Fireproof and antistatic corrosion-resistant glass fiber reinforced plastic cable bridge and preparation method thereof

By adding 4-mercapto-N-(2-hydroxy-4-pentadecanylphenyl)benzamide to fiberglass cable trays, and combining it with low-pressure distillation and alternating dielectric electrophoresis technology, the problems of fiberglass aging and ester contamination were solved, and the corrosion resistance and antistatic properties were improved.

CN123152247APending Publication Date: 2026-11-24HEBEI PENGBO FRP CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611305441.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-26
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing fiberglass cable trays are prone to aging in outdoor environments, and amine antioxidants cause ester contamination, affecting strength and corrosion resistance.

Method used

4-Mercapto-N-(2-hydroxy-4-pentadecanylphenyl)benzamide was used as an additive, and the thermal oxidation stability and antistatic properties of fiberglass were improved by low-pressure distillation, catalytic reduction and dynamic control of alternating dielectric field technology.

Benefits of technology

It effectively solves the problem of ester contamination caused by amine antioxidants, improves the thermal oxidation stability and antistatic properties of fiberglass, and enhances its corrosion resistance and toughness in high-temperature environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123152247A_ABST
    Figure CN123152247A_ABST
Patent Text Reader

Abstract

This invention discloses a fireproof, antistatic, and corrosion-resistant fiberglass cable tray and its preparation method, belonging to the field of organic synthesis technology. The preparation method of the fireproof, antistatic, and corrosion-resistant fiberglass cable tray includes using cashew phenol as a raw material, followed by mixed acid nitration, vacuum distillation separation, and using a Pd / C catalyst to reduce nitro groups to amino groups under pressure catalysis, followed by vacuum distillation separation, and electrochemical reduction to continuously reduce sulfonyl chloride to mercapto groups to obtain an additive. The additive is then mixed into uncured fiberglass resin, and an alternating dielectric electrophoresis field is dynamically controlled according to the resin temperature to remove bubbles, followed by demolding to obtain the finished product. This invention overcomes the shortcomings of existing technologies where amine antioxidants in fiberglass easily cause ester contamination, leading to swelling and decreased strength. The resulting product exhibits excellent flexural strength, impact toughness, aging resistance, flame retardancy, and antistatic properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of organic synthesis technology, and in particular to a fireproof, antistatic, and corrosion-resistant fiberglass cable tray and its preparation method. Background Technology

[0002] Fire-resistant, anti-static, and corrosion-resistant fiberglass cable trays are cable laying devices that combine the rigidity of metal cable trays with the toughness of fiberglass cable trays. They are commonly used in outdoor environments. However, under prolonged outdoor exposure to sunlight, air oxidation, and high temperatures, fiberglass cable trays are prone to aging. When the resin fully absorbs ultraviolet light, the covalent bonds in the resin break, generating free radicals. These free radicals continue to damage the resin, increasing the brittleness of the fiberglass.

[0003] Currently, to address the issue of fiberglass aging under prolonged outdoor exposure to sunlight, air oxidation, and high temperatures, amine antioxidants are typically added. Amine antioxidants, as derivatives of aromatic secondary amines, mainly include diaryl secondary amines, p-phenylenediamine, and aldehyde amines. These antioxidants have good antioxidant effects, but they produce esters during the antioxidant process, leading to ester contamination of the fiberglass. As ester contamination worsens, the fiberglass will swell, thus affecting its strength.

[0004] This invention provides an additive that effectively solves the problem of ester contamination caused by amine antioxidants, while simultaneously improving the thermal oxidation stability of fiberglass. Therefore, developing a sulfur-containing additive to address the ester contamination problem caused by adding amine antioxidants to fire-resistant, anti-static, and corrosion-resistant fiberglass cable trays is of great significance. Summary of the Invention

[0005] The purpose of this invention is to overcome the shortcomings of existing technologies by proposing a fireproof, antistatic, and corrosion-resistant fiberglass cable tray and its preparation method.

[0006] To achieve the above objectives, the present invention adopts the following technical solution:

[0007] A fireproof, antistatic, and corrosion-resistant fiberglass cable tray comprises the following raw materials: 100-120 parts by weight of phenolic resin, 8-10 parts by weight of 4-mercapto-N-(2-hydroxy-4-pentadecanylphenyl)benzamide, 5-8 parts by weight of aluminum hydroxide, and 3-4 parts by weight of benzenesulfonyl chloride;

[0008] The specific preparation method of the 4-mercapto-N-(2-hydroxy-4-pentadecanophenyl)benzamide is as follows:

[0009] S1: Place cashew phenol in mixed acid and heat to 90℃ for 30 min to obtain nitrated cashew phenol. Heat the nitrated cashew phenol to 150-160℃ under a nitrogen atmosphere of 0.1-0.2 kPa and distill to constant weight. Collect the distillate, add Pd / C catalyst to the distillate and react for 2 hours under a catalytic atmosphere of 0.3-0.5 MPa and 40-60℃ to obtain a mixture of 6-aminocainol and 2-aminocainol.

[0010] S2: Aminocainol is distilled under reduced pressure under nitrogen protection, heated to 180~190℃ and purified to constant weight, and the distillate is collected to obtain 6-aminocainol. 6-aminocainol and 4-(chlorosulfonyl)benzoyl chloride are reacted at 0~25℃ in a molar ratio of 1:(1~1.1) for 3 hours to obtain amidated cashewol.

[0011] S3: Add 20-30% by mass of amidated cashew phenol to an ethanol mixed solvent containing 0.2-0.6M H2SO4, stir thoroughly, and add 0.05-0.2M tetrabutylammonium perchlorate to make the electrolyte concentration 0.03-0.12M. Continue stirring for 2 hours in an Ag / AgCl electrolytic cell with lead electrode, control the electrode potential and continue the reaction for 30 minutes. Filter and wash with anhydrous ethanol to obtain 4-mercapto-N-(2-hydroxy-4-pentadecanylphenyl)benzamide additive.

[0012] Preferably, the cashew phenol is a meta-phenol containing a 15-saturated carbon chain; the Pd / C catalyst is a palladium catalyst supported on activated carbon, with a palladium content of 10-15%.

[0013] Preferably, the mixed acid is obtained by uniformly mixing 2M nitric acid and 2M sulfuric acid in a volume ratio of (3~3.5):(1~1.5).

