Cool-feeling thermoplastic elastomer shoe composite material and preparation method thereof
By combining composite cooling functional agents and thermal conductive additives, the sustained cooling sensation and mechanical properties of cooling TPE materials are improved, solving the comfort and durability problems of existing materials in high-temperature summer environments, making them suitable for the footwear industry.
Patent Information
- Application Number
- CN202611426170.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-15
- Publication Date
- 2026-11-24
AI Technical Summary
Existing cooling TPE materials suffer from problems such as short duration of cooling sensation, decreased mechanical properties, poor thermal conductivity, and poor washability in high-temperature summer environments, making it difficult to meet the comprehensive requirements of shoemaking.
A composite cooling functional agent consisting of surface-modified jade micropowder and phase change cooling microcapsules, combined with thermally conductive additives, was used to prepare a cooling thermoplastic elastic shoe composite material by improving interfacial compatibility and establishing a thermally conductive network.
It achieves a high contact cooling coefficient and long-lasting cooling effect. The material retains good performance after multiple washes and has excellent elasticity, abrasion resistance and bending resistance, making it suitable for the footwear industry.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] This invention relates to the field of polymer composite materials technology, and in particular to a cool-feeling thermoplastic elastic shoe composite material and its preparation method. Background Technology
[0002] Thermoplastic elastomers (TPEs) combine the high elasticity of rubber with the thermoplastic processing properties of plastics. They are environmentally friendly, recyclable, and have high molding efficiency, making them widely used in shoe components such as insoles, shoe linings, and outsole layers. In hot summer conditions, the enclosed space inside shoes can easily lead to heat buildup, stuffiness, sweating, and stickiness in the feet, significantly reducing wearing comfort. Therefore, shoe materials with cooling functions have become a hot topic in industry research and development and market demand.
[0003] Existing cooling TPE materials mostly achieve their function through simple blending of a single cooling agent, which has significant drawbacks in footwear applications: First, single organic cooling agents (such as menthol) only provide a temporary sensory cooling sensation, are easily volatilized and lost, decompose significantly during high-temperature processing, have poor water resistance, and the cooling sensation rapidly diminishes after prolonged wear. Second, single inorganic cooling powders (such as ordinary jade powder) rely on contact heat conduction to achieve a cooling sensation, resulting in insufficient cooling intensity. Furthermore, inorganic powders have poor compatibility with non-polar TPE matrices, easily leading to agglomeration, which reduces the material's mechanical properties and flexural strength, causing surface precipitation, whitening, and other problems, affecting the appearance and lifespan of the shoe material. Third, the material lacks an overall thermal conductivity pathway, preventing the rapid transfer of heat from the foot to the material's interior and exterior. The cooling sensation remains only on the contact surface, and heat buildup after continuous wear quickly restores the stuffy feeling. Fourth, it is difficult to simultaneously achieve the cooling function and the essential elasticity, abrasion resistance, flexural strength, and water resistance required for footwear materials, failing to meet the comprehensive requirements of mass production and long-term wear in footwear manufacturing. Summary of the Invention
[0004] The purpose of this invention is to address the shortcomings of existing technologies by proposing a cool-feeling thermoplastic elastic shoe composite material and its preparation method.
[0005] To achieve the above objectives, the present invention adopts the following technical solution: a cool-feeling thermoplastic elastomer shoe composite material, comprising the following components by weight:
[0006] 50-70 parts of styrene-based thermoplastic elastomer;
[0007] 10-20 parts of polyolefin resin;
[0008] 15-35 parts of plasticizer softener;
[0009] 8-18 parts of compound cooling functional agent;
[0010] 3-8 parts of thermal conductive agent;
[0011] 4-9 parts compatibilizer;
[0012] 1-3 parts of wear-resistant additive;
[0013] Antioxidant 0.2-1 part;
[0014] 0.5-1.5 parts lubricant;
[0015] The composite cooling functional agent is composed of surface-modified jade micro powder and phase change cooling microcapsules in a mass ratio of (3-5):1; the surface-modified jade micro powder is natural jade micro powder that has been surface-grafted and modified with a silane coupling agent; the phase change cooling microcapsules use paraffin-based phase change material as the core material and melamine-formaldehyde resin as the wall material.
