Composite insulator glass fiber core rod material and method for manufacturing the same
By using epoxy-functionalized organic-inorganic hybrid toughening modification components, the problems of insufficient toughness and weak interfacial bonding in composite insulator core rod materials have been solved, resulting in a core rod material with high strength and high toughness, suitable for high voltage and ultra-high voltage transmission lines.
Patent Information
- Application Number
- CN202611457578.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-18
- Publication Date
- 2026-11-24
AI Technical Summary
Existing composite insulator core rod materials lack toughness, and the interface between glass fiber and resin matrix is weak. Conventional toughening modification methods lead to deterioration of mechanical strength, affecting the safe operation of transmission lines.
The toughening and modifying component is an epoxy-functionalized organic-inorganic hybrid. Through the synergistic effect of cage-type polysilsesquioxane and polyethylene glycol monooleate, a covalent bond interface is formed to enhance the fiber-resin bond. The preparation method includes surface treatment, premixing, impregnation and pultrusion processes.
It significantly improves the toughness and long-term operational reliability of mandrel materials, increasing impact toughness by 117-199%, tensile strength and flexural strength by 15-36%, and reducing the risk of interface debonding, meeting the DL/T1580-2021 standard.
Smart Images

Figure QLYQS_1
Abstract
Description
Technical Field
[0001] This invention relates to the field of composite insulator core rod material research and development technology, and particularly to epoxy resin / glass fiber core rod material, specifically glass fiber core rod material for composite insulators and its preparation method. Background Technology
[0002] Composite insulators are widely used in high-voltage and ultra-high-voltage transmission lines due to their advantages such as light weight, high mechanical strength, and excellent resistance to flashover. A composite insulator consists of three parts: a core rod, shed sheaths, and end fittings. The core rod is the core component that bears the mechanical load and provides internal insulation. It is typically made of resin-impregnated unidirectional glass fiber (FRP) through a pultrusion process, and its performance directly determines the mechanical strength, electrical insulation performance, and long-term operational reliability of the composite insulator.
[0003] Epoxy resin has become the mainstream matrix resin for high-voltage composite insulator core rods due to its excellent bonding properties and good electrical insulation. However, the cross-linked network structure formed after curing of traditional epoxy resin is dense and has high rigidity, resulting in insufficient toughness and impact resistance of the material, exhibiting brittle characteristics. When subjected to dynamic loads, extreme temperature changes, or long-term stress, microcracks are easily generated and gradually propagate, which can lead to interface debonding or even core rod fracture in severe cases, affecting the safe operation of transmission lines.
[0004] In addition, the surface of glass fiber is inert, and the interface between it and the epoxy resin matrix mainly relies on physical wetting and mechanical locking. Under the action of damp heat, electric field and long-term mechanical stress coupling, it is prone to debonding, hydrolysis and aging, which can become potential causes of mandrel brittle fracture and interface breakdown.
[0005] To improve the toughness of glass fiber / epoxy resin mandrels, existing technologies typically employ the following strategies: First, introducing flexible dispersed phases such as rubber elastomers into the resin matrix to absorb impact energy through mechanisms like crazing and shear band yielding; second, adding inorganic nanofillers to the matrix to inhibit crack propagation using the crack deflection and bridging effects of nanoparticles. However, these methods have significant limitations: while rubber elastomer toughening can improve fracture toughness to some extent, its flexible segments reduce the crosslinking density of the resin matrix, leading to deterioration in mechanical strength properties. Furthermore, the introduction of the rubber phase may increase dielectric loss and reduce electrical insulation performance. Nanoparticle-filled modification faces bottlenecks such as difficulty in nanoscale dispersion, easy aggregation and sedimentation, and poor inorganic-organic interface compatibility and weak interfacial bonding, making it difficult to form a uniform and stable reinforcing network in the resin matrix, and potentially becoming stress concentration points. Summary of the Invention
[0006] This invention addresses the shortcomings of existing epoxy resin core rod materials, such as insufficient toughness, weak interfacial bonding between glass fiber and resin matrix, and mechanical strength degradation associated with conventional toughening modifications. It provides a glass fiber core rod material for composite insulators and its preparation method. By designing epoxy-functionalized organic-inorganic hybrid toughening modification components, and utilizing the synergistic effect of the rigid nanoframework of cage-type polysilsesquioxane (POSS) and the flexible segments of polyethylene glycol monooleate ether, effective toughening is achieved while maintaining the high strength and excellent electrical insulation properties of epoxy resin. Simultaneously, a fiber-resin chemically bonded interface is constructed, significantly improving the toughness and long-term operational reliability of the core rod material.
[0007] The glass fiber core rod material for composite insulators comprises the following raw materials in parts by weight:
[0008] 80-120 parts of bisphenol A type epoxy resin;
[0009] 5-15 parts of epoxy-functionalized organic-inorganic hybrid toughening and modifying components;
[0010] 60-90 parts of acid anhydride curing agent;
[0011] 1-3 parts curing accelerator;
[0012] 1-3 parts release agent;
[0013] 200-300 parts E-glass fiber untwisted roving;
[0014] 2-3 parts epoxy silane coupling agent;
[0015] Among them, the epoxy-functionalized organic-inorganic hybrid toughening and modifying component is prepared by bis(chloropropyl)octaphenyl cage-type polysilsesquioxane and polyethylene glycol monooleate ether through Williamson etherification and epoxidation reaction;
[0016] Preferably, the polyethylene glycol monooleate is one of polyoxyethylene (2) oleate, polyoxyethylene (10) oleate, and polyoxyethylene (20) oleate.
[0017] Preferably, the bisphenol A type epoxy resin is of type E51;
[0018] Preferably, the anhydride curing agent is methyltetrahydrophthalic anhydride curing agent;
[0019] Preferably, the curing accelerator is 2-ethyl-4-methylimidazole;
[0020] Preferably, the E-glass fiber untwisted roving is of type 2400 tex;
[0021] Preferably, the epoxy silane coupling agent is 3-(2,3-epoxypropoxy)propyltrimethoxysilane.
[0022] A method for preparing glass fiber core material for composite insulators includes the following steps:
[0023] Step 1: After hydrolyzing 3-(2,3-epoxypropoxy)propyltrimethoxysilane, surface treatment is performed on E-glass fiber roving to obtain modified glass fiber with surface-grafted epoxy groups.
[0024] Step 2: Premix bisphenol A type epoxy resin with epoxy functionalized organic-inorganic hybrid toughening and modifying components, add methyltetrahydrophthalic anhydride curing agent, 2-ethyl-4-methylimidazolium and internal release agent, and degas under vacuum to obtain epoxy resin adhesive.