[0014] Preferably, the catalytic atmosphere is an atmosphere in which nitrogen and hydrogen are mixed in a volume ratio of (6~7.5):(2.5~3).

[0015] Preferably, the catalytic atmosphere is an atmosphere in which nitrogen and hydrogen are mixed in a volume ratio of (6~7.5):(2.5~3).

[0016] Preferably, the vacuum distillation under nitrogen protection described in S2 is carried out in a nitrogen atmosphere of 0.1~0.2 kPa.

[0017] Preferably, the electrode potential in S3 has a voltage of 2~2.5V and a current density of 10~20mA / cm. 2 .

[0018] Preferably, in step S1, cashew phenol is placed in a mixed acid and heated for 30 minutes to generate 2-nitro cashew phenol, 4-nitro cashew phenol, and 6-nitro cashew phenol. Due to steric hindrance, the yield of 6-nitro cashew phenol is 52-61%, the yield of 4-nitro cashew phenol is 32-35%, and the yield of 2-nitro cashew phenol is 1-2%.

[0019] Preferably, heating nitrated cashew phenol to 150-160°C at 0.1-0.2 kPa effectively removes 4-nitro cashew phenol. Distillation under normal pressure requires heating nitrated cashew phenol to a temperature above 200°C. At high temperatures, the long carbon chain of cashew phenol is unstable and easily breaks, producing a large number of byproducts and impurities. In 4-nitro cashew phenol, the nitro group is located at the para position of the phenolic hydroxyl group and the ortho position of the straight-chain alkyl group. With the same substituents and substitution numbers, the para-substituted benzene has higher molecular symmetry, tighter and more orderly intermolecular arrangement, and stronger intermolecular interactions, resulting in a relatively higher boiling point for 4-nitro cashew phenol.

[0020] Preferably, in step S2, aminocainol is distilled under a nitrogen atmosphere of 0.1~0.2 kPa at 180~190°C, and the distillate is collected as 6-aminocainol. Distillation under a nitrogen atmosphere with reflux can effectively avoid the oxidative decomposition of the product and reduce by-products. The amino group of 2-aminocainol is located between the phenolic hydroxyl group and the long straight alkyl group. The amino group forms an intramolecular hydrogen bond with both functional groups, which significantly increases the boiling point of phenol. The amino group of 6-aminocainol forms a hydrogen bond with the hydroxyl group only within the molecule. The boiling point of 6-aminocainol is significantly lower than that of 2-aminocainol.

[0021] Preferably, the sulfonyl chloride in S3 undergoes four consecutive reduction steps to generate sulfinic acid, thiosulfinic acid ester and disulfide in sequence. Finally, the disulfide is further reduced to the target product thiol by gaining 2 electrons. The added sulfuric acid provides the protons required for the electrochemical reaction.

[0022] Preferably, the additive is an organic compound containing thiol groups, straight-chain alkyl groups, and amides. The longer straight-chain alkyl groups provide a certain degree of toughness, significantly improving compressive strength and flexural strength when added to phenolic resin. The amide groups in the additive have high temperature resistance and good heat aging resistance in outdoor high-temperature applications. The thiol groups in the additive react with the ester groups generated by the anti-aging agent to form thioester bonds under high-temperature outdoor irradiation, effectively solving the problems of ester pollution and ester swelling caused by the anti-aging agent. At the same time, the generated thioester bonds have certain chemical resistance and corrosion resistance. The polar sulfur atoms in the thioester bonds have good surface activity and can form a stable chemical adsorption film on the glass fiber surface, improving the load-bearing capacity of the fiberglass.

[0023] Preferably, the thiol group in the additive molecule also acts as a free radical scavenging group, which can rapidly couple with the peroxide free radicals and alkoxy free radicals generated in the fiberglass resin matrix during thermo-oxidative aging to form stable sulfides or disulfides, thereby interrupting the free radical chain transmission and delaying the oxidative degradation of the resin matrix.

[0024] Furthermore, a method for preparing a fireproof, antistatic, and corrosion-resistant fiberglass cable tray specifically includes the following steps:

[0025] (1) Mix 100-120 parts by weight of phenolic resin with 8-10 parts by weight of additives thoroughly, then add 5-8 parts by weight of aluminum hydroxide and 3-4 parts by weight of benzenesulfonyl chloride in sequence, and stir thoroughly for 5-10 minutes to obtain resin solution.

[0026] (2) Apply release agent to the embedded electrode mold in sequence, then apply phenolic resin liquid containing additives and alkali-free glass fiber cloth. Use a roller to make the resin liquid fully penetrate the glass fiber cloth. The resin coating is controlled to be 1cm and repeated for 5 layers. Apply an alternating dielectric field at 90~100℃ and perpendicular to the direction of the fiberglass, with a frequency of 1~5MHz and a peak voltage of 100~250V for 30min. Heat the resin to 150~160℃ and apply a pressure of 0.5MPa perpendicular to the surface of the fiberglass for 20min. Demold to obtain fiberglass cable tray.

[0027] Preferably, an alternating dielectric electrophoresis field perpendicular to the fiberglass is applied at 90~100℃. 0.1μm-sized bubbles in the fiberglass agglomerate due to electrothermal convection to form 200~300μm bubbles. When the fiberglass is heated to 150~160℃, the bubbles escape from capillary pores of 3~20μm size and are expelled from the fiberglass under a pressure of 0.5MPa.

[0028] Preferably, the alternating dielectric field dynamically controlled according to resin temperature is applied at 80~120℃ with 100~150V and 3~5MHz; the peak voltage is applied at 50~80℃ with 150~200V and 2~3MHz; and the peak voltage is applied at 30~50℃ with 200~250V and 1~2MHz.

[0029] Preferably, the dielectric constant of the bubbles is ε≈1. The antistatic agent added to the composite resin can effectively increase the dielectric constant of the resin, making the dielectric constant ε of the composite resin 3.5~4.5. In a high-frequency alternating electric field, due to the polarization difference, the bubbles in the non-uniform alternating electric field generate a directional motion force due to polarization. This directional motion force is the dielectric electrophoresis force, which can drive the bubbles with low dielectric constant to move, thereby achieving the effect of removing bubbles from the fiberglass.

[0030] Preferably, the alternating dielectric electrophoresis field contains a real-time impedance module that reduces the voltage when the resin impedance drops sharply.

