A method for manufacturing an insulator core rod by high-performance pultrusion

By leveraging the synergistic effect of components such as E-51 epoxy resin, a high-density cross-linked composite insulator core rod was prepared, solving the problem of performance degradation of composite insulators under high temperature and high humidity environments. This resulted in improved glass transition temperature and water resistance, ensuring the stability and electrical insulation performance of the material under harsh conditions.

CN123152253APending Publication Date: 2026-11-24ZHEJIANG GOLDEN PHOENIX POWER TECH CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202611630349.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2025-12-22
Filing Date
2026-10-21
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing composite insulator core rods are prone to water absorption and expansion, and interface hydrolysis in high temperature, high humidity or salt water environments, leading to cracking and delamination. They are also difficult to maintain mechanical strength and electrical insulation performance at high temperatures. Existing improvement methods cannot simultaneously meet the requirements of high glass transition temperature, water boiling time and interface stability.

Method used

Insulator core rods are prepared by impregnation, curing and pultrusion processes using the synergistic effect of components such as E-51 epoxy resin, multifunctional epoxy resin, linear phenolic resin, reactive diluent, silane coupling agent, hydrophobic silica and anti-hydrolysis agent to form a high-density cross-linked structure, enhance the interfacial bonding and physical barrier between resin and glass fiber and optimize material properties.

Benefits of technology

It improves the thermal stability and high-temperature performance of the material, reduces water absorption and interfacial delamination, ensures rigidity, dimensional stability and electrical insulation performance in harsh environments, and extends service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

This invention discloses a method for preparing insulator core rods by pultrusion of high-performance resin, relating to the field of composite materials. The formulation includes E-51 epoxy resin, multifunctional epoxy resin, methyltetrahydrophthalic anhydride, methylnadic anhydride, linear phenolic resin, reactive diluent, KH-560 coupling agent, hydrophobic silica, and an anti-hydrolysis agent, reinforced with S-glass fiber. The core rods are prepared through pre-curing and post-curing processes. This invention combines heat resistance, moisture resistance, hydrolysis resistance, and mechanical and electrical insulation properties, making it suitable for use in high-voltage / ultra-high-voltage transmission lines.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of composite materials, and in particular to a method for preparing insulator core rods by pultrusion of high-performance pultrusion resin. Background Technology

[0002] Composite insulators (or glass fiber-epoxy resin pultruded core rod insulators) are widely used in high-voltage, ultra-high-voltage, and even extra-high-voltage power transmission systems because they offer advantages over porcelain or glass insulators, including lighter weight, higher strength, resistance to flashover pollution, corrosion resistance, and ease of transportation and installation. Composite insulators have become one of the main products used in power transmission lines both in my country and internationally.

[0003] However, in actual operation, the performance of composite insulator core rods (also known as glass fiber pultruded rods, drawn rods, insulating core rods, etc.) still faces several prominent problems, specifically including:

[0004] Prolonged exposure to high temperature, high humidity, or environments containing saline solutions will cause the material to absorb water, leading to resin matrix expansion, interfacial hydrolysis, and damage to the resin-glass fiber bonding interface, ultimately resulting in cracking, delamination, and decreased insulation performance. For example, in some boiling or "water diffusion" tests, high water absorption rates or surface cracks and delamination appear after tens to hundreds of hours. Domestic companies typically require a water absorption rate of ≤0.05% for high-temperature composite insulator core rods, and the current leakage or deformation index in water diffusion tests under boiling conditions for 100 hours (or a similar timescale) must be at a very low level.

[0005] Under high-temperature operating conditions, such as summer environments, high loads, or direct sunlight, the mandrel temperature may rise beyond the tolerance range of traditional epoxy resin materials. If the temperature resistance (Tg) is low (e.g., 150-180℃ or lower), some segments of the resin network may lose rigidity, resulting in a decrease in mechanical strength, electrical insulation strength, and dimensional stability. For harsh conditions such as ultra-high voltage, ultra-long span, or DC environments, the Tg requirements for mandrel materials are becoming increasingly stringent.

[0006] The interfacial bond strength between resin and glass fiber is a crucial factor determining the long-term performance of composite materials. If the interfacial coupling agent is poorly treated or exposed to environments such as acid rain, salt spray, or ultraviolet radiation, the interface is prone to hydrolysis or chemical corrosion, leading to fiber exposure, resin delamination, internal microscopic damage, and even a sharp decrease in mechanical strength. Analysis of "early decay failure of composite insulators" in the literature indicates that in heating or high-humidity areas, the epoxy resin matrix experiences corrosion, glass fiber exposure, and, under high humidity and temperature conditions, the resin-fiber interface detaches.

