Rubber composition, vulcanizate and process for the preparation thereof and tire tread

By optimizing the composition and structure of the rubber composition and using coupling polymers and siloxane coupling centers, the problem of balancing tire anti-skid performance and rolling resistance was solved, achieving high anti-skid performance and low rolling resistance, while reducing Mooney viscosity.

CN123152240APending Publication Date: 2026-11-24CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202510660459.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-05-21
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing technologies struggle to balance improving tire wet grip performance with reducing rolling resistance, and the introduction of silane compounds leads to increased Mooney viscosity.

Method used

A rubber composition containing natural rubber, styrene-butadiene polymer, polybutadiene rubber, vulcanizing agent, vulcanization accelerator, reinforcing agent and activator is used. By using coupling polymer and block polymer with PB1-SB2-PB3 segment structure, combined with siloxane coupling center and end capping agent, the structure of the composition is optimized to improve wet skid resistance and rolling resistance.

Benefits of technology

This achieves the effect of combining high anti-slip properties and low rolling resistance in rubber compositions, reduces Mooney viscosity, and improves the overall performance of rubber.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present application relates to the field of modified rubber, and discloses a rubber composition, vulcanized rubber, a preparation method thereof and a tire tread rubber. The rubber composition of the present application contains natural rubber, styrene-butadiene polymer, polybutadiene rubber, vulcanizing agent, vulcanization accelerator, reinforcing agent and activator. According to the rubber composition of the present application, the contradictory relationship between the wet skid resistance and the rolling resistance of rubber can be effectively improved, and the prepared vulcanized rubber can have both high wet skid resistance and low rolling resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of modified rubber, specifically to a rubber composition, vulcanized rubber, a method for preparing the same, and a tire tread compound. Background Technology

[0002] In recent years, with the development of the automotive industry and the soaring oil prices, people have paid increasing attention to the safety and fuel efficiency of automobiles. This requires tires to have both high anti-skid performance and low rolling resistance. However, it is often difficult to simultaneously improve anti-skid performance and reduce rolling resistance. Therefore, depending on different usage requirements, it is necessary to find the optimal balance between high anti-skid performance and low rolling resistance.

[0003] CN101319064B discloses a tire tread material with high wet skid resistance, low rolling resistance, and excellent physical and mechanical properties obtained by end-capping SSBR with halosilanes; CN118176219A discloses diene rubber with unsaturated siloxanes as coupling agents, which can be used as tire tread compound; CN112521554A discloses a method to reduce the rolling resistance of SSBR by regulating the distribution of butadiene on the molecular chain.

[0004] It is evident that introducing silane compounds into SSBRs is one of the effective methods to improve their anti-slip properties and low rolling resistance. Regulating the distribution of butadiene in SSBRs can also reduce rolling resistance. However, the introduction of siloxanes can cause some Mooney viscosity issues. Summary of the Invention

[0005] The purpose of this invention is to overcome the problem of increased Mooney viscosity caused by the addition of silane compounds in the prior art, and to provide a rubber composition, vulcanized rubber, preparation method thereof, and tire tread compound that can effectively improve the contradictory relationship between the anti-slip properties and rolling resistance of rubber. The vulcanized rubber of this invention can have both high anti-slip properties and low rolling resistance.

[0006] Therefore, the present invention provides a rubber composition (hereinafter also referred to as the composition), wherein the rubber composition contains natural rubber, styrene-butadiene polymer, polybutadiene rubber, vulcanizing agent, vulcanization accelerator, reinforcing agent and activator, wherein the styrene-butadiene polymer contains a coupling polymer and a block polymer having a PB1-SB2-PB3 segment structure, the coupling polymer contains a structure providing a coupling center and a polymer chain bonded to the coupling center, the polymer chain having a PB1-SB2-PB3 segment structure, and based on the total weight of the polymeric monomers in the styrene-butadiene polymer, the content of structural units from styrene is 10-35% by weight, and the content of structural units from butadiene is 65-90% by weight, and the structure providing the coupling center is at least derived from siloxanes, in the PB1-SB2-PB3 segment structure, PB1 represents polybutadiene segment 1, SB2 represents styrene and butadiene copolymer segment 2, and PB3 represents polybutadiene segment 3.

[0007] Preferably, the number-average molecular weights Mn of PB1 and PB3 are 1000-10000, respectively.

[0008] Preferably, the number-average molecular weight Mn of the polymer chain is 90,000-130,000.

[0009] Preferably, the weight ratio of PB1, SB2 and PB3 is 1:5-95:0.2-15, and more preferably 1:8-92:0.5-10.

[0010] Preferably, in SB2, the content of structural units from butadiene is 60-85% by weight, and the content of structural units from styrene is 15-40% by weight.

[0011] Preferably, based on the total weight of the polymeric monomers in the styrene-butadiene polymer, the content of structural units from styrene is 15-30% by weight, and the content of structural units from butadiene is 70-85% by weight.

[0012] Preferably, the structure providing the coupling center is also derived from tin tetrachloride.

[0013] Preferably, the molar ratio of the structure from the coupling center of the siloxane to the structure from the coupling center of tin tetrachloride is 1:0.1-0.5.

[0014] Preferably, the coupling efficiency of the polymer is 30-70%, more preferably 30-60%, and even more preferably 40-60%.

[0015] Preferably, the polymer contains 32-65% by weight of vinyl structural units, more preferably 35-60% by weight, and even more preferably 35-50% by weight.

[0016] Preferably, the polymer has a molecular weight distribution of 1-4, more preferably 1-2.5.

[0017] Preferably, the polymer also has structural units derived from the capping agent.

[0018] Preferably, the end-capping efficiency of the polymer is 35-70%, more preferably 40-60%.

[0019] Preferably, the end-capping agent is selected from siloxane end-capping agents, and more preferably from one or more of tetramethoxysilane, tetraethoxysilane, tetrapropoxysilane, 3-(2,3-epoxypropoxy)propyltrimethoxysilane, 3-(2,3-epoxypropoxy)propyltriethoxysilane, γ-aminopropyltriethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, vinyltri(β-methoxyethoxy)silane, and [3-(diethylamino)propyl]trimethoxysilane.

[0020] Preferably, the polymer further has polar side chains, which have polar groups.

[0021] Preferably, the polar side chain is derived from a compound having at least one group that can react with the polymer and at least one of the polar groups.

[0022] Preferably, the polar group is selected from one or more of siloxane, hydroxyl, carboxyl, ester, amino, imidazole and thiazole, more preferably one or more of siloxane, hydroxyl, carboxyl and ester.

[0023] Preferably, the content of the polar groups is 0.01-1% by weight, more preferably 0.05-0.5% by weight, based on the total weight of the polymer.

[0024] Preferably, the siloxane is selected from one or more of tetramethoxysilane, tetraethoxysilane, tetrapropoxysilane, 3-(2,3-epoxypropoxy)propyltrimethoxysilane, 3-(2,3-epoxypropoxy)propyltriethoxysilane, γ-aminopropyltriethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, vinyltri(β-methoxyethoxy)silane, and [3-(diethylamino)propyl]trimethoxysilane.

[0025] Preferably, based on a total of 100 parts by weight of the natural rubber, the styrene-butadiene polymer, and the polybutadiene rubber, the content of the vulcanizing agent is 1-4 parts by weight, the content of the vulcanization accelerator is 1-5 parts by weight, the content of the reinforcing agent is 60-90 parts by weight, and the content of the activator is 3-7 parts by weight.

[0026] Preferably, based on a total of 100 parts by weight of the natural rubber, the styrene-butadiene polymer, and the polybutadiene rubber, the content of the vulcanizing agent is 1-3 parts by weight, the content of the vulcanization accelerator is 1-4 parts by weight, the content of the reinforcing agent is 65-85 parts by weight, and the content of the activator is 3-5 parts by weight.

[0027] Preferably, based on a total of 100 parts by weight of the natural rubber, the styrene-butadiene polymer, and the polybutadiene rubber, the content of the natural rubber is 15-50 parts by weight, the content of the styrene-butadiene polymer is 50-80 parts by weight, and the content of the polybutadiene rubber is 5-20 parts by weight.

[0028] Preferably, the polybutadiene rubber is low-cis polybutadiene rubber, high-cis polybutadiene rubber, trans polybutadiene rubber, or a mixture thereof.

[0029] Preferably, the vulcanizing agent is one or more of sulfur, dithiomorpholine, and tetrasulfide dimorpholine.

[0030] Preferably, the vulcanization accelerator is a sulfenamide vulcanization accelerator and / or a guanidine vulcanization accelerator.

[0031] Preferably, the reinforcing agent is carbon black and / or silica.

[0032] Preferably, the activator is stearic acid and / or zinc oxide.

[0033] Preferably, the rubber composition further contains a silane coupling agent, and the content of the silane coupling agent is 5-15 parts by weight, preferably 6-8 parts by weight, based on a total of 100 parts by weight of the natural rubber, the styrene-butadiene polymer and the polybutadiene rubber.

[0034] Preferably, the silane coupling agent is selected from one or more of bis(triethoxypropylsilane)tetrasulfide, bis(triethoxypropylsilane)disulfide, 3-thiomercaptopropyl-triethoxysilane, γ-mercaptopropyl-trimethoxysilane, [2-(4-chloromethylphenyl)ethyl]-triethoxysilane and (3-mercaptopropyl)-bis[tetrazylpolyoxyethylene(5)yl]-ethoxysilane.

[0035] Preferably, the rubber composition further contains a tackifying resin, and the content of the tackifying resin is 3-10 parts by weight, preferably 4-7 parts by weight, based on a total of 100 parts by weight of the natural rubber, the styrene-butadiene polymer and the polybutadiene rubber.

