A yellowing-resistant edge band and a production process thereof
By synergistically combining anti-yellowing additives and modified corrosion resistant agents, the yellowing and corrosion problems of ABS edge banding strips under ultraviolet light and acid/alkali environments are solved, achieving long-lasting anti-yellowing and corrosion resistance of the edge banding strips, which are suitable for panel furniture, cabinets, bathroom fixtures and other fields.
Patent Information
- Application Number
- CN202611508370.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-28
- Publication Date
- 2026-11-24
AI Technical Summary
Existing ABS edge banding strips are prone to oxidation and degradation under ultraviolet radiation and long-term heat and oxygen, resulting in yellowing. They are also prone to corrosion and powdering in acidic and alkaline environments, making it difficult to achieve a balance between corrosion resistance and yellowing resistance.
By introducing anti-yellowing additives and modified corrosion resistant agents, the anti-yellowing additives are generated by the condensation of anhydrous citric acid and cysteine hydrochloride to form a pyridone structure, which is then combined with chemical grafting modification of nano-cerium oxide to absorb ultraviolet light and inhibit yellowing; the modified corrosion resistant agents are generated by the esterification reaction of 3,5-diaminobenzoic acid and perfluorohexylethyl alcohol to form perfluoroalkyl groups, thereby improving chemical stability.
It significantly improves the yellowing resistance and chemical corrosion resistance of edge banding, extends service life, is suitable for high humidity and high corrosion environments, and reduces the frequency of product damage caused by aging and corrosion.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] This invention relates to the field of edge banding technology, specifically to an edge banding strip resistant to yellowing and its manufacturing process. Background Technology
[0002] Edge banding is an indispensable core auxiliary material in the production of panel furniture. It is mainly used to cover and seal the cut surfaces of engineered wood panels, preventing external moisture erosion, deformation, and cracking, thus extending the furniture's lifespan. It also blocks the release of free formaldehyde from within the panel, and its performance directly determines the finished quality and long-term user experience of the panel furniture. Currently, the mainstream edge banding materials in the furniture market are divided into four categories: wood, PVC, ABS, and acrylic. ABS edge banding uses ABS resin as its core matrix, achieving a balance between rigidity and toughness through its ternary copolymer structure. It boasts excellent impact resistance and processability, strong compatibility with mainstream hot melt adhesives, no color difference after trimming, and requires no harmful additives, making it environmentally friendly and safe. It has now become the mainstream edge banding material in the mid-to-high-end customized furniture sector. However, the unsaturated carbon-carbon double bonds in the butadiene component of the ABS molecular chain are easily oxidized and degraded under ultraviolet radiation and long-term heat and oxygen, generating chromophores and causing yellowing. Furthermore, ABS resin itself has limited resistance to acids, alkalis, and polar chemicals. In kitchens, bathrooms, and other similar environments, prolonged contact with acidic or alkaline media such as food seasonings and personal care products can easily lead to surface corrosion, powdering, and cracking. Structural damage, in turn, exacerbates aging and yellowing, creating a vicious cycle. Currently, there is a lack of synergistic modification technologies for corrosion resistance and yellowing resistance in edge banding strips, making it difficult to achieve a balance of multiple properties.
[0003] Patent application number 201310676471.X discloses a yellowing-resistant PC / ABS alloy for automotive interior parts and its preparation method. It uses a mixture of benzotriazole and benzophenone UV absorbers and titanium dioxide to obtain a composite yellowing-resistant agent, improving the material's yellowing resistance. However, the physically compounded yellowing-resistant agent has poor compatibility with the matrix, is prone to migration and precipitation, and has insufficient weather resistance. Patent application number 201110245020.1 discloses an aluminum nitride-doped insulating and thermally conductive ABS composite material and its preparation. It uses nano-aluminum nitride to improve the corrosion resistance of the ABS matrix. However, aluminum nitride has limited compatibility with the matrix, is prone to agglomeration affecting appearance, and its durability is insufficient when used alone. Summary of the Invention
[0004] To address the aforementioned technical problems, this invention provides a yellowing-resistant edge banding strip and its manufacturing process.
[0005] The objective of this invention can be achieved through the following technical solutions: A yellowing-resistant edge banding strip comprises the following raw materials in parts by weight: 80-100 parts ABS resin, 20-30 parts nano calcium carbonate, 0.5-2 parts CPE resin, 1-2 parts ACR resin, 1-4 parts yellowing-resistant additive, 0.5-1 part antioxidant, 4-7 parts heat stabilizer, 0.4-0.8 parts lubricant, 0.5-1 part silane coupling agent KH-550, and 2-5 parts modified corrosion resistant agent; The antioxidant is at least one of antioxidant 1010 and antioxidant 1098; The heat stabilizer is at least one of calcium stearate and zinc stearate; The lubricant is at least one of paraffin wax, polyethylene wax, oxidized polyethylene wax and stearic acid; The anti-yellowing agent is prepared by the following steps: Step A1: Mix anhydrous citric acid, cysteine hydrochloride and deionized water to obtain a mixture. Place the mixture in a beaker and shake it in an 80°C drying oven for 30 min. Dry for 1.5 h and then place it in a 130°C forced-air drying oven for 12 h. After the reaction is complete, cool to room temperature, add deionized water, stir for 15 min, filter under reduced pressure, wash and vacuum dry to obtain intermediate product 1. Furthermore, the ratio of the mixed solution to deionized water is 6-18 mL: 150-300 mL; Furthermore, the ratio of anhydrous citric acid, cysteine hydrochloride, and deionized water in the mixture is 0.1-0.3 mol: 0.1-0.3 mol: 6-18 mL; In step A1, anhydrous citric acid and cysteine hydrochloride undergo a condensation reaction to form a ring, introducing a carboxyl group into the system and providing reaction conditions for the subsequent esterification reaction. The resulting pyridone structure contains a pyridine ring and a ketone group, forming a conjugated π-electron system that can effectively absorb ultraviolet light.
