A low-density foamed phenolic resin-based prepreg and a method for manufacturing a composite material thereof

CN123152248APending Publication Date: 2026-11-24CHENGDU LUCHEN NEW MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611574804.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-12
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing technologies struggle to reduce the density of phenolic resin-based composite materials while simultaneously achieving precise control of the cell structure, maintaining good mechanical properties and surface quality, and improving the foaming uniformity of thick-section products.

Method used

A composite foaming system consisting of expandable microspheres and chemical foaming agents is adopted. It combines gradient structure design, nano-toughening filler reinforcement, fiber surface modification and staged foaming and curing, and uses microwave-assisted heating to achieve precise control and uniformity of the cell structure through synergistic foaming.

Benefits of technology

It significantly reduces the density of composite materials, improves the closed-cell rate and uniformity of the foam structure, and enhances the mechanical properties and surface quality of the materials, making it suitable for aerospace, rail transportation, shipbuilding and construction and other fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123152248A_ABST
    Figure CN123152248A_ABST
Patent Text Reader

Abstract

This invention discloses a method for preparing a low-density foamed phenolic resin-based prepreg and its composite material. The prepreg employs a dual-foaming agent synergistic foaming system and a gradient structure design: the core layer contains a composite foaming agent composed of expandable microspheres and a chemical foaming agent, with the initial expansion temperature of the expandable microspheres lower than the decomposition temperature of the chemical foaming agent; the surface layer is a dense phenolic resin layer with no or low foaming agent content; nano-toughening fillers are also added to the resin composition, and the reinforcing fibers undergo surface modification treatment. During preparation, core layer foaming adhesive and surface layer adhesive are prepared separately, and a gradient prepreg is formed through stepwise impregnation coating or lamination. After layering, the prepreg undergoes staged foaming and curing via stepped heating to obtain a dense skin-foamed core integrated composite material. This invention features fine and uniform pores, high closed-cell ratio, and a density as low as 0.25~0.75 g / cm³, while also exhibiting excellent mechanical properties, surface quality, and flame-retardant and thermal insulation properties, making it suitable for the field of lightweight structural and functional integrated materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of composite material technology, specifically relating to a method for preparing a low-density foamed phenolic resin-based prepreg and its composite material, and particularly to a low-density phenolic resin-based prepreg and its composite material with a gradient foaming structure, synergistic foaming by two foaming agents and interface reinforcement. Background Technology

[0002] Phenolic resins possess excellent flame retardancy, heat resistance, low smoke and low toxicity, and dimensional stability, making them important matrix materials in aerospace, rail transportation, shipbuilding, and construction. However, traditional phenolic resin-based composites have a relatively high density, typically 1.2–1.5 g / cm³, which is insufficient to meet increasingly stringent lightweight requirements. Introducing a cellular structure into the resin matrix through foaming can significantly reduce density while simultaneously imparting thermal and sound insulation properties to the material. Combining foamed phenolic resins with continuous fiber reinforcements is an effective way to obtain structural-functional integrated materials that combine low density with high mechanical properties.

[0003] Currently, there are two main routes for preparing foamed phenolic resin-based composite materials: one is to first prepare phenolic foam and then bond it to a fiber layer or panel. This method suffers from poor interfacial bonding between the foam and fiber, easy breakage of the foam cells during the composite process, and cumbersome processes. The other method is to directly introduce the foaming agent into the prepreg system for in-situ foaming during the composite molding process. This method is beneficial for improving interfacial bonding and process efficiency, but it faces the following technical challenges: First, the foaming agent may decompose or volatilize prematurely during the preparation and storage of prepreg, resulting in poor storage stability and reduced foaming capacity of the prepreg. Second, the foaming temperature range of a single foaming agent is narrow, and the foaming process is difficult to precisely match the curing reaction of phenolic resin, which can easily cause cell merging, collapse or uneven distribution, making it difficult to control the foaming ratio and cell size. Third, the surface of the foamed composite material is rough, with openings and defects, resulting in poor surface quality and environmental resistance, making it difficult to use directly as a structural component. Fourth, foaming disrupts the continuity of the resin matrix, significantly reducing mechanical properties, especially compressive strength and interlaminar shear strength, thus limiting its application in load-bearing structures. Fifth, the interfacial bonding between the fiber and the foaming resin is weak, and the cell wall strength is insufficient, making it prone to damage along the fiber / resin interface or cell wall when subjected to stress. Sixth, during the foaming process, thick-section products experience internal and external temperature gradients due to heat conduction, resulting in significant differences in cell size along the thickness direction, making it difficult to guarantee foaming uniformity.

[0004] In the prior art, CN110746738A discloses a phenolic resin foamed prepreg, its preparation method, and its application. This patent involves thoroughly mixing phenolic resin with an expandable microsphere foaming agent to obtain a slurry. Fiber-reinforcing materials are then immersed in the slurry for impregnation. Initial foaming is achieved through continuous impregnation and baking. The prepreg is then rolled and cut into sheets, and the prepreg is stacked and pressed to achieve secondary foaming and final curing. However, this patent uses only expandable microspheres as a single foaming agent. The expansion ratio of the expandable microspheres is limited by the thermoplasticity of the outer polymer and the degree of vaporization of the core hydrocarbons. During the formation of the cross-linked network in the cured phenolic resin, the cell wall strength generated by the microsphere expansion is insufficient to withstand further expansion, resulting in a limited foaming ratio, difficulty in further reducing density, and difficulty in precisely controlling cell size and closed-cell ratio. Meanwhile, the prepreg in this patent contains foaming agent throughout. During the foaming process, bubbles escape freely from the surface of the prepreg, causing the surface cell walls to rupture and form open pores and pinholes. This prevents the formation of a dense and smooth surface layer, resulting in a composite material with a rough surface, high porosity, a water absorption rate as high as 5.2%, and a flexural strength reduced to 42 MPa. Furthermore, this patent does not involve technologies such as nano-toughening fillers to strengthen cell walls and interfaces, fiber surface modification to enhance interfacial bonding, staged foaming and curing to precisely match the curing reaction, or microwave-assisted heating to improve the uniformity of foaming in thick sections.