[0036] Preferably, the tackifying resin is selected from phenolic resins, and more preferably p-tert-octylphenolic resin and / or p-tert-butylphenolic resin.

[0037] Preferably, the rubber composition further contains an anti-slip resin, and the content of the anti-slip resin is 3-10 parts by weight, preferably 4-7 parts by weight, based on a total of 100 parts by weight of the natural rubber, the styrene-butadiene polymer and the polybutadiene rubber.

[0038] Preferably, the anti-slip resin is selected from one or more of C5 resin, C5 and C9 copolymer resin, α-methylstyrene resin, terpene resin and dicyclopentadiene resin.

[0039] Preferably, the rubber composition further contains a compatibilizer, and the content of the compatibilizer is 5-10 parts by weight, preferably 5-7 parts by weight, based on a total of 100 parts by weight of the natural rubber, the styrene-butadiene polymer and the polybutadiene rubber.

[0040] Preferably, the compatibilizer is selected from one or more of polyethylene glycol, polyethylene glycol stearate, and polyvinyl alcohol.

[0041] Preferably, the rubber composition further contains an antioxidant, and the antioxidant content is 2-10 parts by weight, preferably 3-5 parts by weight, based on a total of 100 parts by weight of the natural rubber, the styrene-butadiene polymer and the polybutadiene rubber.

[0042] Preferably, the antioxidant is selected from one or more of antioxidant 6PPD, antioxidant 4020, antioxidant 4010, antioxidant 3100 and microcrystalline wax.

[0043] Preferably, the rubber composition further contains a processing aid, and the content of the processing aid is 10-20 parts by weight, preferably 13-17 parts by weight, based on a total of 100 parts by weight of the natural rubber, the styrene-butadiene polymer and the polybutadiene rubber.

[0044] Preferably, the processing aid is selected from one or more of environmentally friendly aromatic oils, naphthenic oils, and shallow-extracted oils.

[0045] According to a second aspect of the present invention, a vulcanized rubber is provided, wherein it is obtained by mixing and vulcanizing the rubber composition described in the first aspect of the present invention.

[0046] According to a third aspect of the present invention, a method for preparing vulcanized rubber is provided, which is obtained by mixing and vulcanizing the rubber composition described in the first aspect of the present invention.

[0047] According to a fourth aspect of the present invention, a tire tread compound is provided, which is prepared by vulcanized rubber as described in the second aspect of the present invention or by vulcanized rubber prepared by the method for preparing vulcanized rubber as described in the third aspect of the present invention.

[0048] Through the above technical solutions, the present invention can provide a rubber composition, vulcanized rubber and its preparation method, and tire tread compound that can effectively improve the contradictory relationship between the anti-slip performance and rolling resistance of rubber. The vulcanized rubber of the present invention can have both high anti-slip performance and low rolling resistance. Detailed Implementation

[0049] The endpoints and any values ​​of the ranges disclosed herein are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of the various ranges, the endpoint values ​​of the various ranges and individual point values, and individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed herein.

[0050] In this invention, "vinyl structural unit" refers to a structural unit derived from butadiene through 1,2-polymerization. "Vinyl structural unit content" refers to the total content of vinyl structural units in the styrene-butadiene polymer.

[0051] In this invention, "coupling efficiency" refers to the percentage of molecular chains that are bound together by the coupling agent out of the total number of molecular chains.

[0052] In this invention, "end-capping efficiency" refers to the percentage of molecular chains that are end-capped by the end-capping agent out of the total number of molecular chains.

[0053] In this invention, PB1 includes PB1 in block polymers having a PB1-SB2-PB3 segment structure, and also includes PB1 in coupling polymers.

[0054] In this invention, SB2 includes SB2 in block polymers having a PB1-SB2-PB3 segment structure, and also includes SB2 in coupling polymers.

[0055] In this invention, PB3 includes PB3 in block polymers having a PB1-SB2-PB3 segment structure, and also includes PB3 in coupling polymers.

[0056] In a first aspect, the present invention provides a rubber composition comprising natural rubber, a styrene-butadiene polymer, polybutadiene rubber, a vulcanizing agent, a vulcanization accelerator, a reinforcing agent, and an activator. The styrene-butadiene polymer comprises a coupling polymer and a block polymer having a PB1-SB2-PB3 segmental structure. The coupling polymer comprises a structure providing a coupling center and a polymer chain bonded to the coupling center. The polymer chain has a PB1-SB2-PB3 segmental structure. Based on the total weight of the monomers in the styrene-butadiene polymer, the content of structural units from styrene is 10-35% by weight, and the content of structural units from butadiene is 65-90% by weight. Furthermore, the structure providing the coupling center is at least derived from siloxanes. In the PB1-SB2-PB3 segmental structure, PB1 represents a polybutadiene segment 1, SB2 represents a styrene-butadiene copolymer segment 2, and PB3 represents a polybutadiene segment 3.

[0057] In this invention, based on the total weight of the polymeric monomers in the styrene-butadiene polymer, the content of structural units from styrene is 10-35% by weight, and the content of structural units from butadiene is 65-90% by weight; preferably, based on the total weight of the polymeric monomers in the styrene-butadiene polymer, the content of structural units from styrene is 15-30% by weight, and the content of structural units from butadiene is 70-85% by weight.

[0058] In this invention, specific examples of the content of styrene structural units, based on the total weight of the polymeric monomers in the styrene-butadiene polymer, can be given, for example: 10 wt%, 11 wt%, 12 wt%, 13 wt%, 14 wt%, 15 wt%, 16 wt%, 17 wt%, 18 wt%, 19 wt%, 20 wt%, 21 wt%, 22 wt%, 23 wt%, 24 wt%, 25 wt%, 26 wt%, 27 wt%, 28 wt%, 29 wt%, 30 wt%, 31 wt%, 32 wt%, 33 wt%, 34 wt%, 35 wt%, etc., as well as any two of the above ranges and all values ​​within that range.

[0059] In this invention, specific examples of the content of structural units from butadiene, based on the total weight of the polymeric monomers in the styrene-butadiene polymer, include, for example, 65 wt%, 66 wt%, 67 wt%, 68 wt%, 69 wt%, 70 wt%, 71 wt%, 72 wt%, 73 wt%, 74 wt%, 75 wt%, 76 wt%, 77 wt%, 78 wt%, 79 wt%, 80 wt%, 81 wt%, 82 wt%, 83 wt%, 84 wt%, 85 wt%, 86 wt%, 87 wt%, 88 wt%, 89 wt%, 90 wt%, etc., as well as any two of the above ranges and all values ​​within that range.

[0060] In this invention, the content of structural units from styrene and the content of structural units from butadiene in the styrene-butadiene polymer are calculated based on the total weight of the monomers and can also be obtained by nuclear magnetic resonance (NMR) measurement.

[0061] According to the present invention, the number average molecular weight Mn of PB1 can be 1000-10000, for example, 1000, 2000, 5000, 8000, 9900, etc., as well as any two of the above ranges and all values ​​within that range.

[0062] According to the present invention, the number average molecular weight Mn of PB3 can be 1000-10000, for example: 2000, 4100, 5100, 6200, 9000, etc., as well as any two of the above ranges and all values ​​within that range.

[0063] According to the present invention, the number average molecular weight Mn of the polymer chain can be 90,000-130,000, for example, 92,000, 100,000, 101,000, 113,000, 115,000, 120,000, 121,000, 125,000, 130,000, etc., as well as any two of the above ranges and all values ​​within that range.

[0064] According to the present invention, preferably, the weight ratio of PB1, SB2 and PB3 is 1:5-95:0.2-15; more preferably, the weight ratio of PB1, SB2 and PB3 is 1:8-92:0.5-10.

[0065] In this invention, specific examples of the weight ratio of PB1, SB2 and PB3 can be, for example, 1:13.5:0.5, 1:10:0.6, 1:20.5:1, 1:44:1, 1:90:9, etc., as well as any two of the above ranges and all values ​​within that range.

[0066] By keeping the weight ratio of PB1, SB2, and PB3 within the above range, the molecular chain can have the advantages of being soft-hard-soft.

[0067] In this invention, the weight ratio of PB1, SB2 and PB3 is calculated by the feeding ratio of each monomer.

[0068] According to the present invention, the block SB2 is obtained by copolymerizing butadiene and styrene. Preferably, the content of structural units from butadiene in SB2 is 60-85% by weight and the content of structural units from styrene is 15-40% by weight; more preferably, the content of structural units from butadiene in SB2 is 65-80% by weight and the content of structural units from styrene is 20-35% by weight.

[0069] In this invention, specific examples of the content of structural units from butadiene in SB2 include, for example, 65 wt%, 66 wt%, 67 wt%, 68 wt%, 69 wt%, 70 wt%, 71 wt%, 72 wt%, 73 wt%, 74 wt%, 75 wt%, 76 wt%, 77 wt%, 78 wt%, 79 wt%, 80 wt%, 81 wt%, 82 wt%, 83 wt%, 84 wt%, 85 wt%, etc., as well as any two of the above ranges and all values ​​within that range.

[0070] In this invention, specific examples of the content of structural units from styrene in SB2 include, for example, 15 wt%, 16 wt%, 17 wt%, 18 wt%, 19 wt%, 20 wt%, 21 wt%, 22 wt%, 23 wt%, 24 wt%, 25 wt%, 26 wt%, 27 wt%, 28 wt%, 29 wt%, 30 wt%, 31 wt%, 32 wt%, 33 wt%, 34 wt%, 35 wt%, 36 wt%, 37 wt%, 38 wt%, 39 wt%, 40 wt%, etc., as well as any two of the above ranges and all values ​​within that range.

