Pitch direct modification agent for hot and humid regions and preparation method thereof
By using functionalized calcium carbonate and epoxidized terpene phenol resin as components in asphalt direct-injection modifiers, the high-temperature performance and anti-aging problems of asphalt pavement modifiers in hot and humid regions have been solved, thereby improving the water damage resistance and road service life of asphalt mixtures.
Patent Information
- Application Number
- CN202611209348.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-11
- Publication Date
- 2026-11-24
AI Technical Summary
When existing direct-injection modifiers are used in hot and humid regions, it is difficult to simultaneously ensure the high-temperature performance, resistance to thermo-oxidative aging, storage stability, and resistance to water damage of modified asphalt.
Using styrene-butadiene-styrene block copolymer, functionalized calcium carbonate, epoxidized terpene phenol resin and antioxidants, and through silanization treatment and photo-initiated covalent grafting technology, the compatibility and interfacial adhesion between the filler and asphalt are improved, forming a long-lasting anti-aging and interfacial reinforcement function.
It improves the high-temperature mixing performance and long-term service life of asphalt mixtures, reduces water damage, and enhances road performance.
Abstract
Description
Technical Field
[0001] This invention relates to the field of road asphalt modification materials technology, specifically to an asphalt direct-injection modifier for hot and humid regions and its preparation method. Background Technology
[0002] In hot and humid regions, asphalt pavements face severe challenges due to the combined effects of high temperatures, heavy rainfall, and strong ultraviolet radiation, leading to rutting, water damage, and aging. To improve the road performance of asphalt mixtures, polymer modifiers are typically added during the mixing process. Among these, direct-injection modifiers have received widespread attention in engineering applications because they do not require pre-prepared modified asphalt and can be directly added to the mixing drum during mixing. The core requirement for direct-injection modifiers is that they can rapidly melt and uniformly disperse within a limited mixing time after being added to the mixing drum, thereby effectively modifying the asphalt.
[0003] Chinese Patent 202311730372.5 discloses a direct-application, fast-melting adhesive powder modifier, recycled asphalt mixture, and its preparation method. The direct-application, fast-melting adhesive powder modifier is composed of adhesive powder, styrene-based thermoplastic elastomer, thermoplastic resin, rubber softener, grafting agent, coupling agent, crosslinking stabilizer, antioxidant, and dispersant. This modifier uses waste adhesive powder as the main raw material, has a high melt index, and can achieve rapid melting at low temperatures, making it suitable for recycled asphalt mixtures.
[0004] The aforementioned existing technologies mainly focus on the rapid melting modification of rubber powder, combining various components through physical blending and utilizing the elasticity of the swollen rubber powder to improve the low-temperature performance of asphalt. However, in the high-temperature, heavy-load, and continuously humid environments unique to hot and humid regions, asphalt mixtures place higher demands on the modifier's resistance to thermo-oxidative aging and water damage. Functional additives in physically blended systems are easily consumed during high-temperature mixing and long-term service, making it difficult to provide continuous and stable protection to the asphalt matrix. Therefore, developing a direct-injection modifier with both long-lasting anti-aging and interface-enhancing functions is a practical technical need for asphalt pavements in hot and humid regions, specifically addressing their unique service conditions. Summary of the Invention
[0005] (a) Technical problems to be solved The purpose of this invention is to provide a direct-injection modifier for asphalt in humid and hot regions and its preparation method, so as to solve the problem that existing direct-injection modifiers are difficult to simultaneously achieve high-temperature performance, resistance to thermo-oxidative aging, storage stability and resistance to water damage when applied in humid and hot regions.
[0006] (II) Technical Solution To achieve the above objectives, the present invention provides the following technical solution: A direct-injection modifier for asphalt in humid and hot regions comprises the following raw materials in parts by weight: 60-80 parts of styrene-butadiene-styrene block copolymer, 5-15 parts of softening oil, 5-10 parts of tackifying resin, 0.2-0.8 parts of antioxidant, 2-5 parts of lubricant, and 8-15 parts of modified filler.
[0007] Furthermore, the modified filler is prepared by means of the following steps: A1. Add calcium carbonate to a mixed solvent, disperse it by ultrasonication, add γ-methacryloxypropyltrimethoxysilane, adjust the pH to 4-5 with acetic acid, heat and stir the reaction, filter, wash, and vacuum dry to obtain vinyl-functionalized calcium carbonate. A2. Add the vinyl-functionalized calcium carbonate to tetrahydrofuran, add 3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate mercaptoethyl ester and benzoin dimethyl ether, stir under nitrogen protection and irradiate with a UV lamp with a main wavelength of 365 nm for 30-60 min, filter, wash the filter cake with tetrahydrofuran, and vacuum dry to obtain the modified packing.
[0008] Furthermore, the tackifying resin is prepared by the following steps: B1. Dissolve terpene phenol resin in toluene, add epichlorohydrin, heat and add sodium hydroxide solution dropwise, keep the reaction at the temperature, let stand and separate the layers, wash with water until neutral, and distill under reduced pressure to obtain epoxidized terpene phenol resin. B2. The epoxidized terpene phenol resin is heated and melted, γ-aminopropyltriethoxysilane is added, the mixture is heated to react, and then discharged, cooled and crushed to obtain a tackifying resin.
[0009] Furthermore, the styrene-butadiene-styrene block copolymer has a star-shaped structure, a particle size ≤2.0 mm, a melt flow index of 1.0~4.0 g / 10 min, and a styrene content of 25%~35% and a butadiene content of 65%~75%.
[0010] Furthermore, the softening oil is a naphthenic rubber oil.
[0011] Furthermore, the antioxidant is a mixture of antioxidant 1010 and antioxidant 168, wherein the weight ratio of antioxidant 1010 to antioxidant 168 is 1:(1~2).
[0012] Furthermore, the lubricant is calcium stearate.