[0031] Preferably, the curing reaction of the fiberglass system itself is exothermic, and the open tank is laid manually / semi-automatically. Its curing mechanism is a free radical copolymerization reaction, in which free radicals are generated by the decomposition of the initiator, which then initiates chain polymerization. This polymerization is characterized by high speed, concentrated heat release, and large shrinkage rate, which is the main reason for the formation of bubbles. In the actual laying process, the open fiberglass structure with manual coating and semi-automatic laying loses heat quickly during curing, and the temperature difference between the resin surface and the interior is large. This easily leads to the phenomenon that the surface cures first and the internal bubbles cannot escape. Dielectrophoresis is used as a means of bubble removal to achieve defoaming without vacuum assistance.

[0032] Compared with the prior art, the beneficial effects of the present invention are:

[0033] 1. This invention employs a low-pressure distillation method, achieving a yield of 52-61% for 6-nitrocainol, 32-35% for 4-nitrocainol, and 1-2% for 2-nitrocainol in nitrated cashew nut shells. The nitro group in 4-nitrocainol is located para-position to the phenolic hydroxyl group and ortho-position to the aliphatic straight chain. The para-substituted benzene exhibits higher molecular symmetry, tighter and more ordered molecular arrangement, and stronger intermolecular interactions, resulting in a relatively higher boiling point for 4-nitrocainol. This method enables the separation and purification of nitrated cashew nut shells.

[0034] 2. This invention employs a Pd / C catalytic method to convert nitro groups to amino groups, thereby transforming 6-nitro cashew nutshellol and 2-nitro cashew nutshellol into 6-amino cashew nutshellol and 2-amino cashew nutshellol. Since the amino group is located at the ortho position of the phenolic hydroxyl group, it readily forms intramolecular hydrogen bonds. 2-Amino cashew nutshellol, situated between the phenolic hydroxyl group and the aliphatic linear chain, possesses numerous intramolecular hydrogen bonds, resulting in a higher boiling point. The separation of 6-amino cashew nutshellol and 2-amino cashew nutshellol is achieved under a low-pressure nitrogen atmosphere, thus purifying 6-amino cashew nutshellol.

[0035] 3. This invention employs a method of continuous reduction of sulfonyl chloride in an electric field, which causes sulfonyl chloride to sequentially generate sulfinic acid, thiosulfinic ester, and disulfide at the cathode. The disulfide is eventually reduced to thiol, thereby achieving the synthesis of sulfonyl chloride into the target product thiol.

[0036] 4. This invention employs a dynamically controlled alternating dielectric electrophoresis field. Since the dielectric constants of bubbles and resin are different, the polarization difference in the alternating electric field generates a directional motion force, enabling the movement of bubbles with low dielectric constants and achieving the effect of removing bubbles from fiberglass. Attached Figure Description

[0037] Figure 1This is a schematic diagram illustrating the preparation process of a fireproof, antistatic, and corrosion-resistant fiberglass cable tray additive proposed in this invention. Detailed Implementation

[0038] The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with existing known technologies. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments.

[0039] Example 1: A method for preparing a fireproof, antistatic, and corrosion-resistant fiberglass cable tray, comprising the following steps:

[0040] S1: 1.1 mol of cashew phenol was placed in a mixed acid solution of 2M nitric acid and 2M sulfuric acid in a volume ratio of 3:1 and heated to 90°C for 30 min to obtain nitrated cashew phenol. The nitrated cashew phenol was heated to 160°C under a nitrogen atmosphere of 0.1 kPa and distilled to constant weight. The distillate was collected, and 30 g of Pd / C catalyst was added to the distillate and reacted under a catalytic atmosphere of 0.5 MPa and 40°C for 2 hours to obtain a mixture of 6-aminocaucetol and 2-aminocaucetol.

[0041] S2: Amino cashew phenol was distilled under reduced pressure under nitrogen protection at 0.2 kPa, heated to 190 °C and purified to constant weight, and the distillate was collected to obtain 6-amino cashew phenol. 0.7 mol of 4-(chlorosulfonyl)benzoyl chloride was added and stirred for 3 hours to obtain amidated cashew phenol.

[0042] S3: Add 400 mL of a mixed solvent of ethanol containing 1.0 M sulfuric acid to amidated cashew phenol, stir thoroughly, add 600 mL of 0.2 M tetrabutylammonium perchlorate, stir continuously for 2 hours, and in an Ag / AgCl electrolytic cell, control the electrode potential at 2.5 V and continue the reaction for 30 min. Filter and wash with anhydrous ethanol to obtain the additive.

[0043] S4: Mix 100g of phenolic resin with 8g of additive thoroughly, then add 8g of aluminum hydroxide and 3g of benzenesulfonyl chloride in sequence, and stir thoroughly for 5 minutes to obtain resin solution;

[0044] S5: Apply release agent to the embedded electrode mold in sequence, followed by resin adhesive and alkali-free fiberglass cloth. Use a roller to fully saturate the fiberglass cloth with resin adhesive. Control the resin coating to 1cm and repeat the coating 5 times. Apply an alternating dielectric field at 100℃ and perpendicular to the fiberglass direction with a frequency of 2MHz and a peak voltage of 175V for 30 minutes. Heat the resin to 160℃ and apply a pressure of 0.5MPa perpendicular to the fiberglass surface for 20 minutes. Demold to obtain the fiberglass cable tray.

[0045] Example 2: A method for preparing a fireproof, antistatic, and corrosion-resistant fiberglass cable tray, comprising the following steps:

[0046] S1: 1 mol of cashew phenol was placed in a mixed acid solution of 2M nitric acid and 2M sulfuric acid in a volume ratio of 3:1 and heated to 90°C for 30 min to obtain nitrated cashew phenol. The nitrated cashew phenol was heated to 150°C under a nitrogen atmosphere of 0.2 kPa and distilled to constant weight. The distillate was collected, and 25 g of Pd / C catalyst was added to the distillate and reacted under a catalytic atmosphere of 0.3 MPa and 60°C for 2 hours to obtain a mixture of 6-aminocaucetol and 2-aminocaucetol.

[0047] S2: Amino cashew phenol was distilled under reduced pressure under nitrogen protection at 0.1 kPa, heated to 180°C and purified to constant weight, and the distillate was collected to obtain 6-amino cashew phenol. 0.65 mol of 4-(chlorosulfonyl)benzoyl chloride was added and stirred continuously for 3 hours to obtain amidated cashew phenol.

