电子器件密封用高耐热环氧树脂组合物制备方法
By employing a multi-stage modification process involving modified inorganic composite fillers and curing agents, the shortcomings of epoxy resin materials for electronic packaging in terms of interfacial bonding, moisture adsorption, and ion content have been overcome. This process achieves high heat resistance, low ion contamination, and excellent resistance to damp heat and fatigue, meeting the requirements of high-end electronic devices.
Patent Information
- Application Number
- CN202611655539.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-26
- Publication Date
- 2026-11-24
AI Technical Summary
Existing epoxy resin materials for electronic packaging have shortcomings in terms of interfacial bonding density, water vapor adsorption, sodium and chloride ion content, glass transition temperature, and thermal shock resistance, making it difficult to meet the requirements of high heat resistance, high insulation, low ion contamination, and resistance to damp heat and fatigue for high-end electronic devices.
A multi-stage modification process using modified inorganic composite fillers, modified aromatic amine curing agents, and modified latent curing accelerators is employed. Through gallic acid anchoring, epoxy silane grafting, and spermine crosslinking, an organic-inorganic hybrid layer is formed, constructing a uniform and dense crosslinked network. Combined with ion trapping agents and defoamers, the interfacial bonding, crosslinked structure regularity, and curing uniformity are improved.
It significantly reduces the water absorption and ion content of materials, increases the glass transition temperature and high-temperature insulation capability, enhances resistance to thermal shock, and ensures the sealing reliability and high-temperature service performance of electronic devices in humid environments.
Abstract
Description
Technical Field
[0001] This invention relates to the field of epoxy resin composition technology, and in particular to a method for preparing a high heat-resistant epoxy resin composition for sealing electronic devices. Background Technology
[0002] Epoxy resin compositions are polymeric composite materials with epoxy resin as the matrix, which form a three-dimensional network structure through a cross-linking reaction with a curing agent. They typically contain epoxy resin, a curing agent, and possibly fillers, toughening agents, and other additives. By adjusting the formulation, high strength, high adhesion, excellent electrical insulation, and chemical corrosion resistance can be achieved, making them widely used in coatings, adhesives, electronic packaging, composite materials, and other fields.
[0003] Existing epoxy resin materials for electronic packaging generally suffer from the following problems: insufficient interfacial density between unmodified inorganic fillers and the resin matrix, numerous interfacial defects, and easy adsorption of moisture, resulting in high water absorption and poor sealing performance; difficulty in removing free impurity ions from the powder surface, leading to high sodium and chloride ion content in the system, severely reducing the material's high-temperature insulation reliability; limited regularity and stability of the cross-linked network formed by conventional curing systems, resulting in a low glass transition temperature and easy performance degradation under high-temperature conditions; traditional modification and preparation processes cannot achieve orderly modification and performance complementarity of various functional components, resulting in poor curing uniformity and high residual internal stress, leading to low thermal shock resistance and easy cracking failure during long-term service. Overall, the comprehensive performance is difficult to meet the stringent sealing requirements of high heat resistance, high insulation, low ion contamination, and resistance to damp heat and fatigue in high-end electronic devices. Based on this, the present invention provides a method for preparing a high-heat-resistant epoxy resin composition for sealing electronic devices. Summary of the Invention
[0004] The main objective of this invention is to provide a Cl - A method for preparing a high heat-resistant epoxy resin composition for sealing electronic devices with low content and high thermal shock resistance is applied in the preparation method of a high heat-resistant epoxy resin composition for sealing electronic devices.
[0005] To achieve the above objectives, the technical solution adopted by the present invention is as follows: This invention provides a method for preparing a high heat-resistant epoxy resin composition for sealing electronic devices. The method includes the following steps: adding resin to a reaction vessel, heating to 70-90°C at a rate of 1-2°C / min, stirring at 300-500 rpm for 20-30 minutes, sequentially adding stress-modifying agents and functional additives, stirring at a constant temperature for 30-60 minutes, adding modified inorganic composite fillers in 3-5 portions, and adjusting the stirring speed to... Stir at 800-1200 rpm for 40-80 minutes, then cool to 45-60℃ at a cooling rate of 0.8-2℃ / min, adjusting the stirring speed to 200-350 rpm. Add the modified aromatic amine curing agent and the modified latent curing accelerator sequentially, and stir at a constant temperature for 20-40 minutes to obtain a mixture. Degas the mixture under vacuum, setting the vacuum degree to -0.085 to -0.095 MPa, and degas for 15-30 minutes to obtain a high heat-resistant epoxy resin composition for sealing electronic devices.
[0006] Furthermore, the high heat-resistant epoxy resin composition for sealing electronic devices is composed of the following components in parts by weight: 75-90 parts resin, 5-8 parts stress-modifying agent, 1-2 parts functional agent, 150-190 parts modified inorganic composite filler, 42-55 parts modified aromatic amine curing agent, and 0.5-0.9 parts modified latent curing accelerator.
[0007] The phenolic epoxy resin has a total chlorine content of ≤500ppm, a hydrolyzable chlorine content of ≤100ppm, an epoxy equivalent of 160–180g / eq, a moisture content of ≤0.1%, and a single metal ion content of ≤10ppm and a total metal ion content of ≤50ppm.
