Epoxy glass fiber core rod material, preparation method and application in composite insulator

By combining functionalized thermally conductive fillers with epoxy resin and using nano-boron nitride modifiers, the problem of heat dissipation in composite insulator core rods under high voltage was solved, thereby improving thermal conductivity, mechanical properties, and insulation properties, and extending the service life of composite insulators.

CN123152255APending Publication Date: 2026-11-24XINJIANG HENENG ELECTRIC CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611419799.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-14
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing composite insulator core rod materials have difficulty dissipating heat accumulation under high voltage, leading to accelerated aging. Existing thermal conductivity modification schemes cannot simultaneously meet the requirements of high thermal conductivity, excellent mechanical toughness, and good insulation performance.

Method used

Functionalized thermally conductive fillers were used to prepare nano-boron nitride modifiers through mercaptoolefin click reaction, which were then combined with epoxy resin to form a thermally conductive network, reducing interfacial thermal resistance. Epoxy glass fiber core rods were then prepared in a pultrusion molding process.

Benefits of technology

This study achieved a synergistic improvement in the thermal conductivity, mechanical properties, and insulation properties of epoxy glass fiber core rods, reduced the risk of local overheating, and extended the service life of composite insulators.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure QLYQS_1
    Figure QLYQS_1
Patent Text Reader

Abstract

This invention relates to the field of epoxy glass fiber core rod materials, and discloses epoxy glass fiber core rod materials, preparation methods, and applications in composite insulators. The epoxy glass fiber core rod material is made from an alkali-free glass fiber and a curable composite thermally conductive epoxy resin composition through a pultrusion molding process. The curable composite thermally conductive epoxy resin composition includes the following raw materials: epoxy resin, curing agent, accelerator, and functionalized thermally conductive filler. The functionalized thermally conductive filler is added to the epoxy resin, which improves the interfacial compatibility of the two through the dual effects of π-π interactions and interfacial covalent bonds. This not only strengthens stress transmission and improves mechanical properties, but also reduces interfacial thermal resistance and improves thermal conductivity through a thermally conductive network. At the same time, it also improves the hydrophobicity and thermal conductivity of the epoxy resin, synergistically enhancing the tracking resistance of the epoxy resin, while still maintaining excellent insulation levels. The epoxy glass fiber core rod material prepared by this invention meets the performance requirements of composite insulators.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of epoxy glass fiber core rod materials, and more particularly to epoxy glass fiber core rod materials, preparation methods, and applications in composite insulators. Background Technology

[0002] Composite insulators consist of three parts: a core rod that bears mechanical loads and provides internal insulation, outer insulation and weather-resistant silicone rubber sheds, and metal end connectors. Compared with traditional porcelain and glass insulators, composite insulators have significant advantages such as light weight, excellent resistance to pollution flashover, strong hydrophobicity, and low maintenance costs, making them a key insulation device for ultra-high voltage and extra-high voltage transmission lines.

[0003] Among the three main components of a composite insulator, the composite insulator core rod is the core load-bearing component and the main internal insulation material. Currently, the mainstream material for composite insulator core rods is epoxy resin-based glass fiber reinforced composite material (i.e., epoxy glass fiber core rod). This material is prepared using a pultrusion molding process, in which glass fiber yarn is impregnated with an epoxy resin mixture, cured by heating a mold, and continuously drawn into the finished product. The epoxy resin matrix has advantages such as high mechanical strength, excellent electrical insulation properties, low cost, and good processability, while glass fiber provides high strength, high modulus, and a low coefficient of thermal expansion. The combination of the two gives the core rod both excellent mechanical and insulation properties.

[0004] However, as transmission voltage levels continue to rise to ultra-high voltage and extra-high voltage levels, the operating conditions of composite insulators are becoming increasingly harsh. During operation, composite insulators are subjected to the coupling effects of multiple electrical, thermal, and mechanical fields. Among these factors, the epoxy resin in the core rod has extremely low thermal conductivity; the intrinsic thermal conductivity of general-purpose epoxy resin is only about 0.2 W / (m·K), making it difficult for heat to dissipate quickly from localized areas inside the core rod. This abnormal heating further accelerates the aging process of the composite insulator, and can even lead to the core rod rotting and breaking.

[0005] Therefore, the development of high thermal conductivity epoxy resin materials is of great significance for improving the heat resistance of composite insulator core rods, suppressing abnormal heating, and extending their service life.

[0006] Currently, the technical approaches to improving the thermal conductivity of epoxy resin systems are mainly divided into two categories: intrinsic thermal conductivity modification and filler-type thermal conductivity modification.

[0007] Intrinsic thermal conductivity modification involves introducing rigid conjugated structures such as biphenyl groups and naphthalene rings into epoxy resin through molecular structure design. This improves the structural order of the epoxy resin, effectively suppresses phonon scattering, and thus enhances the intrinsic thermal conductivity of the resin matrix. However, the actual increase in thermal conductivity is limited. At the same time, the large-scale introduction of rigid aromatic groups significantly increases the brittleness of the resin and reduces its fracture toughness, leading to a decrease in the impact resistance and stress corrosion resistance of the mandrel. Furthermore, the increased resin viscosity deteriorates the glass fiber impregnation effect, resulting in insufficient compatibility with continuous pultrusion production processes.

[0008] Filler-based thermal conductivity modification is currently the most widely used approach in industry. This involves adding high thermal conductivity inorganic fillers such as alumina, boron nitride, and aluminum nitride to epoxy resin, and then using conventional silane coupling agents to modify the surface of the fillers, thereby improving the filler's dispersion and interfacial bonding in the resin. While this approach can achieve higher thermal conductivity by increasing the filler content, it still has significant drawbacks in practical applications: ordinary silane coupling agents have short-chain aliphatic structures and low intrinsic thermal conductivity. The interfacial layer they form between the filler and the resin matrix cannot effectively mitigate the significant differences in phonon vibration characteristics between the two materials, leading to severe phonon scattering at the interface and persistently high interfacial thermal resistance. This prevents the high thermal conductivity filler from fully realizing its performance potential.

[0009] In summary, existing thermal conductivity modification schemes generally have performance shortcomings and cannot simultaneously meet the multiple requirements of high thermal conductivity efficiency, excellent mechanical toughness, and good insulation performance, becoming the core bottleneck restricting the engineering application of high thermal conductivity epoxy glass fiber core rods. Therefore, developing high thermal conductivity epoxy glass fiber core rod materials with novel interface structures, and simultaneously achieving thermal conductivity gradient transition, toughening, and insulation through multifunctional modification of the filler surface, is a technical problem that urgently needs to be solved in the field of composite insulator core rods. Summary of the Invention

[0010] This invention develops a functionalized thermally conductive filler that can participate in the curing process of epoxy resin through surface carboxyl functional groups. Utilizing the synergistic effect of a bulk thermally conductive network constructed from nano-boron nitride and the reduction effect of interfacial thermal resistance, a curable composite thermally conductive epoxy resin composition with excellent comprehensive performance is prepared. This material possesses excellent mechanical properties, thermal conductivity, and resistance to electrical tracking, while maintaining excellent electrical insulation properties. It can be combined with glass fiber through a pultrusion process to prepare epoxy glass fiber core rods, exhibiting excellent mechanical properties, thermal conductivity, insulation properties, and resistance to damp heat aging, making it suitable as a composite insulator core rod.

