A high impact poly(methyl methacrylate) and a method for its preparation
By controlling the amount of core layer emulsifier and coordinating the process, a multi-layer organic-coated core-shell impact modifier was prepared, which solved the problems of insufficient impact resistance and defects in the polymerization process of PMMA material, and achieved high impact resistance and improved molding quality of the material.
Patent Information
- Application Number
- CN202611551115.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-08
- Publication Date
- 2026-11-24
AI Technical Summary
Existing PMMA materials have insufficient impact resistance, and there are problems such as concentrated release of reaction heat, bubble generation and internal stress during the polymerization process. The dosage of existing modifiers is not accurately controlled, resulting in limited modification effects.
By controlling the amount of core layer emulsifier to 1.2-1.4 wt%, a multi-layer organic-coated core-shell impact modifier was prepared, and combined with a prepolymerization-cooling degassing-segmented heating polymerization process, the impact resistance of PMMA was improved.
It significantly improves the impact resistance of PMMA, reduces volume shrinkage and internal stress defects, and yields a material with high impact resistance and good molding quality.
Smart Images

Figure CN123152233A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of polymer materials technology, specifically relating to a high-impact polymethyl methacrylate and its preparation method. Background Technology
[0002] Polymethyl methacrylate (PMMA) possesses excellent weather resistance, lightweight yet high strength, electrical insulation, and ease of processing, making it widely used in architectural lighting, automotive parts, home appliances, and medical materials. Those skilled in the art have explored ways to improve its performance; for example, Chinese patent application number 201810138873.7 discloses a transparent antistatic PMMA and its preparation method, aiming to improve the antistatic properties of PMMA. However, PMMA itself is brittle and lacks impact resistance, and its polymerization process has significant defects: as polymerization proceeds, the system viscosity increases sharply, chain termination reaction is hindered while chain growth continues, and the heat of reaction is released in a concentrated manner within a short period. Coupled with PMMA's poor thermal conductivity, this easily leads to excessively high local temperatures, causing explosive polymerization or the formation of bubbles. Simultaneously, the volume shrinkage rate of MMA polymerization is approximately 21%. If stress relaxation is insufficient, internal stress easily forms inside the product, leading to defects such as surface ripples, warping, and microcracks.
[0003] To address the aforementioned issues, existing technologies typically employ a prepolymer-casting process, dividing polymerization into two stages: prepolymerization and molding, to release reaction heat in stages and reduce volume shrinkage; or they introduce core-shell structure impact modifiers to improve PMMA toughness. However, existing prepolymerization processes lack precise control over the degree of prepolymerization, making it difficult for air bubbles to escape when the prepolymer slurry viscosity is too high; the toughening effect of core-shell modifiers is highly dependent on the particle size of the core latex particles and the shell coating state, and the amount of core emulsifier is a key factor in controlling particle size. Insufficient dosage leads to excessively large particle size, while excessive dosage causes shell coating defects, both of which prevent the modifier from effectively transferring stress, resulting in limited improvement in impact resistance.
[0004] Therefore, there is an urgent need to develop a PMMA preparation method that can precisely control the amount of core layer emulsifier, keep the particle size and coating state of the core-shell modifier within a suitable range, and coordinate with the prepolymerization and cooling degassing process, so as to significantly improve the impact resistance and reduce the volume shrinkage while ensuring the molding quality of the product. Summary of the Invention
[0005] The purpose of this invention is to provide a method for preparing high-impact polymethyl methacrylate (PMMA). When preparing this high-impact PMMA, the amount of core layer emulsifier is controlled to be 1.2-1.4 wt% of the mass of the core layer raw material, which can produce a core-shell modifier with suitable particle size and complete coating. Combined with the prepolymerization-cooling degassing-segmented heating polymerization process, the impact resistance of PMMA and the molding quality of the product are improved simultaneously.
