Methanol benzoic acid synergistically modified pedot:pss film and preparation method thereof

By treating PEDOT:PSS films with methanol-diluted benzoic acid, the problem of low conductivity was solved, resulting in PEDOT:PSS films with high conductivity and high transmittance, which can be used to prepare high-performance flexible supercapacitors.

CN123152259APending Publication Date: 2026-11-24PEKING UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202610602115.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-05-05
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing PEDOT:PSS films have low electrical conductivity, making it difficult to meet the high power density requirements of flexible supercapacitors, and the use of strong acid modification will damage other materials.

Method used

PEDOT:PSS films were treated with a benzoic acid solution diluted with methanol. Spin coating and methanol cleaning were then used to promote the full reaction between benzoic acid and PSS, forming a highly conductive extended quinone structure.

Benefits of technology

The conductivity of the PEDOT:PSS film was significantly increased to approximately 3680 S/cm, while maintaining high light transmittance and mechanical flexibility. The resulting flexible supercapacitor exhibited excellent energy-power characteristics.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123152259A_ABST
    Figure CN123152259A_ABST
Patent Text Reader

Abstract

The application provides a methanol benzoic acid synergistically modified PEDOT:PSS film and a preparation method thereof. The modified PEDOT:PSS film is obtained by synergistically treating PEDOT:PSS with methanol and benzoic acid. The conductivity of the modified PEDOT:PSS film reaches about 3760 S / cm. The super capacitor prepared by using the material has a surface energy density of 32.8 mu Wh / cm2 under a power density of 1.2 mW / cm2.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of foldable screens, specifically, to methanol. Benzoic acid-synergistic modification of PEDOT:PSS thin films and their preparation methods. Background Technology

[0002] In recent years, foldable screen phones have attracted great interest from consumers and created enormous economic value. Flexible supercapacitors are key components of capacitive touchscreens in foldable screen phones. In the operating environment of a foldable screen, flexible supercapacitors need to possess excellent comprehensive properties such as high power density, lightweight, light transmittance, bendability, stretchability, and long cycle life. To achieve these properties, selecting electrode materials with excellent comprehensive properties of conductivity, flexibility, and light transmittance is crucial. Indium tin oxide (ITO) is currently the material chosen by major foldable screen phone manufacturers for flexible capacitor electrodes due to its high conductivity and high light transmittance. However, ITO has a high density and is inherently brittle, requiring the control of its thickness (≈10 nm) to impart physical flexibility in practical applications. This makes the ITO fabrication process extremely complex. Furthermore, indium is a rare metal with limited supply. These factors result in extremely high ITO manufacturing costs. Therefore, the industry is urgently seeking new alternatives.

[0003] Intrinsically conductive polymers are favored by industry due to their intrinsic conductivity and flexibility, simple preparation processes, and low cost. Among them, poly(3,4-ethylenedioxythiophene):polystyrene sulfonate (PEDOT:PSS) exhibits high transmittance in the visible light range, good mechanical and chemical stability, solution processing capability, and low cost, making it considered one of the important materials that may replace ITO in the future. However, PEDOT:PSS has a low intrinsic conductivity (approximately 0.1~1 S / cm). Therefore, using intrinsic PEDOT:PSS as an electrode material will cause significant energy loss during the charging and discharging of flexible supercapacitors, i.e., reducing the power density of the capacitor. This conflicts with the requirements for flexible supercapacitors in foldable screen phones. Therefore, how to improve the conductivity of PEDOT:PSS while maintaining its other properties, thereby enhancing its overall performance, has significant theoretical and practical value.