[0048] S3: Add 300 mL of a mixed solvent of ethanol containing 0.5 M sulfuric acid to the amidated cashew phenol, stir thoroughly, add 500 mL of 0.05 M tetrabutylammonium perchlorate and stir continuously for 2 hours. In an Ag / AgCl electrolytic cell, control the electrode potential to 2 V and continue the reaction for 30 min. Filter and wash with anhydrous ethanol to obtain the additive.

[0049] S4: Mix 100g of phenolic resin with 8g of additive thoroughly, then add 8g of aluminum hydroxide and 3g of benzenesulfonyl chloride in sequence, and stir thoroughly for 5 minutes to obtain resin solution;

[0050] S5: Apply release agent to the embedded electrode mold in sequence, followed by resin adhesive and alkali-free fiberglass cloth. Use a roller to fully saturate the fiberglass cloth with resin adhesive. Control the resin coating to 1cm and repeat the coating 5 times. Apply an alternating dielectric field at 90℃ and perpendicular to the fiberglass direction with a frequency of 5MHz and a peak voltage of 250V for 30 minutes. Heat the resin to 160℃ and apply a pressure of 0.5MPa perpendicular to the fiberglass surface for 20 minutes. Demold to obtain the fiberglass cable tray.

[0051] Example 3: A method for preparing a fireproof, antistatic, and corrosion-resistant fiberglass cable tray, comprising the following steps:

[0052] S1: 1.1 mol of cashew phenol was placed in a mixed acid solution of 2M nitric acid and 2M sulfuric acid in a volume ratio of 3:1 and heated to 90°C for 30 min to obtain nitrated cashew phenol. The nitrated cashew phenol was heated to 155°C under a nitrogen atmosphere of 0.15 kPa and distilled to constant weight. The distillate was collected, and 27 g of Pd / C catalyst was added to the distillate and reacted under a catalytic atmosphere of 0.4 MPa and 50°C for 2 hours to obtain a mixture of 6-aminocaucetol and 2-aminocaucetol.

[0053] S2: Amino cashew phenol was distilled under reduced pressure under nitrogen protection at 0.15 kPa, heated to 185 °C and purified to constant weight. The distillate was collected to obtain 6-amino cashew phenol. 0.67 mol of 4-(chlorosulfonyl)benzoyl chloride was added and stirred continuously for 3 hours to obtain amidated cashew phenol.

[0054] S3: Add 350 mL of a mixed solvent of ethanol containing 0.7 M sulfuric acid to the amidated cashew phenol, stir thoroughly, add 550 mL of 0.12 M tetrabutylammonium perchlorate, stir continuously for 2 hours, and in an Ag / AgCl electrolytic cell, control the electrode potential at 2.2 V and continue the reaction for 30 min. Filter and wash with anhydrous ethanol to obtain the additive.

[0055] S4: Mix 100g of phenolic resin with 8g of additive thoroughly, then add 8g of aluminum hydroxide and 3g of benzenesulfonyl chloride in sequence, and stir thoroughly for 5 minutes to obtain resin solution;

[0056] S5: Apply release agent to the embedded electrode mold in sequence, followed by resin adhesive and alkali-free fiberglass cloth. Use a roller to fully saturate the fiberglass cloth with resin adhesive. Control the resin coating to 1cm and repeat the coating 5 times. Apply an alternating dielectric field at 90℃ and perpendicular to the fiberglass direction with a frequency of 1MHz and a peak voltage of 100V for 30 minutes. Heat the resin to 150℃ and apply a pressure of 0.5MPa perpendicular to the fiberglass surface for 20 minutes. Demold to obtain the fiberglass cable tray.

[0057] Comparative Example 1: Based on Example 1, the difference is that the defoaming step was not used, and the rest is the same as Example 1.

[0058] S1: 1.1 mol of cashew phenol was placed in a mixed acid solution of 2M nitric acid and 2M sulfuric acid in a volume ratio of 3:1 and heated to 90°C for 30 min to obtain nitrated cashew phenol. The nitrated cashew phenol was heated to 160°C under a nitrogen atmosphere of 0.1 kPa and distilled to constant weight. The distillate was collected, and 30 g of Pd / C catalyst was added to the distillate and reacted under a catalytic atmosphere of 0.5 MPa and 40°C for 2 hours to obtain a mixture of 6-aminocaucetol and 2-aminocaucetol.

[0059] S2: Amino cashew phenol was distilled under reduced pressure under nitrogen protection at 0.2 kPa, heated to 190 °C and purified to constant weight, and the distillate was collected to obtain 6-amino cashew phenol. 0.7 mol of 4-(chlorosulfonyl)benzoyl chloride was added and stirred for 3 hours to obtain amidated cashew phenol.

[0060] S3: Add 400 mL of a mixed solvent of ethanol containing 1.0 M sulfuric acid to amidated cashew phenol, stir thoroughly, add 600 mL of 0.2 M tetrabutylammonium perchlorate, stir continuously for 2 hours, and in an Ag / AgCl electrolytic cell, control the electrode potential at 2.5 V and continue the reaction for 30 min. Filter and wash with anhydrous ethanol to obtain the additive.

[0061] S4: Mix 100g of phenolic resin with 8g of additive thoroughly, then add 8g of aluminum hydroxide and 3g of benzenesulfonyl chloride in sequence, and stir thoroughly for 5 minutes to obtain resin solution;

[0062] S5: Apply release agent to the mold in sequence, then apply resin adhesive and alkali-free fiberglass cloth. Use a roller to fully saturate the fiberglass cloth with resin adhesive. Repeat the coating process for 5 layers, cure and demold to obtain fiberglass cable tray.

[0063] Comparative Example 2: Based on Example 1, the difference is that atmospheric pressure nitrogen distillation is used, and the rest is the same as Example 1.

[0064] S1: 1.1 mol of cashew phenol was placed in a mixed acid solution of 2M nitric acid and 2M sulfuric acid in a volume ratio of 3:1 and heated to 90°C for 30 min to obtain nitrated cashew phenol. The nitrated cashew phenol was heated to 210°C under a nitrogen atmosphere and distilled to constant weight. The distillate was collected, and 30 g of Pd / C catalyst was added to the distillate and reacted under a catalytic atmosphere, 0.5 MPa and 40°C for 2 hours to obtain a mixture of 6-aminocaucetol and 2-aminocaucetol.

[0065] S2: Amino cashew phenol was distilled under reduced pressure under nitrogen protection at 0.2 kPa, heated to 190 °C and purified to constant weight, and the distillate was collected to obtain 6-amino cashew phenol. 0.7 mol of 4-(chlorosulfonyl)benzoyl chloride was added and stirred for 3 hours to obtain amidated cashew phenol.

