A resin composition and use thereof
By combining fillers and phosphorus-containing compounds with specific parameters, a dense packing structure is formed, which solves the problem of yellowing of resin compositions after high-temperature baking, achieving low CTE, high thermal conductivity and excellent yellowing resistance, making it suitable for the manufacture of printed wiring boards.
Patent Information
- Application Number
- CN202510662452.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-05-22
- Publication Date
- 2026-11-24
AI Technical Summary
In the prior art, resin compositions are prone to yellowing after high-temperature baking, and have high thermal conductivity and coefficient of thermal expansion, making it difficult to meet the high-performance requirements of printed wiring boards.
By using a high proportion of fillers and phosphorus-containing compounds with specific parameters, combined with epoxy resin, thermoplastic resin, and curing agent, a dense packing structure is formed, which blocks oxygen permeation and reacts with oxygen, reduces the oxidation rate, and improves thermal conductivity and yellowing resistance.
It achieves low coefficient of thermal expansion, low oxygen permeability, and high thermal conductivity in resin films or cured resins, while not exhibiting significant yellowing after high-temperature baking, thus meeting the high-performance requirements of printed wiring boards.
Smart Images

Figure BDA0005414172380000031 
Figure BDA0005414172380000051 
Figure BDA0005414172380000091
Abstract
Description
Technical Field
[0001] This invention belongs to the field of insulating layer technology and relates to a resin composition and its application. Background Technology
[0002] As a manufacturing technology for printed wiring boards, a manufacturing method based on the stacking of alternating insulating and conductor layers is known. In this stacking-based manufacturing method, the insulating layer is typically formed by curing a resin composition. The insulating layer is usually formed by curing a resin composition containing epoxy resin, a curing agent, thermoplastic resin, and inorganic filler, and a high filler content is required to improve the rigidity of the film, while a thermoplastic resin is used simultaneously to toughen the film. However, the low crosslinking density between the thermoplastic resin and the resin matrix leads to a tendency for yellowing after baking.
[0003] Therefore, there is an urgent need to develop resin compositions that can achieve high thermal conductivity, low coefficient of thermal expansion (CTE), and excellent resistance to yellowing. Summary of the Invention
[0004] In view of the shortcomings of the existing technology, the purpose of the present invention is to provide a resin composition and its application. By using a high proportion of fillers with specific parameters and phosphorus-containing compounds added to the resin composition, the resin film or resin cured product made from the resin composition has a low coefficient of thermal expansion, high thermal conductivity and excellent resistance to yellowing.
[0005] To achieve this objective, the present invention adopts the following technical solution:
[0006] In a first aspect, the present invention provides a resin composition comprising the following components: epoxy resin, thermoplastic resin, curing agent, filler, and phosphorus-containing compound;
[0007] The specific surface area of the filler is 0.3-3.5 m². 2 / g, bulk density is 2.5-3.8g / cm³ 3 .
[0008] The resin composition provided by the present invention comprises a combination of epoxy resin, thermoplastic resin, curing agent, filler and phosphorus-containing compound. Through the screening and synergistic compounding of specific components, the resin film or resin cured product made from the resin composition has low CTE, high thermal conductivity and excellent yellowing resistance.
[0009] It is worth noting that by using fillers with specific parameters in combination with phosphorus-containing compounds, a high proportion of fillers can form a densely packed physical isolation layer in the resin, effectively blocking oxygen permeation. Furthermore, the dense packing forms an effective thermal conductivity path, which can quickly conduct heat away, reducing microcracks caused by high-temperature stress, thereby reducing the exposed area of the oxidation interface. In particular, the addition of phosphorus-containing compounds can also react with the permeated oxygen, reducing the oxygen concentration permeated into the film, thereby slowing down the oxidation rate of the resin composition during processing and further preventing yellowing after baking.