[0011] To achieve the above objectives, the present invention adopts the following technical solution:

[0012] Epoxy glass fiber core material comprises the following raw materials: 70-80 wt% alkali-free glass fiber, 20-30 wt% curable composite thermally conductive epoxy resin composition; wherein the alkali-free continuous glass fiber is E glass fiber roving or ECR glass fiber roving; wherein the curable composite thermally conductive epoxy resin composition comprises the following raw materials in parts by weight: 90-100 parts epoxy resin, 70-80 parts curing agent, 0.1-1 parts accelerator, and 6-10 parts functionalized thermally conductive filler;

[0013] The functionalized thermally conductive filler is prepared by a mercapto-alkene click reaction between an alkenyl carboxyl-type dual long-chain alkyl biphenyl modifier and mercapto-modified nano-boron nitride under the action of a photoinitiator; the mass ratio of the alkenyl carboxyl-type dual long-chain alkyl biphenyl modifier to the mercapto-modified nano-boron nitride is 0.05-0.2:1.

[0014] Preferably, the preparation method of the alkenyl carboxyl type di-long-chain alkyl biphenyl modifier is as follows:

[0015] Under the action of pyridine, the primary amino group in 4-aminobiphenyl undergoes an amidation reaction with the acyl bromide group in bromoacetyl bromide, and the molar equivalent ratio of 4-aminobiphenyl to bromoacetyl bromide is controlled at 1:1 to obtain intermediate 1;

[0016] In the presence of hydrochloric acid, 12-aminododecanoic acid reacts with methanol to form methyl 12-aminododecanoate hydrochloride.

[0017] Under the action of triethylamine, the primary amino group in methyl 12-aminododecanoate hydrochloride undergoes a substitution reaction with the bromine functional group in intermediate 1, and the molar equivalent ratio of methyl 12-aminododecanoate hydrochloride to intermediate 1 is controlled to be 1:1 to obtain intermediate 2.

[0018] Under the action of N,N-diisopropylethylamine, the secondary amino group in intermediate 2 undergoes a substitution reaction with the bromine functional group in undecene bromide, and the molar equivalent ratio of intermediate 2 to undecene bromide is controlled at 1:1. Subsequently, after hydrolysis and acidification treatment, the methyl ester is converted into a carboxyl group to obtain an alkenyl carboxyl type dilong-chain alkyl biphenyl modifier.

[0019] Preferably, the epoxy resin is at least one of bisphenol A type epoxy resin and bisphenol F type epoxy resin.

[0020] Preferably, the curing agent is methylhexahydrophthalic anhydride or methyltetrahydrophthalic anhydride.

[0021] Preferably, the accelerator is 2-methylimidazole or 2,4,6-tris(dimethylaminomethyl)phenol.

[0022] Preferably, the photoinitiator is benzoin dimethyl ether or photoinitiator 1173.

[0023] Preferably, the mercapto-modified boron nitride nanoparticles are prepared by surface modification of boron nitride nanoparticles with a mercaptosilane coupling agent; the mercaptosilane coupling agent is 3-mercaptopropyltrimethoxysilane or 3-mercaptopropyltriethoxysilane; the mass ratio of the mercaptosilane coupling agent to the boron nitride nanoparticles is 0.05-0.15:1.

[0024] A method for preparing epoxy glass fiber core rod material includes the following steps:

[0025] Alkali-free glass fibers are dried at 90-110℃ for 1-3 hours. The dried glass fibers are then evenly guided out through a yarn rack and arranged through a yarn guide plate so that the glass fiber bundles are arranged parallel to each other along the pultrusion direction; thus, pretreated glass fibers are obtained.

[0026] Pretreated glass fibers are introduced into the impregnation tank of curable composite thermally conductive epoxy resin composition to fully wet them. The fiber bundles are gradually extruded through a preforming device to densify them. The content ratio of glass fibers to curable composite thermally conductive epoxy resin composition is controlled by adjusting the aperture of the preforming device, the extrusion pressure and the traction speed to form a blank.

[0027] The preform is fed into a heated pultrusion die, where it is shaped and cured. The heated pultrusion die has multiple temperature zones along the traction direction. The temperature is controlled as follows: inlet preheating zone: 90-110℃; middle gel zone: 120-140℃; outlet curing zone: 150-180℃. The pultrusion speed is controlled at 0.3-0.8 m / min to obtain epoxy glass fiber core rod material.

[0028] Preferably, the preparation method of the composite thermally conductive epoxy resin composition includes the following steps:

[0029] Functionalized thermally conductive fillers are added to epoxy resin, the water bath temperature is raised to 55-65℃, the mixture is stirred at a rate of 200-400r / min for 20-40min, and then ultrasonically dispersed for 30-60min to form a mixture.

[0030] Add curing agent and accelerator to the mixture, stir at 45-55℃ and 200-400r / min for 8-15min, and then vacuum degas for 10-20min to obtain a curable composite thermally conductive epoxy resin composition.

[0031] Application of epoxy glass fiber core rod material, wherein the epoxy glass fiber core rod material is used as a composite insulator core rod.

[0032] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0033] (1) Synergistic improvement of the performance of composite thermally conductive epoxy resin composition: Through the design of functionalized thermally conductive fillers, the thermal conductivity, mechanical properties, insulation and tracking resistance of epoxy resin matrix were synergistically improved; the thermal conductivity of composite thermally conductive epoxy resin composition increased from 0.210 W / (m·K) to 0.446 W / (m·K), the tensile strength increased from 68.4 MPa to 78.5 MPa, and the impact strength increased from 8.2 kJ / m 2 Increased to 12.1 kJ / m 2 The water contact angle increased from 80.2° to 104.1°, while the volumetric conductivity remained at 10. -14 It has excellent electrical insulation properties even at the S / m level;

[0034] (2) Improved comprehensive performance of epoxy glass fiber core rod material: The above-mentioned composite thermally conductive epoxy resin composition and alkali-free glass fiber are pultruded to obtain epoxy glass fiber core rod material; compared with the unmodified system, the tensile strength of the epoxy glass fiber core rod material prepared by the present invention is increased from 759.8MPa to 820.4MPa, the thermal conductivity is increased from 0.621W / (m·K) to 0.846W / (m·K), and the tensile strength retention rate after 90 days of humid heat aging in an 80℃ water bath is increased from 60.4% to 83.5%, and it still maintains excellent insulation performance.

[0035] In summary, the epoxy glass fiber core rod material prepared by this invention maintains excellent insulation performance while achieving synergistic improvement in thermal conductivity, mechanical properties, and resistance to damp heat aging. It is expected to provide a material basis for delaying material aging and improving the safety and service life of composite insulators by promoting rapid and uniform heat dissipation during core rod operation and reducing the risk of local overheating. Detailed Implementation

[0036] The present invention will be further illustrated below with reference to experimental examples, embodiments, and comparative examples. It should be noted that the following embodiments are only for illustrating the technical solutions of the present invention and are not intended to limit the scope of protection of the present invention. Without departing from the technical concept of the present invention, any equivalent substitutions or conventional adjustments made by those skilled in the art to the types and amounts of raw materials, reaction conditions, curing regimes, and pultrusion process parameters should fall within the scope of protection of the present invention.

[0037] This invention first prepares a multifunctional modifier containing alkenyl, carboxyl, biphenyl, and dual long-chain alkyl structures; then, it uses a mercaptosilane coupling agent to perform surface mercaptolation treatment on nano-boron nitride; next, it covalently grafts the multifunctional modifier onto the surface of nano-boron nitride through a mercaptoalkene click reaction to obtain a functionalized thermally conductive filler; subsequently, it disperses the functionalized thermally conductive filler in an anhydride-curing epoxy resin system to obtain a curable composite thermally conductive epoxy resin composition; finally, it uses the resin composition and glass fiber to prepare an epoxy glass fiber core rod material through pultrusion molding, and uses it in composite insulator core rods.