[0066] S3: Add 400 mL of a mixed solvent of ethanol containing 1.0 M sulfuric acid to amidated cashew phenol, stir thoroughly, add 600 mL of 0.2 M tetrabutylammonium perchlorate, stir continuously for 2 hours, and in an Ag / AgCl electrolytic cell, control the electrode potential at 2.5 V and continue the reaction for 30 min. Filter and wash with anhydrous ethanol to obtain the additive.

[0067] S4: Mix 100g of phenolic resin with 8g of additive thoroughly, then add 8g of aluminum hydroxide and 3g of benzenesulfonyl chloride in sequence, and stir thoroughly for 5 minutes to obtain resin solution;

[0068] S5: Apply release agent to the embedded electrode mold in sequence, followed by resin adhesive and alkali-free fiberglass cloth. Use a roller to fully saturate the fiberglass cloth with resin adhesive. Control the resin coating to 1cm and repeat the coating 5 times. Apply an alternating dielectric field at 100℃ and perpendicular to the fiberglass direction with a frequency of 2MHz and a peak voltage of 175V for 30 minutes. Heat the resin to 160℃ and apply a pressure of 0.5MPa perpendicular to the fiberglass surface for 20 minutes. Demold to obtain the fiberglass cable tray.

[0069] Comparative Example 3: Based on Example 1, the difference is that the nitro group is catalyzed to amino group under normal pressure, and the rest is the same as Example 1.

[0070] S1: 1.1 mol of cashew phenol was placed in a mixed acid solution of 2M nitric acid and 2M sulfuric acid in a volume ratio of 3:1 and heated to 90°C for 30 min to obtain nitrated cashew phenol. The nitrated cashew phenol was heated to 160°C under a nitrogen atmosphere of 0.1 kPa and distilled to constant weight. The distillate was collected, and 30 g of Pd / C catalyst was added to the distillate and reacted under a catalytic atmosphere of 0.1 MPa and 60°C for 2 hours to obtain a mixture of 6-aminocaucetol and 2-aminocaucetol.

[0071] S2: Amino cashew phenol was distilled under reduced pressure under nitrogen protection at 0.2 kPa, heated to 190 °C and purified to constant weight, and the distillate was collected to obtain 6-amino cashew phenol. 0.7 mol of 4-(chlorosulfonyl)benzoyl chloride was added and stirred for 3 hours to obtain amidated cashew phenol.

[0072] S3: Add 400 mL of a mixed solvent of ethanol containing 1.0 M sulfuric acid to amidated cashew phenol, stir thoroughly, add 600 mL of 0.2 M tetrabutylammonium perchlorate, stir continuously for 2 hours, and in an Ag / AgCl electrolytic cell, control the electrode potential at 2.5 V and continue the reaction for 30 min. Filter and wash with anhydrous ethanol to obtain the additive.

[0073] S4: Mix 100g of phenolic resin with 8g of additive thoroughly, then add 8g of aluminum hydroxide and 3g of benzenesulfonyl chloride in sequence, and stir thoroughly for 5 minutes to obtain resin solution;

[0074] S5: Apply release agent to the embedded electrode mold in sequence, followed by resin adhesive and alkali-free fiberglass cloth. Use a roller to fully saturate the fiberglass cloth with resin adhesive. Control the resin coating to 1cm and repeat the coating 5 times. Apply an alternating dielectric field at 100℃ and perpendicular to the fiberglass direction with a frequency of 2MHz and a peak voltage of 175V for 30 minutes. Heat the resin to 160℃ and apply a pressure of 0.5MPa perpendicular to the fiberglass surface for 20 minutes. Demold to obtain the fiberglass cable tray.

[0075] Comparative Example 4: Based on Example 1, the difference is that the aminocainol in S2 is distilled at atmospheric pressure, and the rest is the same as in Example 1.

[0076] S1: 1.1 mol of cashew phenol was placed in a mixed acid solution of 2M nitric acid and 2M sulfuric acid in a volume ratio of 3:1 and heated to 90°C for 30 min to obtain nitrated cashew phenol. The nitrated cashew phenol was heated to 160°C under a nitrogen atmosphere of 0.1 kPa and distilled to constant weight. The distillate was collected, and 30 g of Pd / C catalyst was added to the distillate and reacted under a catalytic atmosphere of 0.5 MPa and 40°C for 2 hours to obtain a mixture of 6-aminocaucetol and 2-aminocaucetol.

[0077] S2: Amino cashew phenol was distilled under nitrogen protection at 0.1 MPa and heated to 190 °C to constant weight and the distillate was collected to obtain 6-amino cashew phenol. 0.7 mol of 4-(chlorosulfonyl)benzoyl chloride was added and stirred for 3 hours to obtain amidated cashew phenol.

[0078] S3: Add 400 mL of a mixed solvent of ethanol containing 1.0 M sulfuric acid to amidated cashew phenol, stir thoroughly, add 600 mL of 0.2 M tetrabutylammonium perchlorate, stir continuously for 2 hours, and in an Ag / AgCl electrolytic cell, control the electrode potential at 2.5 V and continue the reaction for 30 min. Filter and wash with anhydrous ethanol to obtain the additive.

[0079] S4: Mix 100g of phenolic resin with 8g of additive thoroughly, then add 8g of aluminum hydroxide and 3g of benzenesulfonyl chloride in sequence, and stir thoroughly for 5 minutes to obtain resin solution;

[0080] S5: Apply release agent to the embedded electrode mold in sequence, followed by resin adhesive and alkali-free fiberglass cloth. Use a roller to fully saturate the fiberglass cloth with resin adhesive. Control the resin coating to 1cm and repeat the coating 5 times. Apply an alternating dielectric field at 100℃ and perpendicular to the fiberglass direction with a frequency of 2MHz and a peak voltage of 175V for 30 minutes. Heat the resin to 160℃ and apply a pressure of 0.5MPa perpendicular to the fiberglass surface for 20 minutes. Demold to obtain the fiberglass cable tray.

[0081] Comparative Example 5: Based on Example 1, the difference is that in S3, an active metal reduction method is used to reduce to thiol, and the rest is the same as in Example 1.