[0008] The trifunctional aromatic epoxy resin has a total chlorine content of ≤500ppm, a hydrolyzable chlorine content of ≤100ppm, an epoxy equivalent of 180–200g / eq, a water content of ≤0.1%, and a single metal ion content of ≤10ppm and a total metal ion content of ≤50ppm.
[0009] The epoxy-terminated polybutadiene has an epoxy value ≥0.05eq / 100g, no free small molecules, a water content ≤0.2%, and metal ions ≤10ppm individually and ≤50ppm in total.
[0010] The organosilicon-modified epoxy resin has good compatibility with epoxy, no free small molecules, a water content of ≤0.2%, and a single metal ion content of ≤10ppm and a total metal ion content of ≤50ppm.
[0011] The ion scavenger is an inorganic cation exchange type ion scavenger, preferably the IXE series (such as IXE-100) or equivalent products from Toa Synthetic Co., Ltd. of Japan, with a chelation capacity ≥1.5 meq / g (for Na+). +The total chlorine content is ≤50ppm, the water content is ≤0.2%, and the individual metal ion content is ≤5ppm and the total metal ion content is ≤20ppm.
[0012] The defoamer is a polyether-modified silicone defoamer, preferably BYK-A530 from BYK Chemical or a product with equivalent performance, with a defoaming time ≤10s, a foam suppression time ≥30min, no residue, a total chlorine content ≤50ppm, and a moisture content ≤0.2%.
[0013] The auxiliary coupling agent is an epoxy silane coupling agent, preferably γ-glycidyl etheroxypropyltrimethoxysilane (GPS) or a product with equivalent performance, with a purity ≥98%, and containing its own Na. + ≤5ppm, total chlorine ≤50ppm, moisture content ≤0.2%.
[0014] Furthermore, the resin is compounded from phenolic epoxy resin and trifunctional aromatic epoxy resin in a mass ratio of (2-4):1.
[0015] The stress-modifying agent is one or more of terminal epoxy-terminated polybutadiene and organosilicon-modified epoxy resin.
[0016] Furthermore, the functional additive is composed of an ion trapping agent, an antifoaming agent, and an auxiliary coupling agent mixed in a mass ratio of (20-35):(15-25):(40-60).
[0017] Furthermore, the preparation of the modified inorganic composite filler includes the following steps: A1. Mix spherical silica and spherical alumina evenly to obtain a composite filler.
[0018] A2. Add the composite packing and solvent to the reactor, set the temperature to 50-65℃, the rotation speed to 600-900 rpm, stir for 20 minutes, add gallic acid, stir at a constant temperature for 40-60 minutes, add γ-glycidoxypropyltrimethoxysilane, stir at a constant temperature for 50-70 minutes, raise the temperature to 65-75℃ at a heating rate of 0.5-1.5℃ / min, add spermine, stir for 60-90 minutes, cool to room temperature at a cooling rate of 0.5-1.5℃ / min, stop stirring, filter, collect the filter cake, wash the filter cake 2-3 times with anhydrous ethanol, vacuum dry the washed filter cake at a temperature of 80-100℃ and a vacuum degree of -0.085MPa for 4-6 hours, cool the dried filter cake to room temperature, grind it through a 200-300 mesh sieve to obtain the modified inorganic composite packing.
[0019] Furthermore, the mass ratio of the spherical silica to the spherical alumina is (1-2.5):1.
[0020] The solvent is a mixture of ethanol and deionized water in a volume ratio of (4-6):1.
[0021] The solid-liquid ratio of the composite filler and solvent is 1:(8-12).
[0022] The gallic acid accounts for 0.8-1.5% of the total mass of the composite filler.
[0023] The γ-glycidyl etheroxypropyltrimethoxysilane accounts for 0.4-0.9% of the total mass of the composite filler.
[0024] The succinamine accounts for 0.3-0.7% of the total mass of the composite filler.
[0025] The spherical silica has a purity ≥99.5%, a D50 of 0.5–30 μm, a sphericity ≥95%, and Na... + ≤5ppm, Cl - ≤5ppm, moisture content ≤0.1%.
[0026] The spherical alumina has a purity ≥99.5%, a D50 of 0.5–30 μm, a sphericity ≥90%, and a Na content of 100%. + ≤5ppm, Cl - ≤5ppm, moisture content ≤0.1%.
[0027] Furthermore, the preparation of the modified aromatic amine curing agent includes the following steps: B1. Add anhydrous ethanol to the reactor and heat to 80-90℃ at a heating rate of 0.5-1.5℃ / min. Start stirring and set the speed to 400-600 rpm. Add m-phenylenediamine and stir at a constant temperature for 20-30 minutes. Adjust the speed to 600-900 rpm and stir for 15 minutes. Add phthalic acid and stir for 40-50 minutes. Add vinyltriethoxysilane and stir for 50-60 minutes. Add polypropylene glycol and stir for 35-45 minutes. Stop stirring and cool to 45-55℃ at a cooling rate of 0.5-1.5℃ / min to obtain material B.
[0028] Although the salt formation reaction reduces the activity of the amine group, during the subsequent stirring and heating process, some ammonium salts can slowly release free amines, or promote the hydrolysis of silanes to produce silanols through trace amounts of water in the system, which then undergo condensation reactions with the amine group to achieve gradual grafting.
