Waterproof low-temperature resistant asphalt modifier and preparation method thereof

By preparing a waterproof and low-temperature resistant asphalt modifier, the problems of asphalt brittleness at low temperatures and poor stability at high temperatures were solved, thereby improving the low-temperature performance and waterproof performance of asphalt, while also enhancing its storage stability. This modifier can be applied to road paving and building waterproofing projects.

CN123152245APending Publication Date: 2026-11-24JIANGSU SILMA ROAD ENVIRONMENTAL PROTECTION MATERIALS GROUP CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611489870.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-23
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing technologies show that asphalt is prone to brittleness at low temperatures, has insufficient waterproofing, and poor high-temperature stability. Furthermore, modified asphalt is prone to segregation during storage, making it impossible to comprehensively improve its low-temperature performance, waterproofing performance, and high-temperature stability.

Method used

A waterproof and low-temperature resistant asphalt modifier is prepared by using styrene-butadiene-styrene block copolymer, epoxy resin, nano silica, aluminum silicate, desulfurized rubber powder and silane coupling agent, etc., through premixing, stirring and melt extrusion, etc., to improve the low-temperature ductility, crack resistance and high-temperature stability of asphalt.

Benefits of technology

It significantly improves the low-temperature ductility, crack resistance, water resistance and high-temperature stability of asphalt. The low-temperature ductility at 5℃ can reach more than 100cm, and the modifier is environmentally friendly and economical.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123152245A_ABST
    Figure CN123152245A_ABST
Patent Text Reader

Abstract

This invention relates to the field of asphalt modifier technology, and discloses a waterproof and low-temperature resistant asphalt modifier and its preparation method. The modifier comprises, by weight, 40-60 parts SBS, 15-30 parts epoxy resin, 2-8 parts nano-silica, 1-5 parts aluminum silicate, 5-15 parts desulfurized rubber powder, 2-6 parts polyvinyl butyral, and 1-3 parts silane coupling agent. The preparation method includes: premixing SBS, desulfurized rubber powder, and nano-silica to obtain a premix; mixing epoxy resin and silane coupling agent, then adding aluminum silicate and polyvinyl butyral to obtain a resin mixture; adding the premix to the resin mixture and stirring at high speed; and extruding and granulating using a twin-screw extruder. This invention significantly improves the low-temperature ductility, crack resistance, waterproofness, high-temperature stability, and storage stability of asphalt through synergistic modification by SBS, nano-silica, and epoxy resin. The low-temperature ductility at 5℃ can reach over 100 cm, and it uses recycled rubber powder, making it environmentally friendly and economical.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of asphalt modifier technology, and in particular to a waterproof and low-temperature resistant asphalt modifier and its preparation method. Background Technology

[0002] Asphalt is widely used in road paving, building waterproofing, bridge deck waterproofing and other engineering fields. Ordinary base asphalt is prone to brittle cracking at low temperatures, and has insufficient crack resistance and ductility; it is prone to softening and flowing at high temperatures, and has poor rutting resistance; at the same time, its density and adhesion are limited, and its waterproof performance may decline with long-term use.

[0003] Existing technologies often use SBS to modify asphalt to improve its low-temperature flexibility and high-temperature stability; however, SBS-modified asphalt alone suffers from poor storage stability and segregation, and there is still room for improvement in low-temperature waterproofing and crack resistance. While nanomaterials can improve the mechanical properties of asphalt, their direct addition easily leads to agglomeration and uneven dispersion. Epoxy resins can improve adhesion and density, but their compatibility with asphalt is limited.

[0004] Therefore, there is a need for an asphalt modifier that can comprehensively improve low-temperature performance, waterproof performance, high-temperature stability, and storage stability. Summary of the Invention

[0005] The purpose of this invention is to provide a waterproof and low-temperature resistant asphalt modifier and its preparation method, which solves the problems of low-temperature brittleness, insufficient waterproofness, poor high-temperature stability, and easy segregation of modified asphalt during storage in the prior art.

[0006] To achieve the above objectives, in a first aspect, the present invention provides a waterproof and low-temperature resistant asphalt modifier, comprising the following raw materials: Styrene-butadiene-styrene block copolymer, epoxy resin, nano silica, aluminum silicate, desulfurized rubber powder, polyvinyl butyral and silane coupling agent.

[0007] The product, by weight, includes the following raw materials: 40-60 parts of styrene-butadiene-styrene block copolymer, 15-30 parts of epoxy resin, 2-8 parts of nano-silica, 1-5 parts of aluminum silicate, 5-15 parts of desulfurized rubber powder, 2-6 parts of polyvinyl butyral, and 1-3 parts of silane coupling agent.

