A foamed thermoplastic elastomer shoe material and a method for producing the same

By preparing low-density, high-resilience, and high-wear-resistant foamed thermoplastic elastomer materials, the problems of high density, poor resilience, and insufficient wear resistance of existing materials in footwear applications have been solved. This has achieved lightweight, environmentally friendly, and recyclable materials suitable for a variety of footwear products.

CN123152244APending Publication Date: 2026-11-24崔仲强
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611426959.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-15
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing foamed thermoplastic elastomer materials have high density, poor resilience, and insufficient abrasion resistance in footwear applications. In particular, the tensile strength and abrasion resistance of the materials decrease significantly at high magnification, making it difficult to meet the requirements of footwear outsoles or high-load midsoles.

Method used

A combination of thermoplastic elastomer matrix, softening plasticizer, filler reinforcing agent, chemical foaming agent, foaming aid, crosslinking system and antioxidant system is used to prepare low-density, high-resilience and high-wear-resistant foamed thermoplastic elastomer shoe material through oil-filled mixing, blending, extrusion granulation and compression molding foaming processes.

Benefits of technology

It achieves low density (0.18~0.38g/cm³), high resilience (≥55%), high abrasion resistance (Akron abrasion loss ≤0.25cm³/1.61km), and excellent cushioning in materials, making it suitable for sports shoe midsoles and casual shoe materials. Moreover, the production process is environmentally friendly and recyclable, and it can meet the performance requirements of different shoe types.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

This invention provides a foamed thermoplastic elastomer shoe material and its preparation method, relating to the field of polymer foaming materials technology. By weight, it comprises the following components: 60-100 parts of thermoplastic elastomer matrix; 20-50 parts of softening plasticizer; 10-40 parts of filler and reinforcing agent; 1.5-6 parts of chemical foaming agent; 0.5-2 parts of foaming aid; 0.2-1.5 parts of crosslinking system; 0.1-1 parts of antioxidant system; and 0.5-2 parts of lubricant. In this invention, through the synergistic effect of oil-filled modification and chemical foaming, the material's appearance... With a density as low as 0.18 g / cm³ and a rebound rate of ≥55%, it provides excellent cushioning and is suitable for midsoles of athletic shoes and casual footwear. Through the synergistic effect of filling reinforcement and moderate cross-linking, the Akron abrasion loss after foaming is ≤0.25cm³ / 1.61km, and the flexural strength is ≥100,000 cycles without cracking. It can be directly used in shoe outsoles without the need for an additional abrasion-resistant layer. It adopts thermoplastic processing technology, and the production process is solvent-free and sulfur-free. Scrap materials and waste products can be crushed, granulated, and reused, which is in line with the trend of green shoe manufacturing.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of polymer foaming materials technology, and in particular to a foamed thermoplastic elastic shoe material and its preparation method. Background Technology

[0002] In the footwear industry, the sole material directly determines the comfort, lightweight nature, and durability of shoes. Traditional sole materials mainly include rubber, EVA (ethylene-vinyl acetate) foam, and polyurethane foam. While EVA foam has low density and low cost, it suffers from poor resilience, tendency to collapse after prolonged wear, and insufficient flexural strength. Rubber offers excellent abrasion resistance, but its high density, long processing time, and non-recyclability make it unsuitable for recycling. Polyurethane foam offers good resilience, but poor hydrolysis resistance and environmental challenges during production.

[0003] Thermoplastic elastomers (TPEs) combine the high elasticity of rubber with the thermoplastic processability of plastics, and are recyclable, leading to their increasingly widespread application in the footwear industry in recent years. However, ordinary unfoamed TPEs have a relatively high density, making it difficult to meet the lightweight requirements of footwear materials. Existing foamed TPE materials generally suffer from uneven cell structure, significant degradation in mechanical properties, and difficulty in achieving a balance between abrasion resistance and resilience. In particular, at high foaming ratios, the tensile strength and abrasion resistance of the material decrease significantly, making it unsuitable for direct use in footwear outsoles or high-load midsoles. Therefore, developing a low-density, high-resilience, high-abrasion-resistant, and easily processed foamed thermoplastic elastomer footwear material has significant application value. Summary of the Invention

[0004] The purpose of this invention is to address the shortcomings of existing technologies by proposing a foamed thermoplastic elastic shoe material and its preparation method.

[0005] To achieve the above objectives, the present invention adopts the following technical solution: a foamed thermoplastic elastomer shoe material, which, by weight, is composed of the following components:

[0006] 60-100 parts of thermoplastic elastomer matrix;

[0007] 20-50 parts of plasticizer softener;

[0008] 10-40 parts of filler and reinforcing agent;

[0009] 1.5 to 6 parts of chemical foaming agent;

[0010] Foaming agent 0.5-2 parts;

[0011] Crosslinking system: 0.2–1.5 parts;

[0012] Antioxidant system 0.1-1 part;

[0013] Lubricant 0.5 to 2 parts.