[0029] B2. Reduce the pressure and rotary evaporate material B at a temperature of 45-55℃, a vacuum degree of -0.07 to -0.09MPa, and a rotation speed of 80-150rpm for 60-120 minutes to obtain a crude product. Vacuum dry the crude product at a temperature of 40-50℃ and a vacuum degree of -0.085MPa for 3-5 hours. Cool the dried crude product to room temperature at a cooling rate of 0.5-1.5℃ / min and grind it through a 300-mesh sieve to obtain the modified aromatic amine curing agent.
[0030] Furthermore, the solid-liquid ratio of the anhydrous ethanol and m-phenylenediamine is (5.6-9):1.
[0031] The mass ratio of phthalic acid, vinyltriethoxysilane, polypropylene glycol and m-phenylenediamine is (0.2-0.45):(0.25-0.5):(0.3-0.65):1.
[0032] Furthermore, the preparation of the modified latent curing accelerator includes the following steps: C1. Add anhydrous ethanol to the reactor and heat to 40-55℃ at a heating rate of 1-2℃ / min. Start stirring and set the speed to 350-550 rpm. Add 2-methylimidazole and stir at a constant temperature for 15-25 minutes. Adjust the speed to 500-800 rpm and stir for 15 minutes. Add salicylic acid and stir for 30-45 minutes. Add γ-mercaptopropyltriethoxysilane and stir for 40-50 minutes. Add glycidyl methacrylate and triethylamine and stir for 30-40 minutes. Stop stirring and cool to 40-50℃ at a cooling rate of 0.5-1.2℃ / min to obtain material C.
[0033] C2. Reduce the pressure and rotary evaporate material C at a temperature of 40-50℃, a vacuum degree of -0.07 to -0.09MPa, and a rotation speed of 80-150rpm for 60-120 minutes to obtain material D. Vacuum dry material D at a temperature of 35-45℃ and a vacuum degree of -0.085MPa for 2-4 hours. Cool the dried material D to room temperature at a cooling rate of 0.5-1.2℃ / min and grind it through a 300-mesh sieve to obtain the modified latent curing accelerator.
[0034] Furthermore, the solid-liquid ratio of the anhydrous ethanol and 2-methylimidazole is (7.3-11.5):1.
[0035] The mass ratio of salicylic acid, γ-mercaptopropyltriethoxysilane, glycidyl methacrylate and 2-methylimidazole is (0.25-0.55):(0.3-0.6):(0.35-0.7):1.
[0036] The amount of triethylamine added is 0.1-1% of the mass of glycidyl methacrylate.
[0037] The present invention has the following beneficial effects: 1. In this invention, a modified inorganic composite filler is added. Its surface, through gallic acid anchoring, epoxy silane grafting, and spermine crosslinking to form an organic-inorganic hybrid layer, can chemically bond with the epoxy resin matrix, filling the nanoscale voids at the filler-resin interface and creating a dense interface structure. This effectively inhibits the penetration and diffusion of water molecules along the interface, reducing the water absorption rate of the composite material. Simultaneously, the ortho-phenolic hydroxyl groups of gallic acid can chelate polyvalent metal ion impurities on the powder surface. Combined with the physical coating barrier of the silane layer and multiple washing processes, this significantly reduces the content of extractable sodium and chloride ions in the system, improving the insulation purity of the material. This endows the composition with excellent resistance to humid heat penetration and high insulation purity, ensuring the sealing reliability of electronic devices in humid environments.
[0038] 2. In this invention, a modified aromatic amine curing agent is added. Through multi-level modification via salt passivation, silane grafting, and the introduction of flexible segments via polyether, additional crosslinking sites and flexible segments are constructed in the m-phenylenediamine molecular structure. This results in a more uniform and dense crosslinking network during curing, improving the regularity and thermal stability of the crosslinking structure. This increases the glass transition temperature and high-temperature insulation capability of the material, giving the composition excellent heat resistance and high-temperature volume insulation properties, meeting the requirements of high-end electronic devices for long-term high-temperature service.
[0039] 3. In this invention, a modified latent curing accelerator is added. Through multi-step modification including salt-forming association activation, silane group hydrolysis and condensation, and glycidyl methacrylate crosslinking end-capping, the highly active imidazole groups are temporarily blocked, resulting in an increased curing initiation temperature and a smoother, more uniform exothermic process. This effectively avoids defects and stress concentration problems caused by localized, intense curing. It improves the material's resistance to thermal shock and prevents the encapsulated body from cracking and failing in alternating temperature environments. Simultaneously, it integrates into the crosslinking network after curing, further improving the overall crosslinking system. Working together with the modified filler and modified curing agent, it continuously optimizes the composition's resistance to damp heat, high-temperature insulation properties, and thermal stability. Detailed Implementation
[0040] The technical solutions of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.
[0041] It should be noted that all raw materials used in the following experiments are commercially available.
