Phosphoric acid modified aluminum nitride / epoxy resin high-thermal-conductivity insulating composite material and preparation method thereof
By generating an aluminum phosphate coating layer in situ on the AlN surface, the problems of high interfacial thermal resistance and easy hydrolysis of AlN in AlN/EP composite materials are solved, achieving a synergistic improvement in thermal conductivity, insulation and mechanical properties. The preparation process is simple and easy to scale up.
Patent Information
- Application Number
- CN202611266695.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-20
- Publication Date
- 2026-11-24
AI Technical Summary
Existing AlN/EP composite materials suffer from high interfacial thermal resistance, easy hydrolysis of AlN, and difficulty in synergistically improving thermal conductivity, insulation, and mechanical properties.
An aluminum phosphate coating layer is generated by reacting phosphoric acid with aluminum nitride under anhydrous conditions. This coating layer serves as an anti-hydrolysis passivation layer, an interfacial bonding layer, and a thermal conductivity bridging layer. By constructing the aluminum phosphate interfacial layer in situ, the interfacial bonding strength is enhanced and the interfacial thermal resistance is reduced.
This method achieves a synergistic improvement in the interfacial compatibility and thermal conductivity of AlN and epoxy resin, significantly reduces interfacial thermal resistance, enhances insulation and mechanical properties, ensures long-term service reliability, and simplifies the preparation process.
Smart Images

Figure CN123152251A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of insulating composite materials technology, and particularly relates to a phosphate-modified aluminum nitride / epoxy resin high thermal conductivity insulating composite material and its preparation method. Background Technology
[0002] With the rapid development of 5G mobile communication, new energy vehicles, high-power power electronic devices, and high-density packaging technologies, the heat flux density generated inside electronic devices is increasing exponentially. Statistics show that over 55% of electronic device failures are caused by heat accumulation due to poor heat dissipation. Therefore, efficient thermal management has become a core challenge for ensuring equipment reliability and extending its service life. Epoxy resin (EP) is widely used as an electronic packaging material, insulating potting compound, copper-clad laminate substrate, and structural adhesive due to its excellent electrical insulation properties, high adhesion, good chemical corrosion resistance, low shrinkage, and ease of processing. However, pure epoxy resin is an amorphous polymer. The disordered arrangement of its molecular chain segments and the presence of numerous phonon scattering centers result in an extremely low intrinsic thermal conductivity, typically only 0.2 W·m. -1 ·K -1 The thermal conductivity of polymer-based composite materials is far from meeting the heat dissipation requirements of modern high-power electronic devices. Currently, the mainstream strategy for improving the thermal conductivity of polymer-based composite materials is to fill them with inorganic fillers with high thermal conductivity.
[0003] Among numerous thermally conductive fillers, aluminum nitride (AlN) has attracted much attention due to its excellent electrical insulation and high theoretical thermal conductivity. However, AlN / EP composite systems face a core challenge: the interfacial thermal resistance between the filler and the matrix. Because of the significant differences in surface energy, polarity, and chemical affinity between inorganic AlN particles and the organic EP matrix, direct blending leads to numerous voids and defects at the interface. Phonons undergo severe scattering when crossing this discontinuous interface, resulting in the actual thermal conductivity of the composite material being far lower than the predicted value based on theoretical models. To address this issue, researchers have proposed various interfacial modification strategies. While silane coupling agent modification can improve the chemical compatibility between AlN and epoxy resin through organic molecular chains, the organic interfacial layer itself has extremely poor thermal conductivity, and its phonon spectrum is mismatched with both the inorganic AlN and epoxy resin matrix, becoming a "thermal barrier" for phonon transmission. This method cannot effectively reduce interfacial thermal resistance from a physical standpoint; it is essentially a compromise of "sacrificing thermal conductivity channels for compatibility." While the three-dimensional continuous skeleton construction method can achieve high thermal conductivity, the process is complex and costly, and the continuous ceramic skeleton may become a leakage current channel. Existing studies generally do not evaluate its electrical insulation performance, resulting in functional blind spots in application scenarios.