[0005] In existing technologies, the conventional approach to addressing the problems of insufficient expansion ratio and difficulty in controlling cell structure with a single foaming agent is to increase the amount of foaming agent or use microspheres with a higher expansion ratio. However, this approach introduces new problems such as uneven dispersion of the foaming agent, cell merging, and further degradation of mechanical properties. Therefore, those skilled in the art, when faced with the specific problems addressed by this invention, would not naturally conceive of a technical solution combining dual foaming agent temperature gradient matching for synergistic foaming, gradient structure design, nano-toughening filler reinforcement, fiber surface modification, staged foaming and curing, and microwave-assisted heating. Summary of the Invention

[0006] The technical problem to be solved by this invention is: how to achieve precise control of the cell structure, maintain good mechanical properties and surface quality, and improve the foaming uniformity of thick cross-section products while significantly reducing density.

[0007] To solve the above-mentioned technical problems, the present invention provides a low-density foamed phenolic resin-based prepreg, comprising reinforcing fibers and a foamed phenolic resin composition loaded on the reinforcing fibers; the foamed phenolic resin composition comprises, by weight, the following components: 55-85 parts phenolic resin, 3-15 parts composite foaming agent, 0-18 parts curing agent, 0.5-3 parts surfactant, 1-10 parts nano-toughening filler, and 10-40 parts solvent; wherein the composite foaming agent is composed of expandable microspheres and a chemical foaming agent in a weight ratio of 1:0.5-1:5; the initial expansion of the expandable microspheres... The expansion temperature is 80~130℃, and the decomposition temperature of the chemical foaming agent is 120~170℃; the initial expansion temperature of the expandable microspheres is lower than the decomposition temperature of the chemical foaming agent, and both are higher than the highest temperature experienced during the preparation of the prepreg, the highest temperature not exceeding 75℃; the prepreg has a gradient structure: including at least one core layer and surface layers located on both sides of the core layer; the core layer contains the foaming phenolic resin composition, the surface layer contains a non-foaming or low-foaming phenolic resin composition, and the foaming agent content in the surface layer is 0~30% of the foaming agent content in the core layer.

[0008] Furthermore, the thickness of the core layer accounts for 40% to 90% of the total thickness of the prepreg, and the thickness of one side of the surface layer accounts for 5% to 30% of the total thickness of the prepreg.

[0009] Furthermore, the phenolic resin is a thermosetting phenolic resin or a thermoplastic phenolic resin; when a thermosetting phenolic resin is used, no curing agent is required, and when a thermoplastic phenolic resin is used, the curing agent is hexamethylenetetramine.

[0010] Furthermore, the expandable microspheres are microcapsules of low-boiling-point hydrocarbons encapsulated in a thermoplastic polymer shell. The outer shell polymer is vinylidene chloride-acrylonitrile copolymer, acrylonitrile-methyl methacrylate copolymer, or acrylonitrile-methacrylonitrile copolymer, and the core is isobutane, isopentane, or n-pentane. The average particle size of the microspheres is 5-40 μm, the initial expansion temperature is 80-130℃, the maximum expansion temperature is 120-190℃, and the maximum expansion ratio is 30-80 times. The chemical foaming agent is selected from one or more of activated azodicarbonamide, p-toluenesulfonyl hydrazine, 4,4'-oxobisbenzenesulfonyl hydrazine, and citric acid-sodium bicarbonate composite foaming agent. The activated azodicarbonamide is activated by zinc oxide, urea, or zinc stearate, and the decomposition temperature is 120-160℃.

[0011] Furthermore, the nano-toughening filler is selected from one or more of nano-silica, nano-calcium carbonate, nano-alumina, multi-walled carbon nanotubes, graphene nanosheets, and nano-montmorillonite; the average particle size or sheet thickness of the nano-toughening filler is 10~200 nm, and the specific surface area is not less than 100 m² / g; the surfactant is selected from one or more of Tween 80, Span 80, organosilicon surfactants, sodium dodecyl sulfate, and polyoxyethylene ether surfactants; the solvent is selected from one or more of ethanol, acetone, methanol, ethyl acetate, and butanone.

[0012] Further, the reinforcing fiber is one of glass fiber, carbon fiber, basalt fiber, aramid fiber, or a fabric thereof; the reinforcing fiber undergoes surface modification treatment, the treatment method being one or more of silane coupling agent impregnation, plasma treatment, or oxidative etching, wherein the silane coupling agent is selected from γ-aminopropyltriethoxysilane, γ-glycidyl etheroxypropyltrimethoxysilane, and γ-methacryloyloxypropyltrimethoxysilane; the mass fraction of the reinforcing fiber in the prepreg is 25%~55%, the unit area mass of the prepreg is 200~3000 g / m², and the volatile matter content at room temperature does not exceed 2%.

[0013] The present invention also provides a low-density foamed phenolic resin-based composite material, which has an integrated structure of a dense surface layer and a foamed core layer, with an overall density of 0.25~0.75 g / cm³, an average cell diameter of 30~150 μm in the core layer, a closed-cell rate of not less than 88%, a surface layer thickness of 0.05~0.5 mm, and a surface layer density of 0.95~1.3 g / cm³; the composite material has a compressive strength of 5~20 MPa, a flexural strength of 30~100 MPa, an interlaminar shear strength of 2~8 MPa, a thermal conductivity of 0.03~0.07 W / (m·K), and an oxygen index of not less than 34%.

[0014] This invention also provides a method for preparing a low-density foamed phenolic resin-based composite material, comprising the following steps: (1) Preparation of core layer foaming resin solution: Phenolic resin, composite foaming agent, curing agent, surfactant, nano toughening filler and solvent are mixed evenly according to the formula to obtain core layer foaming resin solution; (2) Preparation of surface resin solution: Phenolic resin, curing agent, surfactant, nano toughening filler and solvent are mixed evenly according to the formula, with no addition or only a small amount of foaming agent added. The small amount of foaming agent refers to the foaming agent content in the surface layer being 0~30% of the foaming agent content in the core layer, to obtain the surface resin solution. (3) Preparation of gradient prepreg: Impregnate the reinforcing fibers with the core layer foaming resin solution, and dry them to a semi-dry state. The semi-dry state means that the solvent residue is 5%~15% and the surface is not sticky to the touch, has self-supporting properties, and can be laid at room temperature without significant flow or deformation. Then, coat or impregnate the upper and lower surfaces of the core layer with the surface layer resin solution in the semi-dry state, and dry it again to obtain a low-density foamed phenolic resin-based prepreg with a gradient structure; or, impregnate the reinforcing fibers with the core layer foaming resin solution and the surface layer resin solution to make a core layer prepreg sheet and a surface layer prepreg sheet, respectively. Then, attach the surface layer prepreg sheet to the upper and lower sides of the core layer prepreg sheet and combine them into one piece by hot pressing or roller pressing to obtain a gradient prepreg. (4) Lamination and molding: The gradient prepreg is laid in a mold, and firstly, it is kept at 80~130℃ for 10~60 min for the first stage of foaming, then kept at 130~170℃ for 10~60 min for the second stage of foaming and pre-curing, and finally kept at 140~180℃ for 1~4 h for complete curing, while applying a pressure of 0.05~2 MPa to obtain a low-density foamed phenolic resin-based composite material.