[0038] The epoxy glass fiber core rod material of this invention is prepared by pultrusion molding using glass fiber as the reinforcing phase and a curable composite thermally conductive epoxy resin composition as the matrix resin. The curable composite thermally conductive epoxy resin composition includes epoxy resin, an anhydride curing agent, an accelerator, and functionalized thermally conductive filler. The functionalized thermally conductive filler is prepared by a mercapto-modified nano-boron nitride and an alkenyl carboxyl-type double long-chain alkyl biphenyl modifier via a mercapto-alkene click reaction.

[0039] Through the above-mentioned multi-level interface design, the nano-boron nitride in the functionalized thermally conductive filler can form a thermally conductive pathway in the epoxy resin matrix; the biphenyl structure can enhance the interaction between it and the aromatic segments of the epoxy resin, which is beneficial to reducing the thermal resistance of the filler / resin interface; the carboxyl group can participate in the construction of the epoxy curing network and improve the interfacial bonding between the filler and the epoxy resin; the dual long-chain alkyl structure can improve the hydrophobicity and interfacial flexibility of the filler; thus, while improving the thermal conductivity of the epoxy glass fiber core rod material, it can maintain good electrical insulation and mechanical load-bearing properties, and improve its resistance to damp heat and operational reliability.

[0040] Experimental Example 1:

[0041] (1) The preparation mechanism of alkenyl carboxyl type double long-chain alkyl biphenyl modifier is as follows:

[0042] Under the action of pyridine, the primary amino group in 4-aminobiphenyl undergoes an amidation reaction with the acyl bromide group in bromoacetyl bromide, and the molar equivalent ratio of 4-aminobiphenyl to bromoacetyl bromide is controlled at 1:1 to obtain intermediate 1;

[0043] In the presence of hydrochloric acid, 12-aminododecanoic acid reacts with methanol to form methyl 12-aminododecanoate hydrochloride.

[0044] Under the action of triethylamine, the primary amino group in methyl 12-aminododecanoate hydrochloride undergoes a substitution reaction with the bromine functional group in intermediate 1, and the molar equivalent ratio of methyl 12-aminododecanoate hydrochloride to intermediate 1 is controlled to be 1:1 to obtain intermediate 2.

[0045] Under the action of N,N-diisopropylethylamine, the secondary amino group in intermediate 2 undergoes a substitution reaction with the bromine functional group in undecene bromide, and the molar equivalent ratio of intermediate 2 to undecene bromide is controlled at 1:1. Subsequently, hydrolysis is carried out under the action of sodium hydroxide, followed by acidification with dilute hydrochloric acid to hydrolyze the methyl ester to a carboxyl group, thus preparing an alkenyl carboxyl type dilong-chain alkyl biphenyl modifier; its chemical structural formula is:

[0046] ;

[0047] (2) The specific preparation method of the alkenyl carboxyl type double long-chain alkyl biphenyl modifier includes the following steps:

[0048] Nitrogen gas was introduced, and 1.8 g of 4-aminobiphenyl, 30 mL of dichloromethane and 0.7 g of pyridine were added to a three-necked reaction flask. The system was transferred to an ice bath and stirred at 150 r / min until homogeneous. 2.1 g of bromoacetyl bromide was slowly added at 0 °C. The ice bath was removed, and the mixture was refluxed for 4 h. After cooling to room temperature, 30 mL of saturated sodium bicarbonate solution was added, and the organic layer was separated. The dichloromethane was removed by rotary evaporation, and the mixture was washed four times with 8 mL of n-hexane to obtain intermediate 1.

[0049] 2.85 g of 12-aminododecanoic acid, 75 mL of methanol and 2 mL of 12 mol / L hydrochloric acid were added to a round-bottom flask. The mixture was stirred at 200 r / min at room temperature for 8 h. The mixture was then poured into 40 mL of diethyl ether, filtered, the precipitate was collected, and dried under vacuum at 45 °C for 10 h to obtain methyl 12-aminododecanoate hydrochloride.

[0050] A round-bottom flask was placed in an ice bath, and 2.3 g of methyl 12-aminododecanoate hydrochloride, 2.9 g of intermediate 1, and 40 mL of anhydrous tetrahydrofuran were added to the flask. The mixture was stirred at 150 r / min until homogeneous. 2 g of triethylamine was slowly added dropwise at 0 °C, and the mixture was stirred for another 5 min. The ice bath was removed, and the mixture was stirred at room temperature for 5 h. The mixture was then washed with 9 mL of 10 wt% sodium bicarbonate solution and 9 mL of saturated sodium chloride solution, respectively. The organic phases were combined, dried and concentrated with anhydrous sodium sulfate, separated by column chromatography (ethyl acetate to petroleum ether volume ratio of 4:1), and dried under vacuum at 45 °C for 10 h to obtain intermediate 2.

[0051] In a round-bottom flask, add 4.4 g of intermediate 2, 2.2 mL of undecene bromide, and 50 mL of toluene. Raise the temperature to 50 °C and stir at 200 rpm for 15 min. Then add 2 g of N,N-diisopropylethylamine, raise the temperature to 75 °C, and continue stirring for 10 h. Cool to room temperature, filter, and wash the filtrate twice with 30 mL of 3.6 wt% dilute hydrochloric acid. Discard the aqueous layer. Wash the organic layer twice with 60 mL of deionized water and once with 60 mL of saturated sodium chloride solution. Dry the product on anhydrous sodium sulfate and remove the toluene organic layer by vacuum distillation to obtain the crude product. The compound was added to 40 mL of 20 wt% sodium hydroxide aqueous solution, heated to 40 °C and kept at that temperature for 6 h. After the reaction was completed, the temperature was lowered to 0 °C, and 10 wt% dilute hydrochloric acid was added to adjust the pH to 2. The compound was extracted three times with 45 mL of ethyl acetate each time. The organic layers were combined, washed twice with 15 mL of saturated sodium chloride solution, dried over anhydrous sodium sulfate, filtered, concentrated under reduced pressure to dryness, and 45 mL of n-hexane / ethyl acetate (volume ratio 5:1) was added. The mixture was stirred for 1 h, filtered, and the filter cake was washed three times with 6 mL of mixed solvent and dried under vacuum at 45 °C for 10 h to obtain an alkenyl carboxyl type di-long-chain alkyl biphenyl modifier.

[0052] (3) Characterization of alkenyl carboxyl type double long-chain alkyl biphenyl modifiers:

[0053] Hydrogen spectroscopy characterization: 1 H NMR (400MHz, DMSO-D6, δ, ppm): 1.25-1.36 (m, 26H), 1.49-1.62 (m, 6H), 2.01-2.05 (m, 2H), 2.27-2.31 (t, 2H), 2.5 8-2.61(t, 4H), 3.15(s, 2H), 4.95-5.14(m, 2H), 5.72-5.81(m, 1H), 7.36-7.65(m, 9H), 8.19(s, 1H), 11.34(s, 1H);

[0054] Elemental analysis characterization: Theoretical mass fraction: carbon mass fraction 77.04%; hydrogen mass fraction 9.79%; N mass fraction 4.86%; Experimental measured values: carbon mass fraction 76.96%; hydrogen mass fraction 9.84%; N mass fraction 4.81%. The deviation between the theoretical and measured mass fractions is within 0.1%, indicating that the alkenyl carboxyl type double long-chain alkyl biphenyl modifier was successfully synthesized.

[0055] Experimental Example 2:

[0056] (1) The preparation mechanism of mercapto-modified boron nitride nanoparticles is as follows:

[0057] Thiolized boron nitride nanoparticles were prepared by surface modification of boron nitride nanoparticles with mercaptosilane coupling agents, namely 3-mercaptopropyltrimethoxysilane or 3-mercaptopropyltriethoxysilane; in the experimental example, 3-mercaptopropyltrimethoxysilane was selected, wherein the mass ratio of 3-mercaptopropyltrimethoxysilane to boron nitride nanoparticles was 0.05-0.15:1.