[0016] Preferably, the styrene-based thermoplastic elastomer is one or more of SEBS, SEPS, and SEEPS, with a styrene content of 25%-35% by mass and a melt flow rate of 2-9 g / 10 min.
[0017] Preferably, the polyolefin resin is one or a combination of two of copolymer polypropylene and high-density polyethylene; the softening plasticizer is one or a combination of two of naphthenic oil and paraffin oil, with a flash point ≥220℃.
[0018] Preferably, the surface-modified jade micropowder has a particle size of 800-2000 mesh, the silane coupling agent is KH-550, and the modification amount is 1.0%-2.5% of the mass of the jade micropowder; the phase change cooling microcapsules have a particle size of 10-50 μm, a phase change temperature of 28-32℃, and a latent heat value ≥120 J / g.
[0019] Preferably, the thermally conductive agent is flake-shaped hexagonal boron nitride with a flake diameter of 5-20 μm and a thermal conductivity ≥300 W / (m·K).
[0020] Preferably, the compatibilizer is maleic anhydride-grafted SEBS with a grafting rate of 1.2%-2.8%; the wear-resistant additive is one or a combination of two of ultra-high molecular weight polyethylene micro powder and silicone powder.
[0021] Preferably, the antioxidant is a mixture of antioxidant 1010 and antioxidant 168 in a mass ratio of 1:(1-2); the lubricant is one or a combination of two of zinc stearate and ethylene bis-stearamide.
[0022] The method for preparing the cool-feeling thermoplastic elastomer shoe composite material is characterized by comprising the following steps:
[0023] (1) Preparation of surface-modified jade micro powder: natural jade micro powder is added to a high-speed mixer, heated to 80-100℃, sprayed with an ethanol solution containing silane coupling agent, kept warm and stirred for 15-30 min, discharged and dried to obtain surface-modified jade micro powder.
[0024] (2) Premixing of composite cooling functional agent: Add surface modified jade micro powder and phase change cooling microcapsules to a mixer according to the ratio, mix at room temperature for 5-10 minutes to obtain composite cooling functional agent;
[0025] (3) Matrix premixing: Weigh out styrene thermoplastic elastomer, polyolefin resin and softening plasticizer according to the ratio and put them into a high-speed mixer. Mix at 60-80℃ for 8-15 minutes to allow the plasticizer to be fully absorbed and swollen by the elastomer.
[0026] (4) Mixing of all components: Add composite cooling functional agent, thermal conductive agent, compatibilizer, wear-resistant agent, antioxidant and lubricant to the material in step (3), and continue mixing for 4-6 minutes to obtain a uniform premix;
[0027] (5) Melt blending and granulation: The premixed material is added to a twin-screw extruder, and after melt blending, extrusion into strands, and water cooling and pelletizing, cool-feeling TPE composite granules are obtained;
[0028] (6) Molding and processing: The composite particles are processed into sheet material or shoe parts for shoe making through injection molding, calendering or extrusion molding processes.
[0029] Preferably, in step (5), the temperature of each zone of the twin-screw extruder is set as follows: Zone 1 140-155℃, Zone 2 155-170℃, Zone 3 165-175℃, Zone 4 160-170℃, and the die head temperature is 155-165℃; the screw speed is 200-320rpm.
[0030] Preferably, the material has a contact cooling coefficient qmax ≥ 0.35 W / cm², a cooling duration of ≥ 30 min at 35℃, a Shore hardness of 50-70A, a tensile strength ≥ 10 MPa, an elongation at break ≥ 450%, a DIN abrasion loss ≤ 130 mm³, and a cooling retention rate of ≥ 90% after 20 water washes.