[0082] S1: 1.1 mol of cashew phenol was placed in a mixed acid solution of 2M nitric acid and 2M sulfuric acid in a volume ratio of 3:1 and heated to 90°C for 30 min to obtain nitrated cashew phenol. The nitrated cashew phenol was heated to 160°C under a nitrogen atmosphere of 0.1 kPa and distilled to constant weight. The distillate was collected, and 30 g of Pd / C catalyst was added to the distillate and reacted under a catalytic atmosphere of 0.5 MPa and 40°C for 2 hours to obtain a mixture of 6-aminocaucetol and 2-aminocaucetol.

[0083] S2: Amino cashew phenol was distilled under reduced pressure under nitrogen protection at 0.2 kPa, heated to 190 °C and purified to constant weight, and the distillate was collected to obtain 6-amino cashew phenol. 0.7 mol of 4-(chlorosulfonyl)benzoyl chloride was added and stirred for 3 hours to obtain amidated cashew phenol.

[0084] S3: Mix 1.0 mol zinc powder and 0.8 mol dilute sulfuric acid thoroughly and heat to 40°C. Dissolve 0.1 mol sulfonyl chloride substrate in 500 mL anhydrous ethanol and slowly add it to the reaction system at 2000 rpm. Heat the mixture to 75~90°C and continue the reaction for 2 hours to obtain the additive.

[0085] S4: Mix 100g of phenolic resin with 8g of additive thoroughly, then add 8g of aluminum hydroxide and 3g of benzenesulfonyl chloride in sequence, and stir thoroughly for 5 minutes to obtain resin solution;

[0086] S5: Apply release agent to the embedded electrode mold in sequence, followed by resin adhesive and alkali-free fiberglass cloth. Use a roller to fully saturate the fiberglass cloth with resin adhesive. Control the resin coating to 1cm and repeat the coating 5 times. Apply an alternating dielectric field at 100℃ and perpendicular to the fiberglass direction with a frequency of 2MHz and a peak voltage of 175V for 30 minutes. Heat the resin to 160℃ and apply a pressure of 0.5MPa perpendicular to the fiberglass surface for 20 minutes. Demold to obtain the fiberglass cable tray.

[0087] Performance testing

[0088] 1. Bending performance: The bending strength of the materials obtained in Examples 1-3 and Comparative Examples 1-5 was determined by the method in GB / T 1449-2005 "Test method for bending performance of fiber reinforced plastics". The experimental results are shown in Table 1.

[0089] 2. Impact performance: The impact toughness of the materials obtained in Examples 1-3 and Comparative Examples 1-5 was determined by the method in GB / T 1451-2005 "Test Method for Impact Toughness of Fiber Reinforced Plastics in Simply Supported Beams". The experimental results are shown in Table 1.

[0090] 3. Aging performance: The performance retention rate of the materials obtained in Examples 1-3 and Comparative Examples 1-5 was determined by the method in GB / T 2573-2008 "Test Method for Aging Performance of Glass Fiber Reinforced Plastics". The experimental results are shown in Table 1.

[0091] 4. Combustion performance (oxygen index): The oxygen index of the materials obtained in Examples 1-3 and Comparative Examples 1-5 was determined according to the method in GB / T 8924-2005 "Test method for combustion performance of fiber reinforced plastics - oxygen index method". The experimental results are shown in Table 1.

[0092] 5. Antistatic properties: The resistivity of the materials obtained in Examples 1-3 and Comparative Examples 1-5 was determined according to the method in GB / T 15738-2008 "Test Method for Resistivity of Conductive and Antistatic Fiber Reinforced Plastics". The experimental results are shown in Table 1.

[0093] Table 1. Performance tests of each embodiment and comparative example

[0094]

[0095] Data Analysis:

[0096] According to the data in Table 1, the fire-resistant, anti-static, and corrosion-resistant fiberglass cable trays prepared by the method of this invention in Examples 1-3 exhibit superior performance in terms of bending strength, impact toughness, performance retention rate, oxygen index, and resistivity. (Reference) Figure 1 The flowchart illustrates the process. In this example, a reaction is carried out in a mixed acid solution of sulfuric and nitric acids under heating. Cashew nutshellol is converted into 2-nitrocainol, 4-nitrocainol, and 6-nitrocainol. Due to steric hindrance, 6-nitrocainol has the highest yield, followed by 4-nitrocainol, and 2-nitrocainol has the lowest yield. The substituent in nitrocainol is nitro. The main factors affecting the boiling point of nitrocainol are molecular symmetry and intermolecular regularity. 4-nitrocainol has better intermolecular regularity, resulting in a significantly different boiling point compared to the other products. The reduction of 6-nitrocainol and 2-nitrocainol to 6-aminocainol and 2-aminocainol further reduces the substituent... The nitro group is converted to an amino group, which forms intramolecular hydrogen bonds with the phenolic hydroxyl group and the straight chain. In 6-aminocainol, the amino group only forms intramolecular hydrogen bonds with the adjacent phenolic hydroxyl group, while in 2-aminocainol, the amino group forms more intramolecular hydrogen bonds with the adjacent phenolic hydroxyl group and the straight chain. Molecules with more intramolecular hydrogen bonds have higher boiling points, hence the large difference in boiling points between 6-aminocainol and 2-aminocainol. Introducing 4-(chlorosulfonyl)benzoyl chloride under pressurized nitrogen protection yields amidated cashew phenol. When amidated cashew phenol is electrolyzed under acidic conditions, it reacts step by step. The sulfonyl chloride sequentially generates sulfinic acid, thiosulfinic acid ester, and disulfide at the cathode, and the disulfide is eventually reduced to a thiol.

[0097] In Example 1, a higher distillation temperature and a steeper vacuum gradient were used, resulting in more thorough removal of 4-nitrocaerol and higher purity. The separation pyrolysis byproducts were less at lower temperatures, and the more long carbon chains provided a more significant toughening and strengthening effect. In Example 2, the distillation temperature was lower, but the separation efficiency was slightly reduced, and trace amounts of isomers remained in the product. The performance of Example 3 was moderate. In Example 1, the sulfuric acid concentration was higher, the proton supply was sufficient, the potential was higher, and the reduction driving force was stronger, resulting in higher thiol generation efficiency. The thiol directly formed a thioester bond with the ester bond generated by the antioxidant, resulting in a higher performance retention rate of the fiberglass. The conditions in Example 3 were moderate, while the conditions in Example 2 were the worst.