[0006] To achieve the above objectives, the technical solution adopted by the present invention is as follows: The first aspect of this invention provides a method for preparing high-impact polymethyl methacrylate, comprising the following steps: (1) A multilayer organic-coated core-shell impact modifier was prepared by seed polymerization, core-layer polymerization, and shell-layer polymerization. The obtained multilayer organic-coated core-shell impact modifier was added to methyl methacrylate and mixed evenly to obtain a multilayer organic-coated core-shell liquid acrylic resin. The seed polymerization and core-layer polymerization used both core-layer emulsifier and core-layer raw material. When seed polymerization and core-layer polymerization were carried out, the amount of core-layer emulsifier was 1.2-1.4 wt% of the mass of the core-layer raw material. (2) Under stirring and heating conditions, the initiator is dissolved in methyl methacrylate, and after cooling, the accelerator is added and mixed evenly. After heating to 48-50 °C, the prepolymer slurry is obtained. (3) The prepolymer slurry obtained in step (2) is transferred into the cooling and degassing system. While cooling, the multilayer organic core-shell structure liquid acrylic resin described in step (1) is added. After mixing evenly, vacuum degassing is performed, and the mixture is injected into the mold, heated and polymerized, and then naturally cooled to obtain high impact-resistant polymethyl methacrylate.
[0007] In the above technical solution, this application significantly reduces the decomposition activation energy of the initiator through the synergistic effect of the initiator and the accelerator, so that the initiator can efficiently generate free radicals at room temperature, thereby accelerating the polymerization reaction; at the same time, the continuous cooling and degassing can avoid excessive prepolymerization and allow the bubbles entrained during prepolymerization and cooling stirring to be more fully removed.
[0008] Furthermore, the multilayer organic-coated core-shell impact modifier in step (1) is prepared by the following steps: (a) The core layer raw material and core layer emulsifier are added to water and mixed evenly. Under heating and stirring conditions, an initiator is added to polymerize and form a seed emulsion. (b) The core layer raw material, core layer emulsifier and initiator are added to water and mixed evenly, and then the seed emulsion is added dropwise. The second polymerization is carried out under heating and stirring conditions to obtain the core layer emulsion. (c) The shell raw material, shell emulsifier and initiator are added to water and mixed evenly. Then the core emulsion is added dropwise and the third polymerization is carried out under heating and stirring conditions. After drying, a multilayer organic-coated core-shell impact modifier is obtained.
[0009] Further, in step (a), the mass ratio of the core layer raw material to water is 1:(3.8-4); the core layer emulsifier is 1.2-1.4 wt% of the core layer raw material; the initiator is 0.7-0.9 wt% of the core layer raw material; the heating temperature is 75-80℃, the stirring speed is 200-300 rpm; and the polymerization time is 18-20 min.
[0010] Further, in step (b), the mass ratio of the core layer raw material to water is 1:(3.8-4); the core layer emulsifier is 1.2-1.4 wt% of the core layer raw material; the initiator is 0.7-0.9 wt% of the core layer raw material; the heating temperature is 75-80℃, the stirring speed is 200-300 rpm; and the polymerization time is 2.2-2.5 h.
[0011] Further, in step (c), the mass ratio of the shell material to water is 1:(3.8-4); the shell emulsifier is 1.4-1.6 wt% of the shell material; the initiator is 0.4-0.6 wt% of the shell material; the heating temperature is 75-80℃, the stirring speed is 200-300 rpm; and the polymerization time is 2.2-2.5 h.
[0012] Further, the mass ratio of the core material in step (a), the core material in step (b), and the shell material in step (c) is 1:(2-2.1):(4.4-4.5); the core material in step (b) is at least one of butyl acrylate, styrene, butadiene, or propyl methacrylate; the shell material in step (c) is at least one of methyl methacrylate, styrene, ethyl acrylate, or butadiene.
[0013] Furthermore, the core material described in step (a) is the same as the core material described in step (b).
[0014] Furthermore, the core emulsifier and shell emulsifier used are any one of sodium dodecyl sulfate, sodium dodecylbenzene sulfonate and alkylphenol polyoxyethylene ether; the initiator in steps (a), (b) and (c) is any one of ammonium persulfate, sodium persulfate, potassium persulfate and dodecyl peroxide.
[0015] Further, in step (1), the mass ratio of the multilayer organic-coated core-shell impact modifier to methyl methacrylate is 1:(3.8-4); in step (2), the initiator is any one of benzoyl peroxide (BPO), dodecyl peroxide (LPO), and azobisisobutyronitrile (AIBN); and the accelerator is any one of N,N-dimethylanisole (DMA), N,N-dimethyl-p-toluidine (DMT), and N-hydroxyethyl-N-methyl-p-toluidine (HMT).
[0016] Further, in step (2), the stirring speed is 200 rpm; the heating temperature is 38-42 ℃; the heating rate is 0.6 ℃ / min; and the mass ratio of methyl methacrylate to initiator and accelerator is 15:(0.3-0.5):(0.06-0.13).