[0010] In this invention, the specific surface area of the packing material can be obtained by gas adsorption method (BET method), and the testing instrument can be the American Micro GEMINI VII2390(A) specific surface area analyzer; the bulk density of the packing material can be tested according to the method of GB / T 6609.25-2023.
[0011] In this invention, the specific surface area of the filler is 0.3-3.5 m². 2 / g, for example, could be 0.3m 2 / g, 0.5m 2 / g, 1.0m 2 / g, 1.5m 2 / g, 2.0m 2 / g, 2.5m 2 / g, 3.0m 2 / g or 3.5m 2 / g, etc.; the bulk density of the filler is 2.5-3.8 g / cm³. 3 For example, it could be 2.5g / cm³ 3 2.8g / cm 3 3.0g / cm 3 3.2g / cm 3 3.5g / cm 3 3.6g / cm 3 Or 3.8g / cm 3 wait.
[0012] Preferably, the epoxy resin includes any one or a combination of at least two of the following: bisphenol A type epoxy resin, bisphenol F type epoxy resin, phosphorus-containing epoxy resin, MDI-modified epoxy resin, phenolic epoxy resin, biphenyl type epoxy resin, dicyclopentadiene type epoxy resin, naphthalene-containing epoxy resin, or alicyclic epoxy resin.
[0013] Preferably, the thermoplastic resin includes any one or a combination of at least two of the following: phenoxy resin, polyvinyl acetal resin, polyolefin resin, polybutadiene resin, polyimide resin, polyamide-imide resin, polyether-imide resin, polysulfone resin, polyethersulfone resin, polyphenylene ether resin, polycarbonate resin, polyetheretherketone resin, polyester resin, or acrylic resin.
[0014] Preferably, the curing agent comprises any one or a combination of at least two of the following: reactive ester resin, cyanate ester resin, benzoxazine resin, phenolic resin, carbodiimide resin, maleimide resin, or amine curing agent.
[0015] Preferably, the filler comprises any one or a combination of at least two of alumina, aluminum nitride, magnesium oxide, or silicon dioxide.
[0016] Preferably, the average sphericity of the packing material is ≥0.7, for example, it can be 0.7, 0.72, 0.75, 0.78, 0.8, 0.82, 0.85, 0.88, 0.9, or 0.95. Selecting packing material with high average sphericity is beneficial for forming a dense packing structure.
[0017] In this invention, the average sphericity of the filler is ≥0.7, and the average sphericity of the filler can be measured by referring to the corresponding method in GB / T 32661-2016 "Spherical Silica Micropowder".
[0018] Preferably, the phosphorus-containing compound includes any one or a combination of at least two of the structures of formula (I), formula (II), or cyclic phosphazene compounds;
[0019]
[0020] Among them, R C1 -R C5 Each is independently selected from aliphatic hydrocarbon groups or halogen atoms having 1-5 carbon atoms;
[0021] A c Selected from alkylene groups (1-5 carbon atoms), alkenyl groups (2-5 carbon atoms), ether groups, thioether groups, sulfinyl groups, esteryl groups, ketone groups, or single bonds;
[0022] e and f are each independently selected from any integer from 0 to 5 (for example, they can be 0, 1, 2, 3, 4, 5);
[0023] g, h, and i are each independently selected from any integer between 0 and 4 (for example, they can be 0, 1, 2, 3, and 4).
[0024] It is worth noting that phosphorus-containing compounds or cyclic phosphazene compounds with structures (I) and (II) have low molecular polarity and good compatibility with the resin matrix. During high-temperature baking, they can reduce microcracks caused by local thermal stress. On the other hand, the selected phosphorus-containing compounds can react well with the oxygen that permeates in, reducing the oxygen concentration that permeates into the film, thereby slowing down the oxidation rate of the resin composition during baking and improving the problem of yellowing of the film after baking.
[0025] In this invention, the carbon number 1-5 refers to the number of carbon atoms being 1-5, for example, 1, 2, 3, 4 or 5, and other similar expressions are expressed in the same way.