[0008] The nano-silica has an average particle size of 20-100 nm; the desulfurized rubber powder is waste tire desulfurized rubber powder with a particle size of 40-80 mesh; the silane coupling agent is selected from one of KH-550, KH-560, and KH-570; and the epoxy resin is bisphenol A type epoxy resin.

[0009] Secondly, a method for preparing a waterproof and low-temperature resistant asphalt modifier is provided, comprising the following steps: SBS, desulfurized rubber powder and nano silica are premixed in a high-speed mixer to obtain a premixed material. Epoxy resin and silane coupling agent are stirred and mixed in a high-speed mixer, then aluminum silicate and polyvinyl butyral are added, and stirring is continued until uniform to obtain resin mixture. The premixed material is added to the resin mixture and stirred at high speed to ensure that the components are fully and evenly dispersed to obtain a mixture. The mixture is melt-extruded through a twin-screw extruder, cooled, and then granulated to obtain a waterproof and low-temperature resistant asphalt modifier.

[0010] The process of premixing SBS, desulfurized rubber powder, and nano-silica in a high-speed mixer to obtain a premix includes: The SBS, the desulfurized rubber powder, and the nano silica are premixed in a high-speed mixer at a speed of 500-1000 rpm and a temperature of 60-80°C for 15-30 minutes to obtain the premix.

[0011] The process of mixing epoxy resin and silane coupling agent, then adding aluminum silicate and polyvinyl butyral, and continuing to stir until homogeneous, yields a resin mixture comprising: The epoxy resin and the silane coupling agent are added to the high-speed mixer and stirred at 300-600 rpm and 50-60°C for 10-15 minutes. Then, the aluminum silicate and the polyvinyl butyral are added, and stirring is continued until homogeneous to obtain the resin mixture.

[0012] The step of adding the premix to the resin mixture and stirring at high speed to fully disperse and homogenize the components to obtain a mixture includes: The premixed material is added to the resin mixture and stirred at 800-1200 rpm at 80-100°C for 20-40 minutes to ensure that the components are fully dispersed and uniform, thereby obtaining the mixture.

[0013] The step of melting and extruding the mixture under a twin-screw extruder, cooling it, and then granulating it to obtain a waterproof and low-temperature resistant asphalt modifier includes: The resulting mixture is melt-extruded by a twin-screw extruder at a speed of 200-500 rpm and a temperature of 140-160°C, and then granulated after cooling to obtain a waterproof and low-temperature resistant asphalt modifier.

[0014] The high-speed mixer operates at a speed of 300–1500 rpm; the twin-screw extruder operates at a screw speed of 200–600 rpm.

[0015] This invention discloses a waterproof and low-temperature resistant asphalt modifier and its preparation method. The modifier comprises, by weight, 40-60 parts SBS, 15-30 parts epoxy resin, 2-8 parts nano-silica, 1-5 parts aluminum silicate, 5-15 parts desulfurized rubber powder, 2-6 parts polyvinyl butyral, and 1-3 parts silane coupling agent. The preparation method includes: premixing SBS, desulfurized rubber powder, and nano-silica to obtain a premix; mixing epoxy resin and silane coupling agent, then adding aluminum silicate and polyvinyl butyral to obtain a resin mixture; adding the premix to the resin mixture and stirring at high speed; and extruding and granulating using a twin-screw extruder. This invention significantly improves the low-temperature ductility, crack resistance, waterproofness, high-temperature stability, and storage stability of asphalt through synergistic modification by SBS, nano-silica, and epoxy resin. The low-temperature ductility at 5°C can reach over 100 cm, and it can partially utilize recycled rubber powder, making it environmentally friendly and economical. Attached Figure Description

[0016] To more clearly illustrate the technical solutions in the embodiments of this application or the prior art, the accompanying drawings used in the description of the embodiments or the prior art will be briefly introduced below.

[0017] Figure 1 This is a flowchart of a waterproof and low-temperature resistant asphalt modifier and its preparation method according to the present invention. Detailed Implementation

[0018] The embodiments of the present invention are described in detail below. Examples of the embodiments are shown in the accompanying drawings. The embodiments described below with reference to the accompanying drawings are exemplary and intended to explain the present invention, but should not be construed as limiting the present invention.

[0019] In a first aspect, embodiments of the present invention provide a waterproof and low-temperature resistant asphalt modifier, comprising the following raw materials: Styrene-butadiene-styrene block copolymer, epoxy resin, nano silica, aluminum silicate, desulfurized rubber powder, polyvinyl butyral and silane coupling agent.