[0025] Step 3: Immerse the modified glass fiber in the epoxy resin solution and pre-form it to obtain impregnated fiber bundles;
[0026] Step 4: The resin-impregnated fiber bundles are cured by gradient heating through a pultrusion die and then post-treated to obtain the glass fiber core rod material for the composite insulator;
[0027] The epoxy-functionalized organic-inorganic hybrid toughening and modifying component participates in the cross-linking and curing reaction of epoxy resin through epoxy groups and is covalently anchored in the epoxy resin cross-linking network.
[0028] The modified glass fiber participates in the curing reaction simultaneously through surface-grafted epoxy groups, forming a fiber-resin chemically bonded interface.
[0029] Preferably, the preparation method of the epoxy-functionalized organic-inorganic hybrid toughening modification component is as follows:
[0030] Under alkaline conditions with nitrogen protection and the presence of sodium hydride, anhydrous tetrahydrofuran was used as a solvent to achieve the etherification reaction of the terminal chlorine group of 1 molar equivalent of bis(chloropropyl)octaphenyl cage-type polysilsesquioxane with the terminal hydroxyl group of 2.01-2.09 molar equivalent of polyethylene glycol monooleate ether via the Williamson ether synthesis method, resulting in an alkenyl-containing organic-inorganic hybrid toughening and modifying component;
[0031] Under nitrogen protection, anhydrous dichloromethane was used as a solvent to epoxidize the alkenyl functional groups in the alkenyl-containing organic-inorganic hybrid toughening modification component with m-chloroperoxybenzoic acid, resulting in an epoxy-functionalized organic-inorganic hybrid toughening modification component.
[0032] Preferably, the preparation method of the bis(chloropropyl)octaphenyl cage-type polysilsesquioxane is as follows:
[0033] Using phenyltrimethoxysilane as raw material, a hydrolysis-condensation method was adopted. The phenyltrimethoxysilane underwent a hydrolysis-condensation reaction catalyzed by sodium hydroxide to generate an incompletely condensed octaphenyl cage-type polysilsesquioxane sodium salt.
[0034] Using incompletely condensed octaphenyl cage-type polysilsesquioxane sodium salt as raw material, bis(silylhydrogen)octaphenyl cage-type polysilsesquioxane was synthesized by apex-capping method under nitrogen protection and anhydrous tetrahydrofuran solvent, with methyl dichlorosilane as capping agent and triethylamine catalysis.
[0035] Using 1 molar equivalent of bis(silylhydrogen)octaphenyl cage-type polysilsesquioxane and 2.01-2.09 molar equivalents of 3-chloropropene as raw materials, under nitrogen protection and in anhydrous toluene solvent, the alkenyl group of bis(silylhydrogen)octaphenyl cage-type polysilsesquioxane undergoes a hydrosilylation reaction with 3-chloropropene via a Karstedt catalyst to generate bis(chloropropyl)octaphenyl cage-type polysilsesquioxane.
[0036] Preferably, in step one, the hydrolysis conditions are: ethanol-water mixed solvent, pH adjusted to 5.0-6.0, hydrolysis at room temperature for 1-3 hours;
[0037] The surface treatment is an online continuous process, with a fiber traction speed of 0.5-1.5 m / min, a treatment temperature of 35-45℃, and a drying temperature of 100-120℃.
[0038] Preferably, in step two, the premixing temperature is 50-70℃ and the premixing time is 0.5-2h;
[0039] The vacuum degassing process has a vacuum degree of ≤-0.09MPa and a time of 15-30min.
[0040] Preferably, in step three, the impregnation temperature is 45-55℃ and the impregnation time is 60-120s;
[0041] The preforming temperature is 65-75℃.
[0042] Preferably, in step four, the pultrusion die adopts a three-stage temperature control: 100-120℃ in the gelation zone, 140-160℃ in the curing zone, and 170-190℃ in the post-curing zone; the pultrusion speed is 15-30cm / min.
[0043] The post-treatment conditions are 170-180℃ for 2-5 hours.
[0044] The beneficial effects of this invention include:
[0045] (1) A strong and tough synergistic effect was achieved: The epoxy-functionalized organic-inorganic hybrid toughening modifier participated in the curing reaction of the epoxy resin matrix through epoxy groups, and was covalently anchored in the epoxy resin crosslinking network, achieving uniform molecular-level dispersion and excellent interfacial bonding. This avoided the performance degradation caused by phase separation and interfacial debonding of physically blended toughening components. Performance test results showed that the epoxy resin adhesive cured samples in the examples (20.4-28.1 kJ / m) achieved a strong and tough synergistic effect. 2 The impact toughness of the sample was higher than that of the conventional epoxy resin liquid cured sample (9.4 kJ / m). 2 The tensile strength is ≥70MPa and the flexural strength is ≥120MPa (15-29% and 26-36% higher than that of physically blended epoxy resin liquid cured samples, respectively).
[0046] (2) Significantly improves the interfacial bonding force between glass fiber and resin: After the fiber surface is treated with silane coupling agent KH-560, epoxy groups are grafted, forming a covalent bond interface with the toughening modification component and resin matrix. The in-plane shear strength of the mandrel material obtained in this way reaches 53-58MPa, which can reduce the risk of interface debonding under humid heat and long-term stress.
[0047] (3) By adjusting the chain length of polyethylene glycol monooleate, epoxy resin core rod materials with different strength and toughness balance characteristics can be obtained: toughening modification component I (shortest chain) has the highest strength and is suitable for high mechanical load scenarios; toughening modification component II (medium and long chain) has the best comprehensive performance; toughening modification component III (longest chain) has the highest toughness and is suitable for high impact risk scenarios.
[0048] (4) The glass fiber core rod material of the composite insulator prepared by the present invention meets all the technical requirements specified in the DL / T1580-2021 standard and has practical engineering application value. Detailed Implementation
[0049] Example 1:
[0050] Preparation of bis(chloropropyl)octaphenyl cage-type polysilsesquioxane:
[0051] First, using phenyltrimethoxysilane as raw material, a hydrolysis-condensation method is adopted. The phenyltrimethoxysilane undergoes a hydrolysis-condensation reaction catalyzed by sodium hydroxide to generate an incompletely condensed octaphenyl cage-type polysilsesquioxane sodium salt.
[0052] Using incompletely condensed octaphenyl cage-type polysilsesquioxane sodium salt as raw material, under nitrogen protection and in anhydrous tetrahydrofuran solvent, bis(silylhydrogen)octaphenyl cage-type polysilsesquioxane was synthesized by apex-capping method using methyldichlorosilane as capping reagent and triethylamine catalysis.