[0013] Furthermore, in step A1, the mixed solvent is composed of anhydrous ethanol and water in a volume ratio of (8~10):1, the solid-liquid ratio of calcium carbonate to the mixed solvent is 1:(8~12) g / mL, the ultrasonic dispersion time is 15~30 min, the amount of γ-methacryloyloxypropyltrimethoxysilane is 2.0%~3.0% of the weight of calcium carbonate, the heating and stirring reaction temperature is 45~55℃, and the reaction time is 1.5~2.5 h.
[0014] Furthermore, in step A2, the weight ratio of the vinyl-functionalized calcium carbonate, tetrahydrofuran, and 3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate mercaptoethyl ester is 1:(8~15):(0.05~0.12), and the amount of benzoin dimethyl ether used is 3%~8% of the weight of the 3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate mercaptoethyl ester.
[0015] Furthermore, in step B1, the solid-liquid ratio of the terpene phenol resin to toluene is 1:(2~4) g / mL, and the weight ratio of the terpene phenol resin, epichlorohydrin, and sodium hydroxide solution is 1:(0.8~1.2):(0.24~0.6), wherein the mass fraction of the sodium hydroxide solution is 35%~45%, the dropping time is 1~2 h, the heating dropping temperature is 65~75 °C, and the heat preservation reaction time is 2.5~3.5 h.
[0016] Furthermore, in step B2, the heating and melting temperature is 90~100℃, the amount of γ-aminopropyltriethoxysilane is 8%~15% of the weight of the epoxidized terpene phenol resin, the heating reaction temperature is 80~90℃, and the heating reaction time is 1~2h.
[0017] A method for preparing a direct-injection asphalt modifier for hot and humid regions includes the following steps: S1. Add styrene-butadiene-styrene block copolymer and softening oil to a high-speed mixer and stir for 15-30 minutes at a temperature of 60-80℃ and a speed of 200-400 r / min. Then add modified filler, tackifying resin, antioxidant and lubricant, and continue stirring for 5-15 minutes. Discharge the material to obtain the premix. S2. The premixed material is added to a twin-screw extruder. The screw speed is set to 200~350 r / min. The temperatures of each zone are set as follows: Zone 1 130~150℃, Zone 2 150~170℃, Zone 3 160~180℃, Zone 4 160~180℃, Zone 5 150~170℃, and the die head 150~170℃. Vacuum exhaust is performed in the middle section of the extruder, with a vacuum degree of -0.06~-0.09 MPa. The extruded strip is water-cooled, air-dried, and pelletized to obtain a direct-injection modifier for asphalt in humid and hot regions.
[0018] (iii) Beneficial technical effects Compared with the prior art, the beneficial effects of the present invention are: (1) The present invention uses calcium carbonate as a matrix and introduces polymerizable double bonds on its surface through silanization treatment, which can change the surface of calcium carbonate from hydrophilic to hydrophobic, improve the compatibility of filler with styrene-butadiene-styrene block copolymer matrix, and enable the filler to be uniformly dispersed during premixing and extrusion, reducing the uneven performance of modifier caused by filler agglomeration.
[0019] (2) Based on the silanization treatment, this invention further covalently grafts a thiol-containing hindered phenolic antioxidant onto the filler surface via a thioether bond under photoinitiation conditions. This covalent grafting method stably anchors the hindered phenolic antioxidant groups onto the filler surface, making them less prone to migration or volatilization during high-temperature mixing and long-term service of asphalt mixtures. This allows them to continuously exert a free radical scavenging effect, delaying the thermo-oxidative aging process of the asphalt matrix and helping to extend the service life of asphalt pavements.
[0020] (3) The present invention uses terpene phenol resin as the matrix. The phenolic hydroxyl groups are first converted into epoxy groups through epoxidation of phenolic hydroxyl groups, which eliminates some intermolecular hydrogen bonding, helps to reduce the melt viscosity of the resin and improve its processing fluidity in the preparation of direct injection modifier. At the same time, the introduced glycidyl ether structure has good thermal stability, which is beneficial to improving the applicability of the tackifying resin under high temperature extrusion and mixing conditions.
[0021] (4) Based on the epoxidation treatment, this invention further introduces hydrolyzable alkoxysilane groups into the resin molecular chain segments through the epoxy-amine ring-opening reaction of epoxy groups and aminosilanes. When the direct-injection modifier is involved in the mixing of asphalt mixture, the alkoxysilane groups hydrolyze under the action of moisture and temperature to generate silanol groups, which condense with the hydroxyl groups on the aggregate surface to form covalent bonds. This chemical bonding enhances the adhesion between asphalt and aggregate interface, helps reduce asphalt film peeling caused by moisture intrusion, and improves the water damage resistance of asphalt mixture.
[0022] (5) This invention uses modified filler and modified tackifying resin in synergy, which can respectively play the functions of long-term anti-aging and interfacial chemical reinforcement in asphalt mixtures, and the two complement each other. The anti-aging function helps to maintain the flexibility and adhesion of the asphalt matrix and provides a reliable stress transfer medium for interfacial chemical bonding; while good interfacial adhesion reduces the erosion of the asphalt matrix by water penetration along the interface, delays structural aging, and systematically improves the comprehensive road performance of asphalt pavement in humid and hot areas.
[0023] (6) The present invention uses star-shaped styrene-butadiene-styrene block copolymer as the matrix. In its molecular structure, the styrene segments can form physical cross-linking points, and the butadiene segments provide elastic recovery ability. When used in combination with cycloalkyl rubber oil, it can give the direct-injection modifier good melt flowability and basic modification effect, providing favorable conditions for the dispersion and function of functional components. Detailed Implementation
[0024] The technical solutions of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention. Example 1
[0025] A direct-injection modifier for asphalt in humid and hot regions comprises the following raw materials in parts by weight: 60 parts styrene-butadiene-styrene block copolymer, 5 parts softening oil, 5 parts tackifying resin, 0.2 parts antioxidant, 2 parts lubricant, and 8 parts modified filler; The styrene-butadiene-styrene block copolymer has a star-shaped structure, a particle size of 0.5 mm, a melt flow index of 2.0 g / 10 min, a styrene content of 25%, and a butadiene content of 75%. The softening oil is a naphthenic rubber oil. The antioxidant is a mixture of antioxidant 1010 and antioxidant 168, with a weight ratio of antioxidant 1010 to antioxidant 168 of 1:2. The lubricant is calcium stearate.