[0004] Furthermore, existing technologies generally neglect the hydrolysis problem of AlN and the systematic lack of synergistic optimization of multiple properties. AlN is highly susceptible to hydrolysis in humid environments or during processing, forming a loose Al(OH)3 weak boundary layer. However, existing surface modification methods (such as silane coupling agents) cannot provide effective hydrolysis protection for AlN, which directly leads to the long-term reliability degradation of composite materials. At the same time, most existing AlN / EP research falls into the trap of "single-indicator driven"—focusing only on thermal conductivity or compatibility, while ignoring the multi-dimensional synergistic requirements for breakdown strength, volume resistivity, mechanical properties, and long-term service stability in real-world applications. There is a lack of systematic synergistic optimization design for thermal conductivity, insulation, mechanical properties, and reliability. Existing literature reports the use of phosphoric acid or phosphates for surface treatment of various inorganic powders, including aluminum nitride (AlN), such as Al2O3, TiO2, and ZrO2. The basic principle is to utilize the chemical reaction between phosphate ions and metal ions or hydroxyl groups on the surface of inorganic particles to form a phosphate layer. In terms of applications, this technology has been used as a high-temperature inorganic binder, an acid activator for geopolymer building materials, and an inorganic adhesive for the preservation and restoration of cultural relics. A common characteristic of these existing technologies is that the purpose of phosphoric acid / phosphate modification is to utilize its bulk properties as a binder matrix or coating matrix, rather than as a surface functionalized layer for thermally conductive fillers. None of the aforementioned studies have addressed the dispersion of phosphoric acid-modified AlN as a thermally conductive filler in the polymer matrix, nor have they assessed its comprehensive impact on the thermal conductivity, insulation, and mechanical properties of polymer composites. Furthermore, most of these technologies are conducted in aqueous or hydrated systems, failing to consider the crucial role of anhydrous conditions in the structural integrity of the modified layer and the hydrolysis resistance of AlN. Therefore, there is an urgent need to develop a novel interface modification strategy that can simultaneously reduce interfacial thermal resistance, inhibit AlN hydrolysis, enhance interfacial bonding, and achieve a synergistic improvement in thermal conductivity, insulation, and mechanical properties. Summary of the Invention
[0005] The technical problem to be solved by this invention is to address the shortcomings of existing AlN / EP composite materials, such as high interfacial thermal resistance, easy hydrolysis of AlN, and difficulty in synergistically improving thermal conductivity, insulation performance, and mechanical properties. This invention provides a phosphoric acid-modified aluminum nitride / epoxy resin high thermal conductivity insulating composite material and its preparation method, which can simultaneously achieve hydrolysis resistance protection, reduce interfacial thermal resistance, enhance interfacial bonding strength, and achieve synergistic optimization of multiple properties.
[0006] To solve the above-mentioned technical problems, the present invention adopts the following technical solution.
[0007] A method for preparing a phosphoric acid-modified aluminum nitride / epoxy resin high thermal conductivity insulating composite material includes the following steps: (1) Dry the aluminum nitride powder under vacuum at 120-150℃ for 2-4 hours; (2) Prepare a modified mixture by mixing a 10-25 wt% aqueous solution of phosphoric acid with anhydrous ethanol at a volume ratio of 1:5 to 1:15; add the dried aluminum nitride powder from step (1) to the modified mixture, ultrasonically disperse for 15-30 min, and stir at 60-80℃ for 4-8 h to allow the phosphoric acid to react chemically with the surface of aluminum nitride and generate an aluminum phosphate coating layer in situ; after the reaction is completed, centrifuge, wash, and vacuum dry at 100-120℃ for 12-24 h to obtain phosphoric acid modified aluminum nitride powder; (3) Add the phosphoric acid modified aluminum nitride powder obtained in step (2) to the epoxy resin at a mass fraction of 15-40wt%, stir and disperse evenly, add curing agent, degas under vacuum, pour into mold, cure by two-stage thermal curing process, cool and demold to obtain the phosphoric acid modified aluminum nitride / epoxy resin high thermal conductivity insulating composite material.
[0008] Furthermore, the thickness of the aluminum phosphate coating layer in step (2) is 2-6 nm, preferably 3-4 nm.
[0009] Further, in step (2), the concentration of the phosphoric acid aqueous solution is 15 wt%, the volume ratio of the phosphoric acid aqueous solution to anhydrous ethanol is 1:10, the reaction temperature of the constant temperature stirring reaction is 60°C, and the reaction time is 5 h.
[0010] Further, the mass fraction of the phosphoric acid modified aluminum nitride powder in step (3) is 25-40 wt%, preferably 35 wt%.