[0053] Finally, using 1 molar equivalent of bis(silylhydrogen)octaphenyl cage-like polysilsesquioxane and 2.05 molar equivalent of 3-chloropropene as raw materials, under nitrogen protection and in anhydrous toluene solvent, a hydrosilylation reaction was carried out between the alkenyl group of bis(silylhydrogen)octaphenyl cage-like polysilsesquioxane and 3-chloropropene via a Karstedt catalyst to generate bis(chloropropyl)octaphenyl cage-like polysilsesquioxane, the chemical structural formula of which is:
[0054] ;
[0055] The preparation steps are as follows:
[0056] Under nitrogen protection, 25.5 g of phenyltrimethoxysilane, 3.4 g of sodium hydroxide, 120 mL of isopropanol and 4 mL of deionized water were added to a three-necked flask. The mixture was stirred and dissolved at room temperature for 10 min, heated to 90 °C and refluxed for 4 h, cooled to 25 °C and stirred for 15 h, filtered, washed three times with isopropanol, and dried under vacuum at 60 °C for 12 h to obtain incompletely condensed octaphenyl cage-type polysilsesquioxane sodium salt.
[0057] Under nitrogen protection, 11.3 g of incompletely condensed octaphenyl cage-type polysilsesquioxane sodium salt, 3.0 mL of triethylamine, and 100 mL of anhydrous tetrahydrofuran were added to a three-necked flask and stirred for 30 min under ice bath conditions. Then, 10 mL of anhydrous tetrahydrofuran solution containing 3.5 g of methyldichlorosilane was slowly added dropwise to the three-necked flask. The reaction was stirred for 4 h under ice bath conditions. After that, the ice bath was removed, and the reaction was stirred for 20 h at room temperature (25 °C). The insoluble matter was removed by filtration, and the filtrate was collected. The solvent was removed by rotary evaporation, and the filtrate was washed three times with methanol and dried under vacuum at 50 °C for 8 h to obtain bis(silylhydro)octaphenyl cage-type polysilsesquioxane.
[0058] Under nitrogen protection, 8.1 g of bis(silylhydrogen)octaphenyl cage-type polysilsesquioxane and 60 mL of anhydrous toluene were added to a three-necked flask and stirred at room temperature for 10 min to dissolve. Then, 30 μL of Karstedt catalyst (containing 2 wt% Pt) was added and stirred at room temperature for 30 min. The temperature was raised to 50 °C, and 10 mL of anhydrous toluene solution containing 1.1 g of 3-chloropropene was added dropwise to the three-necked flask using a constant pressure dropping funnel. The addition was completed within 1 h. The reaction was stirred at 50 °C for 12 h. After cooling to room temperature, 0.2 g of activated carbon was added and stirred for 15 min. The catalyst was removed by filtration, and the filtrate was collected. The solvent was removed by rotary evaporation of the filtrate to obtain the crude product.
[0059] The crude product was dissolved in 15 mL of hot toluene (60 °C), and methanol was slowly added dropwise until the solution became slightly turbid. After keeping it warm and standing for 30 min, it was naturally cooled to room temperature, and then placed in an ice-water bath to cool to 0 °C. After standing for 4 h, the crystals were collected by filtration, washed three times with methanol, and dried under vacuum at 50 °C for 8 h to obtain bis(chloropropyl)octaphenyl cage-type polysilsesquioxane.
[0060] Characterization of bis(chloropropyl)octaphenyl cage-type polysilsesquioxane:
[0061] 1 H NMR (CDCl3, 400MHz) δ: 0.15 (s, 6H), 0.94-0.97 (t, 4H), 1.72-1.78 (m, 4H), 3.43-3.46 (t, 4H), 7.33-7.54 (m, 40H);
[0062] 1 In the 1H NMR, a 6H singlet (capped -Si-CH3) appears at δ 0.15 ppm; a 4H triplet, a 4H multiplet, and a 4H triplet appear at δ 0.94-0.97, 1.72-1.78, and 3.43-3.46 ppm, respectively (corresponding to the three methylene groups of -Si-CH2-CH2-CH2-Cl); a 40H multiplet (eight phenyl Ar-H) appears at δ 7.33-7.54 ppm; and no Si-H signal peak is generated.
[0063] FTIR (KBr, cm -1 ): 3070-3020, 2960-2855, 1595-1600, 1495, 1450, 1430, 1275, 1120-1080, 750-700, 650, 550, 460;
[0064] 1120-1080cm in FTIR -1 A strong absorption peak of the POSS cage-like Si-O-Si framework appears at 1275 cm⁻¹. -1 A characteristic peak of Si-CH3 symmetric deformation appears at 650 cm⁻¹. -1 A C-Cl stretching vibration peak appears at ~2160 cm⁻¹, and no Si-H stretching vibration absorption peak is generated (~2160 cm⁻¹). -1 (place);
[0065] Combination 1 The results of H NMR and FTIR characterization confirmed that the chemical structure of the bis(chloropropyl)octaphenyl cage-like polysilsesquioxane was consistent with the expected structure.
[0066] Example 2:
[0067] An alkenyl-containing organic-inorganic hybrid toughening and modifying component was prepared, with the following formulation: 1 molar equivalent of bis(chloropropyl)octaphenyl cage-type polysilsesquioxane and 2.05 molar equivalent of polyethylene glycol monooleate ether.
[0068] The chemical structural formula of polyethylene glycol monooleate is as follows:
[0069] ;
[0070] Polyethylene glycol mono-oil ether is one of polyoxyethylene (2) oil ether (Mn~357g / mol), polyoxyethylene (10) oil ether (Mn~710g / mol), and polyoxyethylene (20) oil ether (Mn~1150g / mol);
[0071] The preparation method is as follows: Under alkaline conditions with nitrogen protection and the presence of sodium hydride, using anhydrous tetrahydrofuran as solvent, the terminal chlorine group of 1 molar equivalent of bis(chloropropyl)octaphenyl cage-type polysilsesquioxane is etherified with the terminal hydroxyl group of 2.05 molar equivalent of polyethylene glycol monooleate ether via the Williamson ether synthesis method to obtain an alkenyl-containing organic-inorganic hybrid toughening and modifying component, the chemical structural formula of which is:
[0072] ;
[0073] During the reaction, the unsaturated double bonds in the polyethylene glycol monooleate ether side chain may undergo positional migration or cis-trans isomerization under alkaline conditions in the presence of sodium hydride, but the alkenyl functional group is still retained in the product.