[0071] By keeping the content of structural units from butadiene and structural units from styrene within the above-mentioned range in SB2, the SB2 chain segment can be made to maintain flexibility while being slightly rigid.

[0072] In this invention, the content of structural units from butadiene and the content of structural units from styrene in SB2 are calculated by the feeding ratio.

[0073] According to the present invention, the coupling efficiency of the polymer can be 30-70%; preferably, the coupling efficiency of the polymer is 30-60%; more preferably, the coupling efficiency of the polymer is 40-60%.

[0074] In this invention, specific examples of the coupling efficiency of the polymer may include, for example, 30%, 31%, 32%, 33%, 34%, 35%, 36%, 37%, 38%, 39%, 40%, 41%, 42%, 43%, 44%, 45%, 46%, 47%, 48%, 49%, 50%, 51%, 52%, 53%, 54%, 55%, 56%, 57%, 58%, 59%, 60%, 61%, 62%, 63%, 64%, 65%, 66%, 67%, 68%, 69%, 70%, etc., as well as any two of the above ranges and all values ​​within that range.

[0075] In this invention, the coupling polymer comprises a structure providing a coupling center and a polymer chain bonded to the coupling center, wherein the structure providing the coupling center is at least derived from siloxanes. Preferably, the siloxanes are selected from one or more of tetramethoxysilane, tetraethoxysilane, tetrapropoxysilane, 3-(2,3-epoxypropoxy)propyltrimethoxysilane, 3-(2,3-epoxypropoxy)propyltriethoxysilane, γ-aminopropyltriethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, vinyltri(β-methoxyethoxy)silane, and [3-(diethylamino)propyl]trimethoxysilane.

[0076] In one embodiment of the invention, the structure providing the coupling center is further derived from tin tetrachloride. Preferably, the molar ratio of the structure from the siloxane coupling center to the structure from the tin tetrachloride coupling center is 1:0.1-0.5; more preferably, the molar ratio of the structure from the siloxane coupling center to the structure from the tin tetrachloride coupling center is 1:0.15-0.3.

[0077] According to the present invention, preferably, the polymer further comprises structural units derived from the capping agent. The capping agent is preferably selected from siloxane capping agents, more preferably from one or more of tetramethoxysilane, tetraethoxysilane, tetrapropoxysilane, 3-(2,3-epoxypropoxy)propyltrimethoxysilane, 3-(2,3-epoxypropoxy)propyltriethoxysilane, γ-aminopropyltriethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, vinyltri(β-methoxyethoxy)silane, and [3-(diethylamino)propyl]trimethoxysilane.

[0078] In this invention, the end-capping efficiency of the polymer can be 35-70%, preferably 40-60%, for example, 35%, 36%, 37%, 38%, 39%, 40%, 41%, 42%, 43%, 44%, 45%, 46%, 47%, 48%, 49%, 50%, 51%, 52%, 53%, 54%, 55%, 56%, 57%, 58%, 59%, 60%, 61%, 62%, 63%, 64%, 65%, 66%, 67%, 68%, 69%, 70%, etc., as well as any two of the above ranges and all values ​​within that range.

[0079] In this invention, by making the end-capping efficiency of the polymer within the above-mentioned range, the end of the molecular chain can be made to have affinity with silica, thereby reducing the free movement of the end.

[0080] According to the present invention, preferably, the content of vinyl structural units in the polymer is 32-65% by weight; more preferably, the content of vinyl structural units in the polymer is 35-60% by weight; and even more preferably, the content of vinyl structural units in the polymer is 35-50% by weight.

[0081] In this invention, specific examples of the content of vinyl structural units in the polymer may include, for example, 32 wt%, 33 wt%, 34 wt%, 35 wt%, 36 wt%, 37 wt%, 38 wt%, 39 wt%, 40 wt%, 41 wt%, 42 wt%, 43 wt%, 44 wt%, 45 wt%, 46 wt%, 47 wt%, 48 wt%, 49 wt%, 50 wt%, 51 wt%, 52 wt%, 53 wt%, 54 wt%, 55 wt%, 56 wt%, 57 wt%, 58 wt%, 59 wt%, 60 wt%, 61 wt%, 62 wt%, 63 wt%, 64 wt%, 65 wt%, etc., as well as any two of the above ranges and all values ​​within that range.

[0082] In this invention, by keeping the content of the vinyl structural units within the above-mentioned range, it has the advantage of improving the wet slip resistance of rubber.

[0083] According to the present invention, the molecular weight distribution of the polymer can be 1-4; preferably, the molecular weight distribution of the polymer is 1-2.5.

[0084] According to the present invention, preferably, the polymer further has polar side chains, which have polar groups. By giving the polymer the polar side chains, it is advantageous to improve the compatibility between rubber and silica.

[0085] In this invention, the polar side chain is derived from a compound having at least one group that can react with the polymer and at least one of the polar groups.

[0086] According to the present invention, preferably, the polar group is selected from one or more of siloxane, hydroxyl, carboxyl, ester, amino, imidazole and thiazolyl; more preferably, the polar group is selected from one or more of siloxane, hydroxyl, carboxyl and ester.

[0087] According to the present invention, preferably, the content of the polar groups is 0.01-1% by weight based on the total weight of the polymer; more preferably, the content of the polar groups is 0.05-0.5% by weight based on the total weight of the polymer.

[0088] In a preferred embodiment of the invention, the content of the polar groups is 0.05-0.5% by weight, based on the total weight of the polymer, thereby enabling a significantly lower Mooney viscosity.

[0089] In this invention, the compound having at least one group that can react with the polymer and at least one of the polar groups is preferably selected from compounds having a thiol group and the polar group, and the polar group is selected from one or more of siloxane, hydroxyl, carboxyl, ester, amino, imidazole and thiazole, more preferably from one or more of mercaptosiloxane, mercaptoalcohol, mercaptocarboxylic acid and mercaptoester.

[0090] In a preferred embodiment of the present invention, the method for preparing the styrene-butadiene polymer provided by the present invention includes:

[0091] 1) In the presence of an anionic initiator and a structure modifier, the first part of butadiene undergoes a first polymerization to obtain the PB1 segment, styrene and the second part of butadiene are added to undergo a second polymerization to obtain the PB1-SB2 segment, and the third part of butadiene is added to undergo a third polymerization to obtain the PB1-SB2-PB3 polymer chain.

[0092] 2) The step of coupling the polymerization product obtained in step 1) with the coupling agent;

[0093] 3) The step of capping the coupling product obtained in step 2) with a capping agent;

[0094] 4) The step of reacting the capped product obtained in step 3) with a compound having at least one group that can react with the polymer and at least one polar group in the presence of a free radical initiator.

[0095] The coupling agent includes siloxane coupling agents.

[0096] According to the method of the present invention, in step 1), the polymerization reaction is preferably carried out in the presence of a solvent. The solvent can be a variety of substances capable of serving as a reaction medium, for example, it can be a hydrocarbon solvent and / or an ether solvent. The hydrocarbon solvent can be one or more of C5-C7 cycloalkanes, aromatics, and isoalkanes. Specific examples of the hydrocarbon solvent may include, but are not limited to, one or more of benzene, toluene, pentane, heptane, n-hexane, and cyclohexane. The ether solvent can be a C4-C15 monoether and / or polyether. Specific examples of the ether solvent may include, but are not limited to, tert-butoxyethoxyethane and / or tetrahydrofuran. These solvents can be used alone or in combination.

[0097] According to the method of the present invention, the amount of solvent can be reasonably selected according to the amount of monomer. For example, the amount of solvent can make the total concentration of monomer 1-30% by weight, preferably 5-20% by weight.

[0098] According to the method of the present invention, the anionic initiator can be any existing initiator capable of initiating the polymerization of conjugated dienes, for example, an organolithium initiator. The organolithium initiator can be, for example, a single organolithium initiator with the molecular formula RLi, wherein R is a straight-chain or branched alkyl, cycloalkyl, or aryl group. Specifically, the single organolithium initiator can be selected from one or more of ethyllithium, propyllithium, isopropyllithium, n-butyllithium, sec-butyllithium, pentyllithium, hexyllithium, cyclohexyllithium, phenyllithium, methylphenyllithium, and naphthyllithium, preferably n-butyllithium and / or sec-butyllithium. Furthermore, the present invention can also employ bis-lithium initiators, such as trimethylenedilithium and / or tetramethylenedilithium.

[0099] In a preferred embodiment of the present invention, the organolithium initiator is selected from one or more of n-butyllithium, sec-butyllithium, diisopropylaminolithium, bis(trimethylsilyl)aminolithium, and trimethylsilylmethyllithium.

[0100] The present invention does not impose any particular limitation on the amount of the initiator, and it can be rationally selected according to the designed molecular weight. Those skilled in the art should readily understand that when a polymer with a larger molecular weight is required, the amount of initiator can be reduced, but the polymerization rate will decrease accordingly; conversely, when a polymer with a smaller molecular weight is required, the amount of initiator can be increased, but the polymerization rate will increase accordingly. Therefore, considering both the polymerization rate and the molecular weight of the resulting polymer, preferably, based on 100g of the first portion of butadiene, the amount of initiator is 0.75-1.2 mmol.