[0031] Compared with the prior art, the advantages and positive effects of the present invention are as follows:
[0032] In this invention, surface-modified jade micro powder provides a rapid cooling sensation upon contact, while phase change microcapsules achieve continuous heat absorption and cooling through latent heat of phase change. The two work synergistically to achieve a high coefficient of cooling sensation upon contact and a long duration of cooling sensation, which can effectively alleviate the stuffiness of wearing shoes in summer.
[0033] After surface modification, the jade micro powder is firmly bonded to the matrix, and the phase change core material is encapsulated by the microcapsule wall material, making it difficult for either to migrate or precipitate. Combined with a heat-conducting network to stabilize heat conduction, the cooling performance is well retained after multiple water washes, and the functional life is long.
[0034] Silane modification and compatibilizer synergistically improve the interfacial bonding between inorganic powder and TPE matrix, avoid powder agglomeration, and maintain the material's excellent elasticity, tensile strength and bending resistance, while the wear resistance meets the requirements for footwear materials.
[0035] It can be molded using various commonly used shoemaking processes such as injection molding and calendering, resulting in high production efficiency; the material is a thermoplastic system, and scraps can be recycled and reused, which is in line with the trend of green manufacturing of shoe materials. Detailed Implementation
[0036] The technical solution of the present invention will be further described below with reference to preparation examples, embodiments and comparative examples, but the scope of protection of the present invention is not limited thereto.
[0037] Preparation Example 1: Preparation of Surface-Modified Jade Micropowder
[0038] Weigh 100g of 1250-mesh natural jade powder and add it to a high-speed mixer. Heat the mixture to 90℃. Disperse 2g of silane coupling agent KH-550 in 20mL of 95% ethanol solution and spray it into the mixer. Keep the mixture warm and stir for 20min. After discharge, vacuum dry the mixture at 80℃ for 6h to obtain surface-modified jade powder.
[0039] Preparation Example 2: Preparation of Phase Change Cooling Microcapsules
[0040] The product was prepared by in-situ polymerization: 10g of paraffin (phase change temperature 30℃, latent heat 145J / g) and 2g of emulsifier were added to water and emulsified at high speed to form a stable oil phase emulsion; melamine and formaldehyde were reacted at a molar ratio of 1:2 to prepare a melamine-formaldehyde prepolymer solution; the prepolymer solution was added dropwise to the emulsion, the pH was adjusted to weakly acidic, the temperature was raised to 75℃ and kept at that temperature for 3h, and the product was cooled, filtered and washed to obtain phase change cooling microcapsules with a particle size of 20-30μm.
[0041] Example 1
[0042] Weigh the raw materials according to the following parts by weight: 60 parts of SEBS (YH-503), 15 parts of copolymer polypropylene, 25 parts of naphthenic oil, 12 parts of composite cooling functional agent, 5 parts of flake hexagonal boron nitride, 6 parts of maleic anhydride grafted SEBS (grafting rate 2.0%), 2 parts of ultra-high molecular weight polyethylene micro powder, 0.3 parts of antioxidant 10100, 0.4 parts of antioxidant 1680, and 0.8 parts of zinc stearate.
[0043] The composite cooling functional agent was prepared by combining modified jade micropowder from Preparation Example 1 and phase change microcapsules from Preparation Example 2 at a mass ratio of 4:1.
[0044] Preparation steps:
[0045] Complete the premixing of the compound cooling functional agent using the method described above;
[0046] Add SEBS, copolymer polypropylene, and naphthenic oil to a high-speed mixer and mix at 70°C for 10 minutes.
[0047] Add all remaining components and continue mixing for 5 minutes to obtain the premix;
[0048] Twin-screw extrusion granulation, zone temperatures: Zone 1 150℃, Zone 2 165℃, Zone 3 170℃, Zone 4 165℃, die head 160℃, screw speed 260rpm;
[0049] The granules were calendered into 2mm thick sheet samples.