[0074] When the polyethylene glycol monooleate is polyoxyethylene (2) oleate, polyoxyethylene (10) oleate, and polyoxyethylene (20) oleate respectively, the following organic-inorganic hybrid toughening and modifying components I, II, and III containing alkenyl groups are prepared sequentially.
[0075] The preparation steps of alkenyl-containing organic-inorganic hybrid toughening modification component I are as follows:
[0076] Under nitrogen protection, 3.7g of polyoxyethylene (2) oil ether and 30mL of anhydrous tetrahydrofuran were added to a three-necked flask and stirred at room temperature for 10min. Under ice bath conditions, 0.6g of sodium hydride (60% mineral oil dispersion) was slowly added in 3 batches with an interval of 10min between each batch. After the addition was completed, the ice bath was removed and the reaction was stirred at room temperature for 1h until no bubbles (hydrogen) were generated, and a sodium alkoxide solution of polyoxyethylene (2) oil ether was obtained.
[0077] 6.5 g of bis(chloropropyl)octaphenyl cage-type polysilsesquioxane was dissolved in 50 mL of anhydrous tetrahydrofuran and slowly added dropwise to the above sodium alkoxide solution through a constant pressure dropping funnel. After the addition was completed, the temperature was raised to 60 °C and the reaction was stirred for 12 h. Samples were taken every 4 h, and the reaction progress was tracked by TLC (developing solvent: petroleum ether / ethyl acetate = 3:1) until the starting material spot of bis(chloropropyl)octaphenyl cage-type polysilsesquioxane basically disappeared.
[0078] After the reaction was completed, the mixture was cooled to room temperature, and anhydrous ethanol was slowly added dropwise until no more bubbles were generated (to quench excess NaH). After stirring for 15 min, 50 mL of deionized water was added to dilute the mixture. The mixture was extracted three times with ethyl acetate, the organic phases were combined, washed twice with saturated sodium chloride solution, dried over anhydrous sodium sulfate, filtered, and the filtrate was collected. The solvent in the filtrate was removed by rotary evaporation to obtain the crude product.
[0079] The crude product was dissolved in 15 mL of dichloromethane and slowly added dropwise to 100 mL of cold methanol to precipitate. After standing for 3 h, the solid was collected by filtration, washed three times with cold methanol, and dried under vacuum at 50 °C for 12 h to obtain the alkenyl-containing organic-inorganic hybrid toughening and modifying component I.
[0080] The only difference between the preparation steps of the alkenyl-containing organic-inorganic hybrid toughening modification component II and the alkenyl-containing organic-inorganic hybrid toughening modification component I is that 7.3g of polyoxyethylene (10) oil ether and 70mL of anhydrous tetrahydrofuran are added to a three-necked flask.
[0081] The preparation steps of the alkenyl-containing organic-inorganic hybrid toughening modification component III differ from those of the alkenyl-containing organic-inorganic hybrid toughening modification component I only in that 11.8 g of polyoxyethylene (20) oil ether and 100 mL of anhydrous tetrahydrofuran are added to a three-necked flask.
[0082] Characterization of alkenyl-containing organic-inorganic hybrid toughening and modifying components:
[0083] FTIR (component I, KBr, cm) -1 ): 3070-3020, 2960-2855, 1640, 1595-1600, 1495, 1450, 1420, 1275, 1120-1080, 1100, 960, 750-700, 550, 460;
[0084] FTIR (component II, KBr, cm) -1 ): 3070-3020, 2960-2850, 1645, 1590-1600, 1495, 1450, 1430, 1275, 1120-1080, 1105, 960, 750-700, 550, 460;
[0085] FTIR (component III, KBr, cm) -1 ): 3070-3010, 2960-2850, 1640, 1590-1600, 1490, 1450, 1430, 1275, 1120-1080, 1100, 960, 750-700, 550, 460;
[0086] FTIR characterization results show that:
[0087] 650 cm of the raw material bis(chloropropyl)octaphenyl cage-type polysilsesquioxane -1 The C-Cl stretching vibration peak disappears, and the 1100 cm⁻¹ peak in the product also disappears. -1 The presence of COC ether bond stretching vibration absorption peaks in the vicinity (overlapping with Si-O-Si skeleton peaks) proves that the terminal chlorine group of bis(chloropropyl)octaphenyl cage-type polysilsesquioxane underwent a Williamson etherification reaction with the terminal hydroxyl group of polyethylene glycol monooleate ether, successfully grafting polyethylene glycol monooleate ether segments onto the POSS cage-type core.
[0088] 960cm in the product -1 The characteristic CO absorption peak of the polyoxyethylene chain segment appears at 2960-2850 cm⁻¹. -1 The aliphatic CH stretching vibrations in the vicinity were significantly enhanced, further proving that polyethylene glycol monooleate had been chemically bonded to the POSS cage core;
[0089] 1640cm -1 The presence of C=C stretching vibration peaks in the vicinity indicates that the unsaturated double bonds of the polyethylene glycol mono-oil ether side chain are fully incorporated into the product molecule.
[0090] 1120-1080cm -1 The strong absorption peaks of the POSS cage-like Si-O-Si framework were completely preserved, proving that during the etherification reaction, the silicon-oxygen cage-like framework of POSS did not undergo ring-opening, degradation or structural destruction, and maintained its unique organic-inorganic hybrid cage-like structure.
[0091] The alkenyl groups in the organic-inorganic hybrid toughening modification components I, II, and III, containing alkenyl groups, were determined to be 1.01 mmol / g, 0.74 mmol / g, and 0.55 mmol / g, respectively, by iodometric titration.
[0092] Example 3:
[0093] Preparation of epoxy-functionalized organic-inorganic hybrid toughening modifier: Under nitrogen protection, using anhydrous dichloromethane as solvent, the alkenyl functional groups in the alkenyl-containing organic-inorganic hybrid toughening modifier were epoxidized with mCPBA (m-chloroperoxybenzoic acid) to obtain the epoxy-functionalized organic-inorganic hybrid toughening modifier, whose chemical structural formula is as follows:
[0094] ;
[0095] The preparation steps are as follows:
[0096] Under nitrogen protection, 8g of alkenyl-containing organic-inorganic hybrid toughening and modification component and 80mL of anhydrous dichloromethane were added to a three-necked flask and stirred at room temperature for 10min. Under ice bath conditions, 1.2 times the alkenyl molar equivalent mCPBA was slowly added in 3 batches, with an interval of 10min between each batch, while stirring was maintained.
[0097] After the addition of materials was completed, the reaction was stirred in an ice bath for 1 hour. Then the ice bath was removed and the reaction was stirred at room temperature for 4 hours. Samples were taken every hour and the reaction progress was tracked by TLC (developing solvent: petroleum ether / ethyl acetate = 2:1) until the alkenyl starting material spots basically disappeared.