[0011] Furthermore, the two-stage thermosetting process in step (3) is as follows: first, pre-curing at 80°C for 1 hour, and then curing at 100°C for 10-24 hours.
[0012] Further, the epoxy resin mentioned in step (3) is E51 epoxy resin, the curing agent is D230 polyetheramine curing agent, and the mass ratio of epoxy resin to curing agent is 10:3.
[0013] Furthermore, the average particle size of the aluminum nitride powder in step (1) is 1-3 μm.
[0014] A phosphoric acid-modified aluminum nitride / epoxy resin high thermal conductivity insulating composite material is prepared by any of the above preparation methods.
[0015] Compared with the prior art, the outstanding substantive features and significant progress of the present invention are mainly reflected in the following aspects.
[0016] Firstly, this invention applies a phosphoric acid / aluminum dihydrogen phosphate composite modification system to the field of AlN / EP thermally conductive and insulating composite materials, achieving in-situ construction of an aluminum phosphate inorganic interface layer. While the surface modification of inorganic powders by phosphoric acid and phosphates has been reported, its applications are concentrated in high-temperature inorganic binders, geopolymer building materials, wide-temperature-range lubricating coatings, and cultural relic protection and restoration, where its functional positioning utilizes the bulk properties of phosphates as binder or coating matrices. Compared to the aforementioned prior art, this invention applies an inorganic modification system of Al(H2PO4)3 and H3PO4 to the field of AlN / EP thermally conductive and insulating composite materials, generating a nanoscale aluminum phosphate inorganic coating layer in situ on the AlN surface. This inorganic layer plays a triple role: as an anti-hydrolysis passivation layer, it effectively isolates moisture and prevents AlN from hydrolyzing during processing and service to form a loose AlOOH / Al(OH)3 weak boundary layer, a function that existing silane coupling agent modification technologies cannot achieve; as an interfacial bonding layer, its abundant P-OH groups form a hydrogen bond network with the epoxy resin matrix, significantly enhancing the interfacial bonding strength; and as a thermal conductivity bridging layer, AlPO4 has high intrinsic thermal conductivity, and its phonon spectrum matches well with both AlN and epoxy resin, which can significantly reduce interfacial thermal resistance. This is fundamentally different from the compromise solution in existing technologies where organosilane interfacial layers become phonon transport "thermal barriers" due to their extremely poor thermal conductivity and mismatched phonon spectra with both inorganic AlN and epoxy resin.
[0017] Secondly, this invention achieves a synergistic improvement in interfacial compatibility and thermal conductivity between AlN and epoxy resin through an aluminum phosphate salt interfacial layer, overcoming the prominent contradiction in existing technologies where these two aspects are difficult to balance. In existing technologies, while silane coupling agents can improve the chemical compatibility between AlN and epoxy resin through organic molecular chains, the organic interfacial layer itself has extremely poor thermal conductivity, and its phonon spectrum does not match that of both inorganic AlN and the epoxy resin matrix. Physically, it cannot effectively reduce interfacial thermal resistance, essentially representing a compromise of "sacrificing thermal conductivity channels for compatibility." While the three-dimensional continuous skeleton construction method can achieve high thermal conductivity, it is complex, costly, and the continuous ceramic skeleton may become a leakage path, posing a risk of deterioration in insulation performance. This invention takes a different approach, employing an inorganic aluminum phosphate interface layer to simultaneously address the two core issues of interfacial compatibility and interfacial thermal resistance. On one hand, the P-OH groups on the surface of the aluminum phosphate interface layer form a hydrogen bond network with the epoxy resin matrix, ensuring excellent interfacial compatibility. On the other hand, aluminum phosphate itself has good thermal conductivity, and its phonon spectrum lies between that of inorganic AlN and epoxy resin, acting as a phonon transport bridge and fundamentally reducing interfacial thermal resistance. It is this interface design concept that balances compatibility and thermal conductivity that enables the composite material prepared by this invention to achieve a significant improvement in thermal conductivity while simultaneously enhancing its insulation and mechanical properties, truly realizing synergistic optimization of multiple properties.