[0015] Further, in step (3), the first drying temperature is 50~75℃, and the solvent residue in the semi-dry state of the core layer after drying is 5%~15%; after the second drying, the solvent residue in the final prepreg is 2%~8%, and the volatile content does not exceed 2%; in step (4), the second stage foaming and pre-curing temperature is 125~160℃, the complete curing temperature is 145~180℃, and the applied pressure is 0.1~1.5 MPa.

[0016] Furthermore, in step (4), when the pressure is 0.05~0.1 MPa, vacuum bag pressing or low-pressure molding process is used, which results in low cell growth resistance and high foaming ratio; when the pressure is 1.5~2 MPa, high-pressure molding process is used, which can effectively suppress excessive cell growth and obtain high-density, high-strength foamed composite material; when using autoclave molding, the pressure inside the autoclave is maintained at 0.1~0.5 MPa during the foaming stage, and the pressure is increased to 0.3~1.5 MPa during the curing stage.

[0017] Furthermore, in step (4), the foaming stage is assisted by microwave heating or high-frequency electromagnetic field heating with a frequency of 2450 MHz or 13.56 MHz, a power density of 0.5~5 W / cm², and an auxiliary heating time of 5~20 min.

[0018] Furthermore, in step (4), when the foaming temperature is 80~85℃, the expandable microspheres undergo pre-expansion to form initial cell nuclei, but the chemical foaming agent has not yet decomposed, which is suitable for occasions that require high closed-cell ratio and fine cells; when the foaming temperature is 125~130℃, the expandable microspheres fully expand and the chemical foaming agent begins to decompose, resulting in a higher foaming ratio, which is suitable for occasions that require lower density.

[0019] Compared with the prior art, the present invention has the following beneficial effects: First, this invention employs a composite foaming system composed of expandable microspheres and a chemical foaming agent. By setting the initial expansion temperature of the expandable microspheres lower than the decomposition temperature of the chemical foaming agent, stepwise synergistic foaming is achieved. At a lower temperature, the expandable microspheres expand first, forming uniformly distributed initial cell nuclei within the resin matrix. As the temperature rises, the chemical foaming agent decomposes on top of the existing cell nuclei, generating gas and causing the cells to grow further. The polymer shell of the microspheres remains within the cell walls after expansion, stabilizing the cells and preventing coalescence and collapse. This stepwise synergistic foaming mechanism significantly improves cell size uniformity and closed-cell ratio, with the average cell diameter controllable between 30 and 150 μm and a closed-cell ratio exceeding 88%. In contrast, composite materials obtained with a single chemical foaming agent have a closed-cell ratio of only 76%, a cell diameter of approximately 180 μm, and a density as high as 0.85 g / cm³. This invention achieves a balance between low density and high closed-cell ratio through the synergistic effect of two foaming agents.

[0020] Secondly, this invention employs a gradient structure of "dense surface layer - foamed core layer". The surface layer is a phenolic resin layer with no or low foaming agent content, which forms a dense and smooth surface after curing, effectively sealing the pores of the core layer and preventing the penetration of moisture and external media, while providing high surface hardness and wear resistance. The core layer contains a composite foaming agent, which forms a low-density foam core layer after foaming, achieving weight reduction and heat insulation functions. This integrated gradient structure avoids the defects of rough surface and many openings in traditional foamed composite materials, and can be used directly without subsequent surface treatment. In the comparative example, the water absorption rate is as high as 5.2% and the flexural strength drops to 42 MPa when there is no gradient structure, while the embodiment of this invention has a surface roughness Ra of 0.8 μm, a water absorption rate of 0.8%, and a flexural strength of 68 MPa.

[0021] Third, this invention incorporates nano-toughening fillers into the resin matrix. These fillers are uniformly dispersed within the resin matrix, forming a nano-reinforcing phase within the cell walls. This significantly improves the strength and toughness of the cell walls, inhibits cell breakage and coalescence during foaming, and simultaneously improves stress transfer efficiency at the fiber / resin interface, thereby enhancing the compressive strength and interlaminar shear strength of the composite material. Compared to foamed composites without nano-fillers, the compressive strength can be increased by 30% to 80%. When the amount of nano-silica increases from 1 part to 10 parts, the compressive strength increases from 7.6 MPa to 17.0 MPa.

[0022] Fourth, this invention modifies the surface of the reinforcing fibers through silane coupling agent treatment or plasma treatment, improving the chemical bonding and physical wettability between the fiber surface and the phenolic resin. This ensures uniform nucleation of cells along the fiber surface during foaming, preventing cell aggregation at the fiber / resin interface and the formation of weak interfaces, significantly improving the interlaminar shear strength and resistance to damp heat of the composite material. The interlaminar shear strength of the untreated fibers is only 3.1 MPa, while the interlaminar shear strength in the embodiments of this invention reaches 5.6 MPa.

[0023] Fifth, this invention employs a staged foaming and curing process. The foaming process is divided into a low-temperature microsphere expansion stage and a high-temperature chemical foaming agent decomposition stage, which matches the curing reaction ladder of phenolic resin. This avoids cell defects caused by competition between foaming and curing, resulting in a highly operable process suitable for various molding processes such as compression molding, autoclave molding, and vacuum bagging. When the foaming temperature is between 80 and 85°C, the expandable microspheres undergo pre-expansion to form initial cell nuclei, but the chemical foaming agent has not yet decomposed, making it suitable for applications requiring high closed-cell ratio and fine cell density. When the foaming temperature is between 125 and 130°C, the expandable microspheres fully expand and the chemical foaming agent begins to decompose, resulting in a higher foaming ratio, making it suitable for applications requiring lower density.