[0098] After the reaction was completed, 10 wt% sodium bisulfite aqueous solution was slowly added dropwise until the starch-KI test paper no longer turned blue. The mixture was stirred for 15 min to quench the excess mCPBA, the organic phase was separated, washed twice with saturated sodium bicarbonate solution and twice with saturated sodium chloride solution, dried with anhydrous sodium sulfate, filtered, and the filtrate was collected. The solvent in the filtrate was removed by rotary evaporation to obtain the crude product.
[0099] The crude product was dissolved in 10 mL of dichloromethane and slowly added dropwise to 100 mL of cold methanol to precipitate. After standing for 3 h, the solid was collected by filtration, washed 3 times with cold methanol, and dried under vacuum at 40 °C for 12 h to obtain the epoxy-functionalized organic-inorganic hybrid toughening modified component.
[0100] Among them, the alkenyl-containing organic-inorganic hybrid toughening modification component is one of alkenyl-containing organic-inorganic hybrid toughening modification components I, II, and III;
[0101] When the alkenyl-containing organic-inorganic hybrid toughening modification components are respectively alkenyl-containing organic-inorganic hybrid toughening modification components I, II, and III, epoxy functionalized organic-inorganic hybrid toughening modification components I, II, and III are prepared sequentially.
[0102] Characterization of epoxy-functionalized organic-inorganic hybrid toughening modification components I, II, and III:
[0103] FTIR (component I, KBr, cm) -1): 3070-3020, 2960-2855, 1595-1600, 1495, 1450, 1420, 1275, 1120-1080, 1100, 905-960, 845, 750-700, 550, 460;
[0104] FTIR (component II, KBr, cm) -1 ): 3070-3020, 2960-2855, 1590-1600, 1490, 1450, 1430, 1275, 1120-1080, 1105, 900-960, 840, 750-700, 550, 460;
[0105] FTIR (component III, KBr, cm) -1 ): 3070-3020, 2960-2850, 1590-1600, 1490, 1455, 1430, 1275, 1120-1080, 1105, 900-960, 845, 750-700, 550, 460;
[0106] FTIR characterization results show that:
[0107] Compared with alkenyl-containing raw materials, 1640cm -1 The C=C stretching vibration peak disappears in the nearby region, while the peak at 840 cm⁻¹ disappears. -1 The vicinity exhibits asymmetric stretching vibration peaks of the epoxy ring COC, with peaks at 900-960 cm⁻¹. -1 The enhanced regional broadening demonstrates that the unsaturated double bonds in the oil-based side chain have been transformed into epoxy groups;
[0108] The epoxy group content in epoxy functionalized organic-inorganic hybrid toughening modification components I, II, and III was determined to be 0.98 mmol / g, 0.71 mmol / g, and 0.54 mmol / g, respectively, by the hydrochloric acid-acetone method.
[0109] Example 4:
[0110] The glass fiber core rod material for composite insulators comprises the following raw materials in parts by weight:
[0111] 100 parts of bisphenol A type epoxy resin (model E51)
[0112] Eight epoxy-functionalized organic-inorganic hybrid toughening and modifying components;
[0113] 80 parts of methyltetrahydrophthalic anhydride curing agent (model HKR-0719);
[0114] 1.5 parts of curing accelerator (2-ethyl-4-methylimidazole);
[0115] 2 parts of internal release agent (model NOODA-2490M);
[0116] 250-point E-glass fiber untwisted roving (model 2400tex);
[0117] 2.5 parts of 3-(2,3-epoxypropoxy)propyltrimethoxysilane (silane coupling agent KH-560);
[0118] Among them, the epoxy-functionalized organic-inorganic hybrid toughening modification components are epoxy-functionalized organic-inorganic hybrid toughening modification components I, II, and III.
[0119] Example 5:
[0120] A method for preparing glass fiber core material for composite insulators includes the following steps:
[0121] Step 1, Surface treatment of E-glass fiber untwisted roving: Silane coupling agent KH-560 is used to generate silanol groups under hydrolysis conditions. These silanol groups undergo a dehydration condensation reaction with the hydroxyl groups on the surface of hydrophilic glass fiber, thereby grafting epoxy groups onto the surface of E-glass fiber untwisted roving to obtain E-glass fiber untwisted roving treated with silane coupling agent KH-560.
[0122] The preparation steps are as follows: 2.5 parts by weight of silane coupling agent KH-560 are dissolved in 50 parts by weight of ethanol, 2 parts by weight of deionized water are added, and then the pH of the system is adjusted to 5.5 using glacial acetic acid. The reaction is stirred at room temperature for 2 hours to form a hydrolysis solution of silane coupling agent KH-560.
[0123] 250 parts by weight of E-glass fiber untwisted roving were drawn from the yarn rack and passed through a hydrolysis solution bath of silane coupling agent KH-560 (temperature set at 40℃) at a speed of 1 m / min. After the fiber was impregnated, it was passed through a squeeze roller and air-dried at room temperature for 5 min. Then it was dried in an oven at 110℃ for 15 min, cooled to room temperature, and wound up to obtain E-glass fiber untwisted roving treated with silane coupling agent KH-560.
[0124] Step 2, Preparation of epoxy resin solution:
[0125] 100 parts by weight of bisphenol A type epoxy resin were stirred at 60℃ for 30 min (the viscosity decreased significantly), and 8 parts by weight of epoxy functionalized organic-inorganic hybrid toughening modifier were added. The mixture was stirred at 60℃ for 1 h (the bisphenol A type epoxy resin and the epoxy functionalized organic-inorganic hybrid toughening modifier are compatible and dispersed through the π-π stacking effect between benzene rings and the compatibilizing effect of polyether segments). The mixture was then cooled to 40℃ to obtain a uniform resin premix.
[0126] Add 80 parts by weight of methyltetrahydrophthalic anhydride curing agent, 1.5 parts by weight of 2-ethyl-4-methylimidazolium curing accelerator, and 2 parts by weight of internal release agent to the above resin premix in sequence. Maintain vacuum stirring at 40°C for 20 minutes (vacuum degree ≤ -0.09MPa) to remove air bubbles introduced during the mixing process and obtain epoxy resin solution.
[0127] Step 3, fiber impregnation:
[0128] The E-glass fiber untwisted roving prepared in step one and treated with silane coupling agent KH-560 is drawn out from the yarn frame, sorted by the yarn guide plate, and then put into the resin impregnation tank. The temperature of the impregnation tank is controlled at 50℃, and the fiber is impregnated in the resin for 90 seconds to ensure that the resin fully wets the fiber bundle.