[0058] The specific preparation method of mercapto-modified boron nitride nanoparticles is as follows:

[0059] 1 g of boron nitride nanoparticles (average particle size 50 nm), 72 mL of anhydrous ethanol and 8 mL of deionized water were added to a three-necked flask. After ultrasonic treatment at room temperature for 10 h using a water bath ultrasonic cleaner (300 W), nitrogen gas was introduced, and 0.1 g of 3-mercaptopropyltrimethoxysilane was added to the three-necked flask. The temperature was raised to 100 °C, and the mixture was stirred at a rate of 300 r / min for 8 h. During the heating process, the ethanol gradually evaporated. After cooling to room temperature, the mixture was dispersed with petroleum ether, filtered, washed three times with 9 mL of petroleum ether, and dried in a vacuum environment at 80 °C for 8 h to obtain mercapto-modified boron nitride nanoparticles.

[0060] (2) Characterization of mercapto-modified boron nitride nanoparticles:

[0061] 6 mg of dried boron nitride nanoparticles and 6 mg of dried mercapto-modified boron nitride nanoparticles were taken respectively, and the changes of the two samples under heating conditions were analyzed using a thermogravimetric analyzer. The test was carried out in a nitrogen atmosphere at a temperature of 20-900℃ and a heating rate of 10℃ / min.

[0062] Thermogravimetric analysis results: In the range of 20-300℃, neither nano-boron nitride nor mercapto-based nano-boron nitride showed significant weight loss. The mass decrease was gradual, and this stage was due to the physical adsorption of water on the sample surface and the evaporation of a small amount of residual solvent.

[0063] At 350℃, mercaptolated boron nitride nanoparticles showed significant mass loss, which is presumably due to the thermal decomposition and volatilization of organic components in the silane coupling agent on the surface of the boron nitride nanoparticles.

[0064] When the temperature reaches 900℃, the calculated mass loss rate of boron nitride nanoparticles is 0.8%; the mass loss rate of mercapto-modified boron nitride nanoparticles is 3.2%, thus the grafting rate of 3-mercaptopropyltrimethoxysilane to boron nitride nanoparticles is 2.4%.

[0065] Experimental Example 3:

[0066] (1) The preparation mechanism of functionalized thermally conductive fillers is as follows:

[0067] Under the action of a photoinitiator (benzoin dimethyl ether or photoinitiator 1173), an alkenyl carboxyl-type dilong-chain alkyl biphenyl modifier and mercaptolated boron nitride nanoparticles undergo a mercaptoalkene click reaction to obtain a functionalized thermally conductive filler. The mass ratio of the alkenyl carboxyl-type dilong-chain alkyl biphenyl modifier to the mercaptolated boron nitride nanoparticles is 0.05-0.2:1.

[0068] The specific preparation method of functionalized thermally conductive fillers is as follows:

[0069] 1 g of mercaptolated boron nitride nanoparticles and 50 mL of dimethyl sulfoxide were added to a round-bottom flask. The mixture was stirred at 500 r / min for 30 min at room temperature. 0.15 g of alkenyl carboxyl-type di-long-chain alkyl biphenyl modifier was slowly added. The mixture was reacted under 365 nm ultraviolet light (8 W) for 2 h. The supernatant was removed by centrifugation. The mixture was washed three times with 9 mL of dimethyl sulfoxide and 9 mL of deionized water, respectively. The mixture was then dried in a vacuum environment at 50 °C for 10 h to obtain the functionalized thermally conductive filler.

[0070] (2) Characterization of functionalized thermally conductive fillers:

[0071] The surface carboxyl content was determined by acid-base titration, and the grafting rate of alkenyl carboxyl-type di-long-chain alkyl biphenyl modifier on the surface of mercapto-modified boron nitride nanoparticles was quantitatively calculated. 1 g of the sample was accurately weighed, and excess 0.01 mol / L NaOH standard solution and 50% (v / v) ethanol aqueous solution were added. After ultrasonic dispersion for 10 min, the mixture was stirred at 25℃ for 4 h to allow the surface carboxyl groups to fully neutralize. After high-speed centrifugation, all supernatant was collected, and the remaining NaOH was back-titrated with 0.01 mol / L HCl standard solution. When determining the surface carboxyl content of the functionalized filler using acid-base titration, the systematic error of the titration system was first calibrated by blank titration. Simultaneously, mercapto-modified boron nitride nanoparticles under the same treatment conditions were used as a background control. After deducting the titration deviation caused by its own acidic groups, the effective carboxyl density ρ was calculated using the formula: ρ = [c × (V 对照 -V 样品 )×10 6 ] / m, grafting rate = ρ × M × 10 -6 ×100%; where c is the concentration of HCl standard solution, V control is the volume of HCl consumed in the titration of the base control group, V sample is the volume of HCl consumed in the titration of the functionalized thermally conductive filler group, m is the mass of the sample, and M is the molar mass of the alkenyl carboxyl type dilong-chain alkyl biphenyl modifier. The grafting rate of the alkenyl carboxyl type dilong-chain alkyl biphenyl modifier was calculated to be 5.3%.

[0072] Example 1:

[0073] A curable composite thermally conductive epoxy resin composition a, comprising the following raw materials in parts by weight:

[0074] 100 parts of epoxy resin (model E51, measured epoxy equivalent 196 g / mol).

[0075] 80 parts of methylhexahydrophthalic anhydride;

[0076] 6 portions of functionalized thermally conductive filler;

[0077] 0.3 parts of 2,4,6-tris(dimethylaminomethyl)phenol;

[0078] A method for preparing a curable composite thermally conductive epoxy resin composition a includes the following steps:

[0079] Functionalized thermally conductive fillers were added to epoxy resin, heated to 60°C in a water bath, stirred at 300 r / min for 30 min, and then transferred to a water bath ultrasonic cleaner for ultrasonic dispersion at 60°C and 300 W power for 45 min to form a mixture.

[0080] Methylhexahydrophthalic anhydride and 2,4,6-tris(dimethylaminomethyl)phenol were added to the mixture. After stirring at 50°C and 300 r / min for 10 min, the mixture was placed in a vacuum drying oven and degassed under vacuum conditions of ≤-0.095 MPa for 15 min to obtain curable composite thermally conductive epoxy resin composition a.

[0081] Preparation of composite thermally conductive epoxy resin a casting:

[0082] The curable composite thermally conductive epoxy resin composition a was cast into a mold preheated to 80°C and placed in a vacuum drying oven. Under a vacuum degree ≤ -0.095MPa, the mold was degassed again for 10 minutes. The vacuum was then turned off, and the mold was transferred to the drying oven for curing according to a stepped temperature program: 90°C / 2h, 120°C / 2h, and 160°C / 2h. After curing, the mold was cooled to room temperature and demolded to obtain the composite thermally conductive epoxy resin a casting (for performance testing).

[0083] Example 2:

[0084] The only difference between curable composite thermally conductive epoxy resin composition b and curable composite thermally conductive epoxy resin composition a is that 6 parts of functionalized thermally conductive filler are replaced with 8 parts of functionalized thermally conductive filler.

[0085] The preparation method of the composite thermally conductive epoxy resin b casting is the same as that of the composite thermally conductive epoxy resin a casting.

[0086] Example 3:

[0087] The only difference between curable composite thermally conductive epoxy resin composition c and curable composite thermally conductive epoxy resin composition a is that 6 parts of functionalized thermally conductive filler are replaced with 10 parts of functionalized thermally conductive filler.

[0088] The preparation method of the composite thermally conductive epoxy resin C casting is the same as that of the composite thermally conductive epoxy resin A casting.