[0024] Sixth, this invention introduces microwave or high-frequency electromagnetic field-assisted heating during the foaming stage. It utilizes the dielectric loss of polar molecules in an alternating electromagnetic field to achieve volumetric heating, simultaneously raising the temperature inside and outside the prepreg. This avoids the temperature gradient caused by traditional heat conduction heating, significantly improving the foaming uniformity of thick-section products. With microwave-assisted heating, the average diameter of the cells in the upper, middle, and lower parts of the core layer of thick-section products is approximately 60 μm, the closed-cell rate increases to 93%, and the density difference in the thickness direction decreases to below 0.03 g / cm³. Without microwave-assisted heating, the cell diameter changes from 50 μm at the top to 120 μm at the bottom, and the closed-cell rate decreases to 86%. Attached Figure Description

[0025] Figure 1The diagram shows a gradient prepreg structure, which consists of a core layer and surface layers on both sides of the core layer. The core layer contains expandable microspheres, chemical foaming agents, reinforcing fibers, and nano-toughening fillers. The surface layer is a dense layer. The diagram also indicates that the core layer thickness accounts for 40% to 90% of the total thickness and the surface layer thickness on one side accounts for 5% to 30%.

[0026] Figure 2 This is a process flow diagram for preparing gradient prepreg by a stepwise impregnation coating method. The diagram shows the process of impregnating the reinforcing fiber with a foaming resin solution for the core layer, drying it to a semi-dry state, coating the upper and lower surfaces of the semi-dry core layer with a surface resin solution, and drying it again to obtain the gradient prepreg.

[0027] Figure 3 The temperature-time curve for staged foaming and curing is shown in the figure. The temperature regime is as follows: first stage foaming at 80~130℃ for 10~60 min, second stage foaming and pre-curing at 130~170℃ for 10~60 min, and complete curing at 140~180℃ for 1~4 h. The pressure curve is as follows: 0.05~2 MPa. Detailed Implementation

[0028] The present invention will be further described in detail below with reference to the accompanying drawings and embodiments, but the scope of protection of the present invention is not limited to the following embodiments. In the following embodiments, all parts are parts by weight.

[0029] The performance tests in the following examples adopted the following standards: density was tested according to GB / T 1463-2005 "Test Method for Density and Relative Density of Fiber Reinforced Plastics"; compressive strength was tested according to GB / T 1448-2005 "Test Method for Compression Properties of Fiber Reinforced Plastics"; flexural strength was tested according to GB / T 1449-2005 "Test Method for Flexural Properties of Fiber Reinforced Plastics"; interlaminar shear strength was tested according to GB / T 3357-1982 "Test Method for Interlaminar Shear Strength of Unidirectional Fiber Reinforced Plastics"; thermal conductivity was tested according to GB / T10295-2008 "Determination of Steady-State Thermal Resistance and Related Properties of Thermal Insulation Materials - Heat Flow Meter Method"; oxygen index was tested according to GB / T 2406.2-2009 "Determination of Combustion Behavior by Oxygen Index Method for Plastics - Part 2: Room Temperature Test"; closed-cell rate was tested according to GB / T 10799-2008 "Determination of Open and Closed Cell Volume Percentage of Rigid Foamed Plastics"; water absorption rate was tested according to GB / T Tested according to GB / T 12000-2003 "Determination of water absorption of plastics" (GB 1034-2008); tested according to GB / T 12000-2003 "Determination of the effects of exposure of plastics to damp heat, water spray and salt spray".

[0030] See Figure 1The low-density foamed phenolic resin-based prepreg of the present invention has a gradient structure, comprising at least one core layer and surface layers located on both sides of the core layer. The core layer contains a foamed phenolic resin composition, and the surface layers contain a non-foamed or low-foamed phenolic resin composition. Expandable microspheres, a chemical foaming agent, reinforcing fibers, and nano-toughening fillers are uniformly dispersed in the core layer. The core layer thickness accounts for 40% to 90% of the total thickness of the prepreg, and the thickness of the surface layer on one side accounts for 5% to 30% of the total thickness of the prepreg.

[0031] See Figure 2 The gradient prepreg of the present invention can be prepared by a step-by-step impregnation and coating method: the reinforcing fiber is impregnated with the core layer foaming resin solution, dried to a semi-dry state, and then the upper and lower surfaces of the core layer in the semi-dry state are coated or impregnated with the surface layer resin solution, and dried again to obtain a low-density foamed phenolic resin-based prepreg with a gradient structure; or, the reinforcing fiber is impregnated with the core layer foaming resin solution and the surface layer resin solution to make a core layer prepreg sheet and a surface layer prepreg sheet respectively, and then the surface layer prepreg sheet is attached to the upper and lower sides of the core layer prepreg sheet and laminated together by hot pressing or roll pressing to obtain a gradient prepreg.

[0032] See Figure 3 The layup and molding steps of the present invention adopt a staged foaming and curing system: first, the first stage of foaming is carried out by holding at 80~130℃ for 10~60 min, then the second stage of foaming and pre-curing is carried out by holding at 130~170℃ for 10~60 min, and finally the complete curing is carried out by holding at 140~180℃ for 1~4 h, while applying a pressure of 0.05~2 MPa.

[0033] Example 1 Core layer foaming resin formulation: 75 parts thermosetting phenolic resin (78% solid content); 4 parts expandable microspheres with an outer shell of acrylonitrile copolymer and an inner core of isobutane, with an average particle size of 12 μm; 5 parts azodicarbonamide activated by zinc oxide; 1.5 parts Tween 80; 4 parts nano-silica with an average particle size of 20 nm and a specific surface area of ​​200 m² / g; 25 parts ethanol.

[0034] Surface resin adhesive formulation: 80 parts thermosetting phenolic resin; 1 part Tween 80; 3 parts nano silica; 20 parts ethanol.

[0035] Reinforcing fiber: Plain weave glass fiber fabric with a surface density of 200 g / m², pre-treated with a 1.5% KH550 silane coupling agent aqueous solution and dried at 100℃ for 30 min.

[0036] Preparation process: Core layer foaming resin solution and surface layer resin solution were prepared separately and mechanically stirred for 30 min until homogeneous, followed by vacuum degassing for 15 min. Fiberglass cloth was impregnated with the core layer foaming resin solution and dried in a 65℃ oven for 6 min to obtain a semi-dry core layer with approximately 10% solvent residue. Then, surface layer resin solution was coated onto the upper and lower surfaces of the semi-dry core layer, controlling the surface wet film thickness to approximately 100 μm. It was then dried again at 70℃ for 10 min to obtain a gradient structure prepreg. The total thickness of the prepreg was approximately 0.45 mm, the core layer thickness was approximately 0.35 mm, and the surface layers on both sides were approximately 0.05 mm each. The volatile content was 1.3%, and the solvent residue was 5%. The prepreg was cut into 300 mm × 300 mm pieces, laid in 10 layers, placed in a flat mold, and molded using compression molding. A pressure of 0.3 MPa was applied, and the temperature was increased to 110℃ at 3℃ / min and held for 30 min. Then, the temperature was increased to 140℃ at 2℃ / min and held for 20 min. Finally, the temperature was increased to 160℃ at 2℃ / min and held for 2 h to completely cure the material. After cooling and demolding, a low-density foamed phenolic resin-based composite material was obtained.