[0017] Further, in step (3), the mass ratio of the multilayer organic-coated core-shell structure liquid acrylic resin to the prepolymer slurry is 1:(3-3.5); the heating polymerization step is as follows: first react at 30-35 ℃ for 8-12 h, and then heat to 75-80 ℃ for 1-3 h.
[0018] A second aspect of the present invention provides a high-impact polymethyl methacrylate prepared by the above-described preparation method.
[0019] The beneficial technical effects of this invention are as follows: 1. This invention significantly improves the impact resistance of PMMA by controlling the amount of core layer emulsifier to 1.2-1.4 wt% of the core layer raw material during the preparation process. The amount of core layer emulsifier is a key factor in regulating the average particle size of the core layer particles and the shell coating state. However, those skilled in the art have not yet discovered what kind of multilayer organic-coated core-shell impact modifier with a suitable average particle size and coating state can effectively improve the mechanical strength of PMMA. This application proposes that, within the range of 1.2-1.4 wt%, the multilayer organic-coated core-shell impact modifier has a suitable particle size and complete shell coating. When subjected to external force, it can effectively transfer stress and induce crazes and shear bands to dissipate energy, thereby significantly improving the impact resistance of PMMA while maintaining tensile strength, and synergistically reducing volume shrinkage.
[0020] 2. This invention employs a continuous preparation method combining prepolymerization, cooling degassing, and infusion polymerization, effectively suppressing defects such as burst polymerization, bubbles, and internal stress. The prepolymerization stage consumes some of the reaction heat, lowering the maximum temperature of subsequent polymerization and reducing burst polymerization and bubble generation. The cooling degassing stage rapidly lowers the temperature to slow polymerization, while vacuum degassing ensures the complete removal of bubbles entrained during prepolymerization and stirring. The addition of multilayer organic-coated core-shell structured liquid acrylic resin improves impact resistance and reduces volume shrinkage. The synergistic use of initiators and accelerators significantly reduces the initiator decomposition activation energy, enabling efficient free radical generation at room temperature and accelerating polymerization. Staged heating polymerization can shorten or even skip the induction period, allowing volume shrinkage to occur in segments, reducing internal stress and defects, ultimately yielding PMMA with high impact resistance and excellent molding quality. Attached Figure Description
[0021] Figure 1Differential scanning calorimetry curves of the multilayer organic-coated core-shell impact modifiers prepared in Examples 1-5; Figure 2 The graph shows the impact strength test results of polymethyl methacrylate prepared in Examples 1-3 and Comparative Examples 1-2. Detailed Implementation
[0022] The following is a further detailed description of the present invention in conjunction with specific preferred embodiments, and it should not be construed that the specific implementation of the present invention is limited to these descriptions. For those skilled in the art, various simple deductions or substitutions can be made without departing from the concept of the present invention, and all such modifications and substitutions should be considered within the scope of protection of the present invention. Specific conditions not specified in the embodiments are performed according to conventional conditions or conditions recommended by the manufacturer. Unless otherwise specified, all reagents or instruments used are conventional products obtained through commercial channels.
[0023] (a) Preparation example Preparation Example 1 Preparation Example 1 provides a multilayer organic-coated core-shell impact modifier, which is prepared by the following steps: (a) 32 g water, 6.68 g butyl acrylate, 1.32 g styrene and 0.088 g sodium dodecyl sulfate were placed in a flask and mixed evenly. The mixture was emulsified under stirring at 200 rpm and heated to 80 °C. Then 0.064 g sodium persulfate was added. After polymerization for 5 min, the emulsion turned blue. After polymerization for another 15 min, the seed emulsion was obtained. (b) Mix 64 g water, 13.36 g butyl acrylate, 2.64 g styrene, 0.176 g sodium dodecyl sulfate and 0.128 g sodium persulfate and stir evenly. Then add the mixture dropwise into the seed emulsion in step (a). Polymerize at 80 °C and 200 rpm for 2.5 h to form a core layer emulsion. (c) 144 g water, 34.2 g methyl methacrylate, 1.8 g ethyl acrylate, 0.54 g sodium dodecyl sulfate, and 0.18 g sodium persulfate were mixed and stirred evenly, and then dropped into the core layer emulsion. The mixture was polymerized at 80 °C and 200 rpm for 2.5 h to form a multilayer organic-coated core-shell emulsion. The emulsion was then dried at 35 °C to obtain a multilayer organic-coated core-shell impact modifier, wherein the amount of core layer emulsifier was 1.1 wt% of the mass of the core layer raw material.