[0089] Comparative Example 1:

[0090] The only difference between epoxy resin composition a and curable composite thermally conductive epoxy resin composition a is that no functionalized thermally conductive filler is added.

[0091] The preparation methods for epoxy resin a casting and composite thermally conductive epoxy resin a casting are the same.

[0092] Comparative Example 2:

[0093] The only difference between epoxy resin composition b and curable composite thermally conductive epoxy resin composition b is that 8 parts of functionalized thermally conductive filler are replaced with 8 parts of mercapto-modified nano boron nitride (prepared in Experimental Example 2).

[0094] The preparation methods for epoxy resin B castings and composite thermally conductive epoxy resin B castings are the same.

[0095] Product characterization of epoxy resins prepared in the examples and comparative examples:

[0096] In-situ infrared spectroscopy was used to monitor the consumption of epoxy groups during the curing process in real time. An 872 cm⁻¹ column was selected. -1 The stretching vibration peak of the epoxy group is a characteristic peak of the epoxy group, at 1510 cm⁻¹. -1 The benzene ring skeletal vibration peak was used as an internal standard peak; the difference in sample thickness and concentration was eliminated by normalization, and the epoxy group conversion rate was calculated by the following formula: Epoxy group conversion rate (%) = (1-R t / R0)×100%, where R t R0 is the peak area ratio of the epoxy peak to the benzene ring peak during the curing process; R0 is the peak area ratio of the epoxy peak to the benzene ring peak before curing; the results are shown in Table 1.

[0097] Table 1 Results of epoxy group conversion test

[0098] serial number Epoxy group conversion rate (%) after curing at 90℃ for 2 hours Epoxy group conversion rate (%) after curing Example 1 6.3 96.4 Example 2 7.1 97.3 Example 3 7.7 97.8 Comparative Example 1 5.4 94.7 Comparative Example 2 6.1 95.9

[0099] The following conclusions can be drawn from Table 1:

[0100] (1) The epoxy group conversion rates of Examples 1 to 3 were all higher than those of Comparative Examples 1 and 2. In the 2,4,6-tris(dimethylaminomethyl)phenol-promoted anhydride curing system, the introduction of carboxyl groups on the surface of the functionalized thermally conductive filler provided additional reaction sites, which synergistically consumed epoxy groups with the anhydride, further improving the conversion rate of the examples. In Comparative Example 2, the thiolized boron nitride nanoparticles could not improve the dispersibility of the filler due to the short-chain thiol groups, resulting in lamellar aggregation and a lack of π-π synergistic effect of biphenyl groups, leading to a reduction in effective reaction sites and a slightly lower conversion rate than the examples. However, the boron nitride lamellars were prone to aggregation, resulting in a reduction in effective reaction sites, and therefore the conversion rate was lower than that of the examples.

[0101] (2) After curing, the conversion rate of epoxy groups in Examples 1 to 3 was higher than that in Comparative Example 1 and Comparative Example 2, indicating that the introduction of carboxyl groups on the surface of the functionalized thermally conductive filler increased the number of active sites that could participate in the reaction in the system, and the carboxyl groups and acid anhydrides synergistically promoted the more complete consumption of epoxy groups.

[0102] In summary, in-situ infrared spectroscopy quantitative analysis shows that the carboxyl groups on the surface of the functionalized thermally conductive filler participate in the curing process of the epoxy resin, forming an interfacial chemical bond between the functionalized thermally conductive filler and the epoxy resin.

[0103] Performance testing:

[0104] (1) Mechanical property testing:

[0105] Tensile strength: The epoxy resin casting samples prepared in the examples and comparative examples were subjected to tensile tests using a mechanical testing machine in accordance with the standard GB / T 1040.1-2018 "Determination of tensile properties of plastics - Part 1: General". The tensile speed was 2 mm / min, and the test was repeated at least 3 times. The average value was taken. The test results are shown in Table 2.

[0106] Impact strength test: The epoxy resin casting samples prepared in the unnotched examples and comparative examples were tested using an A-type pendulum impact tester according to the standard GB / T 1043.1-2008 "Determination of impact properties of simply supported plastic beams - Part 1: Non-instrumental impact test". The impact energy was 4J, and the measurement was repeated at least 3 times. The average value was taken. The sample size was 80mm×10mm×4mm. The test results are shown in Table 2.

[0107] Table 2 Test results of mechanical properties of epoxy resin

[0108] serial number Tensile strength (MPa) <![CDATA[Impact strength (kJ / m 2 )]]> Example 1 72.3 10.6 Example 2 78.5 12.1 Example 3 75.1 11.4 Comparative Example 1 68.4 8.2 Comparative Example 2 71.2 9.4

[0109] The following conclusions can be drawn from Table 2:

[0110] Compared with Comparative Example 1 (pure epoxy resin composition), the epoxy resin modified with functionalized thermally conductive filler in the examples can simultaneously improve the tensile strength and impact strength of the curable composite thermally conductive epoxy resin composition, achieving a synergistic effect of reinforcement and toughening.

[0111] Although the thiol groups on the surface of the mercapto-modified boron nitride nanoparticles in Comparative Example 2 can react with epoxy groups to form interfacial covalent bonds, the short-chain thiol groups can only provide limited chemical bonding, which cannot effectively reduce the interfacial energy between the filler and the matrix, nor can they provide sufficient steric hindrance to inhibit the stacking and aggregation of boron nitride sheets, thereby weakening the mechanical property enhancement effect.

[0112] Compared with Comparative Example 2, Example 2, with the same amount of additive, showed significantly improved tensile strength and impact strength, indicating a significant enhancement in the interfacial bonding between the functionalized thermally conductive filler and the epoxy resin. On the one hand, the biphenyl groups on the surface of the functionalized thermally conductive filler form π-π interactions with the benzene rings in the epoxy resin, improving interfacial compatibility; the long alkyl chains on the surface of the functionalized thermally conductive filler are flexible structures, forming a flexible buffer layer at the interface between the filler and the epoxy resin. Under impact, energy is dissipated through molecular chain slippage and entanglement, improving impact toughness; on the other hand, the carboxyl groups on the surface of the functionalized thermally conductive filler participate in the curing process of the epoxy resin and react with the epoxy groups to form chemical bonds. The dual effects of physical compatibility and chemical bonding synergistically enhance the interfacial stress transfer efficiency, reduce interfacial defects, and achieve simultaneous improvement in mechanical properties.

[0113] (2) Thermal conductivity test: The thermal conductivity of the epoxy resin casting sample was tested using a thermal conductivity tester according to the standard GB / T 10297-2015 "Determination of thermal conductivity of non-metallic solids by hot wire method". The test temperature was 25℃. The test results are shown in Table 3.

[0114] Table 3 Test results of thermal conductivity of epoxy resin

[0115] serial number Thermal conductivity [W / (m·K)] Example 1 0.375 Example 2 0.413 Example 3 0.446 Comparative Example 1 0.210 Comparative Example 2 0.354

[0116] The following conclusions can be drawn from Table 3:

[0117] Compared with Comparative Example 1, the thermal conductivity of the curable composite thermally conductive epoxy resin composition prepared in the examples was significantly improved.

[0118] Although the thiol groups on the surface of the mercapto-modified boron nitride nanoparticles in Comparative Example 2 can react with epoxy groups to form interfacial covalent bonds, the short-chain structure cannot effectively reduce the surface energy difference between the boron nitride nanoparticles and the epoxy resin. The steric hindrance is insufficient, which cannot prevent the boron nitride sheets from approaching and agglomerating, thus disrupting the continuity of the thermal conductivity pathway. Therefore, the improvement in thermal conductivity is limited.