[0101] According to the method of the present invention, a structure modifier needs to be added during the preparation of the polymer of the present invention, so as to effectively control the microstructure of the styrene-butadiene polymer. The structure modifier can be any existing substance capable of modifying the microstructure of a polymer, for example, it can be selected from one or more of the following: diethyl ether, dibutyl ether, tetrahydrofuran, ethylene glycol dimethyl ether, diethylene glycol dimethyl ether, dioxane, crown ether, tetrahydrofurfuryl ethyl ether, triethylamine, tetramethylethylenediamine, hexamethylphosphoric triamine, potassium tert-butoxide, potassium tert-pentoxide, potassium lauryloxide, potassium alkylbenzene sulfonate, and sodium alkylbenzene sulfonate. Generally, the amount of the structure modifier is not particularly limited, but is based on achieving a vinyl structure of 32-65% by weight in the polymer. The molar ratio of the structure modifier to the anionic initiator used in the preparation of the polymer is usually 1-100:1, preferably 80-100:1.

[0102] According to the method of the present invention, preferably, the weight ratio of the total weight of the first butadiene and styrene and the second butadiene to the weight ratio of the third butadiene is 1:5-95:0.2-15; more preferably, the weight ratio of the total weight of the first butadiene and styrene and the second butadiene to the weight ratio of the third butadiene is 1:8-92:0.5-10, for example, 1:13.5:0.5, 1:10:0.6, 1:20.5:1, 1:44:1, 1:90:9, etc., as well as any two of the above ranges and all values ​​within that range.

[0103] According to the method of the present invention, preferably, based on the total weight of styrene and butadiene, the amount of butadiene is 60-85% by weight and the amount of styrene is 15-40% by weight; more preferably, based on the total weight of styrene and butadiene, the amount of butadiene is 65-80% by weight and the amount of styrene is 20-35% by weight.

[0104] The present invention does not particularly limit the conditions of the polymerization reaction, which generally include temperature, pressure, and time. Specifically, to better facilitate the polymerization reaction, the anionic initiation polymerization temperature is preferably 35-60℃, more preferably 40-50℃, and the polymerization pressure is preferably 0.05-0.5 MPa, more preferably 0.1-0.3 MPa. Generally, extending the polymerization time is beneficial to improving the conversion rate of reactants and the yield of reaction products. However, excessively long polymerization times do not significantly increase the conversion rate of reactants and the yield of reaction products. Therefore, considering both polymerization efficiency and effect, the polymerization time is preferably 30-100 min, more preferably 30-60 min.

[0105] According to the method of the present invention, preferably, the polymerization reaction in step 1) is carried out under an inert atmosphere. The inert atmosphere refers to any gas or gas mixture that does not chemically react with the reactants and products, such as nitrogen and one or more of the group 0 gases of the periodic table. Maintaining the inert atmosphere can be achieved by introducing any of the aforementioned gases or gas mixtures that do not chemically react with the reactants and products into the reaction system.

[0106] According to the method of the present invention, in step 2), the polymer product obtained in step 1) is subjected to a coupling reaction with a coupling agent, said coupling agent comprising a siloxane coupling agent. By adding a siloxane coupling agent, at least a portion of the polymer chains are coupled together. Preferably, the siloxane coupling agent is selected from one or more of tetramethoxysilane, tetraethoxysilane, tetrapropoxysilane, 3-(2,3-epoxypropoxy)propyltrimethoxysilane, 3-(2,3-epoxypropoxy)propyltriethoxysilane, γ-aminopropyltriethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, vinyltri(β-methoxyethoxy)silane, and [3-(diethylamino)propyl]trimethoxysilane.

[0107] In one embodiment of the present invention, the coupling agent comprises a siloxane coupling agent and tin tetrachloride. Preferably, the molar ratio of the siloxane coupling agent to tin tetrachloride is 1:0.1-0.5; more preferably, the molar ratio of the siloxane coupling agent to tin tetrachloride is 1:0.15-0.3.

[0108] The present invention does not particularly limit the amount of the siloxane coupling agent, which can be adjusted according to the final coupling efficiency of the product being 30-70%. For example, the molar ratio of the siloxane coupling agent to the anionic initiator is 0.1-2:1, preferably 0.1-1:1.

[0109] In this invention, specific examples of the molar ratio of the siloxane coupling agent to the anionic initiator include, for example, 0.1:1, 0.2:1, 0.3:1, 0.4:1, 0.5:1, 0.6:1, 0.7:1, 0.8:1, 0.9:1, 1:1, 1.1:1, 1.2:1, 1.3:1, 1.4:1, 1.5:1, 1.6:1, 1.7:1, 1.8:1, 1.9:1, 2:1, etc., as well as any two of the above ranges and all values ​​within that range.

[0110] According to the method of the present invention, the conditions of the coupling reaction are not particularly limited and can be conventional conditions in the art. Preferably, the conditions of the coupling reaction include: a coupling temperature of 60-90°C, a coupling time of 15-30 min, and a reaction pressure of 0.05-0.3 MPa.

[0111] Generally, anionic polymerization systems do not exhibit obvious termination or transfer reactions; even after all monomers are consumed, the active sites remain. Therefore, according to the present invention, after the polymerization and coupling reactions are completed, a capping agent needs to be added to kill all active ends.

[0112] In this invention, the capping agent is preferably a siloxane, more preferably selected from one or more of tetramethoxysilane, tetraethoxysilane, tetrapropoxysilane, 3-(2,3-epoxypropoxy)propyltrimethoxysilane, 3-(2,3-epoxypropoxy)propyltriethoxysilane, γ-aminopropyltriethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, vinyltri(β-methoxyethoxy)silane, and [3-(diethylamino)propyl]trimethoxysilane.

[0113] The amount of the capping agent can be reasonably selected based on the amount of anionic initiator used to prepare the polymer, with the capping efficiency being 35-70%. Generally speaking, the molar ratio of the capping agent to the anionic initiator is 0.4-0.7:1. For example, 0.4:1, 0.5:1, 0.6:1, 0.7:1, etc., as well as any two of the above ranges and all values ​​within that range.

[0114] According to the method of the present invention, the end-sealing conditions are not particularly limited and can be conventional conditions in the art. Preferably, the end-sealing conditions include: an end-sealing reaction temperature of 60-90°C, an end-sealing reaction time of 15-30 min, and an end-sealing reaction pressure of 0.05-0.3 MPa.

[0115] According to the method of the present invention, the capped product obtained in step 3) is reacted with a compound having at least one group reactive to the polymer and at least one polar group in the presence of a free radical initiator. Preferably, the free radical initiation reaction is carried out in an inert atmosphere.

[0116] The free radical initiator may be one or more of the free radical initiators known to those skilled in the art, such as azo initiators, peroxide initiators, and redox initiators.

[0117] The azo initiator may be selected from one or more of the following: dimethyl azobisisobutyrate, azobisisobutyramidine hydrochloride, azodicarbonamide, azobisisopropylimidazoline hydrochloride, azoisobutylcyanoformamide, azobiscyclohexylformonitrile, azobiscyanopentanoic acid, azobisisopropylimidazoline, azobisisobutyronitrile, azobisisovalerate, and azobisisoheptanenitrile.

[0118] The peroxide initiator may be selected from one or more of hydrogen peroxide, ammonium persulfate, sodium persulfate, potassium persulfate, benzoyl peroxide, and tert-butyl peroxide.

[0119] The redox initiator is selected from one or more of sulfate-sulfite, persulfate-thiourea, persulfate-organic salt, and ammonium persulfate-aliphatic amine. Specifically, the sulfate-sulfite can be selected from one or more of sodium sulfate-sodium sulfite, potassium sulfate-potassium sulfite, and ammonium sulfate-ammonium sulfite; the persulfate-thiourea can be selected from one or more of sodium persulfate-thiourea, potassium persulfate-thiourea, and ammonium persulfate-thiourea; the persulfate-organic salt can be selected from one or more of sodium persulfate-potassium acetate, potassium persulfate-potassium acetate, and ammonium persulfate-ammonium acetate; and the ammonium persulfate-aliphatic amine can be selected from ammonium persulfate-N,N-tetramethylethylenediamine and / or ammonium persulfate-diethylamine.

[0120] According to the method of the present invention, the amount of the free radical initiator can be appropriately selected according to the amount of polar groups grafted to the side chain. Preferably, the amount of the free radical initiator is 0.01-0.1% by weight, based on the weight of the polar groups grafted to the side chain; more preferably, the amount of the free radical initiator is 0.01-0.08% by weight, based on the weight of the polar groups grafted to the side chain.

[0121] According to the method of the present invention, step 4) imparts polar side chains to the polymer. Imparting these polar side chains to the polymer has the advantage of improved compatibility between the rubber and silica.

[0122] According to the method of the present invention, preferably, the polar group is selected from one or more of siloxane, hydroxyl, carboxyl, ester, amino, imidazole and thiazole; more preferably, the polar group is selected from one or more of siloxane, hydroxyl, carboxyl and ester.

[0123] In a preferred embodiment of the invention, the compound having at least one group that can react with the polymer and at least one polar group is preferably selected from compounds having a thiol group and the polar group, and the polar group is selected from one or more of siloxane, hydroxyl, carboxyl, ester, amino, imidazole and thiazole, more preferably from one or more of mercaptosiloxane, mercaptoalcohol, mercaptocarboxylic acid and mercaptoester.

[0124] According to the method of the present invention, the amount of the compound having at least one group that can react with the polymer and at least one polar group is 0.01-1% by weight.

[0125] According to the method of the present invention, preferably, in step 4), the reaction conditions include: a free radical initiation temperature of 60-90°C, a reaction time of 1-2 h, and a reaction pressure of 0.05-0.3 MPa.

[0126] In this invention, all pressures refer to gauge pressure.