[0026] The aliphatic hydrocarbon group with 1-5 carbon atoms refers to an aliphatic hydrocarbon group containing 1-5 carbon atoms, such as methyl, ethyl, propyl, butyl, or pentyl.
[0027] The halogen atoms refer to halogen atoms such as fluorine (F), chlorine (Cl), bromine (Br), or iodine (I).
[0028] The alkylene group with 1-5 carbon atoms refers to an alkylene group containing 1-5 carbon atoms, such as methylene, ethylene, propylene, isopropylene, butylene, or pentylene.
[0029] The term "2-5 carbon atom sub-alkenyl" refers to an sub-alkenyl containing 2-5 carbon atoms, such as vinyl, propenyl, isopropenyl, butenyl, isobutenyl, pentenyl, or isopentenyl.
[0030] In this invention, the cyclic phosphazene compound may be, for example, hexaphenoxycyclotriphosphazene, hexafluorocyclotriphosphazene, pentafluoro(phenoxy)cyclotriphosphazene, ethoxy(pentafluoro)cyclotriphosphazene or a compound with the structure of formula (Ⅲ) below;
[0031]
[0032] In equation (Ⅲ), n is any integer from 3 to 6 (for example, it can be 3, 4, 5, or 6).
[0033] In this invention, the phosphorus-containing compound includes, but is not limited to, products of type PX-200, PX-201, PX-202 or FP-600, and can be commercially available products, such as those manufactured by Daihachi Corporation or ADEKA of Japan.
[0034] Preferably, the resin composition further includes a curing accelerator.
[0035] Preferably, the curing accelerator includes any one or a combination of at least two of pyridine, imidazole, or phosphate accelerators.
[0036] Preferably, the mass ratio of the filler to the phosphorus-containing compound is (30-90):1, for example, it can be 30:1, 35:1, 40:1, 45:1, 50:1, 55:1, 60:1, 65:1, 70:1, 75:1, 80:1, 85:1 or 90:1, etc.
[0037] It is worth noting that by controlling the ratio range of fillers and phosphorus-containing compounds, using a high proportion of fillers in combination with phosphorus-containing compounds can form a dense packing structure, ensuring that oxygen cannot easily penetrate into the resin composition during high-temperature baking.
[0038] Preferably, based on 100% of the total mass of epoxy resin, thermoplastic resin, filler, curing agent, and phosphorus-containing compound in the resin composition, the resin composition comprises 10%-25% epoxy resin, 0.1%-10% thermoplastic resin, 60%-90% filler, 1%-10% curing agent, and 1%-5% phosphorus-containing compound.
[0039] In this invention, based on the total mass of epoxy resin, thermoplastic resin, filler, curing agent, and phosphorus-containing compound in the resin composition as 100%, the content of the epoxy resin is 10%-25%, for example, it can be 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 20%, 22%, or 25%, etc.; the content of the thermoplastic resin is 0.1%-10%, for example, it can be 0.1%, 0.5%, 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, or 10%, etc.; the content of the filler is 60%-90%, for example, The content of the curing agent can be 62%, 65%, 67%, 70%, 72%, 75%, 77%, 80%, 82%, 85%, 87%, 89%, or 90%, etc.; the content of the curing agent is 1%-10%, for example, it can be 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, or 10%, etc.; the content of the phosphorus-containing compound is 1%-5%, for example, it can be 1%, 1.2%, 1.5%, 1.7%, 2%, 2.2%, 2.5%, 2.7%, 3%, 3.2%, 3.5%, 3.7%, 4.0%, 4.2%, 4.5%, or 4.7%, etc.