[0007] For example, to improve Tg or heat resistance, the crosslinking density may be increased or a curing agent / resin with high functionality may be added, which may lead to increased viscosity of the resin system, poor wettability, and difficulties in pultrusion process; or hydrophobic fillers or surface treatment agents may be added to enhance moisture resistance, but these additives may affect mechanical strength or long-term thermal stability.

[0008] Patent CN109233710A discloses an insulating material with high glass transition temperature and high-temperature adhesion. Its resin composition includes a tetrafunctional epoxy resin, an organosilicon epoxy resin, a phenolic resin, a polyurethane-modified epoxy resin, and a dispersant; the curing agent composition includes pyromellitic anhydride, a toughening agent, and a composite accelerator. This patent improves the glass transition temperature and high-temperature adhesion of the insulating material through modification with metallic silicon powder.

[0009] Furthermore, patent document CN110482879B, "A glass fiber impregnating agent for ultra-high voltage composite insulators and its preparation method, product and application process," focuses on the formulation and preparation of glass fiber impregnating agents to improve the wettability and interfacial adhesion of glass fibers in resin, thereby enhancing mechanical, electrical and aging resistance properties.

[0010] Despite these improvements, gaps still exist in reality:

[0011] There are very few reports of material systems achieving such a long water boiling time (continuous exposure to boiling water or high humidity environment) of 500 hours without cracking / delamination;

[0012] Achieving a Tg ≥ 200℃ and high mechanical strength while meeting the requirements of the pultrusion process (i.e., resin viscosity, wettability, and curing process suitable for continuous production) is extremely challenging.

[0013] It maintains interface stability and overall structural integrity under multiple environments such as moisture absorption, acid rain, and salt spray, but there is limited long-term reliability verification. Summary of the Invention

[0014] Based on the problems mentioned above in the background technology, this invention proposes a method for preparing insulator core rods by pultrusion of high-performance pultrusion resin, the technical solution of which is as follows:

[0015] A method for preparing insulator core rods by pultrusion of high-performance resin, wherein the insulator core rod is prepared by fully fusing E-51 epoxy resin, multifunctional epoxy resin, linear phenolic resin, reactive diluent, internal release agent, silane coupling agent KH-560, hydrophobic silica, anti-hydrolysis agent, methyltetrahydrophthalic anhydride, methylnadic anhydride, and ethylene glycol dimercaptoacetate, followed by impregnation, curing, and traction cutting.

[0016] Furthermore, the preparation of the insulator core rod includes the following steps, in parts by weight:

[0017] (A) Stir 100 parts of E-51 epoxy resin and 10-20 parts of multifunctional epoxy resin evenly, and then mix the linear phenolic resin with the mixed epoxy resin again at 70 degrees until the resin is transparent and clear.

[0018] (B) Add 10-20 parts of reactive diluent to (A) and stir to mix evenly;

[0019] (C) Add 1-3 parts of internal release agent and mix well;

[0020] (D) Add 1-3 parts of silane coupling agent KH-560, 1-5 parts of hydrophobic silica, and 0.5-2 parts of anti-hydrolysis agent and stir until homogeneous;

[0021] (E) Add 10-70 parts of methyltetrahydrophthalic anhydride and 10-70 parts of methylnadic anhydride as two curing agents, and stir evenly;

[0022] (F) Add 0.01-0.06 parts of ethylene glycol dimercaptoacetate and 0.1-0.6 parts of triethylamine and stir to fully mix with the acid anhydride and epoxy mixture. Then impregnate, cure and cut to obtain the insulator core rod.

[0023] (G) The impregnation process is as follows: Add 0.5-2 parts of 2-ethyl-4-methylimidazolium, stir evenly, pour into the resin tank for pultrusion, 9600TEXS-glass fiber reinforced, with a content of 78%-82% of the resin, impregnate in the above resin system to make the fiber completely wetted; the temperature of the resin tank is about 30-40℃.

[0024] (H) The resin curing temperature is set in three stages: 120-130℃, 160-170℃, and 180-190℃; the pultrusion speed is 0.4-0.6 cm / min.

[0025] (I) The product is cured by a 4-meter-long tunnel oven located 20-30cm from the mold exit, with a temperature distribution of 190-200℃ and 190-180℃. The last section is not heated and can be heated by residual heat.

[0026] (J) After being pulled out, cut to the required length.

[0027] Furthermore, the epoxy equivalent number of the E-51 epoxy resin is 180-190 g / eq.