[0042] The preparation methods of the modified inorganic composite filler, modified aromatic amine curing agent, and modified latent curing accelerator used in the following embodiments and comparative examples of the present invention are as follows: I. The preparation of the modified inorganic composite filler includes the following steps: A1. Mix 1.8 parts of spherical silica and 1 part of spherical alumina evenly to obtain a composite filler; A2. Add 1 part of composite packing and 10 parts of solvent to a reactor, set the temperature to 58℃, the speed to 750 rpm, and stir for 20 minutes. Add 1.15% gallic acid (by weight of the packing), and stir at a constant temperature for 50 minutes. Add 0.65% γ-glycidoxypropyltrimethoxysilane (by weight of the packing), and stir at a constant temperature for 60 minutes. Increase the temperature to 70℃ at a rate of 1℃ / min. Add 0.5% spermine (by weight of the packing), and stir for 75 minutes. Cool to room temperature at a rate of 1℃ / min, stop stirring, filter, collect the filter cake, wash the filter cake three times with anhydrous ethanol, and vacuum dry the washed filter cake at a temperature of 90℃ and a vacuum of -0.085 MPa for 5 hours. Cool the dried filter cake to room temperature, grind it through a 250-mesh sieve, and obtain the modified inorganic composite packing.
[0043] II. The preparation of modified aromatic amine curing agents includes the following steps: B1. Add 7.5 parts of anhydrous ethanol to the reactor, heat to 85°C at a heating rate of 1°C / min, start stirring, set the speed to 500 rpm, add 1 part of m-phenylenediamine, keep the temperature constant and stir for 25 minutes, adjust the speed to 750 rpm, stir for 15 minutes, add 0.37 parts of phthalic acid, stir for 45 minutes, add 0.37 parts of vinyltriethoxysilane, stir for 55 minutes, add 0.47 parts of polypropylene glycol, stir for 40 minutes, stop stirring, cool to 50°C at a cooling rate of 1°C / min to obtain material B; B2. Reduce the pressure and rotary evaporate material B at a set temperature of 50℃, a vacuum degree of -0.08MPa, and a rotation speed of 80-150rpm for 90 minutes to obtain a crude product. Vacuum dry the crude product at a set temperature of 45℃ and a vacuum degree of -0.085MPa for 4 hours. Cool the dried crude product to room temperature at a cooling rate of 1℃ / min and grind it through a 300-mesh sieve to obtain a modified aromatic amine curing agent.
[0044] III. The preparation of modified latent curing accelerators includes the following steps: C1. Add 9.4 parts of anhydrous ethanol to the reactor, heat to 48°C at a heating rate of 1.5°C / min, start stirring, set the speed to 450 rpm, add 1 part of 2-methylimidazole, keep the temperature constant and stir for 20 minutes, adjust the speed to 650 rpm, stir for 15 minutes, add 0.4 parts of salicylic acid, stir for 38 minutes, add 0.45 parts of γ-mercaptopropyltriethoxysilane, stir for 40-50 minutes, add 0.52 parts of glycidyl methacrylate and 0.0015 parts of triethylamine, stir for 35 minutes, stop stirring, cool to 45°C at a cooling rate of 0.8°C / min to obtain material C; C2. Material C is subjected to reduced pressure rotary evaporation at a set temperature of 45℃, a vacuum degree of -0.08MPa, and a rotation speed of 115rpm for 90 minutes to obtain material D. Material D is then vacuum dried at a set temperature of 40℃ and a vacuum degree of -0.085MPa for 3 hours. The dried material D is then cooled to room temperature at a cooling rate of 0.8℃ / min and ground through a 300-mesh sieve to obtain the modified latent curing accelerator. Example 1: Preparation method of high heat-resistant epoxy resin composition for sealing electronic devices. The preparation method of high heat-resistant epoxy resin composition for sealing electronic devices includes the following preparation steps: adding resin to a reaction vessel, heating to 70°C at a heating rate of 1°C / min, stirring at 300 rpm for 20 minutes, adding stress modifier and functional additive in sequence, stirring at constant temperature for 30 minutes, adding modified inorganic composite filler in 3 portions, adjusting the speed to 800 rpm, stirring for 40 minutes, cooling to 45°C at a cooling rate of 0.8°C / min, adjusting the speed to 200 rpm, adding modified aromatic amine curing agent and modified latent curing accelerator in sequence, stirring at constant temperature for 20 minutes to obtain a mixture, degassing the mixture under vacuum at a vacuum degree of -0.085 MPa for 15 minutes to obtain the high heat-resistant epoxy resin composition for sealing electronic devices.
[0045] The high heat-resistant epoxy resin composition for sealing electronic devices is composed of the following components by weight: 75 parts resin, 5 parts stress-modifying agent, 1 part functional agent, 150 parts modified inorganic composite filler, 42 parts modified aromatic amine curing agent, and 0.5 parts modified latent curing accelerator.
[0046] The resin is a compound of phenolic epoxy resin and trifunctional aromatic epoxy resin in a mass ratio of 2:1.
[0047] The stress-modifying agent is epoxy-terminated polybutadiene.
[0048] The functional additives are composed of an ion trapping agent (IXE series from Toa Synthetic Co., Ltd. of Japan, such as IXE-100), an antifoaming agent (BYK-A530 from BYK Chemicals), and an auxiliary coupling agent (γ-glycidyl etheroxypropyltrimethoxysilane (GPS)) in a mass ratio of 20:20:60.