[0024] Preparation Example 2 Preparation Example 2 is basically the same as Preparation Example 1, except that the amount of sodium dodecyl sulfate in step (a) of Preparation Example 1 is adjusted to 0.096 g; the amount of sodium dodecyl sulfate in step (b) is adjusted to 0.192 g, that is, a multilayer organic-coated core-shell impact modifier is prepared by using a core layer emulsifier at 1.2 wt% of the mass of the core layer raw material.
[0025] Preparation Example 3 Preparation Example 3 is basically the same as Preparation Example 1, except that the amount of sodium dodecyl sulfate in step (a) of Preparation Example 1 is adjusted to 0.104 g; and the amount of sodium dodecyl sulfate in step (b) is adjusted to 0.208 g, that is, a multilayer organic-coated core-shell impact modifier is prepared by using a core layer emulsifier at 1.3 wt% of the mass of the core layer raw material.
[0026] Preparation Example 4 Preparation Example 4 is basically the same as Preparation Example 1, except that the amount of sodium dodecyl sulfate in step (a) of Preparation Example 1 is adjusted to 0.112 g; and the amount of sodium dodecyl sulfate in step (b) is adjusted to 0.224 g, that is, a multilayer organic-coated core-shell impact modifier is prepared by using a core layer emulsifier at 1.4 wt% of the mass of the core layer raw material.
[0027] Preparation Example 5 Preparation Example 5 is basically the same as Preparation Example 1, except that the amount of sodium dodecyl sulfate in step (a) of Preparation Example 1 is adjusted to 0.12 g; and the amount of sodium dodecyl sulfate in step (b) is adjusted to 0.240 g, that is, a multilayer organic-coated core-shell impact modifier is prepared by using a core layer emulsifier at 1.5 wt% of the mass of the core layer raw material.
[0028] (II) Implementation Examples Example 1 Example 1 provides a method for preparing high-impact polymethyl methacrylate, comprising the following steps: (1) At room temperature, 16 g of MMA was placed in a beaker, and 4 g of the multilayer organic-coated core-shell impact modifier prepared in Example 2 with a dosage of 1.2 wt% was added and mixed evenly to obtain a multilayer organic-coated core-shell structure liquid acrylic resin. (2) At room temperature, 64 g of MMA and 1.91 g of dodecyl peroxide (LPO) were placed in a flask, heated to 40°C, and stirred at 200 rpm until the initiator LPO dissolved. After cooling to room temperature, 0.54 g of accelerator N,N-dimethylaniline (DMA) was added to the flask. While maintaining the stirring speed, the temperature was increased to 50°C at a rate of 0.6°C / min to obtain the prepolymer slurry. (3) The prepolymer slurry obtained in step (2) is quickly pumped into the cooling and degassing system, and the multilayer organic core-shell structure liquid acrylic resin obtained in step (1) is added at the same time. The mixture is stirred at 200 rpm to cool the prepolymer slurry quickly and delay its further polymerization. After cooling is completed, vacuum degassing is performed. After degassing is completed, the atmosphere is introduced, and the liquid that has been prepolymerized and degassed is poured into the mold. The mixture is first reacted at 35 ℃ for 8 h, and then heated to 80 ℃ for 2 h. After the reaction is completed, the mold is removed and cooled naturally at room temperature to obtain high impact-resistant polymethyl methacrylate with a core layer emulsifier content of 1.2 wt%.
[0029] This embodiment also provides a high-impact polymethyl methacrylate prepared by the above method.
[0030] Example 2 Example 2 is basically the same as Example 1, except that the multilayer organic-coated core-shell impact modifier with a core layer emulsifier content of 1.2 wt% prepared in Example 2 of Example 1 is replaced with the multilayer organic-coated core-shell impact modifier with a core layer emulsifier content of 1.3 wt% prepared in Example 3.
[0031] Example 3 Example 3 is basically the same as Example 1, except that the multilayer organic-coated core-shell impact modifier with a core layer emulsifier content of 1.2 wt% obtained in Preparation Example 2 of Example 1 is replaced with the multilayer organic-coated core-shell impact modifier with a core layer emulsifier content of 1.4 wt% obtained in Preparation Example 4.