[0028] Furthermore, the multifunctional epoxy resin is one of tetrahydroxymethyltriacrylate triepoxyethyl ether or triepoxymethoxypropane ethyl ether or a mixture thereof, or a tetrafunctional glycidyl ether, and the epoxy equivalent of the tetrafunctional multifunctional epoxy resin is 100-130 g / eq.

[0029] Furthermore, the active diluent is butyl glycidyl ether, cashew phenol glycidyl ether, or phenyl glycidyl ether, and the purity of the active diluent is ≥ 98%.

[0030] Furthermore, the viscosity range suitable for pultrusion impregnation is 2000-5000 mPa·s @ 25℃.

[0031] Furthermore, the linear phenolic resin is a low molecular weight phenolic prepolymer, and the hydroxyl equivalent of the linear phenolic resin is 250-350 g / eq.

[0032] Furthermore, the specific surface area of ​​the hydrophobic silica is 50-200 m². 2 / g, water absorption rate <0.5%.

[0033] Furthermore, the anti-hydrolysis agent is carbodiimide, hydroxy-epoxyphosphate, or 3-glycidyl etheroxypropylmethyldiethoxysilane.

[0034] Reaction mechanism

[0035] Epoxy resin and acid anhydride undergo stepwise addition polymerization under the synergistic effect of catalysts and accelerators: Bisphenol A type E-51 epoxy resin and multifunctional epoxy resin together constitute the epoxy monomer system. The accelerator first activates the carbonyl group of the acid anhydride, causing it to undergo a nucleophilic addition reaction with the epoxy group, promoting the ring opening of the epoxy ring and the formation of ester bonds and hydroxyl groups. The generated hydroxyl groups further react with unreacted acid anhydride and epoxy groups, continuously building cross-linked ester bonds and ether bonds. Among them, the multifunctional epoxy resin, with its multiple epoxy sites, can react with different acid anhydride molecules simultaneously. Combined with the additional cross-linking effect of the hydroxyl and epoxy groups of the linear phenolic resin, a high-density three-dimensional network cross-linked structure is finally formed. The silane coupling agent enhances the interfacial bonding between the resin and glass fiber through chemical action, reducing interfacial defects. The hydrophobic silica and anti-hydrolysis agent reduce the damage of water molecules to the cross-linked network and interface through physical barriers and chemical inhibition, providing a structural basis for the thermal stability, water resistance, mechanical strength and electrical insulation properties of the mandrel.

[0036] Technical effect

[0037] To enhance thermal stability and high-temperature performance retention, a blend of E-51 epoxy resin and multifunctional epoxy resin, combined with synergistic crosslinking modification of linear phenolic resin, and a step-curing and post-curing process, is employed to create a high-density crosslinked structure in the resin network, effectively increasing the glass transition temperature. This improvement ensures that the material maintains rigidity, dimensional stability, and electrical insulation properties under harsh conditions such as high temperature, strong sunlight, or high load, preventing performance degradation due to temperature increases.

[0038] Hydrophobic silica, uniformly dispersed in the resin matrix to enhance hydrothermal resistance and structural integrity, forms a physical barrier to prevent water molecule penetration. An anti-hydrolysis agent reacts with free hydroxyl groups in the resin, reducing easily hydrolyzed groups. Simultaneously, the highly cross-linked resin network further narrows the water molecule diffusion channels. The synergistic effect of these three elements ensures that the material is less prone to increased water absorption, structural cracking, or interfacial delamination in long-term hydrothermal environments, guaranteeing the overall structural and performance stability of the mandrel.

[0039] Optimized interfacial bonding and overall performance reliability: Silane coupling agents achieve strong chemical bonding between the resin and glass fiber interface, reducing the risk of interfacial hydrolysis and delamination under humid and hot conditions; the resin viscosity controlled by reactive diluents ensures full wetting of the glass fiber, and the step-curing process releases internal stress, allowing the material to maintain high mechanical strength and electrical insulation properties even after boiling in water. This improvement balances the long-term stability of mechanical and electrical insulation properties, avoiding a sudden drop in performance due to interfacial failure or structural defects. Detailed Implementation

[0040] The features of the present invention are further illustrated below through embodiments, but the scope of protection of this patent is not limited to the embodiments.

[0041] Example 1

[0042] A method for preparing insulator core rods by pultrusion of high-performance pultrusion resin includes the following steps, based on mass:

[0043] (A) Mix 100 kg of E-51 epoxy resin (epoxy equivalent 180-190 g / eq) with 10 kg of multifunctional epoxy resin (tetramethyloltriacrylate triepoxyethyl ether, epoxy equivalent 100-130 g / eq) until homogeneous; take 20 kg of linear phenolic resin (low molecular weight phenolic prepolymer, hydroxyl equivalent 250-350 g / eq) and mix it again with the above-mixed epoxy resin at 70°C, and continue stirring until the resin system is transparent and clear.