[0040] In this invention, based on 100 parts by weight of the total mass of epoxy resin, thermoplastic resin, filler, curing agent and phosphorus-containing compound in the resin composition, the amount of the curing accelerator is 0.01-2 parts by weight, for example, it can be 0.01 parts by weight, 0.05 parts by weight, 0.1 parts by weight, 0.3 parts by weight, 0.5 parts by weight, 0.7 parts by weight, 1 part by weight, 1.2 parts by weight, 1.5 parts by weight, 1.7 parts by weight or 2 parts by weight, etc.
[0041] The "parts" and "parts by weight" used in this invention are calculated based on solid content and do not include solvents, dispersants, etc.
[0042] In a second aspect, the present invention provides a resin adhesive solution obtained by dissolving or dispersing the resin composition as described in the first aspect in a solvent.
[0043] In this invention, the conventional preparation method of the resin solution includes: first adding solids, then adding liquid solvent, stirring until the solids are completely dissolved, then adding liquid resin and curing accelerator, and continuing to stir until homogeneous.
[0044] The solvent used in this invention is not particularly limited and can be selected from alcohols such as methanol, ethanol, or butanol; ethyl cellosolve, butyl cellosolve, ethylene glycol methyl ether, carbitol, or butyl carbitol; ketones such as acetone, butanone, methyl ethyl ketone, or cyclohexanone; aromatic hydrocarbons such as toluene and xylene; esters such as ethyl acetate and ethoxyethyl acetate; and nitrogen-containing solvents such as N,N-dimethylformamide and N,N-dimethylacetamide. The above solvents can be used alone or in mixtures of two or more. Ketones such as acetone, butanone, methyl ethyl ketone, or cyclohexanone are further preferred. The amount of solvent added is selected by those skilled in the art based on their experience, to achieve a suitable viscosity for the resin solution; no specific limitation is made here.
[0045] Thirdly, the present invention provides a resin film comprising a release film and a resin composition as described in the first aspect, which is attached to the release film after coating and drying.
[0046] Preferably, the oxygen permeability of the resin composition layer of the resin film, after curing at 200°C for 90 minutes, is ≤50cc / m³. 2 ·day, for example 48cc / m 2 ·day, 45cc / m 2 ·day, 42cc / m 2 ·day, 40cc / m 2 ·day, 38cc / m 2 ·day, 35cc / m 2 ·day, 32cc / m 2 ·day, 30cc / m 2 ·day, 20cc / m 2 ·day, 10cc / m 2 ·day, 5cc / m 2 ·day or 0.1cc / m 2 ·day, etc.
[0047] In this invention, the resin composition enables the oxygen permeability of the resin film to be within a suitable range, thereby slowing down the oxidation rate of the resin film during high-temperature baking and curing and preventing yellowing.
[0048] Fourthly, the present invention provides a printed wiring board, the printed wiring board comprising a first conductor layer, a second conductor layer, and an insulating layer formed between the first conductor layer and the second conductor layer.
[0049] Preferably, the insulating layer contains a cured product of the resin composition as described in the first aspect.
[0050] The present invention also provides an application of a resin composition used in the preparation of resin cured products, sheet-like laminates or resin sheets.
[0051] The numerical range described in this invention includes not only the point values listed above, but also any point values within the numerical ranges not listed above. Due to space limitations and for the sake of brevity, this invention will not exhaustively list all the specific point values included in the range.
[0052] Compared with the prior art, the present invention has the following beneficial effects:
[0053] (1) The resin composition provided by the present invention comprises a combination of epoxy resin, thermoplastic resin, curing agent, filler, and phosphorus-containing compound. Through the screening and synergistic compounding of specific components, the resin film or cured resin obtained by the resin composition has low CTE, high thermal conductivity, and excellent resistance to yellowing; wherein, the CTE is 18-24 ppm / ℃, the thermal conductivity is 1.7-2.3 W / m·K, and the oxygen permeability is 32-45 cc / m 2 • Day, it does not yellow after being baked and cured at high temperature.
