 2 The crystallization peak on the cooling crystallization curve is located at around 50℃.

[0048] The temperature was raised again to 180℃ at a rate of 10℃ / min, yielding the second melting curve of the PB sample containing the TMB-5 nucleating agent. This curve corresponds to the melting curve of the crystalline structure obtained during the cooling process from 180℃ to 30℃ at a rate of 10℃ / min. The DSC curve obtained during the second melting process is shown below. Figure 3 PB containing 0.1% and 0.5% TMB5 nucleating agent still only has one melting peak of crystal form III at around 90℃; while the melting peak of PB without nucleating agent appears at 100℃.

[0049] Depend on Figure 1 and Figure 3 The two DSC melting curves show that, without the TMB5 nucleating agent, the melting point of PB corresponding to the first melting peak is 114℃, which is significantly higher than the melting point of 100℃ corresponding to the second melting peak. This is consistent with the characteristic of crystal form I melting and then cooling to crystallize into crystal form II. That is, the melting point of 100℃ obtained in the second heating is the melting point of crystal form II, while the melting point of 114℃ obtained in the first heating is the melting point of crystal form I after crystal form II has been left at room temperature for a long time.

[0050] When containing 0.1% or 0.5% TMB5 nucleating agent, Figure 1 and Figure 3 The DSC curves obtained from the two heating and melting processes were basically the same, both showing a melting peak at 90℃, while their corresponding melting points were lower than the melting point of PB crystal form II. For example... Figure 2 As shown, the addition of TMB5, which acts as a nucleating agent, to PB promotes the melt crystallization of PB. If the melt crystallization yields crystal form II, this typically increases its melting point to some extent, and it should be higher than the melting point of PB crystal form II (100°C) without the nucleating agent. Therefore, when PB contains 0.1% or 0.5% TMB5 as a nucleating agent, the melt crystallization will not yield crystal form II. Furthermore, Figure 1 The samples corresponding to the first heating curve were all subjected to long-term storage at room temperature (storage temperature 25±2℃, for two weeks). If the PB melt crystallization obtained when containing 0.1% or 0.5% TMB5 nucleating agent is of crystal form II, then after long-term storage at room temperature, it will transform into crystal form I. Therefore, Figure 1 and Figure 3 The melting point obtained from the two DSC heating and melting processes should be significantly different from that obtained due to the II-I transformation. Therefore, it can be seen that the crystal structure formed by PB containing 0.1% and 0.5% TMB5 nucleating agent after long-term storage at room temperature, followed by reheating and cooling for crystallization, is not crystal form I or crystal form II, but more likely crystal form I' or crystal form III, which can remain stable at room temperature.

[0051] 10 mm diameter circular samples were cut from PB samples containing TMB5 nucleating agent and stored at room temperature for more than 2 weeks. WAXD scanning tests were performed at room temperature within the 2θ range of 5–35°C, with a wavelength of 0.154 nm and a scan rate of 6°C / min. PB samples containing 0.1% and 0.5% TMB5 nucleating agent, as well as those without TMB5 nucleating agent, were tested after melt molding and long-term storage at room temperature (corresponding to…). Figure 1 The results of WAXD testing on the corresponding first DSC temperature rise curve are as follows: Figure 4 , Figure 5 and Figure 6 As shown. For PB samples containing 0.1% and 0.5% TMB5 nucleating agent, and for PB samples without TMB5 nucleating agent, after... Figure 2 After the corresponding cooling melting and crystallization process shown in the figure (corresponding to) Figure 3 The results of WAXD testing on the melt curve obtained from the second DSC heating in the middle are as follows: Figure 4 , Figure 5 and Figure 6 For PB samples containing 0.1% and 0.5% TMB5 nucleating agent, and for PB samples without TMB5 nucleating agent, in Figure 2 The results of the WAXD test, obtained after the corresponding cooling and melting crystallization as shown in the figure, and then stored at room temperature for 2 weeks, are as follows. Figure 4 , Figure 5 and Figure 6 .