[0014] Preferably, the thermoplastic elastomer matrix is ​​one or more of styrene-based thermoplastic elastomers, polyurethane-based thermoplastic elastomers, and polyester-based thermoplastic elastomers; the styrene-based thermoplastic elastomer is one or more of SEBS, SBS, and SEEPS, with a styrene content of 25% to 40% and a melt flow rate of 2 to 15 g / 10 min (test conditions: 190℃ / 2.16 kg).

[0015] Preferably, the softening plasticizer is one or more of naphthenic oil, paraffin oil, and white oil, with a kinematic viscosity of 80-300 mm² / s at 40°C; the filler and reinforcing agent is one or more of nano-calcium carbonate, talc, silica, and mica powder, with a particle size of 800-3000 mesh.

[0016] Preferably, the chemical foaming agent is one or more of azodicarbonamide, sodium bicarbonate, and p-toluenesulfonyl hydrazine; the foaming aid is one or more of zinc oxide, zinc stearate, and urea-based activators.

[0017] Preferably, the crosslinking system is one or more of dicumyl peroxide, bis-tert-butyl dicumyl peroxide, and trimethylolpropane triacrylate; the antioxidant system is one or more of antioxidant 1010, antioxidant 168, and antioxidant DLTP; and the lubricant is one or more of stearic acid, polyethylene wax, and ethylene bis-stearamide.

[0018] Preferably, the apparent density of the shoe material is 0.18-0.38 g / cm³, the resilience is ≥55%, the Akron abrasion loss is ≤0.25 cm³ / 1.61 km, the tensile strength is ≥2.5 MPa, and the elongation at break is ≥250%.

[0019] The method for producing the foamed thermoplastic elastomer shoe material includes the following steps:

[0020] (1) Pretreatment of ingredients: Weigh each component according to the weight parts, and preheat and dry the thermoplastic elastomer matrix at 60-80℃ for 2-4 hours;

[0021] (2) Oil-filled internal mixing: Put the preheated thermoplastic elastomer matrix into the internal mixer, heat it to 80-100℃, rotate it at 30-50 rpm, add the softening plasticizer in 2-3 batches, and mix for 8-15 minutes until the oil filling is uniform.

[0022] (3) Blending and mixing: Add antioxidant system and lubricant to internal mixer, mix for 3-5 minutes, then add filler, reinforcing agent, chemical foaming agent, foaming aid and crosslinking system, continue mixing for 5-10 minutes, and control the discharge temperature at 115-130℃ to obtain blended rubber compound;

[0023] (4) Extrusion granulation: The blended rubber compound is fed into a twin-screw extruder. The extrusion temperature range is 120-150℃ and the screw speed is 150-300rpm. After water cooling, the compound is stretched and granulated to obtain foaming masterbatch.

[0024] (5) Compression molding: Add the foaming masterbatch into the shoe material mold, and after the mold is closed, heat it to 160-185℃, press it to 10-18MPa, and hold it under pressure for 5-15 minutes; then release the pressure, open the mold, and cool and solidify to obtain the foamed thermoplastic elastic shoe material.

[0025] Preferably, in step (4), the twin-screw extruder adopts segmented temperature control, with the temperature ranges from the feed section to the die head as follows: 120℃, 130℃, 140℃, 145℃, 145℃, 140℃, and the die head temperature is 135℃~140℃.

[0026] Preferably, in step (5), the molding foaming adopts a one-time foaming process, the mold closing and pressurization time is ≤30s, and the pressure release and mold opening time is ≤5s; the cooling and shaping is placed at room temperature of 20~30℃ for 12~24h, or shaped by hot air at 60~80℃ for 30~60min.

[0027] Preferably, the shoe-making material is used to prepare any one of the following: midsole of sports shoes, outsole of casual shoes, upper of slippers, and cushioning layer of safety shoes.

[0028] Compared with the prior art, the advantages and positive effects of the present invention are as follows:

[0029] In this invention, through the synergistic effect of oil-filled modification and chemical foaming, the apparent density of the material can be as low as 0.18 g / cm³, while the rebound rate is ≥55%, providing excellent cushioning and making it suitable for sports shoe midsoles and casual shoe materials.

[0030] Through the synergistic effect of filling reinforcement and moderate cross-linking, Akron abrasion loss after foaming is ≤0.25cm³ / 1.61km, flexural strength is ≥100,000 cycles without cracking, and it can be directly used for shoe outsoles without the need for additional abrasion-resistant layers. It adopts thermoplastic processing technology, and the production process is solvent-free and sulfurized wastewater-free. Scrap materials and waste products can be crushed, granulated and reused, which is in line with the trend of green shoe manufacturing.