[0054] (2) The present invention uses a high proportion of fillers with specific parameters to form a dense stacked structure with phosphorus-containing compounds, which ensures that oxygen is difficult to penetrate into the resin composition during high-temperature baking. At the same time, the proportion range of fillers and phosphorus-containing compounds is controlled. An appropriate amount of phosphorus-containing compounds can also react with the penetrated oxygen, reduce the oxygen concentration in the film, thereby slowing down the oxidation rate of the resin composition during processing and further preventing yellowing after baking. Detailed Implementation
[0055] The technical solution of the present invention will be further illustrated below through specific embodiments. Those skilled in the art should understand that the embodiments described are merely illustrative of the present invention and should not be construed as limiting the invention in any way.
[0056] All materials used in the specific embodiments of this invention can be purchased commercially or prepared using conventional methods in the prior art. Unless otherwise specified, the materials used in this invention are as follows:
[0057] Epoxy Resin 1: Biphenyl type epoxy resin, NC3000, Nippon Kayaku;
[0058] Epoxy Resin 2: Bisphenol A type epoxy resin, NPES-901, Nan Ya;
[0059] Thermoplastic Resin 1: Phenoxy Resin, ERF-001, Nippon Steel Chemicals;
[0060] Thermoplastic resin 2: Polyvinyl alcohol acetal resin, KS-5, Sekisui Chemicals, Japan;
[0061] Curing agent 1: 4,4-Diaminodiphenyl sulfone (DDS), Atul, India;
[0062] Curing agent 2: Reactive ester resin, HPC-8000-65T, DIC Japan;
[0063] Curing agent 3: Phenol-biphenylalkyl type phenolic resin, MEH-7851, Meiwa Kasei Corporation, Japan.
[0064] Filler 1: Alumina 1, with an average sphericity of 0.75 and a specific surface area of 2 m². 2 / g, bulk density is 3.2g / cm³ 3 ;
[0065] Filler 2: Alumina 2, with an average sphericity of 0.8 and a specific surface area of 0.5 m². 2 / g, bulk density is 3.6g / cm³ 3 ;
[0066] Filler 3: Alumina 3, with an average sphericity of 0.75 and a specific surface area of 3.8 m². 2 / g, bulk density is 2.8g / cm³ 3 ;
[0067] Filler 4: Alumina 4, with an average sphericity of 0.75 and a specific surface area of 1.7 m². 2 / g, bulk density is 2.2g / cm³ 3 ;
[0068] Phosphorus-containing compound 1: PX-200, Daihachi Chemical, Japan, resorcinol bis[di(2,6-dimethylphenyl)phosphate], structural formula as follows:
[0069]
[0070] Phosphorus-containing compound 2: PX-202, Daihachi Chemical, Japan, biphenyl bisphenol di(di-2,6-dimethylphosphophosphate), structural formula as follows:
[0071]
[0072] Phosphorus-containing compound 3: FP-600, ADEKA, bisphenol A bis-diphenyl phosphate, with the following structural formula:
[0073]
[0074] Phosphorus-containing compound 4: FP-100, Fushimi Pharmaceutical, hexaphenoxycyclotriphosphazene, structural formula as follows:
[0075]
[0076] Curing accelerator 1: 2-Phenylidene imidazole (2-PZ), BASF, Germany;
[0077] Curing accelerator 2: 4-Dimethylaminopyridine (DMAP), Guangrong Chemical.
[0078] Example 1
[0079] This embodiment provides a resin composition and its application, wherein the preparation method of the resin solution includes:
[0080] First, dissolve 5 parts of curing agent (DDS) and 1 part of curing accelerator (2-PZ) in an appropriate amount of methyl ethyl ketone and stir for more than 60 minutes;
[0081] Then, biphenyl epoxy resin (NC3000, Nippon Kayaku), phenoxy resin (ERF-001, Nippon Steel Chemical), phosphorus-containing compound (PX-200, Daihachi Chemical) and alumina 1 are added in sequence at a solid mass ratio of 18:5:2:70. The mixture is stirred for more than 4 hours to fully mix and form a solution with a solid content of 70%.