[0032] (III) Comparative Example Comparative Example 1 Comparative Example 1 is basically the same as Example 1, except that the multilayer organic-coated core-shell impact modifier with a core layer emulsifier content of 1.2 wt% obtained in Preparation Example 2 of Example 1 is replaced with the multilayer organic-coated core-shell impact modifier with a core layer emulsifier content of 1.1 wt% obtained in Preparation Example 1.
[0033] Comparative Example 2 Comparative Example 2 is basically the same as Example 1, except that the multilayer organic-coated core-shell impact modifier with a core layer emulsifier content of 1.2 wt% obtained in Preparation Example 2 of Example 1 is replaced with the multilayer organic-coated core-shell impact modifier with a core layer emulsifier content of 1.5 wt% obtained in Preparation Example 5.
[0034] (iv) Test Examples Differential scanning calorimetry (DSC) was performed on the multilayer organic-coated core-shell impact modifiers prepared in Examples 1-5. The transition temperature (Tg) of the samples was determined using a differential scanning calorimeter under a nitrogen atmosphere. The test temperature range was −50–140 °C, and the heating rate was 20 °C / min. The test results are as follows: Figure 1 As shown, the multilayer organic-coated core-shell impact modifiers prepared in Examples 1-5 all have two transition temperatures, demonstrating the presence of their core layer (butyl acrylate-styrene copolymer) and shell layer (methyl methacrylate-ethyl acrylate copolymer).
[0035] The polymethyl methacrylates prepared in Examples 1-3 and Comparative Examples 1-2 were subjected to the following performance tests.
[0036] Impact resistance test: Unnotched specimens were prepared and tested according to the GB / T 1043 test standard. The test results are as follows: Figure 2 As shown.
[0037] Figure 2 The impact strength test results of the PMMA materials prepared in Examples 1-3 and Comparative Examples 1-2 of this invention are shown. Each group of samples was tested in parallel five times, and the average value was taken as the data point. As can be seen from the figure, with the increase of the amount of core layer emulsifier (Comparative Example 1, Examples 1-3, Comparative Example 2), the impact strength of the material shows a trend of first increasing and then decreasing. When the amount of core layer emulsifier is 1.2 wt% (Example 1), the impact strength is 16.99 kJ / m. 2 Under these conditions, the core-shell particle interface is tightly bonded and has good rigidity, effectively transferring stress; when the amount of core layer emulsifier is increased to 1.3 wt% (Example 2), the impact strength increases to 20.09 kJ / m. 2 This is because at this dosage, the multilayer organic-coated core-shell impact modifier has a suitable particle size and a complete shell coating, which can effectively transfer stress and induce crazing and shear bands under high-speed impact, efficiently dissipating impact energy; the mechanism of action at 1.4wt% dosage is similar to that at 1.3wt%. For Comparative Examples 1 and 2, the dosage of core layer emulsifier is 1.1wt% and 1.5wt%, respectively, and the impact strength of both is low: insufficient emulsifier dosage will result in excessively large core-shell particle size, while excessive emulsifier will damage the core-shell structure, both of which are not conducive to impact energy absorption. The only difference between Comparative Examples 1-2 and Examples 1-3 is the dosage of core layer emulsifier in the multilayer organic-coated core-shell impact modifier. This application proposes for the first time that by controlling the dosage of core layer emulsifier at 1.2-1.4wt%, a core-shell modifier with suitable particle size and good coating effect can be prepared; combined with the prepolymerization-cooling degassing-segmented heating polymerization process, the impact strength of PMMA material can be significantly improved.
[0038] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, and not to limit them. The basic principles and main features of the present invention have been described above with specific implementation schemes. Based on the present invention, some modifications or substitutions can be made, but these modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the scope of protection claimed by the present invention.
Claims
1. A method for producing a high-impact poly (methyl methacrylate), characterized by, Includes the following steps: (1) A multilayer organic-coated core-shell impact modifier was prepared by seed polymerization, core-layer polymerization and shell-layer polymerization. The obtained multilayer organic-coated core-shell impact modifier was added to methyl methacrylate and mixed evenly to obtain a multilayer organic-coated core-shell liquid acrylic resin. The seed polymerization and core-layer polymerization used both core-layer emulsifier and core-layer raw material. When performing seed polymerization and core-layer polymerization, the amount of core-layer emulsifier used is 1.2-1.4 wt% of the mass of the core-layer raw material; (2) Under stirring and heating conditions, the initiator is dissolved in methyl methacrylate, and after cooling, the accelerator is added and mixed evenly. After heating to 48-50 °C, the prepolymer slurry is obtained. (3) The prepolymer slurry obtained in step (2) is transferred into the cooling and degassing system. While cooling, the multilayer organic core-shell structure liquid acrylic resin described in step (1) is added. After mixing evenly, vacuum degassing is performed, and the mixture is injected into the mold, heated and polymerized, and then naturally cooled to obtain high impact-resistant polymethyl methacrylate.