[0044] (B) Add 10 kg of reactive diluent (butyl glycidyl ether, purity ≥ 98%) to the mixed resin obtained in (A) and stir for 15 minutes until the mixture is uniform.

[0045] (C) Add 1 kg of release agent and continue stirring for 10 minutes until the system is uniform and free of particles;

[0046] (D) Add 1 kg of silane coupling agent KH-560 and 1 kg of hydrophobic silica (specific surface area 50 m²). 2 / g, water absorption rate <0.5%) and 0.5kg anti-hydrolysis agent (carbodiimide), stir at high speed for 20 minutes until all components are evenly dispersed;

[0047] (E) Add 10 kg of methyltetrahydrophthalic anhydride and 10 kg of methylnadic anhydride as curing agents, and stir at low speed for 15 minutes until the system is homogeneous;

[0048] (F) Add 0.01 kg of ethylene glycol dimercaptoacetate and 0.1 kg of triethylamine and stir to fully mix with the acid anhydride and epoxy mixture;

[0049] (G) Add 0.5 kg of 2-ethyl-4-methylimidazole, stir for 10 minutes and pour into the pultrusion resin tank; take 9600 TEX S-glass fiber and lay it in the impregnation area at a ratio of 78% of the resin mass (i.e., the fiber mass to resin mass ratio is 78:22) so that the fiber is completely impregnated with the above resin system; control the temperature of the resin tank at 30℃.

[0050] (H) The resin curing process uses a three-stage temperature control: the first stage is 120℃, the second stage is 160℃, and the third stage is 180℃; the pultrusion speed is set to 0.4cm / min;

[0051] (I) The post-curing of the product is completed through a 4-meter-long tunnel oven located 20cm from the mold outlet. The oven temperature distribution is as follows: 190℃ in the first section, 190℃ in the second section, and no heating in the third section (using residual heat).

[0052] (J) After the core rod is pulled out of the oven, it is cut into the specified length according to the design requirements to obtain the insulator core rod semi-finished product.

[0053] Example 2

[0054] A method for preparing insulator core rods by pultrusion of high-performance pultrusion resin includes the following steps, based on mass:

[0055] (A) Mix 100 kg of E-51 epoxy resin (epoxy equivalent 180-190 g / eq) and 13 kg of multifunctional epoxy resin (triepoxymethoxypropane ethyl ether, epoxy equivalent 100-130 g / eq) until homogeneous; take 25 kg of linear phenolic resin (low molecular weight phenolic prepolymer, hydroxyl equivalent 250-350 g / eq) and mix it with the above mixed epoxy resin at 70°C, stirring until the resin system is transparent and clear;

[0056] (B) Add 13 kg of active diluent (cashew phenolic glycidyl ether, purity ≥ 98%) and stir for 18 minutes until well mixed;

[0057] (C) Add 1.5 kg of internal release agent and stir for 12 minutes until the system is homogeneous;

[0058] (D) Add 1.5 kg of silane coupling agent KH-560 and 2.5 kg of hydrophobic silica (specific surface area 100 m²). 2 / g, water absorption rate <0.5%) and 1kg of anti-hydrolysis agent (hydroxy-epoxyphosphate), stir at high speed for 22 minutes until uniformly dispersed;

[0059] (E) Add 30 kg of methyltetrahydrophthalic anhydride and 30 kg of methylnadic anhydride, and stir at low speed for 18 minutes until the system is free of stratification;

[0060] (F) Add 0.02 kg of ethylene glycol dimercaptoacetate and 0.2 kg of triethylamine and stir to fully mix with the acid anhydride and epoxy mixture;

[0061] (G) Add 1 kg of 2-ethyl-4-methylimidazole, stir for 12 minutes and pour into the pultrusion resin tank; take 9600TEXS glass fiber and lay it in a ratio of 79% of the resin mass to make the fiber completely wet the resin; control the temperature of the resin tank at 33℃.

[0062] (H) Resin curing temperature in three stages: stage 1 123℃, stage 2 163℃, stage 3 183℃; pultrusion speed set to 0.45cm / min;

[0063] (I) Post-curing uses a 4-meter tunnel oven located 23cm from the mold exit, with the following temperature distribution: 193℃ in the first section, 188℃ in the second section, and no heating in the third section;

[0064] (J) After the core rod is pulled out, it is cut to the specified length to obtain the insulator core rod semi-finished product.