[0129] After being impregnated with resin, the fiber bundles are pre-shaped using a pre-forming mold (temperature 70℃), and excess resin is extruded to obtain the pre-shaped fiber bundles after impregnation.
[0130] Step 4, pultrusion curing and molding:
[0131] The pre-formed fiber bundles, after being impregnated with resin, are introduced into a pultrusion die, which employs a three-stage temperature control system.
[0132] First stage (gelation zone): 110℃, the epoxy resin begins to gel and the viscosity increases sharply;
[0133] Second stage (curing zone): 150℃, the curing reaction proceeds fully, forming a cross-linked network;
[0134] In the curing reaction, the epoxy functionalized organic-inorganic hybrid toughening and modifying component, the E-glass fiber untwisted roving treated with silane coupling agent KH-560, and the bisphenol A type epoxy resin undergo a synergistic cross-linking reaction under the action of curing agent and curing accelerator. The organic-inorganic hybrid toughening and modifying component is anchored in the epoxy resin cross-linking network through covalent bonds, while achieving chemical bonding interface compatibility between the fiber and the epoxy resin matrix.
[0135] Third stage (post-curing zone): 180℃, ensure complete curing;
[0136] The pultrusion speed was 20 cm / min, and the traction force was kept stable. After curing, the core rod was led out from the mold outlet, cut to a fixed length by the cutting device, and placed in a 170℃ oven for 4 hours to obtain glass fiber core rod material for composite insulators with a diameter of 30 mm.
[0137] Among them, when the epoxy functionalized organic-inorganic hybrid toughening modification components are epoxy functionalized organic-inorganic hybrid toughening modification components I, II, and III respectively, epoxy resin adhesives I, II, and III and glass fiber core rod materials I, II, and III of composite insulators are prepared sequentially.
[0138] Comparative Example 1:
[0139] The glass fiber core rod material a of the composite insulator comprises the following raw materials in parts by weight:
[0140] 100 parts of bisphenol A type epoxy resin (model E51)
[0141] 80 parts of methyltetrahydrophthalic anhydride curing agent (model HKR-0719);
[0142] 1.5 parts of curing accelerator (2-ethyl-4-methylimidazole);
[0143] 2 parts of internal release agent (model NOODA-2490M);
[0144] 250-point E-glass fiber untwisted roving (model 2400tex);
[0145] 2.5 parts of 3-(2,3-epoxypropoxy)propyltrimethoxysilane (silane coupling agent KH-560);
[0146] The preparation method of glass fiber core rod material a of composite insulator is as follows:
[0147] Step 1, the surface treatment of E-glass fiber untwisted roving is the same as Step 1 in Example 5;
[0148] Step 2, Preparation of epoxy resin adhesive a:
[0149] 100 parts by weight of bisphenol A type epoxy resin were stirred at 60°C for 30 min (the viscosity decreased significantly), cooled to 40°C, and 80 parts by weight of methyltetrahydrophthalic anhydride curing agent, 1.5 parts by weight of 2-ethyl-4-methylimidazolium curing accelerator, and 2 parts by weight of internal release agent were added in sequence. The mixture was stirred under vacuum at 40°C for 20 min (vacuum degree ≤ -0.09MPa) to remove air bubbles introduced during the mixing process, and epoxy resin solution a was obtained.
[0150] Step 3, fiber impregnation, is the same as step 3 in Example 5;
[0151] Step four is pultrusion curing, which is the same as step four in Example five.
[0152] Comparative Example 2:
[0153] The glass fiber core rod material b of the composite insulator comprises the following raw materials in parts by weight:
[0154] 100 parts of bisphenol A type epoxy resin (model E51)
[0155] Eight organic-inorganic blend toughening and modifying components;
[0156] 80 parts of methyltetrahydrophthalic anhydride curing agent (model HKR-0719);
[0157] 1.5 parts of curing accelerator (2-ethyl-4-methylimidazole);
[0158] 2 parts of internal release agent (model NOODA-2490M);
[0159] 250-point E-glass fiber untwisted roving (model 2400tex);
[0160] 2.5 parts of 3-(2,3-epoxypropoxy)propyltrimethoxysilane (silane coupling agent KH-560);
[0161] The preparation method of glass fiber core rod material b for composite insulators is as follows:
[0162] Step 1, the surface treatment of E-glass fiber untwisted roving is the same as Step 1 in Example 5;
[0163] Step 2, Preparation of epoxy resin solution b:
[0164] 100 parts by weight of bisphenol A type epoxy resin were stirred at 60°C for 30 minutes (the viscosity decreased significantly), 8 parts by weight of organic-inorganic blend toughening and modifying component were added, and the mixture was stirred at 60°C for 1 hour. The mixture was then cooled to 40°C to obtain a uniform resin premix.
[0165] 80 parts by weight of methyltetrahydrophthalic anhydride curing agent, 1.5 parts by weight of 2-ethyl-4-methylimidazolium curing accelerator, and 2 parts by weight of internal release agent were added sequentially to the above resin premix. The mixture was stirred under vacuum at 40°C for 20 minutes (vacuum degree ≤ -0.09MPa) to remove the air bubbles introduced during the mixing process, and epoxy resin solution b was obtained.
[0166] Step 3, fiber impregnation, is the same as step 3 in Example 5;
[0167] Step four is pultrusion curing, which is the same as step four in Example five;
[0168] The formulation of the organic-inorganic blend toughening and modifying component is: 1 molar equivalent of octaphenyl cage-type polysilsesquioxane (CAS No. 5256-79-1) and 2.05 molar equivalent of polyoxyethylene (10) oil ether.
[0169] The preparation method of the organic-inorganic blend toughening modified component is as follows: 7.3g of polyoxyethylene (10) oil ether and 70mL of anhydrous tetrahydrofuran are added to a three-necked flask and stirred and dissolved at room temperature for 10min. Then, 50mL of anhydrous tetrahydrofuran solution containing 5.2g of octaphenyl cage-type polysilsesquioxane is slowly added. The mixture is heated to 60℃ and stirred and mixed for 12h. After cooling to room temperature, the solvent is removed by rotary evaporation to obtain the organic-inorganic blend toughening modified component.
[0170] Performance testing:
[0171] 1. Place the epoxy resin sample in a vacuum drying oven to degas for 15 minutes, pour it into a polytetrafluoroethylene mold, cure at 120℃ for 2 hours + at 170℃ for 4 hours, demold, and cure at room temperature for 72 hours before performance testing, as detailed below:
[0172] Mechanical property testing: The mechanical properties of the epoxy resin cured samples were tested in accordance with GB / T 2567-2021 "Test Methods for Properties of Resin Castings". The initial tensile strength (tensile speed of 2 mm / min), flexural strength and impact toughness (dimensions of 80 mm × 10 mm × 4 mm, unnotched, pendulum weight of 5.5 J) of the samples were recorded.