[0098] The oxygen index directly reflects the flame retardant performance of the material. The oxygen index depends on the purity and structural integrity of the additive. The additive in Example 1 has high structural integrity and the highest purity. The C15 long chain exists stably in the additive molecule through chemical bonds, resulting in the highest oxygen index. In Example 2, due to lower separation efficiency, trace amounts of low molecular weight impurities reduce the oxygen index of the material. The oxygen index of Example 3 is moderate. Resistivity reflects the antistatic performance of fiberglass. The additive in Example 1 has the most complete structure and good interfacial bonding in the resin matrix, resulting in low resistivity. In Example 2, a small amount of incompletely reacted intermediate products exist, affecting the dispersibility of the additive and resulting in higher resistivity. The dispersion uniformity of Example 3 is moderate, and the resistivity is moderate.

[0099] Regarding bending strength, Comparative Example 1, which did not employ degassing treatment, retained residual air bubbles during the preparation process. Under bending loads, these bubbles reduced the effective load-bearing area of ​​the resin matrix to withstand tensile stress. Comparative Example 2, which used atmospheric pressure nitrogen distillation to treat nitrated cashew phenol, experienced significant degradation due to the high temperature at 0.1 MPa and 210°C. This high temperature caused the long-chain alkyl groups to break down, generating numerous byproducts and disrupting the long-chain toughening effect of the additives. Furthermore, the product purity decreased significantly, and the effective component content was reduced. Comparative Example 3, involving atmospheric pressure catalytic hydrogenation, showed a decrease in Pd / C catalytic efficiency under atmospheric pressure. The conversion rate of nitro to amino groups decreased, resulting in a lower yield of effective products from subsequent amidation and thiolation. In Comparative Example 4, the amino cashew phenol was distilled at atmospheric pressure. The insufficient temperature of atmospheric distillation made it difficult to distill off 6-amino cashew phenol, and the excessively high temperature easily caused the amino group to oxidize and decompose, resulting in a decrease in product purity and the content of effective additives. In Comparative Example 5, zinc powder chemical reduction was used instead of electrochemical reduction. The zinc powder / acid reduction of sulfonyl chloride could yield a thiol structure, and the long-chain alkyl and amide skeletons were intact. However, the selectivity of chemical reduction was poor, and disulfide byproducts were present. Zinc metal impurities would introduce interface defects, affecting the bending strength of the fiberglass.

[0100] Regarding impact toughness, the impact toughness of fiberglass depends on the fiber-resin interface bonding strength, the plastic deformation capacity of the resin matrix, and the effect of additives. In Comparative Example 1, residual air bubbles occupy the space for plastic slip in the resin matrix, and impact cracks penetrate the air bubbles, shortening the fracture path and causing brittle fracture. In Comparative Example 2, due to the use of high-temperature distillation, the C15 saturated straight chain of cashew phenol undergoes thermal decomposition and fracture, reducing the long alkyl and mercapto components in the product. The additives lack long hydrophobic chains and mercapto polar sites for adsorption to hydroxyl groups on the glass fiber surface, making it difficult to form a stable chemical adsorption film on the glass fiber surface. Under impact, the fiber-resin debonds, making it difficult to effectively transfer the load to the rigid skeleton of the glass fiber. The C15 straight chain is the toughening unit of the resin matrix, and after high-temperature fracture, the additives... The additive loses its flexible chain segments, making it difficult to provide slippage and tensile deformation in the resin crosslinking network. The resin crosslinking network is too rigid and lacks plastic buffering under impact, reducing its impact absorption capacity. In Comparative Example 3, the atmospheric pressure catalysis of nitro hydrogenation resulted in insufficient conversion rate, leading to a decrease in the thiol content of the final product. This made it difficult to adequately alleviate ester swelling, causing microcracks inside the fiberglass matrix and reducing impact toughness. In Comparative Example 4, atmospheric pressure distillation could not effectively separate 2-aminocainol and 6-aminocainol. The 2-aminocainol in the product made it difficult for the additive to spread evenly on the glass fiber surface to form a continuous adsorption film, reducing the glass fiber's impact absorption capacity. In Comparative Example 5, the zinc salt inorganic impurities in the additive were dispersed at the resin-fiber interface, forming stress concentration points. Under impact loads, the impurity particles generated cracks, reducing impact resistance.

[0101] Regarding the performance retention rate, the aging performance retention rate is affected by the reaction between the thiol and ester groups of the additives. In Comparative Example 1, due to the presence of bubbles, the oxygen and water vapor in the bubbles accelerate the production of ester substances from amine antioxidants under outdoor high-temperature irradiation. Water and oxygen penetrate to the interface, and the defects of the bubbles accelerate the erosion of the external medium. In Comparative Examples 2-4, the thiol content is reduced, which weakens the ability to remove ester groups. The aging retention rate decreases in tandem with the proportion of effective ingredients. Comparative Example 5 is prepared by chemical reduction. Under acidic heating conditions, some amide bonds will hydrolyze, and the molecular skeleton of the cashew phenol-benzene ring thiol group will break, losing the structure that reacts with ester groups. It cannot effectively solve the problem of ester contamination. The residual zinc ions will catalyze the free radical oxidation reaction of the resin matrix, accelerating the aging and degradation of the resin, thus reducing the performance retention rate after resin aging.

[0102] Regarding the oxygen index, it is affected by the matrix resin, flame retardant, additives, and reinforcing fibers. In Comparative Example 1, when the flame burns, the bubbles expand due to heat, forming thermal convection, which accelerates the thermal decomposition of the resin. The oxygen in the bubbles provides the reaction conditions for the initial pyrolysis, which greatly increases the external oxygen concentration required by the material. In Comparative Examples 2-4, the effective content of additives is low, the total sulfur content in the system is reduced, and the oxygen index is reduced. In Comparative Example 5, the oxygen index is relatively high. The zinc ions remaining after zinc powder reduction play an inorganic flame retardant synergistic role in flame retardancy, blocking the smoke and producing a synergistic flame retardant effect with the sulfur-containing components in the fiberglass, offsetting the negative impact of the decrease in effective components and achieving an improved oxygen index.