[0006] Step A2: In a glove box, potassium phosphate, 18-crown-6, type 4A molecular sieve and tetrahydrofuran are mixed and placed in a closed reaction system. Polymethylhydrosiloxane, allyl mercaptan and intermediate product 1 are added. The reaction mixture is stirred and refluxed for 12 hours. Ethyl acetate is added, filtered, distilled under reduced pressure and purified to obtain intermediate product 2. Furthermore, the molar ratio of potassium phosphate, 18-crown-6, type 4A molecular sieve, tetrahydrofuran, polymethylhydrosiloxane, allyl mercaptan, intermediate 1, and ethyl acetate is 0.4-0.6 g : 1-1.5 g : 0.8-1.2 g : 130-190 mL : 9-14 mL : 0.02-0.03 mol : 0.06-0.09 mol : 100-120 mL; In step A2, intermediate product 1 and allyl mercaptan undergo a thioesterification reaction, introducing a double bond into the system and providing reaction conditions for subsequent polymerization. This generates a mercaptoester group, which, in synergistic effect with auxochromes containing lone pairs of electrons such as S and N, increases the UV absorption intensity of the system.
[0007] Step A3: Mix nano-cerium oxide powder with 10wt% ethanol aqueous solution to obtain mixture 1. Mix 4-allylcatechol with 10wt% ethanol aqueous solution to obtain mixture 2. Mix mixture 1 and mixture 2, sonicate for 40 min, add acetic acid solution dropwise under stirring to adjust the pH of the system to 6, heat to 50℃ and react for 10 h, cool to room temperature, centrifuge, wash, dry and grind to obtain intermediate product 3. Furthermore, the ratio of nano-cerium oxide powder to ethanol aqueous solution in mixture 1 is 1g:100mL; Furthermore, the ratio of 4-allyl catechol to aqueous ethanol in mixture 2 is 0.01-0.03 mol: 450-650 mL; In step A3, the catechol groups coordinate and chelate with the metal sites on the surface of nano-cerium oxide to achieve chemical grafting modification, introducing double bonds into the system and providing reaction conditions for subsequent polymerization. Nano-cerium oxide has a small band gap, which is conducive to the transition of valence electrons. It has a strong absorption capacity for ultraviolet light in the 200-400nm wavelength band and can also reduce ultraviolet transmission through scattering and reflection. In addition, it has a free radical scavenging effect, which can remove free radicals that cause oxidative breakage or cross-linking of polymer chains and inhibit yellowing.
[0008] Step A4: Add intermediate product 3 to cyclohexane, stir for 30 min, then sonicate for 30 min, add intermediate product 2 and 2-hydroxy-4-(isobutenoyloxy)benzophenone, place in an oil bath and heat to 80°C, stir, add 2 / 3 part of benzoyl peroxide, add 1 / 3 part of benzoyl peroxide after 2 h, continue stirring and react for 7 h, pour the product into anhydrous ethanol, stir for 30 min, wash and vacuum dry to obtain the anti-yellowing agent; Furthermore, the ratio of intermediate 3, cyclohexane, intermediate 2, 2-hydroxy-4-(isobutenoyloxy)benzophenone, benzoyl peroxide, and anhydrous ethanol is 0.4 g : 30-60 mL : 0.01-0.02 mol : 0.01-0.02 mol : 0.4-0.5 g : 50-60 mL; In step A4, intermediate product 2 and 2-hydroxy-4-(isobutenoyloxy)benzophenone undergo in-situ polymerization on the surface of nano-cerium oxide. The introduced benzophenone structure can absorb ultraviolet light in the range of 290-400 nm, preventing photo-oxidation of double bonds in the ABS molecular chain caused by ultraviolet light, thereby inhibiting yellowing. Copolymerizing and grafting it with the pyridone structure onto the surface of nano-cerium oxide helps to reduce the easy migration of organic additives and the easy aggregation of inorganic particles, greatly improving the long-term resistance to yellowing and the compatibility with the matrix.
[0009] The modified corrosion resistant agent is prepared by the following steps: Step B1: Mix 3,5-diaminobenzoic acid, perfluorohexylethyl alcohol, p-toluenesulfonic acid and toluene, stir and heat to 140°C, reflux until no obvious water droplets are formed, after the reaction is complete, add ethyl acetate, wash with 10wt% sodium bicarbonate solution, then wash with deionized water and saturated sodium chloride solution in turn, separate the liquid, dry, filter, distill under reduced pressure and dry to obtain the diamino perfluorinated derivative; Furthermore, the volume ratio of 3,5-diaminobenzoic acid, perfluorohexylethyl alcohol, p-toluenesulfonic acid, toluene, ethyl acetate, sodium bicarbonate solution, deionized water, and saturated sodium chloride solution is 0.1-0.3 mol : 0.095-0.285 mol : 0.01-0.03 mol : 150-350 mL : 200-300 mL : 300-400 mL : 300 mL : 300 mL; In step B1, 3,5-diaminobenzoic acid and perfluorohexylethyl alcohol undergo esterification, introducing a diamino group into the system and providing reaction conditions for subsequent polymerization. The introduced perfluoroalkyl group has extremely strong CF bonds, giving the system high chemical stability, making it difficult to be corroded by acids, alkalis, oxidants, etc. In addition, the perfluoroalkyl group has extremely low surface energy, which can form hydrophobic and oleophobic surfaces, preventing corrosive liquids from wetting and penetrating the material surface, and enhancing the material's corrosion resistance.