[0004] PEDOT is a conjugated, water-insoluble, conductive polymer material. In industrial production, to achieve solution-processable PEDOT, water-soluble, insulating PSS is added during the polymerization of 3,4-ethylenedioxythiophene (EDOT) monomers to induce polymerization and dissolution, thus producing a commercially available PEDOT:PSS solution. Therefore, intrinsic PEDOT:PSS films prepared by spin-coating commercial PEDOT:PSS solutions exhibit low conductivity. Treating the prepared films with chemical reagents to promote phase separation of PEDOT and PSS molecules is a simple and effective method to improve the conductivity of PEDOT:PSS films. Commonly used chemical reagents include high-boiling-point polar solvents, polyhydroxy compounds, ionic liquids, and strong and weak acids. Among these, the use of strong inorganic acids has the most significant effect on improving the conductivity of PEDOT:PSS films. Kim et al. used concentrated sulfuric acid to increase the conductivity of PEDOT:PSS to 4200 S / cm, which is the highest known conductivity value for modified PEDOT:PSS materials. However, strong acids, such as sulfuric acid, are extremely reactive. Using strong acids as modifiers for PEDOT:PSS during flexible device fabrication will inevitably affect other materials in the flexible device, causing serious damage. To reduce such damage, weak acids, such as benzoic acid, can be used to treat the PEDOT:PSS film. Kang et al. added a methanol solution of benzoic acid to the surface of the PEDOT:PSS film, dried it, and then washed the film with methanol, increasing its conductivity to 1500 S / cm. This conductivity value is significantly lower than that obtained using sulfuric acid modification.

[0005] Therefore, there is an urgent need to develop more methods to solve the above problems. Summary of the Invention

[0006] The inventors discovered that the conductivity of PEDOT:PSS films treated with weak acids such as benzoic acid is significantly lower than that obtained by modifying with sulfuric acid, mainly because the benzoic acid dropped onto the film surface has difficulty penetrating the film interior and fully reacting with PSS. If this problem can be solved, it is expected that even mild benzoic acid can greatly improve the conductivity of PEDOT:PSS. Based on this discovery, this invention proposes a method for modifying PEDOT:PSS with a weak acid and its preparation. The method involves adding benzoic acid to a commercially available PEDOT:PSS aqueous solution diluted with methanol, and using the resulting solution to prepare a film by spin coating. The film is then cleaned with methanol. The conductivity of the treated PEDOT:PSS film reaches a maximum of approximately 3680 S / cm. The significant improvement in conductivity is mainly attributed to the full reaction between benzoic acid and PSS. Using the high-conductivity PEDOT:PSS modified by the method of this invention as an electrode material, a flexible supercapacitor with excellent overall performance was prepared.

[0007] In one aspect of the invention, a modified PEDOT:PSS film is provided. According to an embodiment of the invention, the modified PEDOT:PSS film is obtained by co-treating PEDOT:PSS with methanol and benzoic acid.

[0008] According to embodiments of the present invention, the modified PEDOT:PSS film may further include at least one of the following additional technical features: According to an embodiment of the present invention, the PSS content in the modified PEDOT:PSS film is reduced, and PEDOT exhibits a highly conductive extended quinone structure.

[0009] According to an embodiment of the present invention, the electrical conductivity of the modified PEDOT:PSS film is ≥3000 S / cm.

[0010] According to an embodiment of the present invention, the electrical conductivity of the modified PEDOT:PSS film is 3760 S / cm.

[0011] According to an embodiment of the present invention, the modified PEDOT:PSS film has a visible light transmittance of ≥88% at 550 nm.

[0012] In another aspect, the present invention also provides a method for preparing a modified PEDOT:PSS thin film. According to an embodiment of the present invention, the preparation method includes: S1: PEDOT:PSS aqueous solution was diluted with methanol and benzoic acid was added to form a mixed precursor solution; S2: The mixed precursor solution is formed into a film and dried, then soaked and washed with methanol, and finally dried a second time to obtain the modified PEDOT:PSS film.

[0013] According to embodiments of the present invention, the above preparation method may further include at least one of the following additional technical features: According to an embodiment of the present invention, the volume ratio of PEDOT:PSS aqueous solution to methanol in step S1 is 0.1:1-10:1, for example 0.1:1, 1:1, 5:1, 10:1, etc.

[0014] According to an embodiment of the present invention, the concentration of benzoic acid in the mixed precursor solution is greater than 0 mg / mL.