[0037] Performance testing: The composite material has an overall density of 0.52 g / cm³, an average core cell diameter of approximately 65 μm, a closed-cell rate of 94%, a surface layer thickness of approximately 0.12 mm, and a surface layer density of 1.15 g / cm³. It exhibits a compressive strength of 12.5 MPa, a flexural strength of 68 MPa, an interlaminar shear strength of 5.6 MPa, a thermal conductivity of 0.043 W / (m·K), and an oxygen index of 39%. The surface is smooth and flat, with a surface roughness Ra of 0.8 μm, a pencil hardness of 3H, and a water absorption rate (24h) of 0.8%. After 72 hours of humid heat aging at 80℃ / 95%RH, the compressive strength retention rate is 92%, the flexural strength retention rate is 90%, and the interlaminar shear strength retention rate is 88%.

[0038] Example 2 Core layer foaming resin formulation: 68 parts thermoplastic phenolic resin (softening point 100℃, free phenol 1.0%); 10 parts hexamethylenetetramine; 5 parts expandable microspheres with a shell of vinylidene chloride-acrylonitrile copolymer and a core of isopentane, with an average particle size of 20 μm; 6 parts p-toluenesulfonyl hydrazine; 2 parts Span 80; 2 parts multi-walled carbon nanotubes with a diameter of 10~20 nm, a length of 5~20 μm, and a specific surface area of ​​250 m² / g; 30 parts acetone.

[0039] Surface resin formulation: 75 parts thermoplastic phenolic resin; 10 parts hexamethylenetetramine; 1 part Span 80; 1.5 parts multi-walled carbon nanotubes; 25 parts acetone.

[0040] Reinforcing fiber: 200 g / m² carbon fiber twill fabric, plasma treated (power 200 W, treatment time 60 s, atmosphere is air).

[0041] Preparation process: Core layer and surface layer adhesive solutions were prepared separately. Carbon nanotubes were ultrasonically dispersed in acetone for 30 min before adding other components. A gradient prepreg was prepared using a double-layer coating method: carbon fiber cloth was first impregnated with the core layer foaming adhesive solution and dried at 60℃ for 8 min until semi-dry. Then, the surface layer adhesive solution was coated on both sides and dried at 65℃ for 12 min to obtain the gradient prepreg. The total thickness of the prepreg was approximately 0.40 mm, with the core layer approximately 0.30 mm and the surface layers each approximately 0.05 mm, and the volatile matter content was 1.1%. Twelve layers were laid up and formed using an autoclave. Vacuum bag pressing was used, with an internal pressure of 0.2 MPa. The temperature was increased to 100℃ at a rate of 2℃ / min and held for 25 min, then increased to 125℃ and held for 20 min, and finally increased to 150℃ and held for 3 h for curing. During the curing stage, the internal pressure was increased to 0.6 MPa.

[0042] Performance testing: The composite material has an overall density of 0.45 g / cm³, an average core cell diameter of approximately 55 μm, a closed-cell rate of 93%, a surface layer thickness of approximately 0.10 mm, and a surface layer density of 1.18 g / cm³. It exhibits a compressive strength of 10.8 MPa, a flexural strength of 85 MPa, an interlaminar shear strength of 5.2 MPa, a thermal conductivity of 0.039 W / (m·K), and an oxygen index of 36%. The surface is free of pinholes and can be directly painted. After 72 hours of humid heat aging at 80℃ / 95%RH, the compressive strength retention rate is 90%, the flexural strength retention rate is 91%, and the interlaminar shear strength retention rate is 86%.

[0043] Example 3 Core layer foaming resin formulation: 70 parts thermosetting phenolic resin; 6 parts expandable microspheres with an average particle size of 8 μm; 4 parts activated AC foaming agent; 1 part sodium dodecyl sulfate; 1.5 parts graphene nanosheets with a layer thickness of 3~5 nm and a specific surface area of ​​500 m² / g; 8 parts hollow glass microspheres with a density of 0.25 g / cm³ and a particle size of 20~60 μm; 28 parts ethanol.

[0044] Surface resin adhesive formulation: 82 parts thermosetting phenolic resin; 1 part sodium dodecyl sulfate; 1 part graphene nanosheets; 22 parts ethanol.

[0045] Reinforcing fiber: Plain weave fabric of aramid fiber with an areal density of 170 g / m², treated with KH570 silane coupling agent.

[0046] Preparation process: Core and surface layer adhesive solutions were prepared. Graphene nanosheets were ultrasonically dispersed in ethanol for 40 min. Core and surface prepreg sheets were prepared separately: aramid fabric was impregnated with the core and surface adhesive solutions, dried at 65℃ for 8 min to obtain the core prepreg sheet, and dried at 70℃ for 12 min to obtain the surface prepreg sheet. The two surface prepreg sheets were then coated onto the top and bottom sides of a core prepreg sheet, respectively, and rolled at 80℃ and 0.2 MPa pressure for 5 min to obtain a gradient prepreg. The total thickness was approximately 0.50 mm. Six layers were laid up and molded. A pressure of 0.5 MPa was applied, and the temperature was increased to 105℃ at 2℃ / min and held for 35 min, then increased to 140℃ and held for 25 min, and finally increased to 165℃ and held for 2 h for curing.

[0047] Performance testing: The composite material has an overall density of 0.40 g / cm³, an average core cell diameter of approximately 45 μm, a closed-cell rate of 96%, a compressive strength of 9.5 MPa, a flexural strength of 55 MPa, an interlaminar shear strength of 4.8 MPa, a thermal conductivity of 0.035 W / (m·K), and an oxygen index of 38%. The surface is dense and wear-resistant, with a Taber wear loss of 0.05 g / 1000 rpm. After 72 hours of humid heat aging at 80℃ / 95%RH, the compressive strength retention rate is 94%, the flexural strength retention rate is 92%, and the interlaminar shear strength retention rate is 91%.