[0127] According to the method of the present invention, after the polymer preparation is completed, an antioxidant is preferably added. This enables the obtained polymer to have good anti-aging properties and also inhibits Mooney proliferation caused by the introduction of siloxanes. The antioxidants are mainly hindered phenols, such as antioxidants 1520, 1010, 1076, 2088, 1790, 3114, 2264, and 564. More preferably, the hindered phenolic antioxidants are used in combination with phosphite antioxidants, because their main function is to decompose hydroperoxides. Suitable antioxidants include TNP, TNPP, 168, 2018, 2103, and 2105. The total amount of antioxidants is based on 100g of polymer, with a content of 0.5-1.5% by weight. The weight ratio of hindered phenolic antioxidants to phosphite antioxidants can be 0.2-0.5:1.

[0128] According to the method of the present invention, after the addition of antioxidants, the polymer can be precipitated from the solution by methods such as purification precipitation, centrifugation, filtration, decantation, and hot water coagulation. Alternatively, the solvent in the reaction system can be removed by air stripping, which is known to those skilled in the art and will not be described in detail here.

[0129] The other components of the rubber composition of the present invention will now be described.

[0130] According to the present invention, the rubber composition contains, in addition to styrene-butadiene polymer, natural rubber, polybutadiene rubber, vulcanizing agent, vulcanization accelerator, reinforcing agent and activator.

[0131] According to the present invention, preferably, based on a total of 100 parts by weight of the natural rubber, the styrene-butadiene polymer, and the polybutadiene rubber, the content of the vulcanizing agent is 1-4 parts by weight, the content of the vulcanization accelerator is 1-5 parts by weight, the content of the reinforcing agent is 60-90 parts by weight, and the content of the activator is 3-7 parts by weight; more preferably, based on a total of 100 parts by weight of the natural rubber, the styrene-butadiene polymer, and the polybutadiene rubber, the content of the vulcanizing agent is 1-3 parts by weight, the content of the vulcanization accelerator is 1-4 parts by weight, the content of the reinforcing agent is 65-85 parts by weight, and the content of the activator is 3-5 parts by weight.

[0132] According to the present invention, preferably, based on a total of 100 parts by weight of the natural rubber, the styrene-butadiene polymer, and the polybutadiene rubber, the content of the natural rubber is 15-50 parts by weight, the content of the styrene-butadiene polymer is 50-80 parts by weight, and the content of the polybutadiene rubber is 5-20 parts by weight; more preferably, based on a total of 100 parts by weight of the natural rubber, the styrene-butadiene polymer, and the polybutadiene rubber, the content of the natural rubber is 18-22 parts by weight, the content of the styrene-butadiene polymer is 65-75 parts by weight, and the content of the polybutadiene rubber is 8-12 parts by weight.

[0133] According to the present invention, there is no particular limitation on the natural rubber, and various natural rubbers commonly used in the art can be used. The natural rubber can be obtained commercially and will not be described in detail here.

[0134] According to the present invention, the polybutadiene rubber can be low-cis polybutadiene rubber, high-cis polybutadiene rubber, trans polybutadiene rubber, and mixtures thereof. The polybutadiene rubber can be commercially available or prepared according to various methods known to those skilled in the art, which will not be elaborated here.

[0135] According to the present invention, the vulcanizing agent can be various conventional vulcanizing agents, such as one or more of sulfur, dithiomorpholine, and tetrathiodimorpholine, preferably sulfur, and more preferably insoluble sulfur. The insoluble sulfur is an allotrope of sulfur, insoluble in sulfur dioxide and other solvents, and also insoluble in rubber, existing in a dispersed state within the rubber. When the vulcanization temperature is reached, these insoluble sulfur particles dispersed in the rubber undergo an "activation stage," i.e., chain depolymerization, which accelerates the vulcanization rate, reduces the amount of sulfur required, and is beneficial for improving the aging properties of the rubber.

[0136] According to the present invention, the vulcanization accelerator can be any existing substance capable of shortening vulcanization time, lowering vulcanization temperature, reducing the amount of vulcanizing agent, and improving the physical and mechanical properties of rubber. However, in order to obtain a rubber composition with superior environmental performance, the vulcanization accelerator is preferably a sulfenamide vulcanization accelerator and / or a guanidine vulcanization accelerator. The sulfenamide vulcanization accelerator is preferably selected from one or more of N-tert-butyl-2-benzothiazolyl sulfenamide, N-cyclohexyl-2-benzothiazolyl sulfenamide, and N-oxodiethylene-2-benzothiazolyl sulfenamide; the guanidine vulcanization accelerator is preferably diphenylguanidine and / or di-o-tolueneguanidine. The N-tert-butyl-2-benzothiazolyl sulfenamide is commercially known as TBBS or NS and is a vulcanization accelerator with extremely excellent performance.

[0137] According to the present invention, the types of reinforcing agents are known to those skilled in the art. For example, the reinforcing agent can be carbon black and / or silica. The carbon black can be any existing carbon black suitable for use in rubber compositions, such as one or more selected from industrial reference carbon black 7#, high abrasion furnace black N330, and medium-super abrasion furnace black N220. The silica can also be any existing silica capable of improving the strength of the rubber composition, and all silica can be commercially available, for example, silica of grade 115GR purchased from Degussa.

[0138] According to the present invention, the type of activator can also be a conventional choice in the art, such as stearic acid and / or zinc oxide.

[0139] According to the present invention, preferably, the rubber composition further contains a silane coupling agent. The presence of a silane coupling agent improves the dispersion of silica in the rubber.

[0140] As the silane coupling agent, it is preferably selected from one or more of bis(triethoxypropylsilane)tetrasulfide, bis(triethoxypropylsilane)disulfide, 3-thiomercaptopropyl-triethoxysilane, γ-mercaptopropyl-trimethoxysilane, [2-(4-chloromethylphenyl)ethyl]-triethoxysilane and (3-mercaptopropyl)-bis[tetrazylpolyoxyethylene(5)yl]-ethoxysilane.

[0141] In this invention, based on a total of 100 parts by weight of the natural rubber, the styrene-butadiene polymer, and the polybutadiene rubber, the content of the silane coupling agent can be 5-15 parts by weight; preferably, based on a total of 100 parts by weight of the natural rubber, the styrene-butadiene polymer, and the polybutadiene rubber, the content of the silane coupling agent is 6-8 parts by weight.

[0142] According to the present invention, preferably, the rubber composition further comprises a tackifying resin. The presence of a tackifying resin improves processing performance.

[0143] The tackifying resin is preferably selected from phenolic resins, more preferably from p-tert-octylphenolic resins and / or p-tert-butylphenolic resins.

[0144] In this invention, based on a total of 100 parts by weight of the natural rubber, the styrene-butadiene polymer, and the polybutadiene rubber, the content of the tackifying resin can be 3-10 parts by weight; preferably, based on a total of 100 parts by weight of the natural rubber, the styrene-butadiene polymer, and the polybutadiene rubber, the content of the tackifying resin is 4-7 parts by weight.

[0145] According to the present invention, preferably, the rubber composition further comprises an anti-slip resin. By including the anti-slip resin, the grip on both dry and wet surfaces can be further improved.

[0146] The anti-slip resin is preferably selected from one or more of C5 resin, C5 and C9 copolymer resin, α-methylstyrene resin, terpene resin and dicyclopentadiene resin; more preferably, the anti-slip resin is selected from dicyclopentadiene resin and / or α-methylstyrene resin.

[0147] In this invention, based on a total of 100 parts by weight of the natural rubber, the styrene-butadiene polymer, and the polybutadiene rubber, the content of the anti-slip resin can be 3-10 parts by weight; preferably, based on a total of 100 parts by weight of the natural rubber, the styrene-butadiene polymer, and the polybutadiene rubber, the content of the anti-slip resin is 4-7 parts by weight.

[0148] According to the present invention, preferably, the rubber composition further comprises a compatibilizer. The inclusion of a compatibilizer improves the compatibility between the rubber and silica.

[0149] The compatibilizer is preferably selected from one or more of polyethylene glycol, polyethylene glycol stearate, and polyvinyl alcohol, more preferably polyethylene glycol. For example, polyethylene glycol 4000 can be used.

[0150] In this invention, based on a total of 100 parts by weight of the natural rubber, the styrene-butadiene polymer, and the polybutadiene rubber, the content of the compatibilizer can be 5-10 parts by weight; preferably, based on a total of 100 parts by weight of the natural rubber, the styrene-butadiene polymer, and the polybutadiene rubber, the content of the compatibilizer is 5-7 parts by weight.

[0151] According to the present invention, preferably, the rubber composition further comprises an antioxidant. As the antioxidant, physical antioxidants and chemical antioxidants can be used. For example, microcrystalline wax, paraffin wax, etc., can be used as physical antioxidants. For example, antioxidants 6PPD, 4020, 4010, 3100, etc., can be used as chemical antioxidants.

[0152] In a preferred embodiment of the present invention, the antioxidant is selected from one or more of antioxidant 6PPD, antioxidant 4020, antioxidant 4010, antioxidant 3100 and microcrystalline wax.

[0153] In this invention, based on a total of 100 parts by weight of the natural rubber, the styrene-butadiene polymer, and the polybutadiene rubber, the content of the antioxidant is 2-10 parts by weight; preferably, based on a total of 100 parts by weight of the natural rubber, the styrene-butadiene polymer, and the polybutadiene rubber, the content of the antioxidant is 3-5 parts by weight.

[0154] According to the present invention, preferably, the rubber composition further contains processing aids. By containing processing aids, it possesses the processing properties required for rubber compounding.

[0155] The solvent is preferably selected from one or more of environmentally friendly aromatic oils, naphthenic oils, and shallow-extracting oils, and more preferably environmentally friendly aromatic oils.