[0052] like Figure 6 As shown, PB without TMB5, after melting and crystallization and long-term storage at room temperature, exhibited peaks at 9.9°, 17.3°, 20.2°, and 20.5° corresponding to the (110), (300), (220), and (211) crystal planes of crystal form I, respectively, confirming that PB at this time has a crystal form I structure; while after... Figure 1 The heating and melting in the subsequent Figure 2 After the cooling crystallization process, peaks corresponding to the (200), (220), and (213) crystal planes of crystal form II appeared at 11.9°, 16.9°, and 18.4°, respectively, confirming that crystal form II was formed after PB melt crystallization. After being stored at room temperature for 2 weeks, the peaks corresponding to each crystal plane of crystal form I reappeared on the WAXD diagram, while the peaks corresponding to each crystal plane of crystal form II disappeared, completing the II-I transformation. Figure 6 WAXD results obtained from PB samples without TMB5 nucleating agent and Figure 1 and Figure 3 The DSC results are consistent. For example... Figure 4 and Figure 5 As shown, when PB containing 0.1% and 0.5% TMB5 nucleating agent was melt-molded at 200℃ and then rapidly cooled by cold pressing, all showed peaks of 12.2°, 13.9°, 17.6°, and 18.8° in the WAXD plot, corresponding to the (110), (200), (111), and (201) peaks of crystal form III, respectively. This confirms that crystal form III was formed entirely after melt crystallization, which is consistent with... Figure 1 The melting point (90℃) corresponding to the melting peak in the DSC heating and melting curve is lower than the melting point (100℃) of PB crystal form II without TMB5 nucleating agent, which is consistent with this. PB containing 0.1% and 0.5% TMB5 nucleating agent underwent... Figure 1 The heating and melting shown Figure 2 The WAXD diagram obtained after cooling crystallization confirms that all the crystal structures obtained are crystal form III, and after being stored at room temperature for another 2 weeks, the crystal structure is still crystal form III and has not changed.

[0053] PB with fewer chain conformational defects was selected for comparison, such as homopolymer PB with an isotacticity of around 98% (purchased from Zhenhai Refining & Chemical Co., Ltd., number average molecular weight 300,000-400,000). A blending process essentially consistent with the embodiments of this invention was used to obtain homopolymer PB with 0.1% or 0.5% of the amide-based small molecule nucleating agent TMB. Subsequent room temperature storage, heating and melting, and cooling crystallization processes were the same as before. The first DSC heating and melting curve is shown below. Figure 7 As shown, the DSC cooling crystallization curve is as follows: Figure 8 As shown, the melting curve after the second DSC heating is as follows: Figure 9 As shown.

[0054] like Figure 7 Homopolymer PB with an isotacticity of approximately 98% and containing or without 0.1% or 0.5% TMB5 nucleating agent, after melt molding and cold pressing, and then left to stand at room temperature for an extended period (2 weeks), finally measured a melting point of approximately 137°C. Figure 8 The melting curve after the cooling crystallization process shown is as follows: Figure 9As shown, the corresponding melting points are all around 123℃. It can be seen that the melting point difference between the two consecutive heating and cooling cycles is approximately 14℃. The PB corresponding to the two heating curves are crystal form I and crystal form II, respectively. For homopolymer PB with an isotacticity of around 98%, its molecular chain isotacticity is high, and its chain stereodefects are few. When it contains no TMB5 nucleating agent or 0.1% or 0.5% TMB5, the melt crystallization completely yields crystal form II, which can completely transform into crystal form I during room temperature storage. Highly isotactic PB, even with the addition of amides such as TMB5 nucleating agents, still forms thermodynamically metastable crystal form II during melt crystallization, just like when no nucleating agent is added. It cannot obtain crystal form III, which can remain in existence at room temperature for a long time. Because the obtained crystal form II can transform into crystal form I during room temperature storage, it leads to dimensional and property instability caused by the II-I transformation during melt processing.

[0055] In the method of this invention, the melting temperature T used before cooling crystallization of PB containing 4% ethylene copolymer units with added TMB5 nucleating agent is crucial for eliminating the thermal history of the sample. melt This may have a potential impact on the direct formation of crystal form III by the cooling and crystallization of the PB melt at this temperature. Specifically, when the melting temperature T... melt At temperatures approaching 150°C and above, the PB chains can effectively eliminate melt memory. For homopolymer PB with fewer stereodefects and high isotacticity, melt crystallization forms crystal form II, at T... melt Since the melting limit of crystal form II is up to 150℃, crystallization of crystal form II is favorable, exhibiting melt memory. For PB copolymerized with comonomers or containing certain stereodefects of lower isotacticity, its formation from melt crystallization to crystal form III is transformed into complete melt crystallization to crystal form III under the action of nucleating agents, at T melt When the temperature is lowered, the ability of PB to form crystal form III completely during melt crystallization may be weakened. However, when melting PB, the melting temperature is generally about 50°C or higher than the melting point of PB, and the melting temperature usually does not significantly affect the ability of PB to form crystal form III completely during melt crystallization after the addition of nucleating agents.