[0049] Example 2: Preparation method of high heat-resistant epoxy resin composition for sealing electronic devices. The preparation method of high heat-resistant epoxy resin composition for sealing electronic devices includes the following preparation steps: adding resin to a reaction vessel, heating to 80°C at a heating rate of 1.5°C / min, stirring at 400 rpm for 25 minutes, adding stress modifier and functional additive in sequence, stirring at constant temperature for 45 minutes, adding modified inorganic composite filler in 4 portions, adjusting the speed to 1000 rpm, stirring for 60 minutes, cooling to 52.5°C at a cooling rate of 1.4°C / min, adjusting the speed to 275 rpm, adding modified aromatic amine curing agent and modified latent curing accelerator in sequence, stirring at constant temperature for 30 minutes to obtain a mixture, degassing the mixture under vacuum at a vacuum degree of -0.09 MPa for 23 minutes to obtain the high heat-resistant epoxy resin composition for sealing electronic devices.
[0050] The high heat-resistant epoxy resin composition for sealing electronic devices consists of the following components by weight: 82.5 parts resin, 6.5 parts stress-modifying agent, 1.5 parts functional agent, 170 parts modified inorganic composite filler, 48.5 parts modified aromatic amine curing agent, and 0.7 parts modified latent curing accelerator.
[0051] The resin is a compound of phenolic epoxy resin and trifunctional aromatic epoxy resin in a mass ratio of 3:1.
[0052] The stress-modifying agent is an organosilicon-modified epoxy resin.
[0053] The functional additive is composed of an ion trapping agent (IXE series from Toa Synthetic Co., Ltd. of Japan, such as IXE-100), an antifoaming agent (BYK-A530 from BYK Chemicals), and an auxiliary coupling agent (γ-glycidyl etheroxypropyltrimethoxysilane (GPS)) in a mass ratio of 30:15:55.
[0054] Example 3: Preparation method of high heat-resistant epoxy resin composition for sealing electronic devices. The preparation method of high heat-resistant epoxy resin composition for sealing electronic devices includes the following preparation steps: adding resin to a reaction vessel, heating to 90°C at a heating rate of 2°C / min, stirring at 500 rpm for 30 minutes, adding stress modifier and functional additive in sequence, stirring at constant temperature for 60 minutes, adding modified inorganic composite filler in 5 portions, adjusting the speed to 1200 rpm, stirring for 80 minutes, cooling to 60°C at a cooling rate of 2°C / min, adjusting the speed to 350 rpm, adding modified aromatic amine curing agent and modified latent curing accelerator in sequence, stirring at constant temperature for 40 minutes to obtain a mixture, degassing the mixture under vacuum at a vacuum degree of -0.095 MPa for 30 minutes to obtain the high heat-resistant epoxy resin composition for sealing electronic devices.
[0055] The high heat-resistant epoxy resin composition for sealing electronic devices consists of the following components by weight: 90 parts resin, 8 parts stress-modifying agent, 2 parts functional agent, 190 parts modified inorganic composite filler, 55 parts modified aromatic amine curing agent, and 0.9 parts modified latent curing accelerator.
[0056] The resin is a compound of phenolic epoxy resin and trifunctional aromatic epoxy resin in a mass ratio of 4:1.
[0057] The stress-modifying additives are epoxy-terminated polybutadiene and silicone-modified epoxy resin.
[0058] The mass ratio of terminal epoxy group polybutadiene to organosilicon modified epoxy resin is 2:1.
[0059] The functional additive is a mixture of ion trapping agent (IXE series from Toa Synthetic Co., Ltd. of Japan, such as IXE-100), defoamer (BYK-A530 from BYK Chemicals) and auxiliary coupling agent (γ-glycidyl etheroxypropyltrimethoxysilane (GPS)) in a mass ratio of 35:25:40.
[0060] Comparative Example 1: The difference between this comparative example and Example 1 is that: In this comparative example, the modified inorganic composite packing was replaced with an unmodified packing composed of spherical silica and spherical alumina in a ratio of 1.8:1.
[0061] Comparative Example 2: The difference between this comparative example and Example 1 is that: In this comparative example, the modified aromatic amine curing agent was replaced with unmodified m-phenylenediamine.
[0062] Comparative Example 3 differs from Example 1 in that: In this comparative example, the modified latent curing accelerator was replaced with unmodified 2-methylimidazole.
[0063] Comparative Example 4: The difference between this comparative example and Example 1 is that: In this comparative example, the modified inorganic composite filler was replaced with an unmodified spherical silica and spherical alumina compounded in a ratio of 1.8:1; the modified aromatic amine curing agent was replaced with unmodified m-phenylenediamine; and the modified latent curing accelerator was replaced with unmodified 2-methylimidazole.
[0064] Comparative Example 5: The difference between this comparative example and Example 1 is that: In this comparative example, the modified inorganic composite filler was replaced with a bimodal graded filler consisting of spherical silica and spherical alumina surface-treated with γ-glycidoxypropyltrimethoxysilane. The amount of γ-glycidoxypropyltrimethoxysilane was 1.5% of the filler mass, the treatment temperature was 80℃, and the treatment time was 2h. The modified aromatic amine curing agent was replaced with a conventional compound curing agent consisting of a physical mixture of m-phenylenediamine and 4,4'-diaminodiphenyl sulfone (DDS) at a mass ratio of 1:1. The modified latent curing accelerator was replaced with commercially available 2-methylimidazole.