[0048] Example 4 Similar to Example 1, but the first-stage foaming temperature was adjusted to 82℃ and the holding time was extended to 50 min; the second-stage foaming and pre-curing temperature was adjusted to 135℃ and the holding time to 25 min; the complete curing temperature was 160℃ and the holding time was 2 h. The resulting composite material had an overall density of 0.68 g / cm³, an average core cell diameter of 40 μm, a closed-cell rate of 97%, a compressive strength of 16.5 MPa, a flexural strength of 78 MPa, and an interlaminar shear strength of 6.8 MPa.

[0049] Example 5 Similar to Example 1, but the first-stage foaming temperature was adjusted to 128℃, and the holding time was shortened to 15 min; the second-stage foaming and pre-curing temperature was adjusted to 165℃, and the holding time was 15 min; the complete curing temperature was 170℃, and the holding time was 1.5 h. The resulting composite material had an overall density of 0.32 g / cm³, an average core cell diameter of 140 μm, a closed-cell rate of 88%, a compressive strength of 6.2 MPa, a flexural strength of 35 MPa, and an interlaminar shear strength of 2.8 MPa.

[0050] Example 6 Same as in Example 1, but the molding pressure was adjusted to 0.08 MPa (using vacuum bag compression assistance), while other conditions remained unchanged. The resulting composite material had an overall density of 0.38 g / cm³, an average core cell diameter of 120 μm, a closed-cell rate of 89%, a compressive strength of 7.5 MPa, a flexural strength of 42 MPa, and an interlaminar shear strength of 3.2 MPa.

[0051] Example 7 Same as in Example 1, but the molding pressure was adjusted to 1.8 MPa, while all other conditions remained unchanged. The resulting composite material had an overall density of 0.72 g / cm³, an average core cell diameter of 35 μm, a closed-cell rate of 98%, a compressive strength of 18.5 MPa, a flexural strength of 88 MPa, and an interlaminar shear strength of 7.2 MPa.

[0052] Example 8 Similar to Example 1, only the amount of nano-silica added in the core layer was changed, set to 1 part, 2 parts, 4 parts, 7 parts, and 10 parts respectively; the surface layer formulation, reinforcing fiber, prepreg preparation, and molding and curing conditions were all the same as in Example 1. Four parts of this example correspond to Example 1. The results are shown in Table 1.

[0053] Table 1. Effect of nano-silica addition amount on the properties of composite materials

[0054] As shown in Table 1, as the amount of nano-silica increased from 1 part to 10 parts, the average cell diameter gradually decreased, the closed-cell rate increased, and the compressive strength increased from 7.6 MPa to 17.0 MPa, indicating that the nanofiller has a significant reinforcing effect on the cell walls. When the amount is 7 parts, the flexural strength and interlaminar shear strength reach a relatively good balance; when the amount is further increased to 10 parts, the compressive strength still increases, but the flexural strength decreases slightly. This is because high nanoparticle content easily leads to local agglomeration, increases resin viscosity, and reduces impregnation and dispersion uniformity. Therefore, the preferred amount of nano-toughening filler is 1 to 10 parts, and more preferably 2 to 7 parts.

[0055] Example 9 Similar to Example 1, the total thickness of the prepreg was adjusted to approximately 1.0 mm by varying the amount of adhesive applied to the core layer and the thickness of the wet film of the adhesive coating on the surface layer. This resulted in a core layer thickness of approximately 0.40 mm and two surface layers of approximately 0.30 mm each, representing a core layer ratio of 40% and a single-sided surface layer ratio of 30%. The resulting composite material had an overall density of 0.65 g / cm³, an average core layer cell diameter of 52 μm, a closed-cell rate of 95%, a surface layer thickness of approximately 0.30 mm, a surface roughness Ra of 0.5 μm, a 24-hour water absorption rate of 0.5%, a compressive strength of 15.2 MPa, a flexural strength of 75 MPa, and an interlaminar shear strength of 6.3 MPa.

[0056] Example 10 Similar to Example 1, the total thickness of the prepreg was adjusted to approximately 1.0 mm by varying the amount of adhesive applied to the core layer and the thickness of the wet film of the adhesive coating on the surface layer. This resulted in a core layer thickness of approximately 0.90 mm and two surface layers of approximately 0.05 mm each, representing a core layer ratio of 90% and a surface layer ratio of 5% on each side. The resulting composite material had an overall density of 0.48 g / cm³, an average core layer cell diameter of 78 μm, a closed-cell rate of 90%, a surface layer thickness of approximately 0.05 mm, a surface roughness Ra of 2.8 μm, a 24-hour water absorption rate of 1.9%, a compressive strength of 9.8 MPa, a flexural strength of 50 MPa, and an interlaminar shear strength of 4.2 MPa.

[0057] Example 11 Using the core layer adhesive, surface layer adhesive, reinforcing fibers, and gradient prepreg preparation method described in Example 1, a gradient prepreg with a total thickness of approximately 0.45 mm was prepared. The prepreg was cut into 300 mm × 300 mm pieces, laid in 30 layers, and placed in a flat mold to form a thick-section blank with a thickness of approximately 13.5 mm. The molding process was as follows: a pressure of 0.3 MPa was applied, and the temperature was increased to 110°C at a rate of 3°C / min and held for 30 min for the first stage of foaming; microwave-assisted heating was used for the first 10 min at a frequency of 2450 MHz and a power density of 2.0 W / cm²; the temperature was increased to 140°C at a rate of 2°C / min and held for 20 min for the second stage of foaming and pre-curing; the temperature was increased to 160°C at a rate of 2°C / min and held for 2 h for complete curing; after cooling and demolding, a thick-section, low-density foamed phenolic resin-based composite material was obtained.

[0058] As a control, the same formulation and layup as in Example 11 were used, but without microwave-assisted heating; the product was cured by conventional heat conduction only and was designated as Comparative Example 6.

[0059] Table 2. Effect of microwave-assisted heating on the foaming uniformity of thick-section products

[0060] As shown in Table 2, after 10 minutes of microwave-assisted heating at 2450 MHz and a power density of 2.0 W / cm², the cell size distribution along the thickness direction of the thick-section product became significantly more uniform. The average cell diameter in the upper, middle, and lower parts of the core layer was approximately 60 μm, the closed-cell rate increased to 93%, and the density difference along the thickness direction decreased to below 0.03 g / cm³. In Comparative Example 6, due to the temperature gradient caused by conventional heat conduction, the lower part foamed first, followed by the upper part, and the cell diameter changed from 50 μm to 120 μm, resulting in a decrease in the closed-cell rate and a decline in mechanical properties. This indicates that microwave-assisted heating can effectively improve the uniformity of foaming in thick sections.