[0026] The modified filler is prepared by the following steps: A1. Calcium carbonate was added to a mixed solvent, ultrasonically dispersed, γ-methacryloxypropyltrimethoxysilane was added, pH was adjusted to 4 with acetic acid, the reaction was heated and stirred, filtered, washed with anhydrous ethanol, and dried under vacuum at 60°C for 4 h to obtain vinyl-functionalized calcium carbonate. The mixed solvent is composed of anhydrous ethanol and water in a volume ratio of 8:1, the solid-liquid ratio of calcium carbonate to the mixed solvent is 1:8 g / mL, the ultrasonic dispersion time is 30 min, the amount of γ-methacryloyloxypropyltrimethoxysilane is 2.0% of the weight of calcium carbonate, the heating and stirring reaction temperature is 45℃, and the reaction time is 2.5 h. A2. Add the vinyl-functionalized calcium carbonate to tetrahydrofuran, add 3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate mercaptoethyl ester and benzoin dimethyl ether, stir under nitrogen protection and irradiate with a UV lamp with a main wavelength of 365 nm for 60 min, filter, wash the filter cake with tetrahydrofuran, and dry under vacuum at 40 °C for 4 h to obtain the modified filler; The weight ratio of the vinyl-functionalized calcium carbonate, tetrahydrofuran, and 3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate mercaptoethyl ester is 1:8:0.05, and the amount of benzoin dimethyl ether used is 8% of the weight of 3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate mercaptoethyl ester.
[0027] The tackifying resin is prepared by the following steps: B1. Dissolve terpene phenol resin in toluene, add epichlorohydrin, heat and add sodium hydroxide solution dropwise, keep the reaction at the temperature, let stand and separate the layers, wash with water until neutral, and distill under reduced pressure at a vacuum of -0.08 MPa and a temperature of 60℃ for 3 hours to obtain epoxidized terpene phenol resin. The solid-liquid ratio of the terpene phenol resin to toluene is 1:2 g / mL, the weight ratio of the terpene phenol resin, epichlorohydrin, and sodium hydroxide solution is 1:0.8:0.24, the mass fraction of the sodium hydroxide solution is 35%, the dropping time is 2 h, the heating dropping temperature is 65 °C, and the heat preservation reaction time is 3.5 h. B2. The epoxidized terpene phenol resin is heated to 90°C to melt, γ-aminopropyltriethoxysilane is added, and the mixture is heated to 80°C for 2 hours. The mixture is discharged, cooled to room temperature, and crushed to a particle size ≤5mm to obtain the tackifying resin. The amount of γ-aminopropyltriethoxysilane used is 8% of the weight of the epoxidized terpene phenol resin.
[0028] A method for preparing a direct-injection asphalt modifier for hot and humid regions includes the following steps: S1. Add styrene-butadiene-styrene block copolymer and softening oil to a high-speed mixer and stir for 30 minutes at 60°C and 200 r / min. Then add modified filler, tackifying resin, antioxidant and lubricant, and continue stirring for 15 minutes. Discharge the material to obtain the premix. S2. The premixed material is added to a twin-screw extruder, the screw speed is set to 200 r / min, and the temperatures of each zone are set to 130℃ for zone 1, 150℃ for zone 2, 160℃ for zone 3, 160℃ for zone 4, 150℃ for zone 5, and 150℃ for the die. Vacuum exhaust is performed in the middle section of the extruder, with a vacuum degree of -0.06 MPa. The extruded strip is water-cooled, air-dried, and pelletized to obtain a direct-injection modifier for asphalt in humid and hot areas. Example 2
[0029] A direct-injection modifier for asphalt in humid and hot regions comprises the following raw materials in parts by weight: 65 parts styrene-butadiene-styrene block copolymer, 8 parts softening oil, 6 parts tackifying resin, 0.35 parts antioxidant, 3 parts lubricant, and 10 parts modified filler. The styrene-butadiene-styrene block copolymer has a star-shaped structure, a particle size of 0.5 mm, a melt flow index of 2.0 g / 10 min, a styrene content of 28%, and a butadiene content of 72%. The softening oil is a naphthenic rubber oil. The antioxidant is a mixture of antioxidant 1010 and antioxidant 168, with a weight ratio of antioxidant 1010 to antioxidant 168 of 1:1.75. The lubricant is calcium stearate.
[0030] The modified filler is prepared by the following steps: A1. Calcium carbonate was added to a mixed solvent and ultrasonically dispersed. γ-methacryloxypropyltrimethoxysilane was added, and the pH was adjusted to 4.2 with acetic acid. The mixture was heated and stirred to react, filtered, washed with anhydrous ethanol, and dried under vacuum at 65°C for 3.5 h to obtain vinyl-functionalized calcium carbonate. The mixed solvent is composed of anhydrous ethanol and water in a volume ratio of 8.5:1, the solid-liquid ratio of calcium carbonate to the mixed solvent is 1:9 g / mL, the ultrasonic dispersion time is 26 min, the amount of γ-methacryloyloxypropyltrimethoxysilane is 2.2% of the weight of calcium carbonate, the heating and stirring reaction temperature is 48℃, and the reaction time is 2.3 h. A2. The vinyl-functionalized calcium carbonate was added to tetrahydrofuran, along with 3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate mercaptoethyl ester and benzoin dimethyl ether. Under nitrogen protection, the mixture was stirred and irradiated with a 365 nm UV lamp for 50 min. After filtration, the filter cake was washed with tetrahydrofuran and dried under vacuum at 45 °C for 3.5 h to obtain the modified filler. The weight ratio of the vinyl-functionalized calcium carbonate, tetrahydrofuran, and 3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate mercaptoethyl ester is 1:10:0.065, and the amount of benzoin dimethyl ether used is 6.5% of the weight of 3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate mercaptoethyl ester.