[0065] Comparative Example 6: The difference between this comparative example and Example 1 is that: In this comparative example, the modified inorganic composite filler, modified aromatic amine curing agent, and modified latent curing accelerator were all prepared using the binary pre-reaction pathway disclosed in CN117106286A, namely: (1) Filler modification: Gallic acid and γ-glycidyl etheroxypropyltriethoxysilane were pre-mixed and reacted for 30 min to form a binary pre-reactant, which was then mixed with spherical silica-alumina composite filler. The three-step sequential process was not adopted. Spermine was added at the same time as the binary pre-reactant; (2) Curing agent modification: Phthalic acid and vinyltriethoxysilane were pre-mixed to form a binary pre-reactant, which was then reacted with m-phenylenediamine. Polypropylene glycol was added at the same time. The three-step sequential process was not adopted; (3) Accelerator modification: Salicylic acid and γ-mercaptopropyltriethoxysilane were pre-mixed to form a binary pre-reactant, which was then reacted with 2-methylimidazole. Glycidyl methacrylate was added at the same time. The three-step sequential process was not adopted.
[0066] Performance testing: The high heat-resistant epoxy resin compositions for sealing electronic devices prepared in Examples 1, 2, 3, 1, 2, 3, 4, 5, and 6 were tested. The test data are recorded in Table 1 below: Table 1 - Performance Tests of High Heat-Resistant Epoxy Resin Compositions for Sealing Electronic Devices Tg(DSC) / ℃ <![CDATA[Cl - Content / ppm]]> Volume resistivity at 180℃ / Ω・cm Thermal shock / time Boiling water absorption rate (%) in 24 hours <![CDATA[Na + Content / ppm]]> Example 1 166 0.8 <![CDATA[1.8×10 15 ]]> 385 0.18 1.2 Example 2 171 0.6 <![CDATA[2.3×10 15 ]]> 412 0.16 0.9 Example 3 173 0.5 <![CDATA[2.7×10 15 ]]> 450 0.15 0.8 Comparative Example 1 147 6.2 <![CDATA[3.2×10 13 ]]> 155 0.62 6.2 Comparative Example 2 151 3.8 <![CDATA[5.8×10 13 ]]> 176 0.52 3.8 Comparative Example 3 148 4.5 <![CDATA[4.5×10 13 ]]> 163 0.55 4.5 Comparative Example 4 137 9.1 <![CDATA[8.5×10 12 ]]> 75 0.89 9.1 Comparative Example 5 146 5.6 <![CDATA[6.2×10 13 ]]> 195 0.51 5.6 Comparative Example 6 155 2.5 <![CDATA[4.2×10 14 ]]> 240 0.41 3.6 Based on the above data, the following conclusions can be drawn: The high heat-resistant epoxy resin compositions for sealing electronic devices prepared in Examples 1, 2, 3, 1, 2, 3, 4, 5 and 6 were tested according to GB / T19466.2-2004, with a DSC heating rate of 10℃ / min and a nitrogen atmosphere. The Tg (DSC) test was performed on these compositions. The high heat-resistant epoxy resin compositions for sealing electronic devices prepared according to the test methods in GB / T40564-2021 (Examples 1, 2, 3, Comparative Examples 1, 2, 3, 4, 5, and 6) were subjected to Cl...- Content testing; The high heat-resistant epoxy resin compositions for sealing electronic devices prepared according to GB / T31838.7-2021 were subjected to volume resistivity testing at 180℃ after the samples were kept at 180℃ for 30 min and the DC test voltage was 500V. The test was performed according to GB / T2423.22-2012 Test Nc. The test conditions were -40℃ to 125℃, with each temperature held for 30 min and the temperature transition time not exceeding 10 s. The maximum number of cycles without visible cracks in the sample was recorded. The high heat-resistant epoxy resin compositions for sealing electronic devices prepared in Examples 1, 2, 3, 1, 2, 3, 4, 5 and 6 were subjected to thermal shock tests. The high heat-resistant epoxy resin compositions for sealing electronic devices prepared in Examples 1, 2, 3, 1, 2, 3, 4, 5, and 6 of GB / T1034-2008 were subjected to a boiling water 24-hour water absorption test. The samples were immersed in boiling distilled water for 24 hours, cooled and dried, and then weighed to calculate the percentage increase in mass. The high heat-resistant epoxy resin compositions for sealing electronic devices prepared according to the test methods in GB / T40564-2021 (Examples 1, 2, 3, Comparative Examples 1, 2, 3, 4, 5, and 6) were subjected to Na testing. + Content testing.