[0010] Step B2: Under nitrogen protection, the diamino perfluorinated derivative, 2,7-diamino-9-fluorenone, and N,N-dimethylacetamide were mixed and stirred for 30 min. The temperature was lowered to 0°C, and isophthaloyl chloride was added in four portions over 20 min. After the last addition, the stirring speed was increased until the rod-climbing effect occurred. Then, the mixture was heated to 60°C and stirred under nitrogen for 1 h. Finally, calcium hydroxide was added and stirred for 15 min. The mixture was washed and dried to obtain the modified corrosion resistant agent. Furthermore, the molar ratio of the diamino perfluorinated derivative, 2,7-diamino-9-fluorenone, N,N-dimethylacetamide, isophthaloyl chloride, and calcium hydroxide is 0.01-0.02 mol : 0.08-0.09 mol : 90-130 mL : 0.1-0.11 mol : 0.1-0.11 mol; In step B2, the diamino perfluorinated derivative, 2,7-diamino-9-fluorenone, and isophthaloyl chloride undergo an amide polymerization reaction. The resulting polyamide contains a large number of polar amide bonds, which can interact with the polar cyano groups in ABS to form a certain degree of compatibility interface, thereby improving the overall resistance of the material to acid and alkali environments. The fluorenyl group has a large-volume, rigid tricyclic condensed aromatic hydrocarbon structure, which can enhance the compactness and thermal stability of the polyamide chain. It works synergistically with the perfluorinated alkyl group to give the material the advantages of long-term corrosion resistance, no precipitation, and no loss of the mechanical properties of the matrix.
[0011] A manufacturing process for a yellowing-resistant edge banding strip includes the following steps: Step S1: Weigh the raw materials according to the weight parts, and mix ABS resin, nano calcium carbonate, CPE resin, ACR resin, anti-yellowing agent, antioxidant, heat stabilizer, lubricant, silane coupling agent KH-550 and modified corrosion resistant agent, and mix at 800-1500 r / min for 20-40 min to obtain a mixture; Step S2: The mixture is fed into a twin-screw extruder for extrusion, cooled and solidified to obtain a yellowing-resistant edge sealing strip. The operating parameters of the extruder are as follows: Zone 1 of the barrel 1: 180-190℃, Zone 2 of the barrel 2: 180-190℃, Zone 3 of the barrel 3: 180-190℃, Zone 4 of the barrel 4: 180-190℃, Zone 5 of the barrel 5: 190℃, condenser core temperature: 160-170℃, Die Zone 1: 180-190℃, Die Zone 2: 180-190℃.
[0012] The beneficial effects of this invention are: The anti-yellowing edge banding strip of this invention can be widely used in the production of panel furniture, cabinets and bathroom fixtures, interior and exterior decoration, office furniture, and other related fields. Introducing the anti-yellowing additive of this invention into the production process can fundamentally improve the anti-yellowing performance of the edge banding strip and effectively block ultraviolet radiation from corroding the edge banding substrate. The modified corrosion-resistant agent can form a tightly bonded, dense protective system with the edge banding substrate, giving the edge banding strip excellent resistance to chemical corrosion and media erosion, significantly improving its suitability and stability in high-humidity and high-corrosion environments such as kitchens, bathrooms, and balconies. Compared with existing technologies, this invention, through the innovative synergistic combination of the anti-yellowing additive and the modified corrosion-resistant agent, effectively reduces the frequency of product damage and replacement caused by aging, corrosion, and yellowing, significantly extending the product's service life.
[0013] The anti-yellowing agent of this invention first utilizes anhydrous citric acid and cysteine hydrochloride to undergo a condensation cyclization reaction, generating a pyridone structure containing a pyridine ring and a ketone group. This conjugated π-electron system effectively absorbs ultraviolet light. Then, through a thioesterification reaction with allyl mercaptan, a mercaptoester group is generated. This group, in synergistic effect with auxochrome groups containing lone pairs of electrons such as S and N, increases the system's ultraviolet absorption intensity. Subsequently, catechol groups are coordinated and chelated with metal sites on the surface of nano-cerium oxide to achieve chemical grafting modification. Nano-cerium oxide has a small band gap, which is conducive to valence electron transitions, resulting in strong absorption of ultraviolet light in the 200-400 nm wavelength range. It can also reduce ultraviolet transmission through scattering and reflection. Furthermore, it has a free radical scavenging effect, which can eliminate free radicals that cause oxidative breakage or cross-linking of polymer chains, thus inhibiting yellowing. Finally, by utilizing the in-situ polymerization reaction on the surface of nano-cerium oxide, the introduced benzophenone structure can absorb ultraviolet light in the range of 290-400nm, preventing the photo-oxidation reaction of double bonds in the ABS molecular chain caused by ultraviolet light, thereby inhibiting yellowing. By copolymerizing and grafting it with the pyridone structure onto the surface of nano-cerium oxide, it is beneficial to reduce the phenomenon of easy migration of organic additives and easy aggregation of inorganic particles, and significantly improve the long-term resistance to yellowing and the compatibility with the matrix.