[0031] The tackifying resin is prepared by the following steps: B1. Dissolve terpene phenol resin in toluene, add epichlorohydrin, heat and add sodium hydroxide solution dropwise, keep the reaction at the temperature, let stand and separate the layers, wash with water until neutral, and distill under reduced pressure at a vacuum of -0.085 MPa and a temperature of 68℃ for 2.5 h to obtain epoxidized terpene phenol resin. The solid-liquid ratio of the terpene phenol resin to toluene is 1:2.5 g / mL, the weight ratio of the terpene phenol resin, epichlorohydrin, and sodium hydroxide solution is 1:0.9:0.33, the mass fraction of the sodium hydroxide solution is 38%, the dropping time is 1.8 h, the heating dropping temperature is 68 °C, and the heat preservation reaction time is 3.2 h. B2. The epoxidized terpene phenol resin is heated to 93°C to melt, γ-aminopropyltriethoxysilane is added, and the mixture is heated to 83°C for 1.8 hours. The mixture is discharged, cooled to room temperature, and crushed to a particle size ≤5 mm to obtain the tackifying resin. The amount of γ-aminopropyltriethoxysilane used is 10% of the weight of the epoxidized terpene phenol resin.
[0032] A method for preparing a direct-injection asphalt modifier for hot and humid regions includes the following steps: S1. Add the styrene-butadiene-styrene block copolymer and softening oil to a high-speed mixer and stir for 25 minutes at a temperature of 65℃ and a speed of 250r / min. Then add the modified filler, tackifying resin, antioxidant and lubricant, and continue stirring for 12 minutes. Discharge the material to obtain the premix. S2. The premixed material is added to a twin-screw extruder, the screw speed is set to 240 r / min, and the temperatures of each zone are set to 135℃ for zone 1, 155℃ for zone 2, 165℃ for zone 3, 165℃ for zone 4, 155℃ for zone 5, and 155℃ for the die. Vacuum exhaust is performed in the middle section of the extruder, with a vacuum degree of -0.07 MPa. The extruded strip is water-cooled, air-dried, and pelletized to obtain a direct-injection modifier for asphalt in humid and hot areas. Example 3
[0033] A direct-injection asphalt modifier for hot and humid regions comprises the following raw materials in parts by weight: 70 parts styrene-butadiene-styrene block copolymer, 10 parts softening oil, 8 parts tackifying resin, 0.5 parts antioxidant, 4 parts lubricant, and 12 parts modified filler. The styrene-butadiene-styrene block copolymer has a star-shaped structure, a particle size of 0.5 mm, a melt flow index of 2.0 g / 10 min, a styrene content of 30%, and a butadiene content of 70%. The softening oil is a naphthenic rubber oil. The antioxidant is a mixture of antioxidant 1010 and antioxidant 168, with a weight ratio of antioxidant 1010 to antioxidant 168 of 1:1.5. The lubricant is calcium stearate.
[0034] The modified filler is prepared by the following steps: A1. Calcium carbonate was added to a mixed solvent and ultrasonically dispersed. γ-methacryloxypropyltrimethoxysilane was added, and the pH was adjusted to 4.5 with acetic acid. The mixture was heated and stirred to react, filtered, washed with anhydrous ethanol, and dried under vacuum at 70°C for 3 h to obtain vinyl-functionalized calcium carbonate. The mixed solvent is composed of anhydrous ethanol and water in a volume ratio of 9:1, the solid-liquid ratio of calcium carbonate to the mixed solvent is 1:10 g / mL, the ultrasonic dispersion time is 22 min, the amount of γ-methacryloyloxypropyltrimethoxysilane is 2.5% of the weight of calcium carbonate, the heating and stirring reaction temperature is 50℃, and the reaction time is 2.0 h. A2. Add the vinyl-functionalized calcium carbonate to tetrahydrofuran, add 3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate mercaptoethyl ester and benzoin dimethyl ether, stir under nitrogen protection and irradiate with a UV lamp with a main wavelength of 365 nm for 45 min, filter, wash the filter cake with tetrahydrofuran, and dry under vacuum at 50 °C for 3 h to obtain the modified filler; The weight ratio of the vinyl-functionalized calcium carbonate, tetrahydrofuran, and 3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate mercaptoethyl ester is 1:12:0.08, and the amount of benzoin dimethyl ether used is 5.5% of the weight of 3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate mercaptoethyl ester.
[0035] The tackifying resin is prepared by the following steps: B1. Dissolve terpene phenol resin in toluene, add epichlorohydrin, heat and add sodium hydroxide solution dropwise, keep the reaction at the temperature, let stand and separate the layers, wash with water until neutral, and distill under reduced pressure at a vacuum of -0.09 MPa and a temperature of 75°C for 2 hours to obtain epoxidized terpene phenol resin. The solid-liquid ratio of the terpene phenol resin to toluene is 1:3 g / mL, the weight ratio of the terpene phenol resin, epichlorohydrin, and sodium hydroxide solution is 1:1:0.42, the mass fraction of the sodium hydroxide solution is 40%, the dropping time is 1.5 h, the heating dropping temperature is 70 °C, and the heat preservation reaction time is 3.0 h. B2. The epoxidized terpene phenol resin is heated to 95°C to melt, γ-aminopropyltriethoxysilane is added, and the mixture is heated to 85°C for 1.5 hours. The mixture is then discharged, cooled to room temperature, and crushed to a particle size ≤5 mm to obtain the tackifying resin. The amount of γ-aminopropyltriethoxysilane used is 12% of the weight of the epoxidized terpene phenol resin.