[0067] The inorganic composite filler, modified through multiple stages of time, forms an organic-inorganic hybrid layer on its surface through gallic acid anchoring, epoxy silane grafting, and spermine crosslinking. This layer chemically bonds with the epoxy resin matrix, effectively filling the nanoscale voids and creating a dense interfacial structure at the filler-resin interface, thus inhibiting water molecule penetration and diffusion along the interface and reducing the composite material's water absorption. Furthermore, the ortho-phenolic hydroxyl groups of gallic acid chelate polyvalent metal ion impurities on the powder surface. Combined with the physical barrier of the silane layer and multiple washing processes during preparation, this effectively reduces the content of extractable sodium and chloride ions in the system, improving the material's insulation purity. The modified aromatic amine curing agent, through multi-stage modification involving salt passivation, silane grafting, and the introduction of flexible segments via polyether, introduces flexible segments and additional crosslinking sites into the m-phenylenediamine molecular structure. This allows for the formation of a more uniform and dense crosslinking network during curing, improving the regularity and thermal stability of the crosslinking structure. Consequently, it significantly increases the material's glass transition temperature and high-temperature insulation capability, endowing the composition with excellent heat resistance and high-temperature volume insulation properties. Modified latent curing accelerators, through multi-step modification including salt-forming association activation, silane group hydrolysis and condensation, and glycidyl methacrylate crosslinking end-capping, temporarily block highly active imidazole groups, thereby increasing the curing start-up temperature and making the exothermic process more gradual and uniform. This effectively avoids defects and internal stress concentration problems caused by localized intense curing, and improves the material's resistance to thermal shock. At the same time, after participating in the curing reaction, it integrates into the crosslinking network, further improving the overall crosslinking system. Working together with modified fillers and modified curing agents, it continuously optimizes the material's resistance to damp heat, high-temperature insulation properties, and thermal stability.
[0068] Glass transition temperature, volume resistivity at 180℃, and thermal shock cycle count are positive performance indicators; higher values indicate better thermal stability, high-temperature insulation, and resistance to temperature cycling fatigue. Extractable Na + (Sodium ion) content, extractable Cl - The chloride ion content and the boiling water absorption rate over 24 hours are inverse performance indicators. The lower the value, the fewer mobile ionic impurities and the higher the ion purity inside the material. This indicates better resistance to boiling water humid heat penetration and superior sealing performance. The various modified systems work together through process superposition to achieve overall optimization and improvement of the comprehensive sealing performance of the composition.
[0069] Based on the above arguments, this invention addresses the issues of Tg(DSC) and Cl. - Content, volume resistivity at 180℃, thermal shock, water absorption rate in boiling water over 24 hours, and Na + The content of these components was significantly better than that of the control group.
[0070] The preferred embodiments of the present invention disclosed above are merely illustrative of the invention. These preferred embodiments do not exhaustively describe all details, nor do they limit the invention to the specific implementations described. Clearly, many modifications and variations can be made based on the content of this specification. This specification selects and specifically describes these embodiments to better explain the principles and practical applications of the invention, thereby enabling those skilled in the art to better understand and utilize the invention. The invention is limited only by the claims and their full scope and equivalents.
Claims
1. A method for preparing a high heat-resistant epoxy resin composition for sealing electronic devices, characterized in that, The preparation method of the high heat-resistant epoxy resin composition for sealing electronic devices includes the following preparation steps: adding resin to a reaction vessel, heating to 70-90℃ at a heating rate of 1-2℃ / min, stirring at 300-500 rpm for 20-30 minutes, adding stress-modifying additives and functional additives in sequence, stirring at a constant temperature for 30-60 minutes, adding modified inorganic composite fillers in 3-5 portions, adjusting the speed to 800-1200 rpm, stirring for 40-80 minutes, cooling to 45-60℃ at a cooling rate of 0.8-2℃ / min, adjusting the speed to 200-350 rpm, adding modified aromatic amine curing agent and modified latent curing accelerator in sequence, stirring at a constant temperature for 20-40 minutes to obtain a mixture, degassing the mixture under vacuum, setting the vacuum degree to -0.085 to -0.095 MPa, degassing for 15-30 minutes to obtain the high heat-resistant epoxy resin composition for sealing electronic devices; The modified inorganic composite filler is prepared by sequentially modifying bimodal graded inorganic powder composed of spherical silica and spherical alumina through gallic acid anchoring, epoxy silane grafting, and spermine crosslinking into a network. The modified aromatic amine curing agent is prepared by sequentially passing down the amino groups with phthalic acid salt formation, bridging with vinyltriethoxysilane interface, and modifying with polypropylene glycol flexible end-capping, based on m-phenylenediamine as the matrix. The modified latent curing accelerator is prepared by sequentially modifying 2-methylimidazole as a matrix through salicylic acid salt-forming association activation, γ-mercaptopropyltriethoxysilane hydrolysis condensation transition, and glycidyl methacrylate crosslinking and end-capping modification under alkaline catalysis (triethylamine).
2. The method for preparing the high heat-resistant epoxy resin composition for sealing electronic devices according to claim 1, characterized in that, The high heat-resistant epoxy resin composition for sealing electronic devices is composed of the following components by weight: 75-90 parts resin, 5-8 parts stress-modifying agent, 1-2 parts functional agent, 150-190 parts modified inorganic composite filler, 42-55 parts modified aromatic amine curing agent, and 0.5-0.9 parts modified latent curing accelerator.
3. The method for preparing the high heat-resistant epoxy resin composition for sealing electronic devices according to claim 1, characterized in that, The resin is a compound of phenolic epoxy resin and trifunctional aromatic epoxy resin in a mass ratio of (2-4):1; The stress-modifying agent is one or more of terminal epoxy-terminated polybutadiene and organosilicon-modified epoxy resin.
4. The method for preparing the high heat-resistant epoxy resin composition for sealing electronic devices according to claim 1, characterized in that, The functional additive is composed of an ion trapping agent, an antifoaming agent and an auxiliary coupling agent in a mass ratio of (20-35):(15-25):(40-60).