[0050] Example 2
[0051] Weigh the raw materials according to the following parts by weight: 55 parts SEBS (YH-503), 8 parts SEEPS, 12 parts high-density polyethylene, 30 parts paraffin oil, 15 parts composite cooling functional agent, 6 parts flake hexagonal boron nitride, 7 parts maleic anhydride grafted SEBS, 2 parts silicone powder, 0.2 parts antioxidant 10100, 0.5 parts antioxidant 1680, and 1.0 part ethylene bis-stearamide.
[0052] The composite cooling functional agent is a mixture of modified jade micro powder and phase change microcapsules in a mass ratio of 3:1.
[0053] The preparation method is the same as in Example 1.
[0054] Example 3
[0055] Weigh the raw materials according to the following parts by weight: 65 parts SEBS (YH-688), 18 parts copolymer polypropylene, 20 parts naphthenic oil, 9 parts composite cooling functional agent, 4 parts flake hexagonal boron nitride, 5 parts maleic anhydride grafted SEBS, 1.5 parts ultra-high molecular weight polyethylene micro powder, 0.4 parts antioxidant 1010, 0.4 parts antioxidant 168, and 0.7 parts zinc stearate.
[0056] The composite cooling functional agent is a mixture of modified jade micro powder and phase change microcapsules at a mass ratio of 5:1.
[0057] The preparation method is the same as in Example 1.
[0058] Comparative Example 1
[0059] It is basically the same as Example 1, except that the composite cooling functional agent is replaced with an equal mass of unmodified ordinary jade powder.
[0060] Comparative Example 2
[0061] It is basically the same as Example 1, except that the composite cooling functional agent is replaced with an equal mass of a single menthol-based organic cooling agent.
[0062] Comparative Example 3
[0063] It is basically the same as Example 1, except that no sheet-like hexagonal boron nitride thermal conductive agent is added.
[0064] Performance testing
[0065] The performance of the above-described embodiments and comparative samples was tested, and the results are shown in the table below:
[0066]
[0067] The test results show that the cooling thermoplastic elastomer shoe composite material prepared by this invention has both high contact cooling and long-lasting cooling, excellent water washing performance, and maintains good mechanical properties and wear resistance. It can be widely used in the field of shoe manufacturing such as summer cooling insoles, shoe linings, and casual sandal soles.
[0068] The above are merely preferred embodiments of the present invention and are not intended to limit the present invention in any other way. Any person skilled in the art may make changes or modifications to the above-disclosed technical content to create equivalent embodiments that can be applied to other fields. However, any simple modifications, equivalent changes, and modifications made to the above embodiments based on the technical essence of the present invention without departing from the scope of the present invention shall still fall within the protection scope of the present invention.
Claims
1. A cooling thermoplastic elastomer composite material for shoes, characterized in that, By weight, it includes the following components: 50-70 parts of styrene-based thermoplastic elastomer; 10-20 parts of polyolefin resin; 15-35 parts of plasticizer softener; 8-18 parts of compound cooling functional agent; 3-8 parts of thermal conductive agent; 4-9 parts compatibilizer; 1-3 parts of wear-resistant additive; Antioxidant 0.2-1 part; 0.5-1.5 parts lubricant; The composite cooling functional agent is composed of surface-modified jade micro powder and phase change cooling microcapsules in a mass ratio of (3-5):1; the surface-modified jade micro powder is natural jade micro powder that has been surface-grafted and modified with a silane coupling agent; the phase change cooling microcapsules use paraffin-based phase change material as the core material and melamine-formaldehyde resin as the wall material.
2. The cool-feeling thermoplastic elastomer shoe composite material according to claim 1, characterized in that, The styrene-based thermoplastic elastomer is one or more of SEBS, SEPS, and SEEPS, with a styrene content of 25%-35% by mass and a melt flow rate of 2-9 g / 10 min.