[0036] A method for preparing a direct-injection asphalt modifier for hot and humid regions includes the following steps: S1. Add styrene-butadiene-styrene block copolymer and softening oil to a high-speed mixer and stir for 22 minutes at 70°C and 300 r / min. Then add modified filler, tackifying resin, antioxidant and lubricant, and continue stirring for 10 minutes. Discharge the material to obtain the premix. S2. The premixed material is added to a twin-screw extruder, the screw speed is set to 280 r / min, and the temperatures of each zone are set to 140℃ for zone 1, 160℃ for zone 2, 170℃ for zone 3, 170℃ for zone 4, 160℃ for zone 5, and 160℃ for the die. Vacuum exhaust is performed in the middle section of the extruder, with a vacuum degree of -0.08 MPa. The extruded strip is water-cooled, air-dried, and pelletized to obtain a direct-injection modifier for asphalt in humid and hot areas. Example 4
[0037] A direct-injection modifier for asphalt in humid and hot regions comprises the following raw materials in parts by weight: 75 parts styrene-butadiene-styrene block copolymer, 12 parts softening oil, 9 parts tackifying resin, 0.65 parts antioxidant, 4.5 parts lubricant, and 14 parts modified filler. The styrene-butadiene-styrene block copolymer has a star-shaped structure, a particle size of 0.5 mm, a melt flow index of 2.0 g / 10 min, a styrene content of 33%, and a butadiene content of 67%. The softening oil is a naphthenic rubber oil. The antioxidant is a mixture of antioxidant 1010 and antioxidant 168, with a weight ratio of antioxidant 1010 to antioxidant 168 of 1:1.25. The lubricant is calcium stearate.
[0038] The modified filler is prepared by the following steps: A1. Calcium carbonate was added to a mixed solvent and ultrasonically dispersed. γ-methacryloxypropyltrimethoxysilane was added, and the pH was adjusted to 4.7 with acetic acid. The mixture was heated and stirred to react, filtered, washed with anhydrous ethanol, and dried under vacuum at 75°C for 2.5 h to obtain vinyl-functionalized calcium carbonate. The mixed solvent is composed of anhydrous ethanol and water in a volume ratio of 9.5:1, the solid-liquid ratio of calcium carbonate to the mixed solvent is 1:11 g / mL, the ultrasonic dispersion time is 18 min, the amount of γ-methacryloyloxypropyltrimethoxysilane is 2.8% of the weight of calcium carbonate, the heating and stirring reaction temperature is 53℃, and the reaction time is 1.7 h. A2. The vinyl-functionalized calcium carbonate was added to tetrahydrofuran, along with 3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate mercaptoethyl ester and benzoin dimethyl ether. Under nitrogen protection, the mixture was stirred and irradiated with a UV lamp with a main wavelength of 365 nm for 35 min. After filtration, the filter cake was washed with tetrahydrofuran and dried under vacuum at 55 °C for 2.5 h to obtain the modified filler. The weight ratio of the vinyl-functionalized calcium carbonate, tetrahydrofuran, and 3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate mercaptoethyl ester is 1:14:0.10, and the amount of benzoin dimethyl ether used is 4.5% of the weight of 3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate mercaptoethyl ester.
[0039] The tackifying resin is prepared by the following steps: B1. Dissolve terpene phenol resin in toluene, add epichlorohydrin, heat and add sodium hydroxide solution dropwise, keep the reaction at the temperature, let stand and separate the layers, wash with water until neutral, and distill under reduced pressure at a vacuum of -0.095 MPa and a temperature of 82℃ for 1.5 h to obtain epoxidized terpene phenol resin. The solid-liquid ratio of the terpene phenol resin to toluene is 1:3.5 g / mL, the weight ratio of the terpene phenol resin, epichlorohydrin, and sodium hydroxide solution is 1:1.1:0.51, the mass fraction of the sodium hydroxide solution is 42%, the dropping time is 1.2 h, the heating dropping temperature is 73 °C, and the heat preservation reaction time is 2.8 h. B2. The epoxidized terpene phenol resin is heated to 98°C to melt, γ-aminopropyltriethoxysilane is added, and the mixture is heated to 88°C for 1.2 hours. The mixture is then discharged, cooled to room temperature, and crushed to a particle size ≤5 mm to obtain the tackifying resin. The amount of γ-aminopropyltriethoxysilane used is 14% of the weight of the epoxidized terpene phenol resin.
[0040] A method for preparing a direct-injection asphalt modifier for hot and humid regions includes the following steps: S1. Add styrene-butadiene-styrene block copolymer and softening oil to a high-speed mixer and stir for 18 minutes at 75°C and 350 r / min. Then add modified filler, tackifying resin, antioxidant and lubricant, and continue stirring for 8 minutes. Discharge the material to obtain the premix. S2. The premixed material is added to a twin-screw extruder, the screw speed is set to 320 r / min, and the temperatures of each zone are set to 145℃ for zone 1, 165℃ for zone 2, 175℃ for zone 3, 175℃ for zone 4, 165℃ for zone 5, and 165℃ for the die. Vacuum exhaust is performed in the middle section of the extruder, with a vacuum degree of -0.085 MPa. The extruded strip is water-cooled, air-dried, and pelletized to obtain a direct-injection modifier for asphalt in humid and hot areas. Example 5
[0041] A direct-injection asphalt modifier for hot and humid regions comprises the following raw materials in parts by weight: 80 parts styrene-butadiene-styrene block copolymer, 15 parts softening oil, 10 parts tackifying resin, 0.8 parts antioxidant, 5 parts lubricant, and 15 parts modified filler. The styrene-butadiene-styrene block copolymer has a star-shaped structure, a particle size of 0.5 mm, a melt flow index of 2.0 g / 10 min, a styrene content of 35%, and a butadiene content of 65%. The softening oil is a naphthenic rubber oil. The antioxidant is a mixture of antioxidant 1010 and antioxidant 168, with a weight ratio of antioxidant 1010 to antioxidant 168 of 1:1. The lubricant is calcium stearate.