[0119] Compared with Comparative Example 2, the thermal conductivity of Example 2, with the same amount of additive, is significantly higher. Possible reasons include: the high thermal conductivity nano-boron nitride sheets are uniformly dispersed in the epoxy resin matrix, gradually overlapping to form a continuous thermally conductive network, providing a high-speed channel for phonon transmission; the π-π interaction between the biphenyl groups on the surface of the functionalized thermally conductive filler and the benzene rings of the epoxy resin improves the interfacial bonding strength, promotes the local ordered arrangement of molecular chains at the interface, enhances the interfacial phonon transmittance, and effectively reduces the interfacial thermal resistance; simultaneously, the carboxyl groups on the surface of the functionalized thermally conductive filler react with the epoxy groups during epoxy resin curing to form covalent bonds. These multiple effects significantly enhance the interfacial bonding between the functionalized thermally conductive filler and the epoxy resin, reduce interfacial phonon scattering, lower interfacial thermal resistance, and improve thermal conductivity.

[0120] (3) Insulation performance test:

[0121] Volumetric conductivity test: The DC volumetric conductivity of the epoxy resin casting sample was tested using the three-electrode method. The sample size was 30mm×30mm×1mm, and the test temperature was 25℃. The test results are shown in Table 4.

[0122] Dielectric constant testing: The relative permittivity of the epoxy resin casting sample was tested using a broadband dielectric spectrometer. The sample thickness was 1 mm, and the frequency range was set to 10 Hz. 5 The test frequency was Hz, the test temperature was 25℃, the test voltage was 1kV, and the test results are shown in Table 4.

[0123] Water contact angle: The epoxy resin casting sample was tested using a water contact angle measuring instrument. The test solution was 4 μL of deionized water. The solution was dropped at 5 different locations on the sample, and the average value of the measured contact angle was taken. The results are shown in Table 4.

[0124] Table 4 Test results of epoxy resin insulation performance

[0125] serial number <![CDATA[Volume conductivity (×10 -14 S / m)]]> Relative permittivity Water contact angle (°) Example 1 12.3 4.2 99.5 Example 2 13.4 4.3 102.3 Example 3 14.6 4.5 104.1 Comparative Example 1 8.5 4.0 80.2 Comparative Example 2 11.2 4.2 83.1

[0126] The following conclusions can be drawn from Table 4:

[0127] Compared with Comparative Example 1, the volume conductivity and relative permittivity of the curable composite thermally conductive epoxy resin composition prepared in the examples are slightly improved. It is speculated that with the increase of the amount of functionalized thermally conductive filler, the number of interface regions increases and gradually overlaps, and the polarization effect is enhanced, resulting in a slight increase in volume conductivity and permittivity, and a slight decrease in insulation. However, the overall difference is not significant, and the volume conductivity remains at 10. -14 The S / m order of magnitude indicates that the epoxy resin material still maintains excellent insulation properties;

[0128] Compared with Comparative Example 1, in terms of hydrophobic properties, the water contact angle of pure epoxy resin is 80.2°, which is lower than 90°, indicating weak hydrophilicity. The long alkyl chains and biphenyl structures on the surface of the functionalized thermally conductive filler can significantly improve the hydrophobicity of the curable composite thermally conductive epoxy resin composition, with a contact angle of up to 104.1°. The hydrophobic surface can inhibit liquid spreading and wetting, reduce water adhesion and capillary penetration, and hinder the formation of conductive water film, which has a positive effect on improving insulation reliability.

[0129] Tracking resistance test:

[0130] A needle-plate electrode DC tracking test was conducted. A needle electrode with a tip curvature radius of 5 μm and a plate electrode with a width of 15 mm were selected. The distance between the needle and plate electrodes was 4 mm. A DC voltage of 600 V was applied. The needle electrode was connected to the DC power supply terminal, and the plate electrode was connected to ground through a 5 kΩ protective resistor. The electrolyte was a 0.1 wt% NH4Cl solution with a resistivity of 4 Ω·m at 23 °C. The epoxy resin casting sample thickness was 4 mm. The tracking area was quantified using Matlab software. The mass loss of the epoxy resin casting sample was measured using a precision analytical balance. The tracking depth was measured using a micrometer. The test results are shown in Table 5.

[0131] Table 5 Test results of the tracking resistance of epoxy resin

[0132] serial number <![CDATA[Tracking area (mm 2 )]]> Mass loss (mg) Electrical trace depth (mm) Example 1 24.1 9.4 1.3 Example 2 23.4 8.5 1.1 Example 3 22.9 7.7 0.8 Comparative Example 1 25.2 12.3 1.6 Comparative Example 2 24.7 11.2 1.5

[0133] The following conclusions can be drawn from Table 4:

[0134] Compared with Comparative Example 1, the track resistance of the curable composite thermally conductive epoxy resin composition prepared in the examples is improved. As the amount of functionalized thermally conductive filler increases, the track area, mass loss and track depth in track destruction gradually decrease. Track destruction is a phenomenon of material deterioration caused by surface discharge. Track carbonization is mainly due to the large amount of heat generated during the discharge process.

[0135] The improved tracking resistance of the curable composite thermally conductive epoxy resin composition is speculated to be due to the following reasons: the thermally conductive network in the curable composite thermally conductive epoxy resin composition can quickly conduct and dissipate the local heat generated by the discharge, avoiding heat accumulation at the discharge site and inhibiting epoxy resin carbonization and the formation of carbonized conductive channels; the hydrophobicity of the curable composite thermally conductive epoxy resin composition reduces the wetting, spreading and penetration of liquid on the material surface, reduces the formation of continuous water films and conductive channels on the surface, and reduces the discharge intensity and degree of carbonization; the good interfacial bonding between the functionalized thermally conductive filler and the epoxy resin reduces micro-defects and micro-cracks at the filler-epoxy resin interface, thereby reducing the liquid penetration path along the cracks.

[0136] In summary, the curable composite thermally conductive epoxy resin composition with 8 parts of functionalized thermally conductive filler exhibits the best overall performance. The addition of functionalized thermally conductive filler to the epoxy resin improves the interfacial compatibility through both π-π interactions and interfacial covalent bonds. This enhances stress transfer and improves mechanical properties, while reducing interfacial thermal resistance and increasing thermal conductivity. Simultaneously, it improves the hydrophobicity of the epoxy resin, and the combined effect of hydrophobicity and thermal conductivity synergistically enhances its tracking resistance. Furthermore, the curable composite thermally conductive epoxy resin composition maintains excellent insulation levels, meeting the basic performance requirements of insulating components such as composite insulator core rods.

[0137] Example 4:

[0138] Epoxy glass fiber core rod material a, comprising the following raw materials:

[0139] 25wt% Curable composite thermally conductive epoxy resin composition b (prepared in Example 2);

[0140] 75wt% alkali-free glass fiber (E glass fiber untwisted coarse sand, linear density of 2400tex);

[0141] The preparation method of epoxy glass fiber core rod material a is as follows:

[0142] E-glass fiber untwisted coarse sand was dried at 100℃ for 2 hours. The dried E-glass fiber untwisted coarse sand was evenly guided out through a yarn rack and arranged through a yarn guide plate so that the glass fiber bundles were arranged parallel to each other along the pultrusion direction; thus obtaining pretreated glass fiber.

[0143] Pretreated glass fibers are introduced into the impregnation tank of curable composite thermally conductive epoxy resin composition b to fully wet them. The fiber bundles are gradually compressed by a preforming device to make them denser. The content ratio of glass fibers to curable composite thermally conductive epoxy resin composition b is controlled by adjusting the aperture of the preforming device, the extrusion pressure and the traction speed to form a blank.

[0144] The preform is fed into a heated pultrusion die, where it is shaped and cured. The heated pultrusion die is set with multiple temperature zones along the traction direction. The temperature is controlled as follows: inlet preheating zone: 100℃; middle gel zone: 130℃; outlet curing zone: 160℃. The pultrusion speed is controlled at 0.4m / min to obtain epoxy glass fiber core rod material a.