[0065] Example 3

[0066] A method for preparing insulator core rods by pultrusion of high-performance pultrusion resin includes the following steps, based on mass:

[0067] (A) Mix 100 kg of E-51 epoxy resin (epoxy equivalent 180-190 g / eq) with 17 kg of multifunctional epoxy resin (a mixture of tetrahydroxymethyltriacrylate triepoxyethyl ether and triepoxymethoxypropane ethyl ether, mass ratio 1:1, epoxy equivalent 100-130 g / eq) until homogeneous; take 28 kg of linear phenolic resin (low molecular weight phenolic prepolymer, hydroxyl equivalent 250-350 g / eq) and mix it with the mixed epoxy resin at 70°C until transparent and clear;

[0068] (B) Add 17 kg of reactive diluent (phenyl glycidyl ether, purity ≥ 98%) and stir for 20 minutes until homogeneous;

[0069] (C) Add 2.5 kg of internal release agent and stir for 15 minutes until there are no release agent particles in the system;

[0070] (D) Add 2.5 kg of silane coupling agent KH-560 and 4 kg of hydrophobic silica (specific surface area 160 m²). 2 / g, water absorption rate <0.5%) and 1.5kg of anti-hydrolysis agent (3-glycidyl etheroxypropylmethyldiethoxysilane), stirred at high speed for 25 minutes until uniformly dispersed;

[0071] (E) Add 50 kg of methyltetrahydrophthalic anhydride and 50 kg of methylnadic anhydride, and stir at low speed for 20 minutes until the system is homogeneous;

[0072] (F) Add 0.04 kg of ethylene glycol dimercaptoacetate and 0.4 kg of triethylamine and stir to fully mix with the acid anhydride and epoxy mixture;

[0073] (G) Add 1.5 kg of 2-ethyl-4-methylimidazole, stir for 15 minutes and pour into the resin tank; take 9600 TEX S-glass fiber and lay it at a ratio of 81% of the resin mass to ensure that the fiber is completely impregnated; control the temperature of the resin tank at 37℃.

[0074] (H) Resin curing temperature in three stages: first stage 127℃, second stage 167℃, third stage 187℃; pultrusion speed set to 0.55cm / min;

[0075] (I) Post-curing is carried out in a 4-meter tunnel oven 27cm from the mold outlet. The temperature distribution is as follows: 197℃ in the first section, 183℃ in the second section, and no heating in the third section.

[0076] (J) After the core rod is pulled out, it is cut to the designed length to obtain the insulator core rod semi-finished product.

[0077] Example 4

[0078] A method for preparing insulator core rods by pultrusion of high-performance pultrusion resin includes the following steps, based on mass:

[0079] (A) Stir 100 kg of E-51 epoxy resin (epoxy equivalent 180-190 g / eq) and 20 kg of multifunctional epoxy resin (tetramethylolpropionic acid triacrylate, epoxy equivalent 100-130 g / eq) until homogeneous; take 30 kg of linear phenolic resin (low molecular weight phenolic prepolymer, hydroxyl equivalent 250-350 g / eq) and mix it with the mixed epoxy resin at 70°C until the system is transparent and clear;

[0080] (B) Add 20 kg of reactive diluent (butyl glycidyl ether, purity ≥ 98%) and stir for 22 minutes until the mixture is homogeneous;

[0081] (C) Add 3 kg of internal release agent and stir for 18 minutes until the system is homogeneous;

[0082] (D) Add 3 kg of silane coupling agent KH-560 and 5 kg of hydrophobic silica (specific surface area 200 m²). 2 / g, water absorption rate <0.5%) and 2kg of anti-hydrolysis agent (carbodiimide), stir at high speed for 30 minutes until all components are evenly dispersed;

[0083] (E) Add 70 kg of methyltetrahydrophthalic anhydride and 70 kg of methylnadic anhydride, and stir at low speed for 22 minutes until the system is free of stratification;

[0084] (F) Add 0.06 kg of ethylene glycol dimercaptoacetate and 0.6 kg of triethylamine and stir to fully mix with the acid anhydride and epoxy mixture;

[0085] (G) Add 2 kg of 2-ethyl-4-methylimidazole, stir for 18 minutes and pour into the pultrusion resin tank; take 9600TEXS glass fiber and lay it at a ratio of 82% of the resin mass to make the fiber completely wet the resin; control the temperature of the resin tank at 40℃.

[0086] (H) Resin curing temperature in three stages: stage 1 130℃, stage 2 170℃, stage 3 190℃; pultrusion speed set to 0.6cm / min;

[0087] (I) Post-curing uses a 4-meter tunnel oven located 30cm from the mold outlet, with the following temperature distribution: 200℃ in the first section, 180℃ in the second section, and no heating in the third section;

[0088] (J) After the core rod is pulled out, it is precisely cut to the specified length to obtain the insulator core rod semi-finished product.