[0042] The modified filler is prepared by the following steps: A1. Calcium carbonate was added to a mixed solvent, ultrasonically dispersed, γ-methacryloxypropyltrimethoxysilane was added, pH was adjusted to 5 with acetic acid, the reaction was heated and stirred, filtered, washed with anhydrous ethanol, and dried under vacuum at 80°C for 2 h to obtain vinyl-functionalized calcium carbonate. The mixed solvent is composed of anhydrous ethanol and water in a volume ratio of 10:1, the solid-liquid ratio of calcium carbonate to the mixed solvent is 1:12 g / mL, the ultrasonic dispersion time is 15 min, the amount of γ-methacryloyloxypropyltrimethoxysilane is 3.0% of the weight of calcium carbonate, the heating and stirring reaction temperature is 55℃, and the reaction time is 1.5 h. A2. Add the vinyl-functionalized calcium carbonate to tetrahydrofuran, add 3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate mercaptoethyl ester and benzoin dimethyl ether, stir under nitrogen protection and irradiate with a UV lamp with a main wavelength of 365 nm for 30 min, filter, wash the filter cake with tetrahydrofuran, and dry under vacuum at 60 °C for 2 h to obtain the modified filler; The weight ratio of the vinyl-functionalized calcium carbonate, tetrahydrofuran, and 3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate mercaptoethyl ester is 1:15:0.12, and the amount of benzoin dimethyl ether used is 3% of the weight of the 3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate mercaptoethyl ester.
[0043] The tackifying resin is prepared by the following steps: B1. Dissolve terpene phenol resin in toluene, add epichlorohydrin, heat and add sodium hydroxide solution dropwise, keep the reaction at the temperature, let stand and separate the layers, wash with water until neutral, and distill under reduced pressure at a vacuum of -0.1 MPa and 90℃ for 1 h to obtain epoxidized terpene phenol resin. The solid-liquid ratio of the terpene phenol resin to toluene is 1:4 g / mL, the weight ratio of the terpene phenol resin, epichlorohydrin and sodium hydroxide solution is 1:1.2:0.6, the mass fraction of the sodium hydroxide solution is 45%, the dropping time is 1 h, the heating dropping temperature is 75 °C, and the heat preservation reaction time is 2.5 h. B2. The epoxidized terpene phenol resin is heated to 100°C to melt, γ-aminopropyltriethoxysilane is added, and the mixture is heated to 90°C for 1 hour. The mixture is discharged, cooled to room temperature, and crushed to a particle size ≤5mm to obtain the tackifying resin. The amount of γ-aminopropyltriethoxysilane used is 15% of the weight of the epoxidized terpene phenol resin.
[0044] A method for preparing a direct-injection asphalt modifier for hot and humid regions includes the following steps: S1. Add styrene-butadiene-styrene block copolymer and softening oil to a high-speed mixer, stir for 15 minutes at 80℃ and 400r / min, then add modified filler, tackifying resin, antioxidant and lubricant, continue stirring for 5 minutes, and discharge to obtain premix; S2. The premixed material is added to a twin-screw extruder, the screw speed is set to 350 r / min, and the temperatures of each zone are set to 150℃ for zone 1, 170℃ for zone 2, 180℃ for zone 3, 180℃ for zone 4, 170℃ for zone 5, and 170℃ for the die head. Vacuum exhaust is performed in the middle section of the extruder, with a vacuum degree of -0.09 MPa. The extruded strip is water-cooled, air-dried, and pelletized to obtain a direct-injection modifier for asphalt in humid and hot areas.
[0045] Comparative Example 1 A method for preparing a direct-injection modifier for asphalt in humid and hot regions, compared with the method for preparing the direct-injection modifier in Example 1, mainly differs in that: in step S1 of this comparative example, an equal amount of unmodified calcium carbonate is used instead of the modified filler, and an equal amount of unmodified terpene phenol resin is used instead of the tackifying resin; the other components and preparation methods are completely consistent with those in Example 1.
[0046] Comparative Example 2 A method for preparing a direct-injection modifier for asphalt in humid and hot regions, compared with the method for preparing the direct-injection modifier in Example 1, mainly differs in that: in step S1 of this comparative example, an equal amount of unmodified calcium carbonate is used to replace the modified filler, while the other components and preparation methods are completely consistent with those in Example 1.
[0047] Comparative Example 3 A method for preparing a direct-injection modifier for asphalt in humid and hot regions, compared with the method for preparing the direct-injection modifier in Example 1, mainly differs in that: in step S1 of this comparative example, an equal amount of unmodified terpene phenol resin is used instead of the tackifying resin, while the other components and preparation methods are completely consistent with those in Example 1.
[0048] Comparative Example 4 A method for preparing a direct-injection modifier for asphalt in humid and hot regions, compared with the method for preparing the direct-injection modifier in Example 1, mainly differs in that: in step S1 of this comparative example, an equal amount of vinyl-functionalized calcium carbonate modified only in step A1 and not in step A2 is used to replace the modified filler, while the other components and preparation methods are completely consistent with those in Example 1.
[0049] Comparative Example 5 A method for preparing a direct-injection modifier for asphalt in humid and hot regions, compared with the method for preparing the direct-injection modifier in Example 1, mainly differs in that: in step S1 of this comparative example, an equal amount of epoxidized terpene phenol resin modified only in step B1 and not in step B2 is used to replace the tackifying resin, while the other components and preparation methods are completely consistent with those in Example 1.