[0156] In this invention, based on a total of 100 parts by weight of the natural rubber, the styrene-butadiene polymer, and the polybutadiene rubber, the solvent content is 10-20 parts by weight; preferably, based on a total of 100 parts by weight of the natural rubber, the styrene-butadiene polymer, and the polybutadiene rubber, the solvent content is 13-17 parts by weight.

[0157] According to a second aspect of the present invention, a vulcanized rubber is provided, wherein it is obtained by mixing and vulcanizing the rubber composition described in the first aspect of the present invention.

[0158] According to a third aspect of the present invention, a method for preparing vulcanized rubber is provided, wherein the rubber is obtained by mixing and vulcanizing the rubber composition described in the first aspect of the present invention.

[0159] In this invention, there are no particular limitations on the methods and conditions for mixing and vulcanization; conventional methods and conditions in the art can be used.

[0160] In one specific embodiment of the present invention, in the first stage, all components of the rubber composition except for the vulcanizing agent and vulcanization accelerator are mixed in an internal mixer at a speed of 70 r / min and a temperature controlled below 150°C for 5 minutes. The mixture is then discharged, pressed into sheets on an open mill, and left to stand at room temperature for 4 hours. In the second stage, the first stage rubber compound is added to the internal mixer at a speed of 40 r / min and a temperature of 140°C or after mixing for 2 minutes. The mixture is then discharged, pressed into sheets on an open mill, and left to stand at room temperature for 4 hours. In the third stage, the second stage rubber compound is added to the internal mixer at a speed of 40 r / min and a temperature of 40°C. The accelerator and vulcanizing agent are then added, and the mixture is discharged after a temperature of 115°C or after 5 minutes.

[0161] According to a fourth aspect of the present invention, a tire tread compound is provided, which is prepared by vulcanized rubber as described in the second aspect of the present invention or by vulcanized rubber prepared by the method for preparing vulcanized rubber as described in the third aspect of the present invention.

[0162] The present invention will be described in detail below through embodiments, but the present invention is not limited to the following embodiments.

[0163] In the following examples and comparative examples, the thiol conversion rate (i.e., the content of polar side chain groups) and the end-capping efficiency were determined using an Agilent 7890A gas chromatograph. The test conditions included: SPB-5 60m×0.32mm×1.0um capillary column, column flow rate 2.0ml / min, column temperature 220℃, vaporization chamber temperature 220℃, detection chamber temperature 250℃, split ratio 50:1, and injection volume 0.3ul.

[0164] The content of polar side chain groups can also be determined using a nuclear magnetic resonance spectrometer (AVANCE DRX 400MHz) from Bruker, Switzerland, in accordance with GB / T 28728-2012, with deuterated chloroform as the solvent.

[0165] The content of butadiene structural units with double bonds in the side chain was determined using an AVANCEDRX 400MHz nuclear magnetic resonance spectrometer from Bruker, Switzerland, in accordance with GB / T 28728-2012, with deuterated chloroform as the solvent.

[0166] The contents of styrene structural units (structural units derived from styrene) and butadiene structural units (structural units derived from butadiene) were determined using an AVANCE DRX400MHz nuclear magnetic resonance spectrometer from Bruker, Switzerland, in accordance with GB / T 28728-2012, with deuterated chloroform as the solvent.

[0167] Number-average molecular weight, molecular weight distribution, and coupling efficiency were determined using a gel permeation chromatography (GPC) system (WATERS ALLIANCE 2690) from the United States, with THF as the mobile phase, narrow-distribution polystyrene as the standard, and the temperature at 25°C.

[0168] Mooney viscosity was determined using a Shimadzu SMV-300 Mooney viscometer according to the method specified in GB / T1232-92.

[0169] Preparation Example 1

[0170] In a 10-liter stainless steel stirred tank under high-purity nitrogen protection, 5000 g of cyclohexane, 5 g of butadiene, and 35 ml of tetrahydrofuran were added. The mixture was then heated to 55°C, followed by the addition of 5 mmol of tributyltin lithium, with the pressure controlled at 0.2 MPa to initiate the reaction. After the butadiene reaction was complete, 140 g of styrene and 310 g of butadiene were added to continue the reaction. After the monomer conversion was complete, 45 g of butadiene was added until all monomers were converted, ending the polymerization reaction. The reaction time was 60 min. At 60°C and 0.1 MPa, 0.5 mmol of tetraethoxysilane was added, with a coupling time of 15 min. At 60°C and 0.1 MPa, 3 mmol of vinyltrimethoxysilane was added to obtain end-capped modified SSBR. Then, at 70°C and 0.2 MPa, 0.8 g of γ-mercaptopropyltrimethoxysilane and 6.7 mg of azobisisobutyronitrile were added, and the reaction was carried out for 2 hours to obtain the functionalized styrene-butadiene polymer. 4g of antioxidant 3114 and 1g of antioxidant 2018 were added to the above styrene-butadiene polymer, followed by coagulation and drying. The structure of the styrene-butadiene polymer is shown in Table 1. Furthermore, the Mooney viscosity test results are shown in Table 2.

[0171] Preparation Example 2

[0172] In a 10-liter stainless steel stirred tank under high-purity nitrogen protection, 5000 g of cyclohexane, 12 g of butadiene, and 1 g of tetrahydrofurfuryl alcohol ether were added. The mixture was then heated to 50°C, and 6 mmol of diisopropylaminolithium was added while maintaining the pressure at 0.3 MPa to initiate the reaction. After the butadiene reaction was complete, 121 g of styrene and 405 g of butadiene were added to continue the reaction. After the monomer conversion was complete, 12 g of butadiene was added until all the monomers were converted, at which point the polymerization reaction ended. The reaction time was 60 min. At 65°C and 0.2 MPa, 0.1 mmol of tin tetrachloride and 0.58 mmol of tetramethoxysilane were added, with a coupling time of 15 min. Finally, at 65°C and 0.2 MPa, 3.3 mmol of 3-(2,3-epoxypropoxy)propyltrimethoxysilane was added to obtain the end-capped modified SSBR. Then, at a temperature of 75℃ and a pressure of 0.3 MPa, 0.5 g of γ-mercaptopropyltrimethoxysilane, 0.5 g of mercaptoethanol, and 10 mg of azobisisobutyronitrile were added, and the reaction was carried out for 2 hours to obtain a functionalized styrene-butadiene polymer. 4 g of antioxidant 3114 and 1 g of antioxidant 2018 were added to the above styrene-butadiene polymer, followed by coagulation and drying. The structure of the styrene-butadiene polymer is shown in Table 1. Furthermore, the Mooney viscosity test results are shown in Table 2.

[0173] Preparation Example 3

[0174] In a 10-liter stainless steel stirred tank under high-purity nitrogen protection, 5000g of cyclohexane, 20g of butadiene, and 4g of tetrahydrofurfuryl alcohol ether were added. The mixture was then heated to 60°C, and 4mmol of trimethylsilylmethyllithium was added while maintaining the pressure at 0.4MPa to initiate the reaction. After the butadiene reaction was complete, 108g of styrene and 302g of butadiene were added to continue the reaction. After the monomer conversion was complete, 20g of butadiene was added until all the monomers were converted, at which point the polymerization reaction ended. The reaction time was 60min. At 70°C and 0.3MPa, 0.1mmol of tin tetrachloride and 0.4mmol of 3-(2,3-epoxypropoxy)propyltriethoxysilane were added, with a coupling time of 15min. At 70°C and 0.2MPa, 2mmol of 3-(2,3-epoxypropoxy)propyltrimethoxysilane was added to obtain the end-capped modified SSBR. Then, at a temperature of 80℃ and a pressure of 0.3MPa, 1.0g of mercaptopropionic acid, 0.2g of isopropyl mercaptopropionate, and 21mg of azobisisobutyronitrile were added, and the reaction was carried out for 2 hours to obtain a functionalized styrene-butadiene polymer. 4g of antioxidant 3114 and 1g of antioxidant 2018 were added to the above styrene-butadiene polymer, followed by coagulation and drying. The structure of the styrene-butadiene polymer is shown in Table 1. Furthermore, the Mooney viscosity test results are shown in Table 2.

[0175] Preparation Example 4

[0176] In a 10-liter stainless steel stirred tank under high-purity nitrogen protection, 5000g of cyclohexane, 40g of butadiene, and 2g of tetrahydrofurfuryl alcohol ether were added. The mixture was then heated to 50°C, and 5mmol of lithium dimethylamine was added while maintaining the pressure at 0.4MPa to initiate the reaction. After the butadiene reaction was complete, 108g of styrene and 432g of butadiene were added to continue the reaction. After the monomer conversion was complete, 20g of butadiene was added until all the monomers were converted, at which point the polymerization reaction ended. The reaction time was 60min. At 75°C and 0.3MPa, 0.75mmol of vinyltriethoxysilane was added, with a coupling time of 15min. Finally, at 75°C and 0.2MPa, 2mmol of γ-aminopropyltriethoxysilane was added to obtain the end-capped modified SSBR. Then, 0.5 g of 1-mercapto-2-propanol and 18 mg of azobisisoheptanyl cyanide were added at 82 °C and 0.3 MPa, and the reaction was carried out for 2 hours to obtain a functionalized styrene-butadiene polymer. 4 g of antioxidant 3114 and 1 g of antioxidant 2018 were added to the above styrene-butadiene polymer, and the mixture was allowed to coagulate and dry. The structure of the styrene-butadiene polymer is shown in Table 1. Furthermore, the Mooney viscosity test results are shown in Table 2.