[0145] Example 5:

[0146] The only difference between epoxy glass fiber core rod material b and epoxy glass fiber core rod material a is that 25 wt% of epoxy resin a (prepared in Comparative Example 1) is used instead of 25 wt% of curable composite thermally conductive epoxy resin composition b.

[0147] Performance testing:

[0148] (1) Mechanical property testing:

[0149] Tensile strength test: The tensile strength of epoxy glass core rod material was tested according to the standard GB / T 13096-2008 "Test method for mechanical properties of pultruded glass fiber reinforced plastic rods". The test results are shown in Table 6.

[0150] Impact strength test: The impact strength of epoxy glass fiber core rod material was tested according to the standard GB / T 1451-2005 "Test method for impact toughness of fiber reinforced plastics with simply supported beam". The test results are shown in Table 6.

[0151] (2) Thermal conductivity test: The thermal conductivity of epoxy glass fiber core rod material was tested using a thermal conductivity tester according to the standard GB / T 10297-2015 "Determination of thermal conductivity of non-metallic solids by hot wire method". The test temperature was 25℃. The test results are shown in Table 6.

[0152] (3) Insulation performance test:

[0153] Volumetric conductivity test: The DC volumetric conductivity of epoxy glass fiber core rod material was tested using the three-electrode method. The sample size was 30mm×30mm×1mm and the test temperature was 25℃. The test results are shown in Table 7.

[0154] Dielectric constant testing: The relative permittivity of the epoxy glass fiber core rod material was tested using a broadband dielectric spectrometer. The sample thickness was 1 mm, and the frequency range was set to 10 Hz. 5 The test results are shown in Table 7. The test temperature was 25℃ and the test voltage was 1kV.

[0155] (4) Damp heat aging test: The epoxy glass fiber core rod material was subjected to a damp heat aging test in an 80℃ water bath. The test was completed in a constant temperature water bath. After 90 days, the surface condition of the epoxy glass fiber core rod material was observed. The tensile strength of the epoxy glass core rod material was tested again according to the standard GB / T 13096-2008 "Test Method for Mechanical Properties of Pultruded Glass Fiber Reinforced Plastic Rods". The tensile strength retention rate (%) was calculated as (tensile strength after damp heat aging / initial tensile strength) × 100%. The test results are shown in Table 8.

[0156] Table 6 Test results of epoxy glass fiber core rod material properties 1

[0157] product Tensile strength (MPa) <![CDATA[Impact strength (kJ / m 2 )]]> Thermal conductivity [W / (m·K)] Epoxy glass fiber core rod material a 820.4 134.3 0.846 Epoxy glass fiber core material b 759.8 114.7 0.621

[0158] Table 7 Test results of epoxy glass fiber core rod material properties 2

[0159] product <![CDATA[Volume conductivity (×10 -14 S / m)]]> Relative permittivity Epoxy glass fiber core rod material a 6.5 5.2 Epoxy glass fiber core material b 4.2 4.9

[0160] Table 8 Test results of epoxy glass fiber core rod material properties 3

[0161] product Surface state changes Tensile strength retention rate (%) Epoxy glass fiber core rod material a No significant changes 83.5 Epoxy glass fiber core material b The surface becomes rough and fine cracks appear. 60.4

[0162] The following conclusions can be drawn from Tables 6, 7, and 8:

[0163] Mechanical properties: The functionalized thermally conductive filler optimizes the interfacial bonding between epoxy resin and glass fiber through interfacial covalent bonds and π-π stacking, improving stress transfer efficiency. At the same time, the surface double long-chain alkyl forms a flexible buffer layer to achieve interfacial toughening. Therefore, the tensile strength and impact toughness of epoxy glass fiber core rod material a are better than those of epoxy glass fiber core rod material b.

[0164] Thermal conductivity: Continuous glass fiber is the main thermal conduction path of the core rod; functionalized thermally conductive filler builds auxiliary thermal conduction paths in the resin phase on the one hand, and reduces the thermal resistance at the interface between glass fiber and epoxy resin on the other hand. The two work together to improve the overall thermal conductivity; therefore, the thermal conductivity of epoxy glass fiber core rod material a is better than that of epoxy glass fiber core rod material b.

[0165] Insulation performance: Glass fibers divide the continuous epoxy resin phase into isolated regions, binding the movement of migratable ions, resulting in a lower volume conductivity of the epoxy glass fiber core rod material compared to pure resin castings. The introduction of thermally conductive fillers slightly enhances interfacial polarization, causing a slight increase in the volume conductivity and dielectric constant of epoxy glass fiber core rod material a compared to epoxy glass fiber core rod material b, but the material maintains a 10⁻⁶ level. 14 The high insulation level of S / m meets the requirements for the use of composite insulator core rods;

[0166] Resistance to damp heat aging: After 90 days of damp heat aging in an 80℃ water bath, the surface of epoxy glass fiber core rod material b became rough and developed micro-cracks, with a tensile strength retention rate of only 60.4%; while the surface condition of epoxy glass fiber core rod material a showed no significant change, and the tensile strength retention rate reached 83.5%.

[0167] Functionalized thermally conductive fillers form covalent bonds between surface carboxyl groups and epoxy groups, and with the π-π stacking effect of biphenyl groups, they not only strengthen the interfacial bonding between the filler and the resin matrix and eliminate water seepage channels at the filler interface, but also improve the overall crosslinking density and compactness of the resin. This indirectly optimizes the interfacial bonding state between epoxy resin and glass fiber, effectively blocking the penetration path of water molecules along the fiber interface, and reducing matrix hydrolysis and interfacial debonding in hot water environments. Therefore, the epoxy glass fiber core rod material a prepared by this invention has superior resistance to humid heat aging and can meet the long-term service requirements of composite insulator core rods in humid heat environments.

[0168] Application of epoxy glass fiber core material in composite insulators:

[0169] I. Composite Insulator Structure

[0170] Composite insulators were prepared by using the above-mentioned epoxy glass fiber core rod material as the inner load-bearing insulating core rod of the composite insulator.

[0171] The composite insulator includes: epoxy glass fiber core rod material; silicone rubber sheath and shed covering the outer surface of the core rod; end fittings assembled at both ends of the core rod; and a sealing structure provided in the connection area of ​​the core rod, sheath and end fittings, including a silicone rubber sealing layer at the connection between the fittings and the sheath and a sealing ring inside the fitting cavity.

[0172] Among them, the epoxy glass fiber core rod is the main internal load-bearing insulation body, which mainly bears mechanical load and provides main internal insulation; the silicone rubber sheath and sheds are the external insulation structure, providing weather resistance, anti-pollution flashover and water-repellent protection; the end fittings are used to realize the mechanical connection between the composite insulator and the transmission line, tower or other support structure.

[0173] II. Composite Insulator Preparation Method

[0174] Step 1: Pretreatment of mandrel surface:

[0175] Take the epoxy glass fiber core rod material prepared above and cut it to a fixed length according to the design length of the composite insulator; clean and lightly polish the outer surface of the core rod to remove surface contaminants and weak interface layer; then use silane coupling agent (such as KH-560) or special silicone rubber primer to perform interface treatment on the surface of the core rod, and dry it at 100℃ for 15 minutes to improve the bonding strength between the silicone rubber sheath and the surface of the core rod;

[0176] Step 2: Molding of silicone rubber sheath and skirt

[0177] The pre-treated core rod is placed into the composite insulator molding mold, and a continuous sheath and skirt structure is formed on the outer surface of the core rod by liquid silicone rubber injection molding or high-temperature vulcanized silicone rubber compression molding process.