[0014] The modified corrosion resistant agent of this invention first utilizes an esterification reaction between 3,5-diaminobenzoic acid and perfluorohexylethyl alcohol. The introduced perfluoroalkyl group possesses extremely strong CF bonds, endowing the system with high chemical stability, making it difficult to be corroded by acids, alkalis, oxidants, etc. In addition, the perfluoroalkyl group has extremely low surface energy, which can form hydrophobic and oleophobic surfaces, preventing corrosive liquids from wetting and penetrating the material surface, thus enhancing the material's corrosion resistance. Finally, an amide polymerization reaction is used to generate polyamide containing a large number of polar amide bonds, which can interact with the polar cyano groups in ABS to form a certain degree of compatibility interface, improving the overall resistance of the material to acid and alkali environments. The fluorene group has a large-volume, rigid tricyclic condensed aromatic hydrocarbon structure, which can strengthen the compactness and thermal stability of the polyamide chain. Synergistically acting with the perfluoroalkyl group, it endows the material with the advantages of long-term corrosion resistance, no precipitation, and no loss of the mechanical properties of the matrix. Detailed Implementation
[0015] The technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0016] Example 1: The yellowing resistance additive was prepared by the following steps: Step A1: Mix anhydrous citric acid, cysteine hydrochloride, and deionized water to obtain a mixture. Place the mixture in a beaker and shake it in an 80℃ drying oven for 30 min, then dry it for 1.5 h. After that, place it in a 130℃ forced-air drying oven for 12 h. After the reaction is complete, cool it to room temperature, add deionized water, stir for 15 min, filter under reduced pressure, wash, and vacuum dry to obtain intermediate product 1. The volume ratio of the mixture to deionized water is 6 mL: 150 mL, and the volume ratio of anhydrous citric acid, cysteine hydrochloride, and deionized water in the mixture is 0.1 mol: 0.1 mol: 6 mL. Step A2: In a glove box, potassium phosphate, 18-crown-6, type 4A molecular sieve, and tetrahydrofuran are mixed and placed in a closed reaction system. Polymethylhydrosiloxane, allyl mercaptan, and intermediate product 1 are added. The reaction mixture is stirred and refluxed for 12 hours. Ethyl acetate is added, filtered, distilled under reduced pressure, and purified to obtain intermediate product 2. The ratio of potassium phosphate, 18-crown-6, type 4A molecular sieve, tetrahydrofuran, polymethylhydrosiloxane, allyl mercaptan, intermediate product 1, and ethyl acetate is 0.4 g: 1 g: 0.8 g: 130 mL: 9 mL: 0.02 mol: 0.06 mol: 100 mL. Step A3: Mix nano-cerium oxide powder and 10wt% ethanol aqueous solution to obtain mixture 1. Mix 4-allyl catechol and 10wt% ethanol aqueous solution to obtain mixture 2. Mix mixture 1 and mixture 2, sonicate for 40 min, add acetic acid solution dropwise under stirring, adjust the pH of the system to 6, heat to 50℃ and react for 10 h, cool to room temperature, centrifuge, wash, dry and grind to obtain intermediate product 3. The ratio of nano-cerium oxide powder to ethanol aqueous solution in mixture 1 is 1 g: 100 mL, and the ratio of 4-allyl catechol to ethanol aqueous solution in mixture 2 is 0.01 mol: 450 mL. Step A4: Add intermediate product 3 to cyclohexane, stir for 30 min, then sonicate for 30 min, add intermediate product 2 and 2-hydroxy-4-(isobutenoyloxy)benzophenone, place in an oil bath and heat to 80℃, stir, add 2 / 3 part of benzoyl peroxide, add 1 / 3 part of benzoyl peroxide after 2 h, continue stirring and react for 7 h, pour the product into anhydrous ethanol, stir for 30 min, wash and vacuum dry to obtain the anti-yellowing agent. The ratio of intermediate product 3, cyclohexane, intermediate product 2, 2-hydroxy-4-(isobutenoyloxy)benzophenone, benzoyl peroxide and anhydrous ethanol is 0.4 g: 30 mL: 0.01 mol: 0.01 mol: 0.4 g: 50 mL.
[0017] The modified corrosion resistant agent is prepared by the following steps: Step B1: Mix 3,5-diaminobenzoic acid, perfluorohexylethyl alcohol, p-toluenesulfonic acid, and toluene, stir and heat to 140°C, reflux until no obvious water droplets are formed. After the reaction is complete, add ethyl acetate, wash with 10wt% sodium bicarbonate solution, and then wash successively with deionized water and saturated sodium chloride solution. Separate the contents, dry, filter, distill under reduced pressure, and dry to obtain the diamino perfluorinated derivative. The ratio of 3,5-diaminobenzoic acid, perfluorohexylethyl alcohol, p-toluenesulfonic acid, toluene, ethyl acetate, sodium bicarbonate solution, deionized water, and saturated sodium chloride solution is 0.1mol:0.095mol:0.01mol:150mL:200mL:300mL:300mL; Step B2: Under nitrogen protection, the diamino perfluorinated derivative, 2,7-diamino-9-fluorenone, and N,N-dimethylacetamide were mixed and stirred for 30 min. The temperature was lowered to 0℃, and isophthaloyl chloride was added in four portions over 20 min. After the last addition, the stirring speed was increased until the rod-climbing effect occurred. Then, the mixture was heated to 60℃ and stirred under nitrogen for 1 h. Finally, calcium hydroxide was added and stirred for 15 min. The mixture was washed and dried to obtain the modified corrosion resistant agent. The ratio of the diamino perfluorinated derivative, 2,7-diamino-9-fluorenone, N,N-dimethylacetamide, isophthaloyl chloride, and calcium hydroxide was 0.01 mol: 0.08 mol: 90 mL: 0.1 mol: 0.1 mol.