[0173] The results of the above performance experiments are shown in Table 1.
[0174] Table 1. Performance test results of epoxy resin adhesive cured samples
[0175] Product Type Tensile strength (MPa) Bending strength (MPa) <![CDATA[Impact toughness (kJ / m 2 )]]> Epoxy Resin Solution I 79.3 130.2 20.4 Epoxy Resin Liquid II 74.6 127.8 25.3 Epoxy Resin Liquid III 70.9 121.3 28.1 Comparative Example 1 (Epoxy Resin Solution a) 74.2 128.5 9.4 Comparative Example 2 (Epoxy Resin Solution b) 61.5 95.6 17.2
[0176] A comprehensive analysis of the experimental results in Table 1 leads to the following conclusions:
[0177] (1) The enhancing effect of epoxy functionalized organic-inorganic hybrid toughening modifiers on the toughness of epoxy resin
[0178] Impact toughness (20.4-28.1 kJ / m) of epoxy resin adhesive I-III cured samples in the example. 2 Both were significantly higher than those of Comparative Example 1 (which did not contain toughening components) (9.4 kJ / m). 2 Comparative Example 2 (17.2 kJ / m³) and physical blend type 2 This may be attributed to the fact that the nanoscale rigid framework of POSS cage-type polysilsesquioxane acts as a stress transfer node and crack barrier in the epoxy resin matrix. The stress field around it induces shear yielding of the matrix and energy dissipation through microcracks, thereby dissipating impact energy. At the same time, the flexible structure of the long chain of polyethylene glycol monooleate provides the mobility of molecular chain segments, further promoting energy dissipation through plastic deformation. The two achieve synergistic toughening through chemical bonding.
[0179] The longer the chain length of polyethylene glycol monooleate (III>II>I), the higher the proportion of flexible segments, and the better the impact toughness (28.1>25.3>20.4).
[0180] (2) Effect of epoxy functionalized organic-inorganic hybrid toughening modifiers on the strength properties of epoxy resin
[0181] The tensile strength of the epoxy resin adhesive I cured sample in the example was 79.3 MPa and the flexural strength was 130.2 MPa, which were approximately 6.9% and 1.3% higher than those of Comparative Example I (74.2 / 128.5 MPa), respectively, and 28.9% and 36.2% higher than those of Comparative Example II (61.5 / 95.6 MPa), respectively, demonstrating a dual effect of strengthening and toughening.
[0182] The tensile strength and flexural strength of the epoxy resin adhesive II cured sample in the example were 74.6 MPa and 127.8 MPa, respectively, which were basically the same as those of Comparative Example 1 (74.2 / 128.5 MPa) (change of 0.5%), and increased by 21.3% and 33.7% respectively compared with Comparative Example 2 (61.5 / 95.6 MPa). While maintaining high strength, the toughness was significantly improved.
[0183] The tensile strength and flexural strength of the epoxy resin adhesive III cured sample in the example were 70.9 MPa and 121.3 MPa, respectively, which were about 4.4% and 5.6% lower than those of Comparative Example 1, but still 15.3% and 26.9% higher than those of Comparative Example 2, respectively. The optimal toughness improvement was achieved with a limited and controllable decrease in strength.
[0184] The mechanism for the above phenomenon may be as follows: the POSS cage-type rigid inorganic skeleton (Si-O-Si) in the epoxy functionalized organic-inorganic hybrid toughening and modifying component plays a nano-reinforcing role on the epoxy resin matrix, which can effectively bear the load transfer. Its epoxy groups participate in the curing reaction and form covalent bonds with the matrix to anchor, achieving uniform dispersion at the molecular level and excellent interfacial bonding, effectively avoiding the stress concentration defects caused by phase separation and interfacial debonding of traditional physical blend toughening components.
[0185] Meanwhile, the introduction of flexible segments of polyethylene glycol monooleate endows the material with energy dissipation capability. However, the longer the chain length (Ⅲ>Ⅱ>Ⅰ), the more significant the dilution effect of the flexible segments on the rigidity of the crosslinking network, and the strength shows a decreasing trend, but all are significantly higher than those of the physical blend comparative example 2.
[0186] (3) The epoxy resin adhesive II (polyoxyethylene (10) oil ether) cured sample has the best comprehensive performance and exhibits a balance of strength and toughness; the epoxy resin adhesive I (polyoxyethylene (2) oil ether) cured sample achieves double the toughness while maintaining the highest strength, and is suitable for scenarios with higher strength requirements; the epoxy resin adhesive III (polyoxyethylene (20) oil ether) cured sample provides the highest toughness and is suitable for scenarios with higher toughness requirements; in practical applications, the chain length of polyethylene glycol mono-oil ether needs to be optimized according to the comprehensive requirements of toughness and strength.
[0187] 2. The performance of the glass fiber core rod material samples of the composite insulator was tested in accordance with the standard DL / T 1580-2021 "Technical Conditions for Core of AC and DC Composite Insulator". The test results are shown in Table 2 below.
[0188] Table 2 Performance test results of glass fiber core material for composite insulators
[0189] Product Type Glass fiber core rod material I Glass fiber core rod material II Glass fiber core rod material III Technical Requirements Tensile strength (MPa) 1280 1250 1200 ≥1100 Bending strength (MPa) 1110 1060 1030 ≥900 In-plane shear strength (MPa) 58 56 53 ≥45 Water absorption rate (%) 0.03 0.03 0.05 ≤0.05 End face Barcol hardness (HBa) 71 70 68 65-75 Leakage current (μA) 19 21 25 ≤50 dry power frequency withstand voltage pass pass pass After withstanding 80% of the dry power frequency flashover voltage for 30 minutes, the temperature rise does not exceed 5K, with no breakdown or flashover. AC breakdown strength (kV / cm) 51 50 45 ≥30 Positive polarity lightning impulse withstand voltage (kV / 10mm) +120 +120 +115 ≥+100 Volume resistivity (Ω·m) <![CDATA[4.9×10 12 ]]> <![CDATA[4.6×10 12 ]]> <![CDATA[4.1×10 12 ]]> <![CDATA[≥1.0×10 10 ]]> Stress corrosion resistance pass pass pass Passes the stress corrosion resistance test specified in GB / T 34937-2017 Hot bending strength 330 320 305 After being subjected to 150℃±5℃ for 1 hour, the hot bending strength is ≥280 MPa within 5 minutes. Sway fatigue characteristics pass pass pass <![CDATA[1.2×10 6 No cracking or whitening was observed after the second swing fatigue test.