[0050] The preparation method of β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionic acid mercaptoethyl ester used in the embodiments and comparative examples of this invention is as follows: β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionic acid, mercaptoethanol, toluene, and p-toluenesulfonic acid are added to a reactor. The molar ratio of β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionic acid to mercaptoethanol is 1:2.0. The amount of toluene used is 1.2 times the weight of β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionic acid, and the amount of p-toluenesulfonic acid used is... 2% by weight of (3,5-di-tert-butyl-4-hydroxyphenyl)propionic acid was stirred and heated to reflux. The mixture was refluxed at 85°C for 6 hours to remove water. The mixture was then cooled to room temperature and washed with saturated sodium bicarbonate solution until the pH reached 7.5. After standing and separating the layers, the organic phase was collected, washed with deionized water until neutral, dried with anhydrous sodium sulfate for 5 hours, filtered, and then distilled under reduced pressure at -0.095 MPa and 70°C to remove toluene and excess mercaptoethanol, yielding mercaptoethyl 3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionic acid.
[0051] The softening oil used in the embodiments and comparative examples of this invention was purchased from Jinan Runchang Chemical Co., Ltd., and is a naphthenic rubber oil of type 4010.
[0052] Performance testing: The direct-injection modifiers obtained in Examples 1-5 and Comparative Examples 1-5 were respectively added to base asphalt at a mass ratio of 4.5:95.5 at 180°C and sheared at a shear rate of 4500 r / min for 50 min to prepare modified asphalt samples. Part of the modified asphalt samples were tested for softening point, penetration ratio, and segregation softening point difference. Modified asphalt samples were mixed with aggregates and mineral powder at a mixing temperature of 170-175°C to form Marshall specimens, and the water immersion Marshall residual stability ratio was tested. The test results are shown in Table 1. (1) Softening point: The ring and ball method is used to determine the softening point. The modified asphalt sample is injected into the sample ring, cooled in a constant temperature water bath at 5℃ for 30 min, and then heated at a heating rate of 5℃ / min. The temperature at which the steel ball falls from the sample ring to the bottom plate is recorded. (2) Penetration ratio: The modified asphalt sample was first aged in a rotating film oven, and then the 25°C penetration of the residue before and after aging was measured. The penetration test conditions were standard needle, 100g load, and penetration time of 5s. The percentage of penetration after aging was calculated compared with that before aging. (3) Segregation softening point difference: Molten modified asphalt was injected into a vertically placed aluminum tube, and after standing in an oven at 163℃ for 48 hours, it was taken out and cooled. Samples of the upper 1 / 3 section and the lower 1 / 3 section of the aluminum tube were taken and their softening points were measured respectively. The absolute value of the difference between the softening points of the two sections was calculated. (4) Water immersion Marshall residual stability ratio: Two groups of Marshall specimens were formed from the asphalt mixture. One group was kept in a constant temperature water bath at 60℃ for 40 min and the stability was measured. The other group was immersed in water at 60℃ for 48 h and the stability was measured. The percentage of the stability after immersion for 48 h and the stability after immersion for 40 min was calculated, which is the water immersion Marshall residual stability ratio.
[0053] Table 1 Case Softening point (°C) Penetration ratio (%) Segregation softening point difference (°C) Water immersion Marshall residue stability ratio (%) Example 1 88.2 78.6 1.4 89.2 Example 2 89.8 80.3 1.2 90.8 Example 3 91.5 82.5 1.0 92.4 Example 4 90.4 81.7 1.1 91.3 Example 5 89.1 80.1 1.3 90.1 Comparative Example 1 72.6 61.3 4.8 72.4 Comparative Example 2 82.4 67.5 3.1 83.1 Comparative Example 3 79.5 74.8 2.5 76.8 Comparative Example 4 85.7 71.2 1.7 88.6 Comparative Example 5 84.3 79.4 1.9 81.5 As shown in Table 1, the performance of Examples 1-5 is superior to that of Comparative Examples 1-5. Comparative Example 1 uses unmodified calcium carbonate and terpene phenol resin. Calcium carbonate has strong surface hydrophilicity and poor compatibility with the SBS matrix. The terpene phenol resin relies solely on van der Waals forces to interact with the aggregate, resulting in weak interfacial bonding between components and poor overall performance. Comparative Example 2 only modifies the resin through epoxidation and silane grafting, while the filler remains untreated. Its penetration ratio decrease is the most significant among all comparative examples. The filler lacks the hindered phenolic structure covalently anchored by thioether bonds, and therefore cannot effectively capture free radicals generated in the asphalt during the aging process in the rotating thin film oven, leading to a severe decrease in penetration after aging. Comparative Example 3 only modifies the filler through silanization and antioxidant grafting, while the resin remains untreated. Its water immersion Marshall residual stability ratio decreases the most. The terpene phenol resin molecular chain lacks triethoxysilane groups introduced through the ring-opening of epoxy-amine, preventing the formation of covalent bonds on the aggregate surface after water intrusion, resulting in insufficient interfacial anti-peeling ability. In Comparative Example 4, the filler was only silanized without grafting an antioxidant, resulting in a significantly lower penetration ratio compared to the other examples. The methacrylate double bonds introduced onto the calcium carbonate surface only improved the filler's dispersibility but failed to impart a long-term free radical scavenging function, making it difficult to effectively inhibit the degradation of the asphalt matrix during aging. In Comparative Example 5, the resin was only epoxidized without grafting a silane coupling agent, resulting in a significantly lower water immersion Marshall residual stability ratio compared to the other examples. The glycidyl ether groups on the resin molecular chain segments improved the resin's thermal stability but lacked the siloxane structure formed by further ring-opening addition with γ-aminopropyltriethoxysilane, thus failing to construct a chemically bonded layer at the asphalt-aggregate interface.
[0054] This demonstrates that the present invention, by covalently grafting hindered phenolic antioxidants onto the surface of calcium carbonate via thiol-ene click reaction and covalently grafting silane coupling agents onto the molecular chain segments of terpene phenolic resin via epoxy-amine ring-opening reaction, enables the modified filler and modified resin to work synergistically in asphalt mixtures. The former continuously captures free radicals to delay the aging of asphalt and SBS, while the latter forms chemical bonds at the aggregate interface to resist moisture stripping, thereby systematically improving the high-temperature performance, anti-aging performance, storage stability, and water damage resistance of modified asphalt.