[0089] Comparative Example 1

[0090] A method for preparing insulator core rods by pultrusion of high-performance pultrusion resin includes the following steps, based on mass:

[0091] (A) Mix 100 kg of E-51 epoxy resin (epoxy equivalent 180-190 g / eq) with 10 kg of multifunctional epoxy resin (tetramethyloltriacrylate triepoxyethyl ether, epoxy equivalent 100-130 g / eq) until homogeneous; take 20 kg of linear phenolic resin (low molecular weight phenolic prepolymer, hydroxyl equivalent 250-350 g / eq) and mix it again with the above-mixed epoxy resin at 70°C, and continue stirring until the resin system is transparent and clear.

[0092] (B) Add 10 kg of reactive diluent (butyl glycidyl ether, purity ≥ 98%) to the mixed resin obtained in (A) and stir for 15 minutes until the mixture is uniform.

[0093] (C) Add 1 kg of release agent and continue stirring for 10 minutes until the system is uniform and free of particles;

[0094] (D) Add 1 kg of silane coupling agent KH-560 and 1 kg of hydrophobic silica (specific surface area 50 m²). 2 / g, water absorption rate <0.5%) and 0.5kg anti-hydrolysis agent (carbodiimide), stir at high speed for 20 minutes until all components are evenly dispersed;

[0095] (E) Add 10 kg of methyltetrahydrophthalic anhydride and 10 kg of methylnadic anhydride as curing agents, and stir at low speed for 15 minutes until the system is homogeneous;

[0096] (F) Add 0.1 kg of triethylamine and stir to fully mix it with the acid anhydride and epoxy mixture;

[0097] (G) Add 0.5 kg of 2-ethyl-4-methylimidazole, stir for 10 minutes and pour into the pultrusion resin tank; take 9600 TEX S-glass fiber and lay it in the impregnation area at a ratio of 78% of the resin mass (i.e., the fiber mass to resin mass ratio is 78:22) so that the fiber is completely impregnated with the above resin system; control the temperature of the resin tank at 30℃.

[0098] (H) The resin curing process uses a three-stage temperature control: the first stage is 120℃, the second stage is 160℃, and the third stage is 180℃; the pultrusion speed is set to 0.4cm / min;

[0099] (I) The post-curing of the product is completed through a 4-meter-long tunnel oven located 20cm from the mold outlet. The oven temperature distribution is as follows: 190℃ in the first section, 190℃ in the second section, and no heating in the third section (using residual heat).

[0100] (J) After the core rod is pulled out of the oven, it is cut into the specified length according to the design requirements to obtain the insulator core rod semi-finished product.

[0101] Comparative Example 2

[0102] A method for preparing insulator core rods by pultrusion of high-performance pultrusion resin includes the following steps, based on mass:

[0103] (A) Mix 100 kg of E-51 epoxy resin (epoxy equivalent 180-190 g / eq) with 10 kg of multifunctional epoxy resin (tetramethyloltriacrylate triepoxyethyl ether, epoxy equivalent 100-130 g / eq) until homogeneous; take 20 kg of linear phenolic resin (low molecular weight phenolic prepolymer, hydroxyl equivalent 250-350 g / eq) and mix it again with the above-mixed epoxy resin at 70°C, and continue stirring until the resin system is transparent and clear.

[0104] (B) Add 10 kg of reactive diluent (butyl glycidyl ether, purity ≥ 98%) to the mixed resin obtained in (A) and stir for 15 minutes until the mixture is uniform.

[0105] (C) Add 1 kg of release agent and continue stirring for 10 minutes until the system is uniform and free of particles;

[0106] (D) Add 1 kg of silane coupling agent KH-560 and 1 kg of hydrophobic silica (specific surface area 50 m²). 2 / g, water absorption rate <0.5%) and 0.5kg anti-hydrolysis agent (carbodiimide), stir at high speed for 20 minutes until all components are evenly dispersed;

[0107] (E) Add 10 kg of methyltetrahydrophthalic anhydride and 10 kg of methylnadic anhydride as curing agents, and stir at low speed for 15 minutes until the system is homogeneous;

[0108] (F) Add 0.01 kg of ethylene glycol dimercaptoacetate and stir to fully mix it with the acid anhydride and epoxy mixture;

[0109] (G) Add 0.5 kg of 2-ethyl-4-methylimidazole, stir for 10 minutes and pour into the pultrusion resin tank; take 9600 TEX S-glass fiber and lay it in the impregnation area at a ratio of 78% of the resin mass (i.e., the fiber mass to resin mass ratio is 78:22) so that the fiber is completely impregnated with the above resin system; control the temperature of the resin tank at 30℃.