[0018] Thirdly, the anhydrous conditions used in this invention for phosphoric acid modification offer two key advantages. Firstly, the anhydrous conditions prevent competitive adsorption of water molecules on the AlN surface, allowing phosphate groups to more fully contact and graft onto the AlN surface, maximizing the effective grafting density and ensuring the density and integrity of the aluminum phosphate coating. Secondly, the anhydrous conditions fundamentally prevent the hydrolysis of AlN during the modification process, ensuring the structural integrity of the interface layer and avoiding the formation of a loose Al(OH)3 weak boundary layer beneath the phosphoric acid coating. This technical feature enables the composite material prepared by this invention to exhibit excellent long-term service reliability under humid and hot environments, effectively overcoming the shortcomings of existing technologies that generally neglect AlN hydrolysis, leading to long-term reliability degradation of composite materials.
[0019] Fourth, the preparation method of the present invention adopts the E51 epoxy resin / D230 polyetheramine curing agent system. The curing process is simple (80℃ / 1h + 100℃ / 10-24h), without the need for complex three-dimensional skeleton construction processes such as freeze drying, ice template or foam gel. The raw materials are readily available, the operation is simple, and it is easy to scale up production, which has significant industrial practical value. Attached Figure Description
[0020] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0021] Figure 1 The figure shows the variation of thermal conductivity of two epoxy resin composite samples with doping concentration.
[0022] Figure 2 The figure shows the variation of interfacial thermal resistance fitting based on the HS model for two epoxy resin composite samples with doping concentration.
[0023] Figure 3 Cross-sectional morphology images of composite material samples with P-AlN filler mass fractions of 0 wt%, 15 wt%, 35 wt%, and 40 wt%.
[0024] Figure 4 The graph shows the change in flashover voltage of the P-AlN / EP composite sample with doping concentration.
[0025] Figure 5 The graph shows the change in bulk resistivity of the P-AlN / EP composite sample with doping concentration.
[0026] Figure 6The graph shows the variation of Young's modulus of the P-AlN / EP composite sample with doping concentration.
[0027] Figure 7 The figure shows the variation of tensile strength of P-AlN / EP composite material samples with doping concentration.
[0028] Figure 8 The figure shows the change in elongation at break of P-AlN / EP composite material samples with doping concentration.
[0029] Figure 9 This is a schematic diagram of the preparation method for P-AlN / EP composite material samples. Detailed Implementation
[0030] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as a limitation of the present invention, but rather as a more detailed description of certain aspects, features, and embodiments of the present invention.
[0031] All raw materials used in this invention are not particularly limited in their source; they can be purchased from the market or prepared using conventional methods known to those skilled in the art.
[0032] There are no particular restrictions on the purity of any of the raw materials used in this invention. However, this invention preferably uses raw materials of analytical grade or purity commonly used in the field of chemical synthesis.
[0033] This invention provides a method for preparing a phosphoric acid-modified aluminum nitride / epoxy resin high thermal conductivity insulating composite material, comprising the following steps: Step 1: Pretreatment of aluminum nitride (AlN) powder. Micron-sized aluminum nitride powder is placed in a vacuum oven and dried at 120-150℃ for 2-4 hours to remove physically adsorbed moisture from the powder surface. The average particle size of the AlN powder is 1-3 μm.
[0034] Step 2: Preparation of anhydrous phosphoric acid-modified AlN (P-AlN). A 10-25 wt% aqueous solution of phosphoric acid was mixed with anhydrous ethanol at a volume ratio of 1:5 to 1:15 and stirred until homogeneous to obtain a modified mixture. The AlN powder pretreated in Step 1 was added to the modified mixture and ultrasonically dispersed for 15-30 min. Then, the mixture was stirred at 60-80℃ for 4-8 h to allow a chemical reaction between the phosphoric acid and the AlN surface, resulting in an in-situ aluminum phosphate coating layer. After the reaction, the mixture was centrifuged and washed 3-5 times with deionized water and anhydrous ethanol, respectively. Finally, it was vacuum dried at 100-120℃ for 12-24 h to obtain phosphoric acid-modified aluminum nitride powder, denoted as P-AlN. Characterization by high-resolution transmission electron microscopy (HR-TEM) showed that the phosphate coating layer thickness was 2-6 nm, preferably 3-4 nm.