3. The cool-feeling thermoplastic elastomer shoe composite material according to claim 1, characterized in that, The polyolefin resin is one or a combination of two of copolymer polypropylene and high-density polyethylene; the softening plasticizer is one or a combination of two of naphthenic oil and paraffin oil, with a flash point ≥220℃.
4. The cool-feeling thermoplastic elastomer shoe composite material according to claim 1, characterized in that, The surface-modified jade micropowder has a particle size of 800-2000 mesh, the silane coupling agent is KH-550, and the modification amount is 1.0%-2.5% of the mass of the jade micropowder; the phase change cooling microcapsules have a particle size of 10-50 μm, a phase change temperature of 28-32℃, and a latent heat value ≥120 J / g.
5. The cool-feeling thermoplastic elastomer shoe composite material according to claim 1, characterized in that, The thermally conductive additive is a sheet-like hexagonal boron nitride with a sheet diameter of 5-20 μm and a thermal conductivity ≥300 W / (m·K).
6. The cool-feeling thermoplastic elastomer shoe composite material according to claim 1, characterized in that, The compatibilizer is maleic anhydride-grafted SEBS with a grafting rate of 1.2%-2.8%; the wear-resistant additive is one or a combination of two of ultra-high molecular weight polyethylene micro powder and silicone powder.
7. The cool-feeling thermoplastic elastomer shoe composite material according to claim 1, characterized in that, The antioxidant is a mixture of antioxidant 1010 and antioxidant 168 in a mass ratio of 1:(1-2); the lubricant is one or a combination of two of zinc stearate and ethylene bis-stearamide.
8. A method for preparing a cool-feeling thermoplastic elastomer shoe composite material as described in any one of claims 1-7, characterized in that, Includes the following steps: (1) Preparation of surface-modified jade micro powder: natural jade micro powder is added to a high-speed mixer, heated to 80-100℃, sprayed with an ethanol solution containing silane coupling agent, kept warm and stirred for 15-30 min, discharged and dried to obtain surface-modified jade micro powder. (2) Premixing of composite cooling functional agent: Add surface modified jade micro powder and phase change cooling microcapsules to a mixer according to the ratio, mix at room temperature for 5-10 minutes to obtain composite cooling functional agent; (3) Matrix premixing: Weigh out styrene thermoplastic elastomer, polyolefin resin and softening plasticizer according to the ratio and put them into a high-speed mixer. Mix at 60-80℃ for 8-15 minutes to allow the plasticizer to be fully absorbed and swollen by the elastomer. (4) Mixing of all components: Add composite cooling functional agent, thermal conductive agent, compatibilizer, wear-resistant agent, antioxidant and lubricant to the material in step (3), and continue mixing for 4-6 minutes to obtain a uniform premix; (5) Melt blending and granulation: The premixed material is added to a twin-screw extruder, and after melt blending, extrusion into strands, and water cooling and pelletizing, cool-feeling TPE composite granules are obtained; (6) Molding and processing: The composite particles are processed into sheet material or shoe parts for shoe making through injection molding, calendering or extrusion molding processes.
9. The preparation method according to claim 8, characterized in that, In step (5), the temperature of each zone of the twin-screw extruder is set as follows: Zone 1 140-155℃, Zone 2 155-170℃, Zone 3 165-175℃, Zone 4 160-170℃, and the die head temperature is 155-165℃; the screw speed is 200-320rpm.
10. The cool-feeling thermoplastic elastomer shoe composite material according to claim 1, characterized in that, The material has a contact cooling coefficient qmax ≥ 0.35 W / cm², a cooling duration of ≥ 30 min at 35℃, a Shore hardness of 50-70A, a tensile strength of ≥ 10 MPa, an elongation at break of ≥ 450%, and a DIN abrasion loss of ≤ 130 mm³. The cooling retention rate is ≥ 90% after 20 water washes.