[0082] The resin solution provided in Example 1 was coated onto a release film, dried, and then baked in an oven at 130°C for 3 minutes to obtain a resin film with a semi-cured resin layer. Subsequently, the semi-cured resin film (40 μm thick) and the browned PCB (Printed Circuit Board) were pressed and cured to form a printed wiring board with circuits.
[0083] The performance testing methods for the obtained printed wiring board are as follows:
[0084] (1) Coefficient of thermal expansion (CTE): A fully cured resin film sample with a length of 60 mm, a width of 4 mm, and a thickness of 40 μm (curing conditions: 200 °C, 90 min) was taken, dried in an oven at 105 °C for 1 h, and then cooled to room temperature in a desiccator. The mechanical thermal analysis (TMA) method was used for measurement. The heating rate was 10 °C / min, and the temperature was increased from room temperature to 300 °C twice. After the first heating was completed and the sample was cooled to room temperature, it was repositioned for the second heating. The result was the coefficient of thermal expansion in the plane from 25 °C to 150 °C during the second heating, and the unit was ppm / °C.
[0085] (2) Thermal conductivity: In accordance with the ASTM D5470 test method, the cured resin film (curing conditions 200℃, 90min) was prepared into a sample of 25.4mm×25.4mm to test the thermal conductivity of the board.
[0086] (3) Oxygen permeability: After the resin film is cured at 200℃ for 90 min, the release film is removed, exposing the two surfaces of the resin layer. The measured value is obtained according to JIS K7126-2:2006 (isobaric method) at 23℃ and 0%RH atmosphere, where RH represents relative humidity.
[0087] (4) Yellowing after high temperature baking: After the resin film is cured at 200℃ for 240 min, it is taken out and the color change is observed. The criteria for judging the color change are to use a colorimeter to test the L, a, and b values of the sample release film surface. Compared with the uncured state, if ΔE*≤3.0, it is judged as no color change; if ΔE*≥6.0, it is judged as severe color change; and the rest are slight color change.
[0088] The performance test results are shown in Tables 1 and 2.
[0089] Examples 2-8 and Comparative Examples 1-3
[0090] Except for changes in the materials and proportions of the resin mixture used in Example 1, the component formulations of the resin adhesive are shown in Tables 1 and 2. Other methods, such as the preparation methods of the printed wiring board and the fixing sheet, and the performance testing methods, are all performed in accordance with Example 1.
[0091] Table 1
[0092]
[0093]
[0094] Table 2
[0095]
[0096]
[0097] From Table 1 and Table 2, we can see that:
[0098] The resin compositions provided in Examples 1-6 of this invention produce resin films or cured resins with low CTE, high thermal conductivity, and excellent resistance to yellowing. Specifically, the CTE is 18-24 ppm / ℃, the thermal conductivity is 1.7-2.3 W / m·K, and the oxygen permeability is 32-45 cc / m². 2 ·day.
[0099] A comparison of Examples 1 and 7-8 shows that when the mass ratio of filler to phosphorus-containing compound is not within the preferred range of (30-90):1, slight discoloration will occur after high-temperature baking.
[0100] As can be seen from the comparison between Example 1 and Comparative Examples 1-2, when the specific surface area or bulk density of the filler is not within the range of the present invention, the oxygen permeability will increase significantly, and severe discoloration will occur after high-temperature baking.
[0101] As can be seen from the comparison between Example 1 and Comparative Example 3, when phosphorus-containing compounds are not used in the resin composition, the oxygen permeability will increase significantly, and severe discoloration will occur after high-temperature baking.
[0102] The applicant declares that the above description is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily conceived by those skilled in the art within the technical scope disclosed in the present invention fall within the protection and disclosure scope of the present invention.