[0110] (H) The resin curing process uses a three-stage temperature control: the first stage is 120℃, the second stage is 160℃, and the third stage is 180℃; the pultrusion speed is set to 0.4cm / min;

[0111] (I) The post-curing of the product is completed through a 4-meter-long tunnel oven located 20cm from the mold outlet. The oven temperature distribution is as follows: 190℃ in the first section, 190℃ in the second section, and no heating in the third section (using residual heat).

[0112] (J) After the core rod is pulled out of the oven, it is cut into the specified length according to the design requirements to obtain the insulator core rod semi-finished product.

[0113] Test methods

[0114] 1. Glass transition temperature (Tg) — DSC / DMA

[0115] Standard: ISO 11357-2 / ISO 11357-1 (Differential Scanning Calorimetry, DSC).

[0116] Sample preparation: The rod was sliced ​​and ground flat. Sample drying treatment: Vacuum drying at 80℃ for 4 h.

[0117] Test parameters (DSC): Nitrogen protection, heating / cooling rate 10 ℃ / min; sweep from 25 ℃ to 300–350 ℃; Tg is taken from the midpoint of the baseline displacement or heat capacity step in the heat flux curve or the half-width at half-maximum method.

[0118] Table 1. Test results of glass transition temperature

[0119]

[0120] 2. Water absorption and resistance to boiling / soaking in water

[0121] Standard: ASTM D570 (Water Absorption) is used for water absorption determination; for long-term boiling immersion, the "boiling water" clause in ASTM D570 or the industry accelerated aging / immersion procedure can be extended to 100°C, long-term immersion and periodic testing.

[0122] Sample preparation: Dimensions and weight can refer to the standard (50×10×3 mm small pieces or standard specimens). First, dry according to standard and weigh (m0); immerse in boiling water at 100 ℃ (sealed or open container, deionized water recommended); remove the sample after 500 hours, cool to room temperature, wipe the surface dry, weigh (mt), and perform a visual inspection (cracks, delamination, peeling). Water absorption rate (%) = (mt - m0) / m0 × 100%. Record whether cracks / delamination occur.

[0123] Table 2 Results of boiling water test

[0124]

[0125] 3. Mechanical properties

[0126] Tensile strength:

[0127] Standard: ASTM D638 (Stretchable Plastics).

[0128] Samples: Prepared according to standards or cut from mandrels of appropriate size. Test conditions: 20 ± 2 ℃, relative humidity 50 ± 5%; tensile rate according to standards (5 mm / min or as specified in the standard).

[0129] Bending strength:

[0130] Standard: ASTM D790 Three-point bending test.

[0131] Samples: Prepare beam-shaped specimens according to standard dimensions or cut appropriate lengths from bars for testing. Record bending strength, bending modulus, and fracture mode.

[0132] Table 3 Mechanical Test Results

[0133]

[0134] 4. Electrical properties—Surface resistivity

[0135] Standard: ASTM D257 (Surface / Volume Resistivity) is used to evaluate the effect of moisture absorption on electrical insulation.

[0136] Samples: Prepare flat samples (thickness 1–6 mm) according to standards. Measure the surface resistivity (Ω) at room temperature and after boiling in water; the breakdown voltage is determined using the electrode spacing / sample thickness specification. Record the performance changes before and after boiling in water.

[0137] Table 4 Electrical Performance Test Results

[0138]

[0139] Based on the test results of the four types of core performance, the insulator core rods prepared in Examples 1-4 show significantly better overall performance than those in Comparative Examples 1-2, specifically as follows:

[0140] Superior thermal stability: The glass transition temperature (Tg) of the examples is higher than that of the comparative example, indicating that their resin cross-linking structure is more compact and their performance retention ability is stronger at high temperatures;

[0141] Better water and heat resistance: The water absorption rate of the examples was lower than that of the comparative examples, and all samples were free of appearance defects such as cracks and delamination, demonstrating that the synergistic effect of hydrophobic components and anti-hydrolysis components effectively improved the material's resistance to water erosion.

[0142] More stable mechanical properties: The tensile strength and flexural strength of the example before boiling were higher, and the strength retention rate after boiling for 500 hours was also better, which verified the reliability of the resin-fiber interface bonding and the structure's resistance to hydrolysis.

[0143] The electrical insulation performance is stronger and the water resistance is more stable: the surface resistivity before boiling is higher and the resistivity decreases by a smaller percentage after boiling, indicating that its electrical insulation performance is less affected by the hydrothermal environment.