[0035] Step 3: Preparation of P-AlN / epoxy resin (P-AlN / EP) composite material. The P-AlN filler obtained in Step 2 was added to the E51 epoxy resin matrix at a predetermined mass fraction (0-40 wt%). The mixture was stirred continuously at 60°C for 2 hours to ensure uniform dispersion of the P-AlN filler in the epoxy resin matrix. Curing agent was added at a mass ratio of E51 to D230 curing agent of 10:3, and stirring continued for 30 minutes. The uniformly mixed slurry was placed in a vacuum chamber for degassing until no obvious bubbles were observed, thus eliminating entrained air. The degassed mixture was poured into a polytetrafluoroethylene (PTFE) mold and cured using a two-stage thermosetting process: first, pre-curing at 80°C for 1 hour, and then curing at 100°C for 10-24 hours to complete the crosslinking reaction. After curing, the mixture was allowed to cool naturally to room temperature and demolded to obtain the phosphate-modified aluminum nitride / epoxy resin high thermal conductivity insulating composite material.
[0036] The flowchart of the above preparation method is shown below. Figure 9 As shown. The core of this invention lies in the in-situ generation of an aluminum phosphate nanocoating layer by reacting anhydrous phosphoric acid with the active sites on the AlN surface. This inorganic layer has three functions: first, as an anti-hydrolysis passivation layer, it effectively isolates moisture and prevents AlN from hydrolyzing during processing and service to form a weak Al(OH)3 boundary layer; second, as an interfacial bonding layer, its abundant P-OH groups can form a hydrogen bond network with the epoxy resin matrix, enhancing the interfacial bonding strength; third, as a thermal conductivity bridging layer, AlPO4 has high intrinsic thermal conductivity, and its phonon spectrum matches well with both AlN and epoxy resin, significantly reducing interfacial thermal resistance. This is fundamentally different from the compromise solution in existing technologies where organosilane interfacial layers sacrifice thermal conductivity for compatibility. Furthermore, the present invention employs anhydrous conditions for modification, which on the one hand avoids competitive adsorption of water molecules on the AlN surface, allowing phosphate groups to more fully contact and graft onto the AlN surface, maximizing the effective grafting density; on the other hand, it avoids the hydrolysis reaction of AlN, ensuring the structural integrity of the interface layer and preventing the formation of a loose Al(OH)3 weak boundary layer under the phosphate coating.
[0037] The present invention will be further described in detail below through specific embodiments, but the scope of protection of the present invention is not limited thereto.
[0038] Example 1 Step 1: Place AlN powder with an average particle size of 2μm in a vacuum oven and dry it at 120℃ for 3h.
[0039] Step 2: Mix a 15wt% aqueous solution of phosphoric acid with anhydrous ethanol at a volume ratio of 1:10, stir until homogeneous, and prepare a modified mixture. Add the pretreated AlN powder from Step 1 to the modified mixture, ultrasonically disperse for 20 min, and then stir at 60℃ for 5 h. After the reaction is complete, centrifuge, wash three times each with deionized water and anhydrous ethanol, and then vacuum dry at 120℃ for 24 h to obtain P-AlN powder.
[0040] Step 3: Add P-AlN to E51 epoxy resin at a mass fraction of 15 wt%, and stir at 60℃ for 2 hours. Add curing agent at a mass ratio of E51 to D230 curing agent of 10:3, and continue stirring for 30 minutes. After vacuum degassing, pour into a PTFE mold, pre-cur at 80℃ for 1 hour, cure at 100℃ for 10 hours, and demold naturally to obtain P-AlN / EP composite material.
[0041] Example 2 The mass fraction of P-AlN filler is 25wt%, and the remaining steps are the same as in Example 1.
[0042] Example 3 The P-AlN filler mass fraction was 35 wt%, and the remaining steps were the same as in Example 1. This example is the optimal example, and the thickness of the obtained P-AlN coating layer is approximately 3.57 nm, resulting in the best overall performance of the composite material.
[0043] Example 4 The mass fraction of P-AlN filler is 40 wt%, and the remaining steps are the same as in Example 1.
[0044] Example 5 Step 1: Place AlN powder with an average particle size of 2μm in a vacuum oven and dry it at 150℃ for 2h.
[0045] Step 2: Mix a 10wt% aqueous solution of phosphoric acid with anhydrous ethanol at a volume ratio of 1:5 and stir until homogeneous. Add AlN powder, ultrasonically disperse for 15 min, and stir at 80℃ for 4 h. Centrifuge, wash three times each with deionized water and anhydrous ethanol, and vacuum dry at 100℃ for 12 h to obtain P-AlN powder.
[0046] Step 3: Add P-AlN to E51 epoxy resin at a mass fraction of 35wt%, and follow the same steps as in Example 1.
[0047] Example 6 Step 1: Same as in Example 1, dry AlN powder at 120℃ for 3 hours.