2. The method for preparing high-impact polymethyl methacrylate according to claim 1, characterized in that, The multilayer organic-coated core-shell impact modifier in step (1) is prepared by the following steps: (a) The core layer raw material and core layer emulsifier are added to water and mixed evenly. Under heating and stirring conditions, an initiator is added to polymerize and form a seed emulsion. (b) The core layer raw material, core layer emulsifier and initiator are added to water and mixed evenly, and then the seed emulsion is added dropwise. The second polymerization is carried out under heating and stirring conditions to obtain the core layer emulsion. (c) The shell raw material, shell emulsifier and initiator are added to water and mixed evenly. Then the core emulsion is added dropwise and the third polymerization is carried out under heating and stirring conditions. After drying, a multilayer organic-coated core-shell impact modifier is obtained.
3. The method for preparing high-impact polymethyl methacrylate according to claim 2, characterized in that, In step (a), the mass ratio of the core layer raw material to water is 1:(3.8-4); the core layer emulsifier is 1.2-1.4 wt% of the core layer raw material; the initiator is 0.7-0.9 wt% of the core layer raw material; the heating temperature is 75-80 ℃, the stirring speed is 200-300 rpm; and the polymerization time is 18-20 min.
4. The method for preparing high-impact polymethyl methacrylate according to claim 2, characterized in that, In step (b), the mass ratio of the core layer raw material to water is 1:(3.8-4); the core layer emulsifier is 1.2-1.4 wt% of the core layer raw material; the initiator is 0.7-0.9 wt% of the core layer raw material; the heating temperature is 75-80 ℃, the stirring speed is 200-300 rpm; and the polymerization time is 2.2-2.5 h.
5. The method for preparing high-impact polymethyl methacrylate according to claim 2, characterized in that, In step (c), the mass ratio of the shell material to water is 1:(3.8-4); the shell emulsifier is 1.4-1.6 wt% of the shell material; the initiator is 0.4-0.6 wt% of the shell material; the heating temperature is 75-80 ℃, the stirring speed is 200-300 rpm; and the polymerization time is 2.2-2.5 h.
6. The method for preparing high-impact polymethyl methacrylate according to claim 2, characterized in that, The mass ratio of the core material in step (a), the core material in step (b), and the shell material in step (c) is 1:(2-2.1):(4.4-4.5); the core material in step (b) is at least one of butyl acrylate, styrene, butadiene, or propyl methacrylate; the shell material in step (c) is at least one of methyl methacrylate, styrene, ethyl acrylate, or butadiene.
7. The method for preparing high-impact polymethyl methacrylate according to claim 1, characterized in that, The mass ratio of the multilayer organic-coated core-shell impact modifier and methyl methacrylate in step (1) is 1:(3.8-4); the initiator in step (2) is any one of benzoyl peroxide (BPO), dodecyl peroxide (LPO), and azobisisobutyronitrile (AIBN); the accelerator is any one of N,N-dimethylanisole (DMA), N,N-dimethyl-p-toluidine (DMT), and N-hydroxyethyl-N-methyl-p-toluidine (HMT).
8. The method for preparing high-impact polymethyl methacrylate according to claim 1, characterized in that, The stirring speed in step (2) is 200 rpm; the heating temperature is 38-42 ℃; the heating rate is 0.6 ℃ / min; and the mass ratio of methyl methacrylate to initiator and accelerator is 15:(0.3-0.5):(0.06-0.13).
9. The method for preparing high-impact polymethyl methacrylate according to claim 1, characterized in that, The mass ratio of the multilayer organic-coated core-shell structure liquid acrylic resin to the prepolymer slurry in step (3) is 1:(3-3.5); the heating polymerization step is as follows: first react at 30-35 ℃ for 8-12 h, and then heat to 75-80 ℃ for 1-3 h.
10. High-impact polymethyl methacrylate prepared by the preparation method according to any one of claims 1-9.
Citation Information
Patent Citations
A transparent antistatic PMMA and its preparation method
CN108314753B