[0018] Example 2: The yellowing resistance agent was prepared by the following steps: Step A1: Mix anhydrous citric acid, cysteine hydrochloride, and deionized water to obtain a mixture. Place the mixture in a beaker and shake it in an 80℃ drying oven for 30 min, then dry it for 1.5 h. After that, place it in a 130℃ forced-air drying oven for 12 h. After the reaction is complete, cool it to room temperature, add deionized water, stir for 15 min, filter under reduced pressure, wash, and vacuum dry to obtain intermediate product 1. The ratio of the mixture to deionized water is 12 mL: 225 mL, and the ratio of anhydrous citric acid, cysteine hydrochloride, and deionized water in the mixture is 0.2 mol: 0.2 mol: 12 mL. Step A2: In a glove box, potassium phosphate, 18-crown-6, type 4A molecular sieve, and tetrahydrofuran are mixed and placed in a closed reaction system. Polymethylhydrosiloxane, allyl mercaptan, and intermediate product 1 are added. The reaction mixture is stirred and refluxed for 12 hours. Ethyl acetate is added, filtered, distilled under reduced pressure, and purified to obtain intermediate product 2. The ratio of the amounts of potassium phosphate, 18-crown-6, type 4A molecular sieve, tetrahydrofuran, polymethylhydrosiloxane, allyl mercaptan, intermediate product 1, and ethyl acetate is 0.5 g: 1.25 g: 1 g: 160 mL: 11.5 mL: 0.025 mol: 0.0075 mol: 110 mL. Step A3: Mix nano-cerium oxide powder and 10wt% ethanol aqueous solution to obtain mixture 1. Mix 4-allyl catechol and 10wt% ethanol aqueous solution to obtain mixture 2. Mix mixture 1 and mixture 2, sonicate for 40 min, add acetic acid solution dropwise under stirring, adjust the pH of the system to 6, heat to 50℃ and react for 10 h, cool to room temperature, centrifuge, wash, dry and grind to obtain intermediate product 3. The ratio of nano-cerium oxide powder to ethanol aqueous solution in mixture 1 is 1 g: 100 mL, and the ratio of 4-allyl catechol to ethanol aqueous solution in mixture 2 is 0.02 mol: 550 mL. Step A4: Add intermediate product 3 to cyclohexane, stir for 30 min, then sonicate for 30 min. Add intermediate product 2 and 2-hydroxy-4-(isobutenoyloxy)benzophenone, place in an oil bath and heat to 80℃, stir, add 2 / 3 part of benzoyl peroxide, add 1 / 3 part of benzoyl peroxide after 2 h, continue stirring and react for 7 h, pour the product into anhydrous ethanol, stir for 30 min, wash and vacuum dry to obtain the anti-yellowing agent. The ratio of intermediate product 3, cyclohexane, intermediate product 2, 2-hydroxy-4-(isobutenoyloxy)benzophenone, benzoyl peroxide and anhydrous ethanol is 0.4 g: 45 mL: 0.015 mol: 0.015 mol: 0.45 g: 55 mL.
[0019] The modified corrosion resistant agent is prepared by the following steps: Step B1: Mix 3,5-diaminobenzoic acid, perfluorohexylethyl alcohol, p-toluenesulfonic acid, and toluene, stir and heat to 140°C, reflux until no obvious water droplets are formed. After the reaction is complete, add ethyl acetate, wash with 10wt% sodium bicarbonate solution, then wash with deionized water and saturated sodium chloride solution in sequence, separate the contents, dry, filter, distill under reduced pressure, and dry to obtain the diamino perfluorinated derivative. The ratio of 3,5-diaminobenzoic acid, perfluorohexylethyl alcohol, p-toluenesulfonic acid, toluene, ethyl acetate, sodium bicarbonate solution, deionized water, and saturated sodium chloride solution is 0.2mol:0.19mol:0.02mol:250mL:250mL:350mL:300mL:300mL. Step B2: Under nitrogen protection, the diamino perfluorinated derivative, 2,7-diamino-9-fluorenone, and N,N-dimethylacetamide were mixed and stirred for 30 min. The temperature was lowered to 0℃, and isophthaloyl chloride was added in four portions over 20 min. After the last addition, the stirring speed was increased until the rod-climbing effect occurred. Then, the mixture was heated to 60℃ and stirred under nitrogen for 1 h. Finally, calcium hydroxide was added and stirred for 15 min. The mixture was washed and dried to obtain the modified corrosion resistant agent. The ratio of the diamino perfluorinated derivative, 2,7-diamino-9-fluorenone, N,N-dimethylacetamide, isophthaloyl chloride, and calcium hydroxide was 0.015 mol: 0.085 mol: 110 mL: 0.105 mol: 0.105 mol.
[0020] Example 3: The yellowing resistance additive was prepared by the following steps: Step A1: Mix anhydrous citric acid, cysteine hydrochloride, and deionized water to obtain a mixture. Place the mixture in a beaker and shake it in an 80℃ drying oven for 30 min, then dry it for 1.5 h. After that, place it in a 130℃ forced-air drying oven for 12 h. After the reaction is complete, cool it to room temperature, add deionized water, stir for 15 min, filter under reduced pressure, wash, and vacuum dry to obtain intermediate product 1. The ratio of the mixture to deionized water is 18 mL: 300 mL, and the ratio of anhydrous citric acid, cysteine hydrochloride, and deionized water in the mixture is 0.3 mol: 0.3 mol: 18 mL. Step A2: In a glove box, potassium phosphate, 18-crown-6, type 4A molecular sieve, and tetrahydrofuran are mixed and placed in a closed reaction system. Polymethylhydrosiloxane, allyl mercaptan, and intermediate product 1 are added. The reaction mixture is stirred and refluxed for 12 hours. Ethyl acetate is added, filtered, distilled under reduced pressure, and purified to obtain intermediate product 2. The ratio of potassium phosphate, 18-crown-6, type 4A molecular sieve, tetrahydrofuran, polymethylhydrosiloxane, allyl mercaptan, intermediate product 1, and ethyl acetate is 0.6 g: 1.5 g: 1.2 g: 190 mL: 14 mL: 0.03 mol: 0.09 mol: 120 mL. Step A3: Mix nano-cerium oxide powder and 10wt% ethanol aqueous solution to obtain mixture 1. Mix 4-allyl catechol and 10wt% ethanol aqueous solution to obtain mixture 2. Mix mixture 1 and mixture 2, sonicate for 40 min, add acetic acid solution dropwise under stirring, adjust the pH of the system to 6, heat to 50℃ and react for 10 h, cool to room temperature, centrifuge, wash, dry and grind to obtain intermediate product 3. The ratio of nano-cerium oxide powder to ethanol aqueous solution in mixture 1 is 1 g: 100 mL, and the ratio of 4-allyl catechol to ethanol aqueous solution in mixture 2 is 0.03 mol: 650 mL. Step A4: Add intermediate product 3 to cyclohexane, stir for 30 min, then sonicate for 30 min. Add intermediate product 2 and 2-hydroxy-4-(isobutenoyloxy)benzophenone, place in an oil bath and heat to 80℃, stir, add 2 / 3 part of benzoyl peroxide, add 1 / 3 part of benzoyl peroxide after 2 h, continue stirring and react for 7 h, pour the product into anhydrous ethanol, stir for 30 min, wash and vacuum dry to obtain the anti-yellowing agent. The ratio of intermediate product 3, cyclohexane, intermediate product 2, 2-hydroxy-4-(isobutenoyloxy)benzophenone, benzoyl peroxide and anhydrous ethanol is 0.4 g: 60 mL: 0.02 mol: 0.02 mol: 0.5 g: 60 mL.