[0178] The preferred method is liquid silicone rubber injection molding: mold temperature is 150℃, injection pressure is 15MPa, and vulcanization time is 30min, which can be adjusted according to the sheath thickness to ensure that the silicone rubber is fully vulcanized and crosslinked.

[0179] Step 3: Assembly and sealing of end fittings

[0180] End fittings are assembled at both ends of the mandrel; the fittings and the mandrel can be connected by crimping, wedge bonding or adhesive bonding, with crimping being preferred; the end fittings are hot-dip galvanized steel fittings or aluminum alloy fittings, and the crimping length is 5 times the diameter of the mandrel;

[0181] After crimping, room temperature vulcanizing silicone rubber sealant is applied to the joint area between the fitting and the silicone rubber sheath, and a sealing ring is installed to form a double moisture-proof sealing structure, preventing external moisture from entering the mandrel through the interface between the fitting, sheath, and mandrel.

[0182] III. Application Effects of Composite Insulators

[0183] The composite insulator prepared using the epoxy glass fiber core material of this invention retains the advantages of traditional composite insulators, such as light weight, high strength, resistance to pollution flashover, and good hydrophobicity, while significantly improving the internal thermal conductivity of the core rod. During long-term operation, factors such as dielectric loss, partial discharge, and ambient temperature rise can generate localized heat within the core rod. The uniformly dispersed functionalized nano-boron nitride sheets within the core rod, in synergy with the continuous glass fiber skeleton, construct a multi-scale thermally conductive network, simultaneously improving the axial and radial thermal conductivity of the core rod. This promotes rapid heat transfer from the interior to the sheath surface, reduces the internal hot spot temperature of the core rod, and slows down the thermal aging rate of the epoxy resin matrix. Simultaneously, the functionalized thermally conductive filler optimizes the interfacial compatibility between the filler and the resin, and the hydrophobic effect of the long-chain alkyl groups on the surface enhances the overall hydrophobicity of the material, strengthens the interfacial bonding strength between the resin and glass fiber, and further enhances the long-term reliability of the core rod in humid and hot environments.

[0184] Therefore, the epoxy glass fiber core rod material prepared by this invention is suitable for the inner load-bearing insulating core rod of composite insulators, and can meet the requirements of high voltage, ultra-high voltage and extra-high voltage transmission lines for the core rod's thermal conductivity, insulation performance, damp heat resistance and long-term operational stability.

Claims

1. An epoxy glass fiber core rod material, characterized in that, Including the following raw materials: The composition comprises 70-80 wt% alkali-free glass fiber and 20-30 wt% curable composite thermally conductive epoxy resin; the alkali-free continuous glass fiber is E-glass fiber roving or ECR glass fiber roving; the curable composite thermally conductive epoxy resin composition comprises the following raw materials in parts by weight: 90-100 parts epoxy resin, 70-80 parts curing agent, 0.1-1 part accelerator, and 6-10 parts functionalized thermally conductive filler; The functionalized thermally conductive filler is prepared by a mercapto-alkene click reaction between an alkenyl-carboxyl-type dual long-chain alkyl biphenyl modifier and mercapto-modified nano-boron nitride under the action of a photoinitiator; the mass ratio of the alkenyl-carboxyl-type dual long-chain alkyl biphenyl modifier to the mercapto-modified nano-boron nitride is 0.05-0.2:1; The chemical structural formula of the alkenyl carboxyl type double long-chain alkyl biphenyl modifier is: 。 2. The epoxy glass fiber core rod material according to claim 1, characterized in that, The preparation method of the alkenyl carboxyl type double long-chain alkyl biphenyl modifier is as follows: Under the action of pyridine, the primary amino group in 4-aminobiphenyl undergoes an amidation reaction with the acyl bromide group in bromoacetyl bromide, and the molar equivalent ratio of 4-aminobiphenyl to bromoacetyl bromide is controlled at 1:1 to obtain intermediate 1; In the presence of hydrochloric acid, 12-aminododecanoic acid reacts with methanol to form methyl 12-aminododecanoate hydrochloride. Under the action of triethylamine, the primary amino group in methyl 12-aminododecanoate hydrochloride undergoes a substitution reaction with the bromine functional group in intermediate 1, and the molar equivalent ratio of methyl 12-aminododecanoate hydrochloride to intermediate 1 is controlled to be 1:1 to obtain intermediate 2. Under the action of N,N-diisopropylethylamine, the secondary amino group in intermediate 2 undergoes a substitution reaction with the bromine functional group in undecene bromide, and the molar equivalent ratio of intermediate 2 to undecene bromide is controlled at 1:

1. Subsequently, after hydrolysis and acidification treatment, the methyl ester is converted into a carboxyl group to obtain an alkenyl carboxyl type dilong-chain alkyl biphenyl modifier.

3. The epoxy glass fiber core rod material according to claim 1, characterized in that, The epoxy resin is at least one of bisphenol A type epoxy resin and bisphenol F type epoxy resin.

4. The epoxy glass fiber core rod material according to claim 1, characterized in that, The curing agent is methylhexahydrophthalic anhydride or methyltetrahydrophthalic anhydride.

5. The epoxy glass fiber core rod material according to claim 1, characterized in that, The accelerator is 2-methylimidazole or 2,4,6-tris(dimethylaminomethyl)phenol.

6. The epoxy glass fiber core rod material according to claim 1, characterized in that, The photoinitiator is benzoin dimethyl ether or photoinitiator 1173.

7. The epoxy glass fiber core rod material according to claim 1, characterized in that, The mercaptolated boron nitride nanoparticles are prepared by surface modification of boron nitride nanoparticles with a mercaptosilane coupling agent; the mercaptosilane coupling agent is 3-mercaptopropyltrimethoxysilane or 3-mercaptopropyltriethoxysilane; the mass ratio of the mercaptosilane coupling agent to boron nitride nanoparticles is 0.05-0.15:

1.

8. The method for preparing the epoxy glass fiber core rod material according to any one of claims 1-7, characterized in that, Includes the following steps: The alkali-free glass fiber is dried at 90-110℃ for 1-3 hours. The dried glass fiber is then evenly guided out through a yarn rack and arranged through a yarn guide plate so that the glass fiber bundles are arranged parallel to each other along the pultrusion direction. Pretreated glass fibers are obtained; Pretreated glass fibers are introduced into the impregnation tank of curable composite thermally conductive epoxy resin composition to fully wet them. The fiber bundles are gradually extruded through a preforming device to densify them. The content ratio of glass fibers to curable composite thermally conductive epoxy resin composition is controlled by adjusting the aperture of the preforming device, the extrusion pressure and the traction speed to form a blank. The preform is fed into a heated pultrusion die, where it is shaped and cured. The heated pultrusion die has multiple temperature zones along the traction direction. The temperature is controlled as follows: inlet preheating zone: 90-110℃; middle gel zone: 120-140℃; outlet curing zone: 150-180℃. The pultrusion speed is controlled at 0.3-0.8 m / min to obtain epoxy glass fiber core rod material.

9. The method for preparing the epoxy glass fiber core rod material according to claim 8, characterized in that, The preparation method of the composite thermally conductive epoxy resin composition includes the following steps: Functionalized thermally conductive fillers are added to epoxy resin, the water bath temperature is raised to 55-65℃, the mixture is stirred at a rate of 200-400r / min for 20-40min, and then ultrasonically dispersed for 30-60min to form a mixture. Add curing agent and accelerator to the mixture, stir at 45-55℃ and 200-400r / min for 8-15min, and then vacuum degas for 10-20min to obtain a curable composite thermally conductive epoxy resin composition.

10. The application of the epoxy glass fiber core rod material according to any one of claims 1-7, characterized in that, The epoxy glass fiber core rod material is used as the core rod of the composite insulator.