[0177] Preparation Example 5

[0178] In a 10-liter stainless steel stirred tank under high-purity nitrogen protection, 5000 g of cyclohexane, 52 g of butadiene, and 4 g of bis(tetrahydrofurfuryl)propane were added. The mixture was then heated to 45°C, and 5.2 mmol of n-butyllithium was added while maintaining the pressure at 0.4 MPa to initiate the reaction. After the butadiene reaction was complete, 120 g of styrene and 397 g of butadiene were added to continue the reaction. After the monomer conversion was complete, 31 g of butadiene was added until all the monomers were converted, at which point the polymerization reaction ended. The reaction time was 60 min. At 80°C and 0.3 MPa, 0.95 mmol of N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane was added, with a coupling time of 15 min. At 80°C and 0.2 MPa, 2.34 mmol of [3-(diethylamino)propyl]trimethoxysilane was added to obtain the end-capped modified SSBR. Then, 3g of γ-mercaptopropyltriethoxysilane and 30mg of azobisisoheptacyanide were added at 81℃ and 0.3MPa, and the reaction was carried out for 2 hours to obtain a functionalized styrene-butadiene polymer. 4g of antioxidant 3114 and 1g of antioxidant 2018 were added to the above styrene-butadiene polymer, and the mixture was allowed to coagulate and dry. The structure of the styrene-butadiene polymer is shown in Table 1. Furthermore, the Mooney viscosity test results are shown in Table 2.

[0179] Preparation of Comparative Example 1

[0180] Styrene-butadiene polymers were prepared according to the method in Example 5, except that styrene, isoprene, and butadiene were added to the polymerization reactor at once to obtain diene hydrocarbon polymers, the structures of which are shown in Table 1. Furthermore, the Mooney viscosity test results are shown in Table 2.

[0181] Preparation of Comparative Example 2

[0182] Styrene-butadiene polymers were prepared according to the method in Example 5, except that silicon tetrachloride was used as the coupling agent. The resulting styrene-butadiene polymers are shown in Table 1. Furthermore, the Mooney viscosity test results are shown in Table 2.

[0183] Preparation of Comparative Example 3

[0184] The styrene and butadiene polymer before coupling was prepared according to method CN112521554A. Specifically, in a 10-liter stainless steel stirred tank under high-purity nitrogen protection, 5000g of cyclohexane, 120g of styrene, 240g of butadiene, and 4g of bis(tetrahydrofurfuryl)propane were added. The mixture was then heated to 45°C, and 5.2mmol of n-butyllithium was added while maintaining the pressure at 0.2MPa to initiate the reaction. After reaching the maximum temperature, 240g of butadiene was added until all monomers were converted, ending the polymerization reaction. The polymer was then coupled, end-capped, and modified according to the method in Example 5 to obtain the styrene-butadiene polymer, the structure of which is shown in Table 1. Furthermore, the Mooney viscosity test results are shown in Table 2.

[0185] Table 1

[0186] Z1 Z2 Z3 Z4 Z5 ZD1 ZD2 ZD3 Styrene structural units (wt%) 28 22 24 18 20 20 20 20 Butadiene structural units (wt%) 72 78 76 82 80 80 80 80 Vinyl (wt%) 38 48 53 55 59 57 59 59 Mn(PB1) / 10,000 0.10 0.20 0.50 0.80 0.99 - 0.99 - Mn(PB3) / 10,000 0.90 0.20 0.51 0.41 0.62 - 0.62 - Single-arm Mn / 10,000 10.1 9.2 11.3 12.1 11.5 11.4 11.5 11.5 Coupling efficiency (%) 40 45 50 60 55 56 56 56 End capping efficiency (%) 60 55 50 40 45 44 44 44 Side chain polar groups (wt%) 0.15 0.16 0.23 0.07 0.45 0.45 0.45 0.45

[0187] - indicates that it was not measured.

[0188] Table 2

[0189] project Z1 Z2 Z3 Z4 Z5 ZD1 ZD2 ZD3 Mooney viscosity of raw rubber 57.6 51.1 58.2 55.3 60.3 62.1 61.5 61.0 24h Mooney viscosity* 57.5 51.1 58.3 55.6 60.4 62.2 67.7 61.0 48h Mooney viscosity* 57.8 51.5 58.5 55.9 60.8 62.6 67.6 61.6

[0190] *Mooney viscosity of the dried sample after aging in air at 100°C is intended to simulate a longer storage time for the sample.

[0191] Examples 1-5 and Comparative Examples 1-3

[0192] Examples 1-5 illustrate the vulcanized rubber and its preparation method provided by the present invention.

[0193] Preparation of compound rubber:

[0194] 70 parts by weight of styrene-butadiene polymers prepared in Preparation Examples 1-5 and Comparative Preparation Examples 1-3, 20 parts of natural rubber, 10 parts of cis-butadiene rubber, 2 parts by weight of stearic acid (Hong Kong Siwen Chemical Co., Ltd., SA1801), 9 parts by weight of high abrasion resistant furnace black N330 (Tianjin Jinqiushi Carbon Black Chemical Co., Ltd.), 60 parts by weight of silica 115GR (Degussa), and 5 parts by weight of p-tert-octylphenol resin (DuPont Surlyn). 1801); 6 parts α-methylstyrene resin (product of Kertész Chemical Co., Ltd.), 2 parts zinc oxide (Liuzhou Zinc Products Co., Ltd.), 2 parts antioxidant 4020, 1.9 parts N-tert-butyl-2-benzothiazole sulfenamide TBBS (purchased from Hebi Lianhao Chemical Co., Ltd.), 1.7 parts diphenylguanidine (Guangzhou Lida Rubber Raw Material Trading Co., Ltd., DPG), 1.5 parts sulfur, 6 parts silane coupling agent Si69 (Degussa), 1 part microcrystalline wax, 5.6 parts polyethylene glycol 4000, and 15 parts aromatic oil (Hansheng V500).

[0195] All components of the rubber composition, except for sulfur and vulcanization accelerator, were mixed in an internal mixer at a speed of 70 r / min and a temperature below 150℃ for 5 minutes. The mixture was then discharged, pressed into sheets on an open mill, and left to stand at room temperature for 4 hours. The mixture was then returned to the internal mixer at a speed of 40 r / min and a temperature of 140℃, or after 2 minutes of mixing, it was discharged and pressed into sheets on an open mill, left to stand at room temperature for 4 hours. The mixture was then returned to the internal mixer at a speed of 40 r / min and a temperature of 40℃, after which the accelerator and vulcanizing agent were added, and the mixture was discharged after 5 minutes of mixing at 115℃. The mixed rubber was then vulcanized at 150℃ and 12 MPa on a flat vulcanizing machine for 35 minutes to obtain vulcanized rubbers S1-S5 and DS1-DS3.

[0196] The present invention provides a test for the properties of vulcanized rubber.

[0197] (1) Mechanical property testing:

[0198] Vulcanized rubber was made into 2mm thick vulcanized rubber sheets. The vulcanized rubber sheets were cut into dumbbell-shaped standard pieces according to the type 1 dumbbell cutter specified in GB / T528-1998. The mechanical properties of the vulcanized rubber sheets were tested using a rubber tensile testing machine (manufactured by Shimadzu Corporation, Japan, model AG-20KNG). The test temperature was 25℃ and the traction speed was 500 mm / min. The tensile strength and elongation at break of the vulcanized rubber were obtained.

[0199] (2) Shore A hardness test:

[0200] The test shall be conducted according to the method specified in GB / T531-1999.

[0201] (3) Deformation resistance test:

[0202] Cut the vulcanized rubber into dumbbell-shaped standard pieces using a type 1 dumbbell cutter as specified in GB / T528-92. The samples are then tensile-broken at a test temperature of 25℃ and a traction speed of 500 mm / min. After the tensile fracture, the samples are left to stand for 3 minutes, then the two broken parts are joined together. The distance between the two parallel lines after joining is measured, and the permanent tensile deformation is calculated using the following formula:

[0203] S b =100(L) t -L0) / L0, where S b To break permanent deformation, %; L t L1 is the distance between the two parallel lines after the sample matches, in mm; L0 is the initial test length, in mm.

[0204] (4) Testing of wet skid resistance and rolling resistance:

[0205] The wet skid resistance and rolling resistance of vulcanized rubber were determined using a DMA-2980 viscoelastic spectrometer from TA Instruments (USA). The test frequency was 2 Hz, the heating rate was 5 °C / min, the test temperature was 100 °C, and the sample size was 40 mm × 5 mm × 1 mm. The wet skid resistance of vulcanized rubber was represented by tanδ at 0 °C; a larger tanδ indicates better wet skid resistance. The rolling resistance of vulcanized rubber was represented by tanδ at 60 °C; a smaller tanδ indicates lower rolling resistance.

[0206] The test results are shown in Table 3.

[0207] Table 3

[0208] project S1 S2 S3 S4 S5 DS1 DS2 DS3 Tensile strength / MPa 17.8 18.0 18.2 18.4 18.5 18.3 18.4 18.4 Elongation / % 338 377 374 368 373 350 382 375 Shore hardness A 72 72 72 72 72 72 72 72 Permanent deformation / % 10 10 10 8 8 10 8 8 tanδ(0℃) 0.3012 0.2972 0.2997 0.2971 0.2993 0.2961 0.2931 0.2901 tanδ(60℃) 0.1091 0.1036 0.0999 0.1026 0.1014 0.1193 0.1029 0.1160

[0209] As shown in Table 2, the rubber composition provided by this invention has a lower Mooney viscosity. Furthermore, as shown in Table 3, the rubber composition provided by this invention has better wet skid resistance and lower rolling resistance, making it suitable for green tire tread compounds.