[0021] The modified corrosion resistant agent is prepared by the following steps: Step B1: Mix 3,5-diaminobenzoic acid, perfluorohexylethyl alcohol, p-toluenesulfonic acid, and toluene, stir and heat to 140°C, reflux until no obvious water droplets are formed. After the reaction is complete, add ethyl acetate, wash with 10wt% sodium bicarbonate solution, and then wash successively with deionized water and saturated sodium chloride solution. Separate, dry, filter, distill under reduced pressure, and dry to obtain the diamino perfluorinated derivative. The ratio of 3,5-diaminobenzoic acid, perfluorohexylethyl alcohol, p-toluenesulfonic acid, toluene, ethyl acetate, sodium bicarbonate solution, deionized water, and saturated sodium chloride solution is 0.3mol:0.285mol:0.03mol:350mL:300mL:400mL:300mL:300mL. Step B2: Under nitrogen protection, the diamino perfluorinated derivative, 2,7-diamino-9-fluorenone, and N,N-dimethylacetamide were mixed and stirred for 30 min. The temperature was lowered to 0℃, and isophthaloyl chloride was added in four portions over 20 min. After the last addition, the stirring speed was increased until the rod-climbing effect occurred. Then, the mixture was heated to 60℃ and stirred under nitrogen for 1 h. Finally, calcium hydroxide was added and stirred for 15 min. The mixture was washed and dried to obtain the modified corrosion resistant agent. The ratio of the diamino perfluorinated derivative, 2,7-diamino-9-fluorenone, N,N-dimethylacetamide, isophthaloyl chloride, and calcium hydroxide was 0.02 mol: 0.09 mol: 130 mL: 0.11 mol: 0.11 mol.
[0022] Example 4: A production process for a yellowing-resistant edge banding strip, comprising the following steps: 80 parts ABS resin, 20 parts nano calcium carbonate, 0.5 parts CPE resin, 1 part ACR resin, 1 part of the yellowing resistance additive prepared in Example 1, 0.5 parts antioxidant 1010, 4 parts calcium stearate, 0.4 parts paraffin, 0.5 parts silane coupling agent KH-550, and 2 parts modified corrosion resistant agent prepared in Example 1. Step S1: Weigh the raw materials according to the weight parts, and mix ABS resin, nano calcium carbonate, CPE resin, ACR resin, anti-yellowing additive prepared in Example 1, antioxidant 1010, calcium stearate, paraffin wax, silane coupling agent KH-550 and modified corrosion resistant agent prepared in Example 1. Mix at 800 r / min for 20 min to obtain a mixture. Step S2: The mixture is fed into a twin-screw extruder for extrusion, cooled and solidified to obtain a yellowing-resistant edge sealing strip. The operating parameters of the extruder are: barrel zone 1 180℃, barrel zone 2 182℃, barrel zone 3 185℃, barrel zone 4 188℃, barrel zone 5 190℃, confluence core temperature 160℃, die zone 1 180℃, and die zone 2 180℃.
[0023] Example 5: A production process for a yellowing-resistant edge banding strip, comprising the following steps: 90 parts ABS resin, 25 parts nano calcium carbonate, 1 part CPE resin, 1.5 parts ACR resin, 2 parts of the yellowing resistance additive prepared in Example 2, 0.5 parts antioxidant 1098, 5 parts zinc stearate, 0.6 parts polyethylene wax, 0.5 parts silane coupling agent KH-550, and 4 parts modified corrosion resistant agent prepared in Example 2. Step S1: Weigh the raw materials according to the weight parts, and mix ABS resin, nano calcium carbonate, CPE resin, ACR resin, anti-yellowing additive prepared in Example 2, antioxidant 1098, zinc stearate, polyethylene wax, silane coupling agent KH-550 and modified corrosion resistant agent prepared in Example 2. Mix at 1000 r / min for 30 min to obtain a mixture. Step S2: The mixture is fed into a twin-screw extruder for extrusion, cooled and solidified to obtain a yellowing-resistant edge sealing strip. The operating parameters of the extruder are: barrel zone 1 182℃, barrel zone 2 184℃, barrel zone 3 186℃, barrel zone 4 188℃, barrel zone 5 190℃, confluence core temperature 165℃, die zone 1 185℃, and die zone 2 190℃.