[0144] Comparative Example 1, lacking ethylene glycol dimercaptoacetate, and Comparative Example 2, lacking triethylamine, resulted in slightly inferior performance indicators compared to the examples. This further demonstrates the crucial significance of the synergistic effect of the components in the formulation of this invention for performance improvement. Overall, it verifies that the preparation method can effectively balance the thermal stability, hydrothermal resistance, mechanical properties, and electrical insulation properties of the mandrel.

[0145] Although embodiments of the present invention have been disclosed above, they are not limited to the applications listed in the specification and embodiments. They can be applied to various fields suitable for the present invention. Other modifications can be easily made by those skilled in the art. Therefore, without departing from the general concept defined by the claims and their equivalents, the present invention is not limited to the specific details and the illustrations shown and described herein.

Claims

1. A method for preparing insulator core rods by pultrusion of high-performance pultrusion resin, characterized in that, The insulator core rod is made by fully fusing E-51 epoxy resin, multifunctional epoxy resin, linear phenolic resin, reactive diluent, internal release agent, silane coupling agent KH-560, hydrophobic silica, anti-hydrolysis agent, methyltetrahydrophthalic anhydride, methylnadic anhydride, and ethylene glycol dimercaptoacetate, followed by impregnation, curing, and traction cutting.

2. The method for preparing insulator core rods by pultrusion of high-performance resin according to claim 1, characterized in that: The preparation process of the insulator core rod includes the following steps, in parts by weight: (A) Stir 100 parts of E-51 epoxy resin and 10-20 parts of multifunctional epoxy resin evenly, and then mix the linear phenolic resin with the mixed epoxy resin again at 70 degrees until the resin is transparent and clear. (B) Add 10-20 parts of reactive diluent to (A) and stir until well mixed; add 1-3 parts of internal release agent and stir until well mixed; then add 1-3 parts of silane coupling agent KH-560, 1-5 parts of hydrophobic silica, and 0.5-2 parts of anti-hydrolysis agent and stir until well mixed. (C) Then add 10-70 parts of methyltetrahydrophthalic anhydride and 10-70 parts of methylnadic anhydride as curing agents, and stir evenly; then add 0.01-0.06 parts of ethylene glycol dimercaptoacetate and 0.1-0.6 parts of triethylamine and stir to fully integrate with the anhydride and epoxy mixture; then impregnate, cure, and cut to obtain the insulator core rod.

3. The method for preparing insulator core rods by high-performance pultrusion resin extrusion according to claim 2, characterized in that: The epoxy equivalent number of the E-51 epoxy resin is 180-190 g / eq.

4. The method for preparing insulator core rods by high-performance pultrusion resin extrusion according to claim 2, characterized in that: The multifunctional epoxy resin is one of tetrahydroxymethyltriacrylate triepoxyethyl ether or triepoxymethoxypropane ethyl ether or a mixture thereof, or a tetrafunctional glycidyl ether.

5. The method for preparing insulator core rods by high-performance pultrusion resin extrusion according to claim 2, characterized in that: The active diluent is butyl glycidyl ether, cashew phenol glycidyl ether, or phenyl glycidyl ether, and the purity of the active diluent is ≥ 98%.

6. The method for preparing insulator core rods by high-performance pultrusion resin extrusion according to claim 2, characterized in that: The impregnation process is as follows: Add 0.5-2 parts of 2-ethyl-4-methylimidazole, stir evenly, and pour into a resin tank for pultrusion. 9600TEXS-glass fiber reinforced, with a content of 78%-82% of the resin, is impregnated in the above resin system to ensure complete fiber wetting. The temperature of the resin tank is about 30-40℃.

7. The method for preparing insulator core rods by high-performance pultrusion resin extrusion according to claim 2, characterized in that: The product post-curing equipment is a long tunnel-type oven, where the last section is not heated and only the residual heat is used; after being pulled out, it is cut to the required length.

8. The method for preparing insulator core rods by high-performance pultrusion resin extrusion according to claim 2, characterized in that: The anti-hydrolysis agent is carbodiimide, hydroxy-epoxyphosphate, or 3-glycidyl etheroxypropylmethyldiethoxysilane.

9. The method for preparing insulator core rods by pultrusion of high-performance pultrusion resin according to claim 2, wherein the resin curing temperature is in three stages: 120-130℃, 160-170℃, and 180-190℃; and the pultrusion speed is 0.4-0.6cm / min.

Citation Information

Patent Citations

  • Insulating material with high glass transition temperature and high-temperature cohesiveness and preparation method of insulating material

    CN109233710A

  • A glass fiber impregnating agent for ultra-high voltage composite insulators, its preparation method, product and application

    CN110482879B