[0031] By adjusting the ratio of foaming agent to crosslinking agent, the foaming ratio and mechanical properties can be flexibly adjusted to meet the performance requirements of different shoe types. The molding process is compatible with existing shoe manufacturing equipment and is easy to scale up. Detailed Implementation

[0032] The technical solution of the present invention will be further described below with reference to embodiments, comparative examples and performance tests, but the scope of protection of the present invention is not limited thereto.

[0033] Example 1

[0034] A foamed thermoplastic elastic shoe material, by weight, comprises: 70 parts SEBS (YH-503), 30 parts naphthenic oil (KN4010), 20 parts nano-calcium carbonate (1500 mesh), 3 parts AC foaming agent, 1 part zinc oxide, 0.6 parts DCP, 0.3 parts TMPTA, 0.3 parts antioxidant 1010, and 1 part stearic acid.

[0035] Preparation steps:

[0036] Dry the SEBS at 70℃ for 3 hours;

[0037] Add the naphthenic oil in two batches at 90℃ and 40rpm in an internal mixer and mix for 10 minutes until the oil filling is uniform.

[0038] Add antioxidant 1010 and stearic acid and mix for 4 minutes. Then add nano calcium carbonate, AC foaming agent, zinc oxide, DCP and TMPTA, and continue mixing for 7 minutes. The discharge temperature is 122℃.

[0039] Twin-screw extrusion granulation, temperature range 125-135-140-140-135℃, screw speed 200rpm, pelletizing to obtain masterbatch;

[0040] Compression molding: Temperature 170℃, pressure 15MPa, pressure holding for 10min, quick pressure release and mold opening, leave at room temperature for 24h to set.

[0041] Performance tests: apparent density 0.26 g / cm³, resilience 58%, tensile strength 3.2 MPa, elongation at break 310%, Akron abrasion 0.21 cm³ / 1.61 km.

[0042] Example 2

[0043] A foamed thermoplastic elastic shoe material, by weight, comprises: 80 parts SEBS (YH-602), 35 parts paraffin oil, 15 parts talc (2000 mesh), 2.5 parts AC foaming agent, 0.8 parts zinc stearate, 0.5 parts BIPB, 0.2 parts antioxidant 168, and 0.8 parts polyethylene wax.

[0044] The preparation steps are basically the same as in Example 1, with a molding temperature of 175℃, a pressure of 14MPa, and a holding time of 12min.

[0045] Performance tests: apparent density 0.22 g / cm³, resilience 62%, tensile strength 2.8 MPa, elongation at break 280%, Akron abrasion 0.23 cm³ / 1.61 km.

[0046] Example 3

[0047] A foamed thermoplastic elastic shoe material, by weight, comprises: 100 parts of SEBS / TPU compounded in a 7:3 ratio, 40 parts of white oil, 25 parts of silica, 4 parts of sodium bicarbonate, 1.2 parts of urea-based foaming agent, 0.8 parts of DCP, 0.4 parts of TMPTA, 0.5 parts of antioxidant DLTP, and 1.2 parts of EBS.

[0048] The preparation steps are basically the same as in Example 1, with an extrusion temperature of 130-145℃, a molding temperature of 180℃, and a holding pressure of 8min.

[0049] Performance tests: apparent density 0.32 g / cm³, resilience 56%, tensile strength 4.1 MPa, elongation at break 260%, Akron abrasion 0.18 cm³ / 1.61 km.

[0050] Comparative Example 1

[0051] No crosslinking system was added; the remaining components and processes were the same as in Example 1.

[0052] Performance testing: apparent density 0.30 g / cm³, resilience 48%, tensile strength 2.1 MPa, uneven cell size, with obvious merging of large pores.

[0053] Comparative Example 2

[0054] Ordinary EVA foam shoe material (commercially available).

[0055] Performance testing: apparent density 0.25 g / cm³, resilience 42%, Akron abrasion 0.38 cm³ / 1.61 km, cracks appeared after 30,000 folds.

[0056] As can be seen from the above embodiments and comparative examples, the foamed thermoplastic elastomer material prepared by the present invention through the synergistic regulation of the cross-linked foaming system still has excellent resilience, wear resistance and mechanical properties at low density. Its comprehensive performance is significantly better than that of traditional EVA foam materials, and fully meets the performance requirements of the footwear industry for midsole and outsole materials.

[0057] The above are merely preferred embodiments of the present invention and are not intended to limit the present invention in any other way. Any person skilled in the art may make changes or modifications to the above-disclosed technical content to create equivalent embodiments that can be applied to other fields. However, any simple modifications, equivalent changes, and modifications made to the above embodiments based on the technical essence of the present invention without departing from the scope of the present invention shall still fall within the protection scope of the present invention.