[0020] The product, by weight, includes the following raw materials: 40-60 parts of styrene-butadiene-styrene block copolymer, 15-30 parts of epoxy resin, 2-8 parts of nano-silica, 1-5 parts of aluminum silicate, 5-15 parts of desulfurized rubber powder, 2-6 parts of polyvinyl butyral, and 1-3 parts of silane coupling agent.

[0021] Secondly, the average particle size of the nano-silica is 20-100 nm; the desulfurized rubber powder is waste tire desulfurized rubber powder with a particle size of 40-80 mesh; the silane coupling agent is selected from one of KH-550, KH-560, and KH-570; and the epoxy resin is bisphenol A type epoxy resin.

[0022] This invention discloses a waterproof and low-temperature resistant asphalt modifier, which comprises, by weight: 40-60 parts SBS, 15-30 parts epoxy resin, 2-8 parts nano silica, 1-5 parts aluminum silicate, 5-15 parts desulfurized rubber powder, 2-6 parts polyvinyl butyral, and 1-3 parts silane coupling agent. This invention significantly improves the low-temperature ductility, crack resistance, waterproofness, high-temperature stability, and storage stability of asphalt through synergistic modification by SBS, nano silica, and epoxy resin. The low-temperature ductility at 5℃ can reach over 100 cm, and it can partially utilize recycled rubber powder, making it environmentally friendly and economical.

[0023] Secondly, please refer to Figure 1 , Figure 1 This is a flowchart of a waterproof and low-temperature resistant asphalt modifier and its preparation method according to the present invention.

[0024] A method for preparing a waterproof and low-temperature resistant asphalt modifier includes the following steps: S1 premixes SBS, desulfurized rubber powder and nano silica in a high-speed mixer to obtain a premix; Specifically, the SBS, the desulfurized rubber powder, and the nano-silica are premixed in a high-speed mixer at a speed of 500–1000 rpm and a temperature of 60–80°C for 15–30 minutes to obtain the premix. S2 involves mixing epoxy resin and silane coupling agent in a high-speed mixer, then adding aluminum silicate and polyvinyl butyral, and continuing to stir until homogeneous to obtain a resin mixture. Specifically, the epoxy resin and the silane coupling agent are added to the high-speed mixer and stirred at 300-600 rpm and 50-60°C for 10-15 minutes. Then, the aluminum silicate and the polyvinyl butyral are added, and stirring is continued until homogeneous to obtain the resin mixture.

[0025] S3. The premixed material is added to the resin mixture and stirred at high speed to ensure that the components are fully dispersed and uniform, thereby obtaining a mixture. Specifically, the premix is ​​added to the resin mixture and stirred at 800-1200 rpm at 80-100°C for 20-40 minutes to ensure that the components are fully dispersed and uniform, thereby obtaining the mixture.

[0026] S4 The mixture is melt-extruded through a twin-screw extruder, cooled, and then granulated to obtain a waterproof and low-temperature resistant asphalt modifier; Specifically, the obtained mixture is melt-extruded by a twin-screw extruder at a speed of 200-500 rpm and a temperature of 140-160°C, and then granulated after cooling to obtain a waterproof and low-temperature resistant asphalt modifier.

[0027] Furthermore, the high-speed mixer operates at a speed of 300–1500 rpm; the twin-screw extruder operates at a screw speed of 200–600 rpm. Specific Implementation

[0029] Example: Raw material formula, in parts by weight: 50 parts SBS; 22 parts bisphenol A type epoxy resin E-51; 5 parts nano silica, average particle size 30nm; 3 parts aluminum silicate; 10 parts desulfurized rubber powder, 60 mesh; 4 parts polyvinyl butyral; 2 parts silane coupling agent KH-550.

[0030] Preparation method: Step 1: Add SBS, desulfurized rubber powder and nano silica to a high-speed mixer and premix at 70℃ and 800rpm for 20 minutes to obtain a premix.

[0031] Step 2: Stir epoxy resin E-51 and KH-550 at 55℃ for 12 minutes, add aluminum silicate and polyvinyl butyral, and continue stirring until uniform to obtain resin mixture.

[0032] Step 3: Add the premix to the resin mixture and stir at 90°C and 1000 rpm for 30 minutes.

[0033] Step 4: Feed the mixture into a twin-screw extruder, melt-extrude at 150°C, cool and granulate to obtain a waterproof and low-temperature resistant asphalt modifier.