[0103] Regarding resistivity, the factors affecting resistivity are mainly influenced by the polar groups and conductive additives in the additives. Polar groups can effectively improve the polarization ability of the resin. As the carrier migration efficiency increases, the resistivity of the monomer volume decreases. In Comparative Example 1, due to the ineffective removal of bubbles, the presence of bubbles in the fiberglass is equivalent to an insulating barrier, making it difficult for carriers to form a conductive path through the bubbles. In Comparative Examples 2-4, due to the low content of effective additives, the density of polar groups decreases, resulting in weaker antistatic ability of the fiberglass. In Comparative Example 4, due to the hydrolysis of amide bonds, the reduction of effective polar groups, and the decrease in matrix polarization ability, as zinc salt impurities exist as independent particles in the resin, they cannot form a continuous and stable conductive path, which disrupts the uniform distribution of polar groups, increases resistivity, and reduces antistatic performance.

[0104] The difference between Example 1 and Comparative Example 5 is that Comparative Example 5 uses an active metal reduction method to reduce to thiols. In contrast, the chemical reduction involves acidic heating conditions that cause partial hydrolysis of amide bonds, destroying the cashew phenol-benzene ring thiol group. At the same time, zinc salt impurities remain in the resin-fiber interface, forming stress concentration, which significantly reduces bending strength and impact toughness. The breakage of amide groups reduces the high-temperature resistance of additives, reduces polar groups, and reduces thiol content, making it impossible to fully form thioester bonds with antioxidants. Residual zinc ions catalyze the free radical oxidation of resin, accelerating aging and degradation. The electrochemical method of Example 1 can effectively avoid these side reactions. In terms of oxygen index, due to the synergistic effect of zinc ions as inorganic flame retardants in Comparative Example 5, they form a synergistic carbonization and smoke barrier effect with the sulfur-containing components in fiberglass, which improves flame retardancy to a certain extent. Compared with Example 1 and Comparative Example 5, the electrochemical method of Example 1 has the advantages of mild reaction conditions, high product selectivity, no introduction of metal impurities, and intact molecular structure.

[0105] The above description is only a preferred embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any equivalent substitutions or modifications made by those skilled in the art within the scope of the technology disclosed in the present invention, based on the technical solution and inventive concept of the present invention, should be covered within the scope of protection of the present invention.

Claims

1. A fireproof, antistatic, and corrosion-resistant fiberglass cable tray, characterized in that, Includes the following raw material components: 100-120 parts by weight of phenolic resin, 8-10 parts by weight of 4-mercapto-N-(2-hydroxy-4-pentadecanylphenyl)benzamide, 5-8 parts by weight of aluminum hydroxide, and 3-4 parts by weight of benzenesulfonyl chloride; The specific preparation method of the 4-mercapto-N-(2-hydroxy-4-pentadecanophenyl)benzamide is as follows: S1: Place cashew phenol in mixed acid and heat to 90℃ for 30 min to obtain nitrated cashew phenol. Heat the nitrated cashew phenol to 150-160℃ under a nitrogen atmosphere of 0.1-0.2 kPa and distill to constant weight. Collect the distillate, add Pd / C catalyst to the distillate and react for 2 hours under a catalytic atmosphere of 0.3-0.5 MPa and 40-60℃ to obtain a mixture of 6-aminocainol and 2-aminocainol. S2: Aminocainol is distilled under reduced pressure under nitrogen protection, heated to 180~190℃ and purified to constant weight, and the distillate is collected to obtain 6-aminocainol. 6-aminocainol and 4-(chlorosulfonyl)benzoyl chloride are reacted at 0~25℃ in a molar ratio of 1:(1~1.1) for 3 hours to obtain amidated cashewol. S3: Add 20-30% by mass of amidated cashew phenol to an ethanol mixed solvent containing 0.2-0.6M H2SO4, stir thoroughly, and add 0.05-0.2M tetrabutylammonium perchlorate to make the electrolyte concentration 0.03-0.12M. Continue stirring for 2 hours in an Ag / AgCl electrolytic cell with lead electrode, control the electrode potential and continue the reaction for 30 minutes. Filter and wash with anhydrous ethanol to obtain 4-mercapto-N-(2-hydroxy-4-pentadecanylphenyl)benzamide additive.

2. The fireproof, antistatic, and corrosion-resistant fiberglass cable tray according to claim 1, characterized in that, The cashew phenol is a meta-phenol with a 15-saturated carbon chain; the Pd / C catalyst is a palladium catalyst supported on activated carbon, with a palladium content of 10-15%.

3. The fireproof, antistatic, and corrosion-resistant fiberglass cable tray additive according to claim 1, characterized in that, The mixed acid is obtained by uniformly mixing 2M nitric acid and 2M sulfuric acid in a volume ratio of (3~3.5):(1~1.5).

4. The fireproof, antistatic, and corrosion-resistant fiberglass cable tray additive according to claim 1, characterized in that, The catalytic atmosphere is an atmosphere in which nitrogen and hydrogen are mixed in a volume ratio of (6~7.5):(2.5~3).

5. The fireproof, antistatic, and corrosion-resistant fiberglass cable tray additive according to claim 1, characterized in that, The vacuum distillation described in S2 is carried out under nitrogen protection in a nitrogen atmosphere of 0.1~0.2 kPa.

6. The fireproof, antistatic, and corrosion-resistant fiberglass cable tray additive according to claim 1, characterized in that, The electrode potential described in S3 has a voltage of 2~2.5V and a current density of 10~20mA / cm. 2 .

7. The method for preparing the fireproof, antistatic, and corrosion-resistant fiberglass cable tray according to any one of claims 1 to 6, characterized in that, Includes the following steps: (1) Mix 100-120 parts by weight of phenolic resin with 8-10 parts by weight of additives thoroughly, then add 5-8 parts by weight of aluminum hydroxide and 3-4 parts by weight of benzenesulfonyl chloride in sequence, and stir thoroughly for 5-10 minutes to obtain resin solution. (2) Apply release agent to the embedded electrode mold in sequence, then apply phenolic resin liquid containing additives and alkali-free glass fiber cloth. Use a roller to make the resin liquid fully penetrate the glass fiber cloth. The resin coating is controlled to be 1cm and repeated for 5 layers. Apply an alternating dielectric field at 90~100℃ and perpendicular to the direction of the fiberglass, with a frequency of 1~5MHz and a peak voltage of 100~250V for 30min. Heat the resin to 150~160℃ and apply a pressure of 0.5MPa perpendicular to the surface of the fiberglass for 20min. Demold to obtain fiberglass cable tray.

8. The preparation method of the fireproof, antistatic, and corrosion-resistant fiberglass cable tray additive according to claim 7, characterized in that, The alternating dielectric electrophoresis field contains a real-time impedance module that reduces voltage when the resin impedance drops sharply.