[0024] Example 6: A production process for a yellowing-resistant edge banding strip, comprising the following steps: 100 parts ABS resin, 30 parts nano calcium carbonate, 2 parts CPE resin, 2 parts ACR resin, 4 parts of the yellowing resistance additive prepared in Example 3, 0.5 parts antioxidant 1010, 0.5 parts antioxidant 1098, 3 parts calcium stearate, 4 parts zinc stearate, 0.4 parts oxidized polyethylene wax, 0.4 parts stearic acid, 1 part silane coupling agent KH-550, and 5 parts modified corrosion resistant agent prepared in Example 3; Step S1: Weigh the raw materials according to the weight parts, and mix ABS resin, nano calcium carbonate, CPE resin, ACR resin, anti-yellowing additive prepared in Example 3, antioxidant 1010, antioxidant 1098, calcium stearate, zinc stearate, oxidized polyethylene wax, stearic acid, silane coupling agent KH-550 and modified corrosion resistant agent prepared in Example 3. Mix at 1500 r / min for 40 min to obtain a mixture. Step S2: The mixture is fed into a twin-screw extruder for extrusion, cooled and solidified to obtain a yellowing-resistant edge sealing strip. The operating parameters of the extruder are: barrel zone 1 183℃, barrel zone 2 185℃, barrel zone 3 186℃, barrel zone 4 189℃, barrel zone 5 190℃, confluence core temperature 170℃, die zone 1 190℃, and die zone 2 190℃.
[0025] Comparative Example 1: This comparative example is an edge sealing strip. The difference between this example and Example 6 is that nano-cerium oxide is used instead of the anti-yellowing agent prepared in Example 3. All other aspects are the same.
[0026] Comparative Example 2: This comparative example is an edge sealing strip, which differs from Example 6 in that polyamide is used instead of the modified corrosion resistant agent prepared in Example 3, and all other aspects are the same.
[0027] Comparative Example 3: This comparative example is an edge sealing strip. The difference between it and Example 6 is that nano-cerium oxide is used instead of the anti-yellowing agent prepared in Example 3, and polyamide is used instead of the modified corrosion resistant agent prepared in Example 3. All other aspects are the same.
[0028] The edge banding strips prepared in Examples 4-6 and Comparative Examples 1-3 were subjected to performance tests: Tensile strength: The tensile strength was obtained by referring to the standard ASTM D638, and the result was the average of 10 parallel tests. Bending strength: The bending strength was obtained by referring to the standard ASTM D790, and the result was the average of 10 parallel tests. Notched impact strength: The notched impact strength of the cantilever beam was obtained with reference to the standard ASTM D256. The result was the average of 10 parallel tests. Yellowing resistance test: According to the test method of yellow index of plastics in HG / T 3862-2006, the yellow index was measured to obtain the yellowing index △YI; Corrosion resistance test: The edge banding sample was placed in a 40wt% sodium hydroxide solution and a 30wt% hydrochloric acid solution and placed in a constant temperature and humidity chamber for 90 days. The mass of the sample before and after the experiment was weighed and the percentage change in weight before and after the experiment was calculated.
[0029] The test results are shown in Table 1: Table 1: Performance Test Results
[0030] As can be seen from Table 1, the anti-yellowing edge banding prepared by this invention possesses excellent mechanical properties. The tensile strength of the edge banding prepared in the examples is all above 44.7 MPa, and the notched impact strength is above 25.8 KJ / m. 2 The bending strength is above 47.7 MPa. As shown in Example 6 and Comparative Example 1, the anti-yellowing additive prepared by this invention improves the UV absorption capacity of the ABS matrix and reduces the change in the yellowing index of the material. Comparative Example 6 and Comparative Example 2 show that the modified corrosion resistant agent prepared by this invention improves the stability of the ABS matrix in acidic and alkaline environments, which is beneficial to the stability of the edge banding strip in daily use. This demonstrates that the anti-yellowing edge banding strip of this invention has good mechanical properties, anti-yellowing properties, and corrosion resistance.
[0031] The above content is merely an example and illustration of the concept of the present invention. Those skilled in the art can make various modifications or additions to the specific embodiments described or use similar methods to replace them, as long as they do not deviate from the scope defined by the inventive concept, they should all fall within the protection scope of the present invention.
Claims
1. A yellowing-resistant edge banding strip, characterized in that, The raw materials include the following parts by weight: 80-100 parts ABS resin, 20-30 parts nano calcium carbonate, 0.5-2 parts CPE resin, 1-2 parts ACR resin, 1-4 parts anti-yellowing agent, 0.5-1 part antioxidant, 4-7 parts heat stabilizer, 0.4-0.8 parts lubricant, 0.5-1 part silane coupling agent KH-550, and 2-5 parts modified corrosion resistant agent; The anti-yellowing agent is prepared by the following steps: Step A1: Mix anhydrous citric acid, cysteine hydrochloride and deionized water to obtain a mixture. Place the mixture in a beaker and shake it in an 80°C drying oven for 30 min. Dry for 1.5 h and then place it in a 130°C forced-air drying oven for 12 h. After the reaction is complete, cool to room temperature, add deionized water, stir for 15 min, filter under reduced pressure, wash and vacuum dry to obtain intermediate product 1. Step A2: In a glove box, potassium phosphate, 18-crown-6, type 4A molecular sieve and tetrahydrofuran are mixed and placed in a closed reaction system. Polymethylhydrosiloxane, allyl mercaptan and intermediate product 1 are added. The reaction mixture is stirred and refluxed for 12 hours. Ethyl acetate is added, filtered, distilled under reduced pressure and purified to obtain intermediate product 2. Step A3: Mix nano-cerium oxide powder with 10wt% ethanol aqueous solution to obtain mixture 1. Mix 4-allylcatechol with 10wt% ethanol aqueous solution to obtain mixture 2. Mix mixture 1 and mixture 2, sonicate for 40 min, add acetic acid solution dropwise under stirring to adjust the pH of the system to 6, heat to 50℃ and react for 10 h, cool to room temperature, centrifuge, wash, dry and grind to obtain intermediate product 3. Step A4: Add intermediate product 3 to cyclohexane, stir for 30 min, then sonicate for 30 min, add intermediate product 2 and 2-hydroxy-4-(isobutenoyloxy)benzophenone, place in an oil bath and heat to 80°C, stir, add 2 / 3 part of benzoyl peroxide, add 1 / 3 part of benzoyl peroxide after 2 h, continue stirring and react for 7 h, pour the product into anhydrous ethanol, stir for 30 min, wash and vacuum dry to obtain the anti-yellowing agent.