Claims
1. A resin composition, characterized in that, The resin composition comprises the following components: epoxy resin, thermoplastic resin, curing agent, filler, and phosphorus-containing compound; The specific surface area of the filler is 0.3-3.5 m². 2 / g, bulk density is 2.5-3.8g / cm³ 3 .
2. The resin composition according to claim 1, characterized in that, The epoxy resin includes any one or a combination of at least two of the following: bisphenol A type epoxy resin, bisphenol F type epoxy resin, phosphorus-containing epoxy resin, MDI modified epoxy resin, phenolic epoxy resin, biphenyl type epoxy resin, dicyclopentadiene type epoxy resin, naphthalene-containing epoxy resin, or alicyclic epoxy resin. Preferably, the thermoplastic resin includes any one or a combination of at least two of the following: phenoxy resin, polyvinyl acetal resin, polyolefin resin, polybutadiene resin, polyimide resin, polyamide-imide resin, polyether-imide resin, polysulfone resin, polyethersulfone resin, polyphenylene ether resin, polycarbonate resin, polyetheretherketone resin, polyester resin, or acrylic resin.
3. The resin composition according to claim 1 or 2, characterized in that, The curing agent includes any one or a combination of at least two of the following: reactive ester resin, cyanate ester resin, benzoxazine resin, phenolic resin, carbodiimide resin, maleimide resin, or amine curing agent; Preferably, the filler comprises any one or a combination of at least two of alumina, aluminum nitride, magnesium oxide, or silicon dioxide; Preferably, the average sphericity of the packing is ≥0.
7.
4. The resin composition according to any one of claims 1-3, characterized in that, The phosphorus-containing compound includes any one or a combination of at least two of the structures of formula (I), formula (II), or cyclic phosphazene compounds; Among them, R C1 -R C5 Each is independently selected from aliphatic hydrocarbon groups or halogen atoms having 1-5 carbon atoms; A c Selected from alkylene groups (1-5 carbon atoms), alkenyl groups (2-5 carbon atoms), ether groups, thioether groups, sulfinyl groups, esteryl groups, ketone groups, or single bonds; e and f are each independently selected from any integer between 0 and 5; g, h, and i are each independently selected from any integer between 0 and 4.
5. The resin composition according to any one of claims 1-4, characterized in that, The resin composition further includes a curing accelerator; Preferably, the curing accelerator includes any one or a combination of at least two of pyridine, imidazole, or phosphate accelerators.
6. The resin composition according to any one of claims 1-5, characterized in that, The mass ratio of the filler to the phosphorus-containing compound is (30-90):
1.
7. The resin composition according to claim 5, characterized in that, Based on the total mass of epoxy resin, thermoplastic resin, filler, curing agent and phosphorus-containing compound in the resin composition as 100%, the resin composition comprises 10%-25% epoxy resin, 0.1%-10% thermoplastic resin, 60%-90% filler, 1%-10% curing agent and 1%-5% phosphorus-containing compound; Preferably, the amount of curing accelerator is 0.01-2 parts by weight, based on 100 parts by weight of the total mass of epoxy resin, thermoplastic resin, filler, curing agent and phosphorus-containing compound in the resin composition.
8. A resin adhesive, characterized in that, The resin solution is obtained by dissolving or dispersing the resin composition as described in any one of claims 1-7 in a solvent.
9. A resin film, characterized in that, The resin film includes a release film and a resin composition as described in any one of claims 1-7, which is applied to and dried on the release film. Preferably, the oxygen permeability of the resin composition layer of the resin film, after curing at 200°C for 90 minutes, is ≤50cc / m³. 2 ·day.
10. A printed wiring board, characterized in that, The printed wiring board includes a first conductor layer, a second conductor layer, and an insulating layer formed between the first conductor layer and the second conductor layer; Preferably, the insulating layer contains a cured product of the resin composition as described in any one of claims 1-7.