[0190] The following conclusions can be drawn from the performance test results in Table 2:
[0191] The glass fiber core rod material of the composite insulator prepared by this invention meets all the technical requirements specified in the DL / T1580-2021 standard and has practical application value.
Claims
1. A fiberglass core rod material for composite insulators, characterized in that, The ingredients include the following parts by weight: 80-120 parts of bisphenol A type epoxy resin; 5-15 parts of epoxy-functionalized organic-inorganic hybrid toughening and modifying components; 60-90 parts of acid anhydride curing agent; 1-3 parts curing accelerator; 1-3 parts release agent; 200-300 parts E-glass fiber untwisted roving; 2-3 parts epoxy silane coupling agent; Among them, the epoxy-functionalized organic-inorganic hybrid toughening and modifying component is prepared by bis(chloropropyl)octaphenyl cage-type polysilsesquioxane and polyethylene glycol monooleate ether through Williamson etherification and epoxidation reaction; The chemical structural formula of the epoxy-functionalized organic-inorganic hybrid toughening and modifying component is as follows: 。 2. The fiberglass core rod material for composite insulators according to claim 1, characterized in that, The anhydride curing agent is methyltetrahydrophthalic anhydride curing agent; The curing accelerator is 2-ethyl-4-methylimidazol; The epoxy silane coupling agent is 3-(2,3-epoxypropoxy)propyltrimethoxysilane.
3. The fiberglass core rod material for composite insulators according to claim 1, characterized in that, The type of bisphenol A epoxy resin is E51; The E-glass fiber untwisted roving is of type 2400tex.
4. The method of making a fiberglass core rod material for a composite insulator according to any one of claims 1-3, characterized in that, Includes the following steps: Step 1: After hydrolyzing 3-(2,3-epoxypropoxy)propyltrimethoxysilane, surface treatment is performed on E-glass fiber roving to obtain modified glass fiber with surface-grafted epoxy groups. Step 2: Premix bisphenol A type epoxy resin with epoxy functionalized organic-inorganic hybrid toughening and modifying components, add methyltetrahydrophthalic anhydride curing agent, 2-ethyl-4-methylimidazolium and internal release agent, and degas under vacuum to obtain epoxy resin adhesive. Step 3: Immerse the modified glass fiber in the epoxy resin solution and pre-form it to obtain impregnated fiber bundles; Step 4: The resin-impregnated fiber bundles are cured by gradient heating through a pultrusion die and then post-treated to obtain the glass fiber core rod material for the composite insulator; The epoxy-functionalized organic-inorganic hybrid toughening and modifying component participates in the cross-linking and curing reaction of epoxy resin through epoxy groups and is covalently anchored in the epoxy resin cross-linking network. The modified glass fiber participates in the curing reaction simultaneously through surface-grafted epoxy groups, forming a fiber-resin chemically bonded interface.
5. The method of making a fiberglass core rod material for a composite insulator according to claim 4, wherein, The preparation method of the epoxy-functionalized organic-inorganic hybrid toughening and modifying component is as follows: Under alkaline conditions with nitrogen protection and the presence of sodium hydride, anhydrous tetrahydrofuran was used as a solvent to achieve the etherification reaction of the terminal chlorine group of 1 molar equivalent of bis(chloropropyl)octaphenyl cage-type polysilsesquioxane with the terminal hydroxyl group of 2.01-2.09 molar equivalent of polyethylene glycol monooleate ether via the Williamson ether synthesis method, resulting in an alkenyl-containing organic-inorganic hybrid toughening and modifying component; Under nitrogen protection, anhydrous dichloromethane was used as a solvent to epoxidize the alkenyl functional groups in the alkenyl-containing organic-inorganic hybrid toughening modification component with m-chloroperoxybenzoic acid, resulting in an epoxy-functionalized organic-inorganic hybrid toughening modification component.
6. The method of making a fiberglass core rod material for a composite insulator according to claim 5, wherein, The preparation method of the bis(chloropropyl)octaphenyl cage-type polysilsesquioxane is as follows: Using phenyltrimethoxysilane as raw material, a hydrolysis-condensation method was adopted. The phenyltrimethoxysilane underwent a hydrolysis-condensation reaction catalyzed by sodium hydroxide to generate an incompletely condensed octaphenyl cage-type polysilsesquioxane sodium salt. Using incompletely condensed octaphenyl cage-type polysilsesquioxane sodium salt as raw material, bis(silylhydrogen)octaphenyl cage-type polysilsesquioxane was synthesized by apex-capping method under nitrogen protection and anhydrous tetrahydrofuran solvent, with methyl dichlorosilane as capping agent and triethylamine catalysis. Using 1 molar equivalent of bis(silylhydrogen)octaphenyl cage-type polysilsesquioxane and 2.01-2.09 molar equivalents of 3-chloropropene as raw materials, under nitrogen protection and in anhydrous toluene solvent, the alkenyl group of bis(silylhydrogen)octaphenyl cage-type polysilsesquioxane undergoes a hydrosilylation reaction with 3-chloropropene via a Karstedt catalyst to generate bis(chloropropyl)octaphenyl cage-type polysilsesquioxane.
7. The method for preparing the glass fiber core rod material of the composite insulator according to claim 4, characterized in that, In step one, the hydrolysis conditions are: ethanol-water mixed solvent, pH adjusted to 5.0-6.0, hydrolysis at room temperature for 1-3 hours; The surface treatment is an online continuous process, with a fiber traction speed of 0.5-1.5 m / min, a treatment temperature of 35-45℃, and a drying temperature of 100-120℃.
8. The method for preparing the glass fiber core rod material of the composite insulator according to claim 4, characterized in that, In step two, the premixing temperature is 50-70℃, and the premixing time is 0.5-2h; The vacuum degassing process has a vacuum degree of ≤-0.09MPa and a time of 15-30min.
9. The method for preparing the glass fiber core rod material of the composite insulator according to claim 4, characterized in that, In step three, the impregnation temperature is 45-55℃ and the impregnation time is 60-120s; The preforming temperature is 65-75℃.
10. The method for preparing the glass fiber core rod material of the composite insulator according to claim 4, characterized in that, In step four, the pultrusion die adopts a three-stage temperature control: 100-120℃ in the gelation zone, 140-160℃ in the curing zone, and 170-190℃ in the post-curing zone; the pultrusion speed is 15-30cm / min. The post-treatment conditions are 170-180℃ for 2-5 hours.