[0048] Step 2: Mix a 25wt% aqueous solution of phosphoric acid with anhydrous ethanol at a volume ratio of 1:15 and stir until homogeneous. Add AlN powder, ultrasonically disperse for 30 min, and stir at a constant temperature of 60℃ for 8 h. Centrifuge, wash 5 times each with deionized water and anhydrous ethanol, and vacuum dry at 120℃ for 24 h to obtain P-AlN powder.
[0049] Step 3: Add P-AlN to E51 epoxy resin at a mass fraction of 35wt%, and follow the same steps as in Example 1.
[0050] Example 7 Step 1: Place AlN powder with an average particle size of 2μm in a vacuum oven and dry it at 120℃ for 4h.
[0051] Steps 2 and 3 are the same as in Example 3, with a phosphoric acid concentration of 15 wt%, a volume ratio of 1:10, ultrasonication for 20 min, reaction at 60°C for 5 h, and P-AlN filler of 35 wt%.
[0052] Comparative Example 1 No fillers were added. E51 epoxy resin was added to D230 curing agent at a mass ratio of 10:3, stirred for 30 minutes, vacuum degassed, poured into PTFE mold, pre-cured at 80℃ for 1 hour, cured at 100℃ for 10 hours, and demolded naturally to obtain pure EP sample.
[0053] Comparative Example 2 AlN powder with an average particle size of 2 μm was dried at 120 °C for 3 h without phosphoric acid modification. It was then added to E51 epoxy resin at a mass fraction of 35 wt%, with the remaining steps the same as in Example 1, to obtain an unmodified AlN / EP composite material.
[0054] Comparative Example 3 AlN was surface modified using silane coupling agent KH-550. KH-550 was added at 2 wt% of AlN to a 95 wt% ethanol aqueous solution and hydrolyzed for 1 h. AlN powder dried at 120°C for 3 h was added, and the mixture was stirred at 80°C for 4 h. After washing and drying, silane-modified AlN was obtained. This modified AlN was then added at 35 wt% of E51 epoxy resin, with the remaining steps the same as in Example 1, to obtain a silane-modified AlN / EP composite material.
[0055] Comparative Example 4 The modification solution used only a 15wt% aqueous solution of phosphoric acid, without the addition of anhydrous ethanol. AlN powder dried at 120℃ for 3 hours was added, ultrasonically dispersed for 20 minutes, and reacted at a constant temperature of 60℃ for 5 hours. After centrifugation, washing, and drying, P-AlN powder was obtained. This powder was added to E51 epoxy resin at a mass fraction of 35wt%, and the remaining steps were the same as in Example 1, yielding an aqueous phosphoric acid-modified AlN / EP composite material.
[0056] Experimental Example 1: Thermal Conductivity and Interfacial Thermal Resistance The thermal conductivity was measured using a Hot Disk TPS2500 S thermal conductivity meter based on the transient plane heat source method. A Kapton probe (model 7577) with a radius of 2.001 mm was selected, with a heating power of 0.2 W and a transient test time of 20 s. Five parallel samples were tested for each type of sample, and the average value was taken. Simultaneously, the interfacial thermal resistance was calculated using a Hashin-Shtrikman model. The test results are as follows: Figure 1 and Figure 2 As shown.
[0057] The thermal conductivity of Comparative Example 1 (pure EP) is 0.23 W·m. -1 ·K -1 Example 1 (15wt%) has a thermal conductivity of 0.28 W·m. -1 ·K -1 Example 2 (25wt%) was 0.35 W·m -1 ·K -1 Example 3 (35wt%) was 0.41 W·m -1 ·K -1 Example 4 (40wt%) was 0.38 W·m -1 ·K -1 It can be seen that the thermal conductivity of the P-AlN / EP composite material first increases and then slightly decreases with the filler content, reaching its maximum value in Example 3, which is 78.3% higher than that of pure EP. The thermal conductivity of Examples 5-7 is comparable to that of Example 3, all ranging from 0.40 to 0.42 W·m. -1 ·K -1 Within the range, it indicates that good thermal conductivity can be obtained by different combinations of preparation parameters.