Claims

1. A foamed thermoplastic elastomer shoe material, characterized in that, By weight, it consists of the following components: 60-100 parts of thermoplastic elastomer matrix; 20-50 parts of plasticizer softener; 10-40 parts of filler and reinforcing agent; 1.5 to 6 parts of chemical foaming agent; Foaming agent 0.5-2 parts; Crosslinking system: 0.2–1.5 parts; Antioxidant system 0.1-1 part; Lubricant 0.5 to 2 parts.

2. The foamed thermoplastic elastomer shoe material according to claim 1, characterized in that: The thermoplastic elastomer matrix is ​​one or more of styrene-based thermoplastic elastomers, polyurethane-based thermoplastic elastomers, and polyester-based thermoplastic elastomers; the styrene-based thermoplastic elastomer is one or more of SEBS, SBS, and SEEPS, with a styrene content of 25% to 40% and a melt flow rate of 2 to 15 g / 10 min (test conditions: 190℃ / 2.16 kg).

3. The foamed thermoplastic elastomer shoe material according to claim 1, characterized in that: The softening plasticizer is one or more of naphthenic oil, paraffin oil, and white oil, with a kinematic viscosity of 80-300 mm² / s at 40°C; the filler and reinforcing agent is one or more of nano-calcium carbonate, talc, silica, and mica powder, with a particle size of 800-3000 mesh.

4. The foamed thermoplastic elastomer shoe material according to claim 1, characterized in that: The chemical foaming agent is one or more of azodicarbonamide, sodium bicarbonate, and p-toluenesulfonyl hydrazine; the foaming aid is one or more of zinc oxide, zinc stearate, and urea-based activators.

5. The foamed thermoplastic elastomer shoe material according to claim 1, characterized in that: The crosslinking system is one or more of dicumyl peroxide, bis-tert-butyldicumyl peroxide, and trimethylolpropane triacrylate; the antioxidant system is one or more of antioxidant 1010, antioxidant 168, and antioxidant DLTP; and the lubricant is one or more of stearic acid, polyethylene wax, and ethylene bis-stearamide.

6. The foamed thermoplastic elastomer shoe material according to claim 1, characterized in that: The apparent density of the shoe material is 0.18-0.38 g / cm³, the resilience is ≥55%, the Akron abrasion is ≤0.25 cm³ / 1.61 km, the tensile strength is ≥2.5 MPa, and the elongation at break is ≥250%.

7. A method for preparing the foamed thermoplastic elastomer shoe material as described in any one of claims 1 to 6, characterized in that, Includes the following steps: (1) Pretreatment of ingredients: Weigh each component according to the weight parts, and preheat and dry the thermoplastic elastomer matrix at 60-80℃ for 2-4 hours; (2) Oil-filled internal mixing: Put the preheated thermoplastic elastomer matrix into the internal mixer, heat it to 80-100℃, rotate it at 30-50 rpm, add the softening plasticizer in 2-3 batches, and mix for 8-15 minutes until the oil filling is uniform. (3) Blending and mixing: Add antioxidant system and lubricant to internal mixer, mix for 3-5 minutes, then add filler, reinforcing agent, chemical foaming agent, foaming aid and crosslinking system, continue mixing for 5-10 minutes, and control the discharge temperature at 115-130℃ to obtain blended rubber compound; (4) Extrusion granulation: The blended rubber compound is fed into a twin-screw extruder. The extrusion temperature range is 120-150℃ and the screw speed is 150-300rpm. After water cooling, the compound is stretched and granulated to obtain foaming masterbatch. (5) Compression foaming: Add the foaming masterbatch into the shoe material mold, and after the mold is closed, heat it to 160-185℃, press it to 10-18MPa, and hold it under pressure for 5-15 minutes; then release the pressure, open the mold, and cool and solidify to obtain foamed thermoplastic elastic shoe material.

8. The preparation method according to claim 7, characterized in that: In step (4), the twin-screw extruder adopts segmented temperature control, with the temperature ranges from the feed section to the die head as follows: 120℃, 130℃, 140℃, 145℃, 145℃, 140℃, and the die head temperature is 135℃ to 140℃.

9. The preparation method according to claim 7, characterized in that: In step (5), the molding foaming adopts a one-time foaming process, with the mold closing and pressurization time ≤30s and the pressure release and mold opening time ≤5s; the cooling and shaping is carried out at room temperature of 20~30℃ for 12~24h, or by hot air shaping at 60~80℃ for 30~60min.

10. The preparation method according to claim 7, characterized in that: The shoe-making material is used to prepare any one of the following: midsole of sports shoes, outsole of casual shoes, upper of slippers, and cushioning layer of safety shoes.