[0034] Application: Heat 1000 kg of base asphalt to 160°C, add 80 kg of the above modifier, and stir at 160°C for 45 min until evenly dispersed to obtain modified asphalt.

[0035] The above-disclosed embodiments are merely one or more preferred embodiments of this application and should not be construed as limiting the scope of this application. Those skilled in the art can understand that all or part of the processes for implementing the above embodiments and equivalent changes made in accordance with the claims of this application still fall within the scope of this application.

Claims

1. A waterproof and low-temperature resistant asphalt modifier, characterized in that, Including the following raw materials: Styrene-butadiene-styrene block copolymer, epoxy resin, nano silica, aluminum silicate, desulfurized rubber powder, polyvinyl butyral and silane coupling agent.

2. The waterproof and low-temperature resistant asphalt modifier as described in claim 1, characterized in that, By weight, it includes the following raw materials: 40-60 parts of styrene-butadiene-styrene block copolymer, 15-30 parts of epoxy resin, 2-8 parts of nano silica, 1-5 parts of aluminum silicate, 5-15 parts of desulfurized rubber powder, 2-6 parts of polyvinyl butyral and 1-3 parts of silane coupling agent.

3. The waterproof and low-temperature resistant asphalt modifier as described in claim 2, characterized in that, The average particle size of the nano-silica is 20-100 nm; the desulfurized rubber powder is waste tire desulfurized rubber powder with a particle size of 40-80 mesh; the silane coupling agent is selected from one of KH-550, KH-560, and KH-570; and the epoxy resin is bisphenol A type epoxy resin.

4. A method for preparing a waterproof and low-temperature resistant asphalt modifier, used to prepare the waterproof and low-temperature resistant asphalt modifier according to any one of claims 1 to 3, characterized in that, Includes the following steps: SBS, desulfurized rubber powder and nano silica are premixed in a high-speed mixer to obtain a premixed material. Epoxy resin and silane coupling agent are stirred and mixed in a high-speed mixer, then aluminum silicate and polyvinyl butyral are added, and stirring is continued until uniform to obtain resin mixture. The premixed material is added to the resin mixture and stirred at high speed to ensure that the components are fully and evenly dispersed to obtain a mixture. The mixture is melt-extruded through a twin-screw extruder, cooled, and then granulated to obtain a waterproof and low-temperature resistant asphalt modifier.

5. The method for preparing a waterproof and low-temperature resistant asphalt modifier as described in claim 4, characterized in that, The process of premixing SBS, desulfurized rubber powder, and nano-silica in a high-speed mixer to obtain a premixed material includes: The SBS, the desulfurized rubber powder, and the nano silica are premixed in a high-speed mixer at a speed of 500-1000 rpm and a temperature of 60-80°C for 15-30 minutes to obtain the premix.

6. The method for preparing a waterproof and low-temperature resistant asphalt modifier as described in claim 4, characterized in that, Epoxy resin and silane coupling agent are mixed in a high-speed mixer, then aluminum silicate and polyvinyl butyral are added, and stirring is continued until homogeneous to obtain a resin mixture comprising: The epoxy resin and the silane coupling agent are added to the high-speed mixer and stirred at 300-600 rpm and 50-60°C for 10-15 minutes. Then, the aluminum silicate and the polyvinyl butyral are added, and stirring is continued until homogeneous to obtain the resin mixture.

7. The method for preparing a waterproof and low-temperature resistant asphalt modifier as described in claim 4, characterized in that, The process involves adding the premix to the resin mixture and stirring at high speed to ensure thorough and uniform dispersion of all components, resulting in a mixture comprising: The premixed material is added to the resin mixture and stirred at 800-1200 rpm at 80-100°C for 20-40 minutes to ensure that the components are fully dispersed and uniform, thereby obtaining the mixture.

8. The method for preparing a waterproof and low-temperature resistant asphalt modifier as described in claim 4, characterized in that, The mixture is melt-extruded under a twin-screw extruder, cooled, and then granulated to obtain a waterproof and low-temperature resistant asphalt modifier, comprising: The resulting mixture is melt-extruded by a twin-screw extruder at a speed of 200-500 rpm and a temperature of 140-160°C, and then granulated after cooling to obtain a waterproof and low-temperature resistant asphalt modifier.

9. The method for preparing a waterproof and low-temperature resistant asphalt modifier as described in claim 4, characterized in that, The high-speed mixer operates at a speed of 300–1500 rpm; the twin-screw extruder operates at a screw speed of 200–600 rpm.