[0058] Regarding interfacial thermal resistance, Comparative Example 2 (unmodified AlN / EP, 35wt%) had an interfacial thermal resistance of 0.285 m·K·W. -1 In Example 3, the interfacial thermal resistance was reduced to 0.177 m·K·W. -1 The thermal resistance decreased by 37.9%, fully demonstrating the significant effect of the aluminum phosphate interface layer as a thermal bridging layer. Comparative Example 3 (silane modified) had an interface thermal resistance of 0.248 m·K·W. -1 The thermal resistance of Comparative Example 4 (modified under aqueous conditions) is higher than that of Example 3, reflecting the inherent defect of poor thermal conductivity in the organosilane interface layer. The interfacial thermal resistance is 0.205 m·K·W. -1 The results are higher than in Example 3, illustrating the necessity of anhydrous conditions for forming a high-quality interface layer.
[0059] Experimental Example 2: Evaluation of Packing Dispersibility The cross-sectional morphology of the composite material was observed using a scanning electron microscope (SEM, Thermo Fisher Scientific Quattro-S), and quantitative image analysis was performed using ImageJ software to calculate the nearest neighbor distance (NND) and Morita index (I), where I=1 represents a completely random distribution (ideally homogeneous), I>1 represents aggregation, and I<1 represents a regular distribution. The test results are as follows: Figure 3 As shown.
[0060] The NND of Example 1 (15 wt%) was 0.42 μm, and the Morita index was 0.89; the NND of Example 2 (25 wt%) was 0.25 μm, and the Morita index was 0.95; the NND of Example 3 (35 wt%) was 0.18 ± 0.07 μm, and the Morita index was 1.07, the closest to 1 among all samples, indicating that the filler dispersion was the most uniform and the filler network was the densest; the NND of Example 4 (40 wt%) rose to 0.35 μm, and the Morita index increased to 1.21, indicating that excessive filler led to significant agglomeration. In contrast, the Morita index of Comparative Example 2 (unmodified AlN / EP, 35 wt%) reached 1.35, showing severe agglomeration, fully demonstrating that phosphoric acid modification significantly improved the dispersion uniformity of AlN in the epoxy resin matrix. The dispersibility of Comparative Example 4 (modified under aqueous conditions) was also inferior to that of Example 3, indicating that the phosphate coating formed under anhydrous conditions is more conducive to filler dispersion.
[0061] Test Example 3: Insulation Performance Surface flashover testing was performed using finger electrodes with an electrode spacing of 10 mm and a voltage of 0.5 kV·s. -1 A constant voltage boost rate was applied until flashover occurred, and the flashover voltage value was recorded. Simultaneously, the volume resistivity was measured using the three-electrode method: a 1kV DC voltage was applied, and the steady-state volume current was recorded after 10 minutes using an electrometer (Keithley 6517b). The volume resistivity was calculated using the formula ρV=(TS×S) / (U×IV), where TS is the sample thickness, S is the area of the collecting electrode, U is the applied voltage, and IV is the volume current. The test results are as follows: Figure 4 and Figure 5 As shown.
[0062] Comparative Example 1 (pure EP) has a flashover voltage of 14.6 kV and a volume resistivity of 2.73 × 10⁻⁶. -14 Ω·m. Example 3 (35wt%) achieved a flashover voltage of 15.9kV, an 8.9% improvement over pure EP; the volume resistivity reached 4.12×10⁻⁶ Ω·m. -14The Ω·m value was improved by 50.91% compared to pure EP. The flashover voltage and volume resistivity of Examples 1, 2, and 4 were also superior to those of the unmodified AlN / EP composite material with the same content. The insulation performance of Comparative Examples 2 and 3 decreased to varying degrees. These results indicate that the aluminum phosphate inorganic interface layer constructed on the AlN surface through the anhydrous phosphoric acid modification strategy of this invention effectively suppresses charge migration within the composite material, not only preventing the formation of leakage channels but also significantly improving insulation performance.
[0063] Test Example 4: Mechanical Properties The tensile properties of each sample were tested using an electronic universal testing machine (PK-106). Five parallel samples were tested for each type of sample, and the average value was taken. Young's modulus, tensile strength, and elongation at break were extracted from the recorded force-displacement data. The test results are as follows: Figure 6 , Figure 7 and Figure 8 As shown.