[0061] Example 12 Similar to Example 1, but with the addition of a composite foaming agent to the surface resin adhesive. The amount added is 10% of the total amount of the core foaming agent, i.e., 0.9 parts, including 0.4 parts of expandable microspheres and 0.5 parts of activated AC foaming agent. The resulting composite material has an overall density of 0.515 g / cm³, an average core cell diameter of 66 μm, a closed-cell rate of 93.5%, a surface layer thickness of approximately 0.13 mm, a surface layer density of 1.12 g / cm³, a surface roughness Ra of 1.0 μm, a 24-hour water absorption rate of 0.9%, a compressive strength of 12.3 MPa, a flexural strength of 67 MPa, and an interlaminar shear strength of 5.5 MPa.

[0062] Example 13 Similar to Example 1, but with the addition of a composite foaming agent to the surface resin adhesive. The amount added is 20% of the total amount of the core foaming agent, i.e., 1.8 parts, including 0.8 parts of expandable microspheres and 1.0 part of activated AC foaming agent. The resulting composite material has an overall density of 0.508 g / cm³, an average core cell diameter of 67 μm, a closed-cell rate of 93%, a surface layer thickness of approximately 0.14 mm, a surface layer density of 1.06 g / cm³, a surface roughness Ra of 1.8 μm, a 24-hour water absorption rate of 1.1%, a compressive strength of 12.0 MPa, a flexural strength of 64 MPa, and an interlaminar shear strength of 5.3 MPa.

[0063] Example 14 Similar to Example 1, but a composite foaming agent was added to the surface resin adhesive at an amount equal to 30% of the core foaming agent content, i.e., 2.7 parts, including 1.2 parts expandable microspheres and 1.5 parts activated AC foaming agent. The resulting composite material has an overall density of 0.50 g / cm³, an average core cell diameter of 68 μm, a closed-cell rate of 92%, a surface layer thickness of approximately 0.14 mm, a surface layer density of 0.95 g / cm³, a surface roughness Ra of 3.2 μm, a compressive strength of 11.8 MPa, a flexural strength of 62 MPa, an interlaminar shear strength of 5.0 MPa, and a 24-hour water absorption rate of 1.5%.

[0064] Comparative Example 1 Similar to Example 1, but using only activated AC foaming agent without adding expandable microspheres, and the total amount of foaming agent was the same as the total mass of the composite foaming agent in Example 1. The resulting composite material had a density of 0.68 g / cm³, an average cell diameter of approximately 180 μm, a closed-cell rate of 76%, and a compressive strength of 6.8 MPa. The cell structure was significantly non-uniform, with both macropores and open cells present, indicating that a single chemical foaming agent is insufficient to obtain a fine and uniform cell structure.

[0065] Comparative Example 2 Similar to Example 1, but using only expandable microspheres without adding chemical foaming agents. The resulting composite material had a density of 0.85 g / cm³, an average cell diameter of approximately 40 μm, and a closed-cell rate of 90%, but the foaming ratio was insufficient and the density was too high. This indicates that the foaming capacity of a single microsphere is limited, and chemical foaming agents are needed to synergistically improve the foaming ratio.

[0066] Comparative Example 3 Similar to Example 1, but the prepreg did not employ a gradient structure; instead, the entire prepreg contained foaming agent. The resulting composite material had a rough surface with numerous open holes and pinholes, a water absorption rate (24h) as high as 5.2%, a surface hardness of only HB, and a flexural strength reduced to 42 MPa. This demonstrates that a dense surface layer is crucial for surface quality and mechanical properties.

[0067] Comparative Example 4 Similar to Example 1, but without the addition of nano-silica. The resulting composite material had a compressive strength of only 7.2 MPa, a decrease of approximately 42% compared to Example 1, with thinner cell walls and localized cracking. This indicates that the nano-toughening filler plays an important role in strengthening the cell walls and improving compressive strength.

[0068] Comparative Example 5 Similar to Example 1, but the reinforcing fibers were not treated with a silane coupling agent. The resulting composite material had an interlaminar shear strength of only 3.1 MPa, a decrease of approximately 45% compared to Example 1. Cross-sectional observation showed that the cells aggregated along the fiber / resin interface, forming a weak interfacial layer. This indicates that fiber surface modification is crucial for improving interfacial bonding and cell distribution uniformity.

[0069] Comparative Example 6 The same formulation and layup as in Example 11 were used, but without microwave-assisted heating; curing was performed solely through conventional heat conduction. The resulting thick-section composite material had an overall density of 0.55 g / cm³, with an average cell diameter of 50 μm in the upper core, 85 μm in the middle, and 120 μm in the lower core, an average closed-cell rate of 86%, a thickness-direction density difference ≥0.08 g / cm³, a compressive strength of 10.5 MPa, a flexural strength of 58 MPa, and an interlaminar shear strength of 4.7 MPa.

[0070] The above examples and comparative examples demonstrate that the present invention, through the combined effects of synergistic foaming with dual foaming agents, gradient structure design, nano-toughening fillers, and fiber surface modification, successfully prepared foamed phenolic resin-based composite materials with low density, high closed-cell ratio, fine and uniform pores, excellent mechanical properties, and superior surface quality. These materials are significantly superior to traditional foamed prepreg systems with a single foaming agent or no gradient structure.

Claims

1. A low-density foamed phenolic resin-based prepreg, characterized in that, The invention comprises reinforcing fibers and a foamed phenolic resin composition loaded on the reinforcing fibers; the foamed phenolic resin composition comprises, by weight, the following components: 55-85 parts phenolic resin, 3-15 parts composite foaming agent, 0-18 parts curing agent, 0.5-3 parts surfactant, 1-10 parts nano-toughening filler, and 10-40 parts solvent; wherein the composite foaming agent is composed of expandable microspheres and a chemical foaming agent in a weight ratio of 1:0.5-1:5; the initial expansion temperature of the expandable microspheres is 80-130℃, and the chemical foaming agent... The decomposition temperature of the foaming agent is 120~170℃; the initial expansion temperature of the expandable microspheres is lower than the decomposition temperature of the chemical foaming agent, and both are higher than the highest temperature experienced during the preparation of the prepreg, which does not exceed 75℃; the prepreg has a gradient structure: including at least one core layer and surface layers located on both sides of the core layer; the core layer contains the foaming phenolic resin composition, the surface layer contains a non-foaming or low-foaming phenolic resin composition, and the foaming agent content in the surface layer is 0~30% of the foaming agent content in the core layer.