[0055] In the description of this specification, references to terms such as "an embodiment," "example," "specific example," etc., indicate that a specific feature, structure, material, or characteristic described in connection with that embodiment or example is included in at least one embodiment or example of the invention. In this specification, illustrative expressions of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments or examples.
[0056] Although embodiments of the present invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and variations can be made to these embodiments without departing from the principles and spirit of the present invention. All equivalent changes and improvements made within the scope of the present invention should still fall within the scope of the present invention.
Claims
1. A direct-injection asphalt modifier for use in hot and humid regions, characterized in that, The raw materials include the following parts by weight: 60-80 parts styrene-butadiene-styrene block copolymer, 5-15 parts softening oil, 5-10 parts tackifying resin, 0.2-0.8 parts antioxidant, 2-5 parts lubricant, and 8-15 parts modified filler; The modified filler is prepared by the following steps: A1. Add calcium carbonate to a mixed solvent, disperse it by ultrasonication, add γ-methacryloxypropyltrimethoxysilane, adjust the pH to 4-5 with acetic acid, heat and stir the reaction, filter, wash, and vacuum dry to obtain vinyl-functionalized calcium carbonate. A2. Add the vinyl-functionalized calcium carbonate to tetrahydrofuran, add 3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate mercaptoethyl ester and benzoin dimethyl ether, stir under nitrogen protection and irradiate with a UV lamp with a main wavelength of 365nm for 30~60min, filter, wash the filter cake with tetrahydrofuran, and vacuum dry to obtain the modified packing material; The tackifying resin is prepared by the following steps: B1. Dissolve terpene phenol resin in toluene, add epichlorohydrin, heat and add sodium hydroxide solution dropwise, keep the reaction at the temperature, let stand and separate the layers, wash with water until neutral, and distill under reduced pressure to obtain epoxidized terpene phenol resin. B2. The epoxidized terpene phenol resin is heated and melted, γ-aminopropyltriethoxysilane is added, the mixture is heated to react, and then discharged, cooled and crushed to obtain a tackifying resin.
2. The asphalt direct-injection modifier for hot and humid regions according to claim 1, characterized in that, The styrene-butadiene-styrene block copolymer has a star-shaped structure, a particle size ≤2.0 mm, and a melt flow index of 1.0~4.0 g / 10 min, wherein the styrene content is 25%~35% and the butadiene content is 65%~75%.
3. The asphalt direct-injection modifier for hot and humid regions according to claim 1, characterized in that, The softening oil is a naphthenic rubber oil.
4. The asphalt direct-injection modifier for hot and humid regions according to claim 1, characterized in that, The antioxidant is a mixture of antioxidant 1010 and antioxidant 168, wherein the weight ratio of antioxidant 1010 to antioxidant 168 is 1:(1~2).
5. The asphalt direct-injection modifier for hot and humid regions according to claim 1, characterized in that, The lubricant is calcium stearate.
6. The asphalt direct-injection modifier for hot and humid regions according to claim 1, characterized in that, In step A1, the mixed solvent is composed of anhydrous ethanol and water in a volume ratio of (8~10):1, the solid-liquid ratio of calcium carbonate to the mixed solvent is 1:(8~12) g / mL, the ultrasonic dispersion time is 15~30 min, the amount of γ-methacryloyloxypropyltrimethoxysilane is 2.0%~3.0% of the weight of calcium carbonate, the heating and stirring reaction temperature is 45~55℃, and the reaction time is 1.5~2.5 h.
7. The asphalt direct-injection modifier for hot and humid regions according to claim 1, characterized in that, In step A2, the weight ratio of the vinyl-functionalized calcium carbonate, tetrahydrofuran, and 3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate mercaptoethyl ester is 1:(8~15):(0.05~0.12), and the amount of benzoin dimethyl ether used is 3%~8% of the weight of the 3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate mercaptoethyl ester.
8. The asphalt direct-injection modifier for hot and humid regions according to claim 1, characterized in that, In step B1, the solid-liquid ratio of the terpene phenol resin to toluene is 1:(2~4) g / mL, and the weight ratio of the terpene phenol resin, epichlorohydrin, and sodium hydroxide solution is 1:(0.8~1.2):(0.24~0.6). The mass fraction of the sodium hydroxide solution is 35%~45%. The dropping time is 1~2 h, the heating dropping temperature is 65~75 °C, and the heat preservation reaction time is 2.5~3.5 h.
9. The asphalt direct-injection modifier for hot and humid regions according to claim 1, characterized in that, In step B2, the heating and melting temperature is 90~100℃, the amount of γ-aminopropyltriethoxysilane is 8%~15% of the weight of the epoxidized terpene phenol resin, the heating reaction temperature is 80~90℃, and the heating reaction time is 1~2h.
10. A method for preparing a direct-injection asphalt modifier for hot and humid regions, characterized in that, Includes the following steps: S1. Add styrene-butadiene-styrene block copolymer and softening oil to a high-speed mixer and stir for 15-30 minutes at a temperature of 60-80℃ and a speed of 200-400 r / min. Then add modified filler, tackifying resin, antioxidant and lubricant, and continue stirring for 5-15 minutes. Discharge the material to obtain the premix. S2. The premixed material is added to a twin-screw extruder. The screw speed is set to 200~350 r / min. The temperatures of each zone are set as follows: Zone 1 130~150℃, Zone 2 150~170℃, Zone 3 160~180℃, Zone 4 160~180℃, Zone 5 150~170℃, and the die head 150~170℃. Vacuum exhaust is performed in the middle section of the extruder, with a vacuum degree of -0.06~-0.09 MPa. The extruded strip is water-cooled, air-dried, and pelletized to obtain a direct-injection modifier for asphalt in humid and hot regions.
Citation Information
Patent Citations
Direct vat set quick-melting rubber powder modifier, recycled asphalt mixture and preparation method of recycled asphalt mixture
CN117624753A