[0064] Comparative Example 1 (pure EP) had a tensile strength of 63.4 MPa, a Young's modulus of 3.17 GPa, and an elongation at break of 4.33%. Example 1 (15 wt%) had a tensile strength of 68.2 MPa and a Young's modulus of 3.52 GPa; Example 2 (25 wt%) had a tensile strength of 73.1 MPa and a Young's modulus of 4.12 GPa; Example 3 (35 wt%) achieved the best mechanical properties, with a tensile strength of 77.45 MPa (22.2% higher than pure EP), a Young's modulus of 4.68 GPa (47.6% higher than pure EP), and an elongation at break of 7.45% (72.1% higher than pure EP); Example 4 (40 wt%) showed a decrease in tensile strength to 62.2 MPa, a Young's modulus of 4.49 GPa, and an elongation at break of 6.83% due to filler agglomeration. The mechanical properties of Examples 5-7 were comparable to those of Example 3.
[0065] Comparative Example 2 (unmodified AlN / EP, 35 wt%) had a tensile strength of 58.7 MPa and a Young's modulus of 3.89 GPa, both lower than that of Example 3. Comparative Example 3 (silane modified) had a tensile strength of 71.3 MPa, lower than that of Example 3. Comparative Example 4 (modified under aqueous conditions) had a tensile strength of 70.1 MPa, also lower than that of Example 3. These results indicate that the aluminum phosphate interfacial layer forms a hydrogen bond network with the epoxy resin through P-OH groups, significantly enhancing the interfacial bonding strength and thus achieving a substantial improvement in mechanical properties. The phosphate coating layer prepared under anhydrous conditions has a more complete structure and stronger interfacial bonding.
[0066] The embodiments described above are merely preferred embodiments of the present invention and are not intended to limit the scope of the present invention. Various modifications and improvements made by those skilled in the art to the technical solutions of the present invention without departing from the spirit of the present invention should fall within the protection scope defined by the claims of the present invention.
Claims
1. A method for preparing a phosphoric acid-modified aluminum nitride / epoxy resin high thermal conductivity insulating composite material, characterized in that, Includes the following steps: (1) Dry the aluminum nitride powder under vacuum at 120-150℃ for 2-4 hours; (2) Prepare a modified mixture by mixing a 10-25 wt% aqueous solution of phosphoric acid with anhydrous ethanol at a volume ratio of 1:5 to 1:15; add the dried aluminum nitride powder from step (1) to the modified mixture, ultrasonically disperse for 15-30 min, and stir at 60-80℃ for 4-8 h to allow the phosphoric acid to react chemically with the surface of aluminum nitride and generate an aluminum phosphate coating layer in situ; after the reaction is completed, centrifuge, wash, and vacuum dry at 100-120℃ for 12-24 h to obtain phosphoric acid modified aluminum nitride powder; (3) Add the phosphoric acid modified aluminum nitride powder obtained in step (2) to the epoxy resin at a mass fraction of 15-40wt%, stir and disperse evenly, add curing agent, degas under vacuum, pour into mold, cure by two-stage thermal curing process, cool and demold to obtain the phosphoric acid modified aluminum nitride / epoxy resin high thermal conductivity insulating composite material.
2. The production method according to claim 1, characterized by, The thickness of the aluminum phosphate coating layer in step (2) is 2-6 nm.
3. The production method according to claim 2, characterized by, The thickness of the aluminum phosphate coating layer is 3-4 nm.
4. The method of claim 1, wherein, The concentration of the phosphoric acid aqueous solution in step (2) is 15wt%, the volume ratio of the phosphoric acid aqueous solution to anhydrous ethanol is 1:10, the reaction temperature of the constant temperature stirring reaction is 60℃, and the reaction time is 5h.
5. The preparation method according to claim 1, characterized in that, The mass fraction of the phosphoric acid modified aluminum nitride powder in step (3) is 25-40 wt%.
6. The production method according to claim 5, wherein The mass fraction of the phosphoric acid-modified aluminum nitride powder is 35 wt%.
7. The preparation method according to claim 1, characterized in that, The two-stage thermosetting process described in step (3) is as follows: first, pre-curing at 80℃ for 1 hour, and then curing at 100℃ for 10-24 hours.
8. The method of claim 1, wherein, The epoxy resin mentioned in step (3) is E51 epoxy resin, the curing agent is D230 polyetheramine curing agent, and the mass ratio of epoxy resin to curing agent is 10:
3.
9. The method of claim 1, wherein, The average particle size of the aluminum nitride powder in step (1) is 1-3 μm.
10. A phosphoric acid-modified aluminum nitride / epoxy resin high thermal conductivity insulating composite material, characterized in that, It is prepared by the preparation method according to any one of claims 1 to 9.