2. The anti-yellowing edge banding strip according to claim 1, characterized in that, In step A1, the ratio of the mixture to deionized water is 6-18 mL: 150-300 mL, and the ratio of anhydrous citric acid, cysteine hydrochloride, and deionized water in the mixture is 0.1-0.3 mol: 0.1-0.3 mol: 6-18 mL.
3. The anti-yellowing edge banding strip according to claim 1, characterized in that, In step A2, the ratio of potassium phosphate, 18-crown-6, type 4A molecular sieve, tetrahydrofuran, polymethylhydrosiloxane, allyl mercaptan, intermediate product 1, and ethyl acetate is 0.4-0.6g: 1-1.5g: 0.8-1.2g: 130-190mL: 9-14mL: 0.02-0.03mol: 0.06-0.09mol: 100-120mL.
4. The anti-yellowing edge banding strip according to claim 1, characterized in that, In step A3, the ratio of nano-cerium oxide powder to ethanol aqueous solution in mixture 1 is 1g:100mL, and the ratio of 4-allylcatechol to ethanol aqueous solution in mixture 2 is 0.01-0.03mol:450-650mL.
5. The anti-yellowing edge banding strip according to claim 1, characterized in that, In step A4, the ratio of intermediate product 3, cyclohexane, intermediate product 2, 2-hydroxy-4-(isobutenoyloxy)benzophenone, benzoyl peroxide, and anhydrous ethanol is 0.4g: 30-60mL: 0.01-0.02mol: 0.01-0.02mol: 0.4-0.5g: 50-60mL.
6. The anti-yellowing edge banding strip according to claim 1, characterized in that, The modified corrosion resistant agent is prepared by the following steps: Step B1: Mix 3,5-diaminobenzoic acid, perfluorohexylethyl alcohol, p-toluenesulfonic acid and toluene, stir and heat to 140°C, reflux until no obvious water droplets are formed, after the reaction is complete, add ethyl acetate, wash with 10wt% sodium bicarbonate solution, then wash with deionized water and saturated sodium chloride solution in turn, separate the liquid, dry, filter, distill under reduced pressure and dry to obtain the diamino perfluorinated derivative; Step B2: Under nitrogen protection, the diamino perfluorinated derivative, 2,7-diamino-9-fluorenone, and N,N-dimethylacetamide are mixed and stirred for 30 min. The temperature is then lowered to 0°C, and isophthaloyl chloride is added in four portions over 20 min. After the last addition, the stirring speed is increased until the rod-climbing effect occurs. The mixture is then heated to 60°C and stirred under nitrogen for 1 h. Finally, calcium hydroxide is added and stirred for 15 min. The mixture is then washed and dried to obtain the modified corrosion resistant agent.
7. The anti-yellowing edge banding strip according to claim 6, characterized in that, In step B1, the ratio of the amounts of 3,5-diaminobenzoic acid, perfluorohexylethyl alcohol, p-toluenesulfonic acid, toluene, ethyl acetate, sodium bicarbonate solution, deionized water, and saturated sodium chloride solution is 0.1-0.3 mol: 0.095-0.285 mol: 0.01-0.03 mol: 150-350 mL: 200-300 mL: 300-400 mL: 300 mL: 300 mL.
8. The anti-yellowing edge banding strip according to claim 6, characterized in that, In step B2, the ratio of the amount of the diamino perfluorinated derivative, 2,7-diamino-9-fluorenone, N,N-dimethylacetamide, isophthaloyl chloride, and calcium hydroxide is 0.01-0.02 mol: 0.08-0.09 mol: 90-130 mL: 0.1-0.11 mol: 0.1-0.11 mol.
9. The anti-yellowing edge banding strip according to claim 1, characterized in that, The antioxidant is at least one of antioxidant 1010 and antioxidant 1098, the heat stabilizer is at least one of calcium stearate and zinc stearate, and the lubricant is at least one of paraffin wax, polyethylene wax, oxidized polyethylene wax, and stearic acid.
10. A manufacturing process for the anti-yellowing edge banding strip according to any one of claims 1-9, characterized in that, Includes the following steps: Step S1: Weigh the raw materials according to the weight parts, and mix ABS resin, nano calcium carbonate, CPE resin, ACR resin, anti-yellowing agent, antioxidant, heat stabilizer, lubricant, silane coupling agent KH-550 and modified corrosion resistant agent, and mix at 800-1500 r / min for 20-40 min to obtain a mixture; Step S2: The mixture is fed into a twin-screw extruder for extrusion, cooled and solidified to obtain a yellowing-resistant edge sealing strip. The operating parameters of the extruder are as follows: Zone 1 of the barrel 1: 180-190℃, Zone 2 of the barrel 2: 180-190℃, Zone 3 of the barrel 3: 180-190℃, Zone 4 of the barrel 4: 180-190℃, Zone 5 of the barrel 5: 190℃, condenser core temperature: 160-170℃, Die Zone 1: 180-190℃, Die Zone 2: 180-190℃.
Citation Information
Patent Citations
Insulating heat-conducting ABS composite material doped with aluminum nitride and preparation thereof
CN102408663A
Yellowing-resistant PC / ABS (polycarbonate-acrylonitrile-butadiene-styrene) alloy for automobile interior ornaments and preparation method thereof