[0056] PB with appropriate chain stereodefects was obtained through copolymerization, such as PB copolymerized with 4% ethylene. After adding the amide molecule TMB5, the effect of different melting and cooling processes on the yield of crystal form III was examined. Figure 10As shown, PB copolymerized with 4% ethylene without nucleating agent has crystal form I before melting. After melting at 180°C, the crystal structure obtained by direct cold pressing at room temperature (the molten material at 180°C is placed on a molding machine with the upper and lower molds at room temperature of 20-25°C, and the molten material is cold pressed using the molds), natural cooling from 180°C to room temperature, and natural cooling from 180°C to 90°C and holding at that temperature for 24 hours before natural cooling to room temperature are all crystal form II. After being stored at room temperature for 2 weeks, the crystal structure of all of them has changed to crystal form I.

[0057] like Figure 11 As shown, PB with 0.1% nucleating agent TMB5 has a crystal form III structure before melting. After melting at 180℃, it is directly cold-pressed at room temperature, resulting in a crystal form III structure. After being stored at room temperature for 2 weeks, the crystal form III structure remains. When PB is melted at 180℃ and then naturally cooled to room temperature, the resulting crystal form contains a certain amount of crystal form II in addition to crystal form III. After being stored at room temperature for another 2 weeks, the crystal form II transforms into crystal form I, forming a crystal structure where crystal forms III and I coexist. It can be seen that when the melt is naturally cooled from 180℃ to room temperature, the cooling rate is slower than when it is directly cold-pressed at room temperature, which is conducive to the formation of some crystal form II. When PB is melted at 180℃ and then naturally cooled to 90℃, held at that temperature for 24 hours, and then naturally cooled to room temperature, the resulting structure is almost entirely crystal form II. After being stored at room temperature for 2 weeks, all of these crystal forms II transform into crystal form I. Increasing the holding temperature of the PB melt to 90℃ promotes the formation of crystal form II and inhibits the formation of crystal form III; furthermore, even if crystal form III forms during the process of naturally cooling from 180℃ to 90℃ and holding for 24 hours, it will transform into crystal form II at 90℃. Figure 12 As shown, PB with 0.5% nucleating agent TMB5 was in crystal form III before melting. After melting at 180℃, it was directly cold-pressed at room temperature, resulting in crystal form III. After being stored at room temperature for 2 weeks, the crystal form remained crystal form III, which is basically consistent with the result with 0.1% nucleating agent TMB5. When PB was melted at 180℃ and then naturally cooled to room temperature, the resulting crystal form was entirely crystal form III. This is different from the partial formation of crystal form II when 0.1% nucleating agent TMB5 was added. The increased amount of nucleating agent TMB5 helps to reduce the amount of crystal form II formed when the cooling rate is slow, thus facilitating complete melting and crystallization to obtain crystal form III. However, when PB was first naturally cooled from 180℃ to 90℃ and held for 24 hours before being naturally cooled to room temperature, almost all crystal form II was obtained. After being kept at room temperature for 2 weeks, all crystal form II crystals transformed into crystal form I. It should be added that... Figure 10-12Characteristic peaks for various crystal forms were identified. Due to the close similarity of some peaks, selective highlighting was employed. For details regarding characteristic peaks of crystal form III, such as those obtained through natural cooling or room temperature cold pressing, please refer to [link to relevant documentation]. Figure 5 As shown. To further demonstrate the obtained crystal form III and its stability, PB / 0.1%TMB5 was used as an example and WAXD characterization was performed, proving that the crystal structure of PB / 0.1%TMB5 is crystal form III and that it can exist stably at room temperature.