5. The method for preparing the high heat-resistant epoxy resin composition for sealing electronic devices according to claim 1, characterized in that, The preparation of the modified inorganic composite filler includes the following steps: A1. Mix spherical silica and spherical alumina evenly to obtain a composite filler; A2. Add the composite packing and solvent to the reactor, set the temperature to 50-65℃, the rotation speed to 600-900 rpm, stir for 20 minutes, add gallic acid, stir at a constant temperature for 40-60 minutes, add γ-glycidoxypropyltrimethoxysilane, stir at a constant temperature for 50-70 minutes, raise the temperature to 65-75℃ at a heating rate of 0.5-1.5℃ / min, add spermine, stir for 60-90 minutes, cool to room temperature at a cooling rate of 0.5-1.5℃ / min, stop stirring, filter, collect the filter cake, wash the filter cake 2-3 times with anhydrous ethanol, vacuum dry the washed filter cake at a temperature of 80-100℃ and a vacuum degree of -0.085MPa for 4-6 hours, cool the dried filter cake to room temperature, grind it through a 200-300 mesh sieve to obtain the modified inorganic composite packing.
6. The method for preparing the high heat-resistant epoxy resin composition for sealing electronic devices according to claim 5, characterized in that, The mass ratio of the spherical silica to the spherical alumina is (1-2.5):1; The solvent is a mixture of ethanol and deionized water in a volume ratio of (4-6):
1. The solid-liquid ratio of the composite filler and the solvent is 1:(8-12); The gallic acid accounts for 0.8-1.5% of the total mass of the composite filler; The γ-glycidyl etheroxypropyltrimethoxysilane accounts for 0.4-0.9% of the total mass of the composite filler; The succinamine accounts for 0.3-0.7% of the total mass of the composite filler.
7. The method for preparing the high heat-resistant epoxy resin composition for sealing electronic devices according to claim 1, characterized in that, The preparation of the modified aromatic amine curing agent includes the following steps: B1. Add anhydrous ethanol to the reactor and heat to 80-90℃ at a heating rate of 0.5-1.5℃ / min. Start stirring and set the speed to 400-600 rpm. Add m-phenylenediamine and stir at a constant temperature for 20-30 minutes. Adjust the speed to 600-900 rpm and stir for 15 minutes. Add phthalic acid and stir for 40-50 minutes. Add vinyltriethoxysilane and stir for 50-60 minutes. Add polypropylene glycol and stir for 35-45 minutes. Stop stirring and cool to 45-55℃ at a cooling rate of 0.5-1.5℃ / min to obtain material B. B2. Reduce the pressure and rotary evaporate material B at a temperature of 45-55℃, a vacuum degree of -0.07 to -0.09MPa, and a rotation speed of 80-150rpm for 60-120 minutes to obtain a crude product. Vacuum dry the crude product at a temperature of 40-50℃ and a vacuum degree of -0.085MPa for 3-5 hours. Cool the dried crude product to room temperature at a cooling rate of 0.5-1.5℃ / min and grind it through a 300-mesh sieve to obtain the modified aromatic amine curing agent.
8. The method for preparing the high heat-resistant epoxy resin composition for sealing electronic devices according to claim 7, characterized in that, The solid-liquid ratio of the anhydrous ethanol and m-phenylenediamine is (5.6-9):1; The mass ratio of phthalic acid, vinyltriethoxysilane, polypropylene glycol and m-phenylenediamine is (0.2-0.45):(0.25-0.5):(0.3-0.65):
1.
9. The method for preparing the high heat-resistant epoxy resin composition for sealing electronic devices according to claim 1, characterized in that, The preparation of the modified latent curing accelerator includes the following steps: C1. Add anhydrous ethanol to the reactor and heat to 40-55℃ at a heating rate of 1-2℃ / min. Start stirring and set the speed to 350-550 rpm. Add 2-methylimidazole and stir at a constant temperature for 15-25 minutes. Adjust the speed to 500-800 rpm and stir for 15 minutes. Add salicylic acid and stir for 30-45 minutes. Add γ-mercaptopropyltriethoxysilane and stir for 40-50 minutes. Add glycidyl methacrylate and triethylamine and stir for 30-40 minutes. Stop stirring and cool to 40-50℃ at a cooling rate of 0.5-1.2℃ / min to obtain material C. C2. Reduce the pressure and rotary evaporate material C at a temperature of 40-50℃, a vacuum degree of -0.07 to -0.09MPa, and a rotation speed of 80-150rpm for 60-120 minutes to obtain material D. Vacuum dry material D at a temperature of 35-45℃ and a vacuum degree of -0.085MPa for 2-4 hours. Cool the dried material D to room temperature at a cooling rate of 0.5-1.2℃ / min and grind it through a 300-mesh sieve to obtain the modified latent curing accelerator.
10. The method for preparing the high heat-resistant epoxy resin composition for sealing electronic devices according to claim 9, characterized in that, The solid-liquid ratio of the anhydrous ethanol and 2-methylimidazole is (7.3-11.5):1; The mass ratio of salicylic acid, γ-mercaptopropyltriethoxysilane, glycidyl methacrylate, and 2-methylimidazole is (0.25-0.55):(0.3-0.6):(0.35-0.7):1; The amount of triethylamine added is 0.1-1% of the mass of glycidyl methacrylate.
Citation Information
Patent Citations
LED composite packaging material and preparation method thereof
CN117106286A