[0210] The preferred embodiments of the present invention have been described in detail above; however, the present invention is not limited thereto. Within the scope of the inventive concept, various simple modifications can be made to the technical solutions of the present invention, including combinations of various technical features in any other suitable manner. These simple modifications and combinations should also be considered as the content disclosed in the present invention and are all within the protection scope of the present invention.

Claims

1. A rubber composition, characterized in that, The rubber composition contains natural rubber, styrene-butadiene polymer (SBR), polybutadiene rubber, vulcanizing agent, vulcanization accelerator, reinforcing agent, and activator. The SBR contains a coupling polymer and a block polymer having a PB1-SB2-PB3 segmental structure. The coupling polymer contains a structure providing a coupling center and polymer chains bonded to the coupling center. The polymer chains have a PB1-SB2-PB3 segmental structure. Based on the total weight of the monomers in the SBR, the content of structural units from styrene is 10-35% by weight, and the content of structural units from butadiene is 65-90% by weight. Furthermore, the structure providing the coupling center is at least derived from siloxanes. In the PB1-SB2-PB3 segmental structure, PB1 represents polybutadiene segment 1, SB2 represents a styrene-butadiene copolymer segment 2, and PB3 represents polybutadiene segment 3.

2. The rubber composition according to claim 1, wherein, The number-average molecular weights (Mn) of PB1 and PB3 are 1000-10000, respectively. Preferably, the number-average molecular weight Mn of the polymer chain is 90,000-130,000; Preferably, the weight ratio of PB1, SB2 and PB3 is 1:5-95:0.2-15, and more preferably 1:8-92:0.5-10; Preferably, in SB2, the content of structural units from butadiene is 60-85% by weight, and the content of structural units from styrene is 15-40% by weight.

3. The rubber composition according to claim 1, wherein, Based on the total weight of the polymeric monomers in the styrene-butadiene polymer, the content of structural units from styrene is 15-30% by weight, and the content of structural units from butadiene is 70-85% by weight.

4. The rubber composition according to any one of claims 1-3, wherein, The structure providing the coupling center also originates from tin tetrachloride; Preferably, the molar ratio of the structure from the coupling center of siloxane to the structure from the coupling center of tin tetrachloride is 1:0.1-0.5; Preferably, the coupling efficiency of the polymer is 30-70%, more preferably 30-60%, and even more preferably 40-60%.

5. The rubber composition according to any one of claims 1-3, wherein, The polymer contains 32-65% by weight of vinyl structural units, preferably 35-60% by weight, and more preferably 35-50% by weight. Preferably, the polymer has a molecular weight distribution of 1-4, more preferably 1-2.

5.

6. The rubber composition according to any one of claims 1-3, wherein, The polymer also has structural units derived from the capping agent; Preferably, the end-capping efficiency of the polymer is 35-70%, more preferably 40-60%; Preferably, the end-capping agent is selected from siloxane end-capping agents, and more preferably from one or more of tetramethoxysilane, tetraethoxysilane, tetrapropoxysilane, 3-(2,3-epoxypropoxy)propyltrimethoxysilane, 3-(2,3-epoxypropoxy)propyltriethoxysilane, γ-aminopropyltriethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, vinyltri(β-methoxyethoxy)silane, and [3-(diethylamino)propyl]trimethoxysilane.

7. The rubber composition according to any one of claims 1-3, wherein, The polymer also has polar side chains, which have polar groups; Preferably, the polar side chain is derived from a compound having at least one group that can react with the polymer and at least one of the polar groups; Preferably, the polar group is selected from one or more of siloxane, hydroxyl, carboxyl, ester, amino, imidazole and thiazole, more preferably one or more of siloxane, hydroxyl, carboxyl and ester; Preferably, the content of the polar groups is 0.01-1% by weight, more preferably 0.05-0.5% by weight, based on the total weight of the polymer.

8. The rubber composition according to any one of claims 1-3, wherein, The siloxanes are selected from one or more of tetramethoxysilane, tetraethoxysilane, tetrapropoxysilane, 3-(2,3-epoxypropoxy)propyltrimethoxysilane, 3-(2,3-epoxypropoxy)propyltriethoxysilane, γ-aminopropyltriethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, vinyltri(β-methoxyethoxy)silane, and [3-(diethylamino)propyl]trimethoxysilane.

9. The rubber composition according to any one of claims 1-3, wherein, Based on a total of 100 parts by weight of the natural rubber, the styrene-butadiene polymer and the polybutadiene rubber, the content of the vulcanizing agent is 1-4 parts by weight, the content of the vulcanization accelerator is 1-5 parts by weight, the content of the reinforcing agent is 60-90 parts by weight, and the content of the activator is 3-7 parts by weight. Preferably, based on a total of 100 parts by weight of the natural rubber, the styrene-butadiene polymer, and the polybutadiene rubber, the content of the vulcanizing agent is 1-3 parts by weight, the content of the vulcanization accelerator is 1-4 parts by weight, the content of the reinforcing agent is 65-85 parts by weight, and the content of the activator is 3-5 parts by weight. Preferably, based on a total of 100 parts by weight of the natural rubber, the styrene-butadiene polymer, and the polybutadiene rubber, the content of the natural rubber is 15-50 parts by weight, the content of the styrene-butadiene polymer is 50-80 parts by weight, and the content of the polybutadiene rubber is 5-20 parts by weight.

10. The rubber composition according to any one of claims 1-3, wherein, The polybutadiene rubber is low-cis polybutadiene rubber, high-cis polybutadiene rubber, trans polybutadiene rubber, and mixtures thereof.

11. The rubber composition according to any one of claims 1-3, wherein, The vulcanizing agent is one or more of sulfur, dithiomorpholine and tetrasulfide dimorpholine; Preferably, the vulcanization accelerator is a sulfenamide vulcanization accelerator and / or a guanidine vulcanization accelerator; Preferably, the reinforcing agent is carbon black and / or silica; Preferably, the activator is stearic acid and / or zinc oxide.

12. The rubber composition according to any one of claims 1-3, wherein, The rubber composition further contains a silane coupling agent, and the content of the silane coupling agent is 5-15 parts by weight, preferably 6-8 parts by weight, based on a total of 100 parts by weight of the natural rubber, the styrene-butadiene polymer and the polybutadiene rubber. Preferably, the silane coupling agent is selected from one or more of bis(triethoxypropylsilane)tetrasulfide, bis(triethoxypropylsilane)disulfide, 3-thiomercaptopropyl-triethoxysilane, γ-mercaptopropyl-trimethoxysilane, [2-(4-chloromethylphenyl)ethyl]-triethoxysilane and (3-mercaptopropyl)-bis[tetrazylpolyoxyethylene(5)yl]-ethoxysilane.

13. The rubber composition according to any one of claims 1-3, wherein, The rubber composition further contains a tackifying resin, and the content of the tackifying resin is 3-10 parts by weight, preferably 4-7 parts by weight, based on a total of 100 parts by weight of the natural rubber, the styrene-butadiene polymer and the polybutadiene rubber. Preferably, the tackifying resin is selected from phenolic resins, and more preferably p-tert-octylphenolic resin and / or p-tert-butylphenolic resin.

14. The rubber composition according to any one of claims 1-3, wherein, The rubber composition further contains an anti-slip resin, and the content of the anti-slip resin is 3-10 parts by weight, preferably 4-7 parts by weight, based on a total of 100 parts by weight of the natural rubber, the styrene-butadiene polymer and the polybutadiene rubber. Preferably, the anti-slip resin is selected from one or more of C5 resin, C5 and C9 copolymer resin, α-methylstyrene resin, terpene resin and dicyclopentadiene resin.

15. The rubber composition according to any one of claims 1-3, wherein, The rubber composition further contains a compatibilizer, and the content of the compatibilizer is 5-10 parts by weight, preferably 5-7 parts by weight, based on a total of 100 parts by weight of the natural rubber, the styrene-butadiene polymer and the polybutadiene rubber. Preferably, the compatibilizer is selected from one or more of polyethylene glycol, polyethylene glycol stearate, and polyvinyl alcohol.

16. The rubber composition according to any one of claims 1-3, wherein, The rubber composition further contains an antioxidant, and the antioxidant content is 2-10 parts by weight, preferably 3-5 parts by weight, based on a total of 100 parts by weight of the natural rubber, the styrene-butadiene polymer and the polybutadiene rubber. Preferably, the antioxidant is selected from one or more of antioxidant 6PPD, antioxidant 4020, antioxidant 4010, antioxidant 3100 and microcrystalline wax.

17. The rubber composition according to any one of claims 1-3, wherein, The rubber composition further contains processing aids, and the content of the processing aids is 10-20 parts by weight, preferably 13-17 parts by weight, based on a total of 100 parts by weight of the natural rubber, the styrene-butadiene polymer and the polybutadiene rubber. Preferably, the processing aid is selected from one or more of environmentally friendly aromatic oils, naphthenic oils, and shallow-extracted oils.

18. A vulcanized rubber, characterized in that, It is obtained by mixing and vulcanizing the rubber composition according to any one of claims 1-17.

19. A method for preparing vulcanized rubber, characterized in that, It is obtained by mixing and vulcanizing the rubber composition according to any one of claims 1-17.

20. A tire tread compound, which is prepared by using the vulcanized rubber of claim 18 or the vulcanized rubber prepared by the method of preparing the vulcanized rubber of claim 19.

Citation Information

Patent Citations

  • Method for preparing terminal group functional solution polymerized butadiene styrene rubber filling white carbon black composite material

    CN101319064B

  • Synthesis method of solution polymerized styrene-butadiene rubber, low-heat-generation solution polymerized styrene-butadiene rubber and automobile tire

    CN112521554A

  • Diene rubbers prepared with unsaturated siloxane-based coupling agents