[0058] Taking PB / 1%TMB5 as an example, its WAXS test results in the initial state (i.e., after granulation and storage at room temperature for 2 weeks) are as follows: Figure 16 As shown, after melting at 180°C and cold pressing at 25°C, a WAXS test was performed, and the results are as follows. Figure 17 As shown, it can be found Figure 16 and Figure 17 The results are largely consistent, proving that cold pressing after melting yielded all crystal form III. When PB / 1% TMB5 was melted at 180°C and allowed to cool naturally to room temperature, WAXS characterization was performed. Figure 18 As shown, this demonstrates that directly cooling the melt after melting yields crystal form III, and the same result is obtained by cooling at a rate of 10 °C / min. This PB / 1% TMB5, melted at 180 °C and then naturally cooled to room temperature, was stored at room temperature (20-25 °C) for two weeks before being characterized by WAXS. Figure 19 As shown, its crystal structure is crystal form III, and it showed no change after being stored at room temperature for 2 weeks, proving its stability. For example, PB / 1% TMB5 was melted at 180℃, then naturally cooled to 90℃ and stored for 24 hours, followed by natural cooling to room temperature, and then characterized by WAXS. Figure 20 As shown, crystal form III can be transformed into crystal form II after storage at 90℃.

[0059] According to the description of this invention, by adding antioxidants and nucleating agents to copolymerized or stereochemically defective PB, followed by melt extrusion granulation, a PB material with a fully melt-crystallized crystal structure of crystal form III, which is stable at room temperature, can be obtained. DSC and WAXD tests have demonstrated that crystal form III, which is stable at room temperature, can be directly formed from isotactic 1-butene bulk through complete melt crystallization. The above description of this invention is exemplary. It should be noted that any simple modifications, alterations, or equivalent substitutions that can be made by those skilled in the art without creative effort, without departing from the core of this invention, fall within the protection scope of this invention.

Claims

1. A method for directly forming polybutene bulk melt crystallization into crystal form III, which is stable at room temperature, characterized in that... Polybutene, an antioxidant, and a nucleating agent N,N′-dicyclohexyl-2,6-naphthalenediamide are uniformly blended, heated to melt, and then molded in an apparatus at room temperature to obtain a polybutene material or product that can melt and crystallize to form crystal form III. The antioxidant is a combination of antioxidant 1010 and antioxidant 168 in equal mass ratios, and the polybutene is polybutene with chain stereodefects. In the polybutene, antioxidant, and nucleating agent N,N′-dicyclohexyl-2,6-naphthalenediamide, the mass percentage of the antioxidant is 0.5%, and the mass percentage of the nucleating agent is 0.1%-1%. The melting temperature is 150-230 degrees Celsius.

2. The method according to claim 1 for directly forming crystal form III of polybutene through bulk melt crystallization, which is stable at room temperature, is characterized in that... In polybutene, antioxidants, and nucleating agent N,N′-dicyclohexyl-2,6-naphthalenediamide, the mass percentage of the nucleating agent is 0.5%-1%.

3. The method according to claim 1 for directly forming polybutene bulk melt crystallization into crystal form III, which is stable at room temperature, is characterized in that... The isotacticity of polybutene is lower than that of homopolymer polybutene (98%).

4. The method for directly forming crystal form III, which is stable at room temperature, entirely by bulk melt crystallization of polybutene according to claim 1, is characterized in that... Polybutene is a copolymer of ethylene and 1-butene. In its preparation, PB with chain stereodefects is obtained by copolymerizing ethylene monomer with 1-butene monomer to reduce isotacticity.

5. The method according to claim 1 for directly forming crystal form III of polybutene through bulk melt crystallization, which is stable at room temperature, is characterized in that... Polybutene is polybutene copolymerized with 4% ethylene. The copolymerization of ethylene and 1-butene is selected, wherein the mass of ethylene is 4% of the sum of the masses of the two monomers, and the isotacticity is reduced to 93-95%.

6. The method for directly forming crystal form III, which is stable at room temperature, entirely by bulk melt crystallization of polybutene according to claim 1, is characterized in that... The melting temperature is 180-200 degrees Celsius.

7. The method for directly forming crystal form III, which is stable at room temperature, entirely by bulk melt crystallization of polybutene according to claim 1, characterized in that... After being heated and melted, it is shaped in a device at room temperature, using extrusion granulation equipment, extrusion molding equipment, or injection molding equipment.