2. The low-density foamed phenolic resin-based prepreg according to claim 1, characterized in that, The core layer has a thickness of 40% to 90% of the total thickness of the prepreg, and the surface layer has a single-sided thickness of 5% to 30% of the total thickness of the prepreg.

3. The low-density foamed phenolic resin-based prepreg according to claim 1, characterized in that, The phenolic resin is a thermosetting phenolic resin or a thermoplastic phenolic resin; when a thermosetting phenolic resin is used, no curing agent is required, and when a thermoplastic phenolic resin is used, the curing agent is hexamethylenetetramine.

4. The low-density foamed phenolic resin-based prepreg according to claim 1, characterized in that, The expandable microspheres are microcapsules of low-boiling-point hydrocarbons encapsulated in a thermoplastic polymer shell. The outer shell polymer is vinylidene chloride-acrylonitrile copolymer, acrylonitrile-methyl methacrylate copolymer, or acrylonitrile-methacrylonitrile copolymer, and the core is isobutane, isopentane, or n-pentane. The average particle size of the microspheres is 5-40 μm, the maximum expansion temperature is 120-190℃, and the maximum expansion ratio is 30-80 times. The chemical foaming agent is selected from one or more of activated azodicarbonamide, p-toluenesulfonyl hydrazine, 4,4'-oxobisbenzenesulfonyl hydrazine, and citric acid-sodium bicarbonate composite foaming agent. The activated azodicarbonamide is activated by zinc oxide, urea, or zinc stearate, and the decomposition temperature is 120-160℃.

5. The low-density foamed phenolic resin-based prepreg according to claim 1, characterized in that, The nano-toughening filler is selected from one or more of nano-silica, nano-calcium carbonate, nano-alumina, multi-walled carbon nanotubes, graphene nanosheets, and nano-montmorillonite; the average particle size or sheet thickness of the nano-toughening filler is 10~200 nm, and the specific surface area is not less than 100 m² / g; the surfactant is selected from one or more of Tween 80, Span 80, organosilicon surfactants, sodium dodecyl sulfate, and polyoxyethylene ether surfactants; the solvent is selected from one or more of ethanol, acetone, methanol, ethyl acetate, and butanone.

6. The low-density foamed phenolic resin-based prepreg according to claim 1, characterized in that, The reinforcing fiber is one of glass fiber, carbon fiber, basalt fiber, aramid fiber, or a fabric thereof; the reinforcing fiber undergoes surface modification treatment, the treatment method being one or more of silane coupling agent impregnation, plasma treatment, or oxidative etching, wherein the silane coupling agent is selected from γ-aminopropyltriethoxysilane, γ-glycidyl etheroxypropyltrimethoxysilane, and γ-methacryloyloxypropyltrimethoxysilane; the mass fraction of the reinforcing fiber in the prepreg is 25%~55%, the unit area mass of the prepreg is 200~3000 g / m², and the volatile matter content at room temperature does not exceed 2%.

7. A low-density foamed phenolic resin-based composite material, characterized in that, It has an integrated structure with a dense surface layer and a foamed core layer, with an overall density of 0.25~0.75 g / cm³, an average cell diameter of 30~150 μm in the core layer, a closed-cell rate of not less than 88%, a surface layer thickness of 0.05~0.5 mm, and a surface layer density of 0.95~1.3 g / cm³. The composite material has a compressive strength of 5~20 MPa, a flexural strength of 30~100 MPa, an interlaminar shear strength of 2~8 MPa, a thermal conductivity of 0.03~0.07 W / (m·K), and an oxygen index of not less than 34%.

8. A method for preparing a low-density foamed phenolic resin-based composite material, characterized in that, Includes the following steps: (1) Preparation of core layer foaming resin solution: Phenolic resin, composite foaming agent, curing agent, surfactant, nano toughening filler and solvent are mixed evenly according to the formula to obtain core layer foaming resin solution; (2) Preparation of surface resin solution: Phenolic resin, curing agent, surfactant, nano toughening filler and solvent are mixed evenly according to the formula, with no addition or only a small amount of foaming agent added. The small amount of foaming agent refers to the foaming agent content in the surface layer being 0~30% of the foaming agent content in the core layer, to obtain the surface resin solution. (3) Preparation of gradient prepreg: Impregnate the reinforcing fibers with the core layer foaming resin solution, and dry them to a semi-dry state. The semi-dry state means that the solvent residue is 5%~15% and the surface is not sticky to the touch, has self-supporting properties, and can be laid at room temperature without significant flow or deformation. Then, coat or impregnate the upper and lower surfaces of the core layer with the surface layer resin solution in the semi-dry state, and dry it again to obtain a low-density foamed phenolic resin-based prepreg with a gradient structure; or, impregnate the reinforcing fibers with the core layer foaming resin solution and the surface layer resin solution to make a core layer prepreg sheet and a surface layer prepreg sheet, respectively. Then, attach the surface layer prepreg sheet to the upper and lower sides of the core layer prepreg sheet and combine them into one piece by hot pressing or roller pressing to obtain a gradient prepreg. (4) Lamination and molding: The gradient prepreg is laid in a mold, and firstly, it is kept at 80~130℃ for 10~60 min for the first stage of foaming, then kept at 130~170℃ for 10~60 min for the second stage of foaming and pre-curing, and finally kept at 140~180℃ for 1~4 h for complete curing, while applying a pressure of 0.05~2 MPa to obtain a low-density foamed phenolic resin-based composite material.

9. The preparation method according to claim 8, characterized in that, In step (3), the first drying temperature is 50~75℃, and the solvent residue in the semi-dry state of the core layer after drying is 5%~15%; after the second drying, the solvent residue in the final prepreg is 2%~8%, and the volatile content does not exceed 2%; in step (4), the second stage foaming and pre-curing temperature is 125~160℃, the complete curing temperature is 145~180℃, and the applied pressure is 0.1~1.5 MPa; when the pressure is 0.05~0.1 MPa, vacuum bag pressing or low-pressure molding process is used; when the pressure is 1.5~2 MPa, high-pressure molding process is used; when using autoclave molding, the pressure inside the autoclave is maintained at 0.1~0.5 MPa during the foaming stage, and the pressure is increased to 0.3~1.5 MPa during the curing stage.

10. The preparation method according to claim 8, characterized in that, In step (4), the foaming stage is assisted by microwave heating or high-frequency electromagnetic field heating with a frequency of 2450 MHz or 13.56 MHz, a power density of 0.5~5 W / cm², and an auxiliary heating time of 5~20 min.