[0015] According to an embodiment of the present invention, the concentration of benzoic acid in the mixed precursor solution is greater than 0 mg / mL and less than or equal to 500 mg / mL.

[0016] According to an embodiment of the present invention, the concentration of benzoic acid in the mixed precursor solution is 50 mg / mL.

[0017] According to an embodiment of the present invention, the film formation method in step S2 is spin coating, blade coating or spray coating.

[0018] According to an embodiment of the present invention, the film formation in step S2 is performed by spin-coating the mixed precursor liquid onto the substrate.

[0019] According to embodiments of the present invention, the substrate is a glass substrate, a polyethylene terephthalate (PET) substrate, a polyurethane (PUR) substrate, or a titanium foil (Ti) substrate.

[0020] According to an embodiment of the present invention, the drying is carried out at a temperature of 80–160°C for 5–60 minutes.

[0021] According to an embodiment of the present invention, the drying is carried out at a temperature of 120°C for 20 minutes.

[0022] According to an embodiment of the present invention, the methanol soaking and cleaning time in step S2 is 1 to 60 minutes.

[0023] According to an embodiment of the present invention, the electrical conductivity of the modified PEDOT:PSS film is ≥3000 S / cm.

[0024] According to an embodiment of the present invention, the electrical conductivity of the modified PEDOT:PSS film is 3760 S / cm.

[0025] According to an embodiment of the present invention, the modified PEDOT:PSS film has a visible light transmittance of ≥88% at 550 nm.

[0026] In another aspect, the present invention also provides a flexible electrode. According to an embodiment of the present invention, the flexible electrode comprises the modified PEDOT:PSS film described above or the modified PEDOT:PSS film prepared according to the methods described above.

[0027] In another aspect, the present invention also proposes a flexible supercapacitor. According to an embodiment of the present invention, the flexible supercapacitor for foldable screens includes the flexible electrodes described above.

[0028] According to an embodiment of the present invention, the flexible supercapacitor has an area energy density of 32.8 μWh / cm² at a power density of 1.2 mW / cm².

[0029] In another aspect, the present invention also proposes the application of the modified PEDOT:PSS film described above or the modified PEDOT:PSS film prepared according to the method described above in flexible electronics, wearable devices, flexible energy storage devices, and foldable screen terminals.

[0030] In another aspect, this invention proposes a method of synergistic modification of PEDOT:PSS with methanol and benzoic acid. Through a process involving methanol dilution, benzoic acid blending, and subsequent methanol washing, the insulating PSS component is partially removed, causing the PEDOT molecular chain to transform from a coiled aromatic structure to a highly conductive extended quinone structure. This significantly improves the film's conductivity, visible light transmittance, bending flexibility, and environmental stability. Flexible transparent electrodes and flexible supercapacitors based on this modified film exhibit high specific capacitance, long cycle life, and excellent bending resistance, making them widely applicable in foldable screen devices, flexible electronics, wearable energy storage devices, and other fields. The process is simple, low-cost, and easily scalable. Attached Figure Description

[0031] The above and / or additional aspects and advantages of the present invention will become apparent and readily understood from the description of the embodiments taken in conjunction with the following drawings, in which: Figure 1 Schematic diagram of the process for PEDOT:PSS methanol-benzoic acid co-modification; Figure 2 The conductivity and total transmittance of PEDOT:PSS after modification with different concentrations of benzoic acid; Figure 3A schematic diagram of the PEDOT:PSS / BA flexible supercapacitor device (a), GCD curves at different current densities (b), area Lagrangian plot of the capacitor (c), and actual working diagram of the capacitor (d). Detailed Implementation

[0032] Embodiments of the present invention are described in detail below, examples of which are illustrated in the accompanying drawings, wherein the same or similar reference numerals denote the same or similar elements or elements having the same or similar functions throughout. The embodiments described below with reference to the accompanying drawings are exemplary and intended to explain the present invention, and should not be construed as limiting the present invention.

[0033] Furthermore, the terms "first" and "second" are used for descriptive purposes only and should not be construed as indicating or implying relative importance or implicitly specifying the number of technical features indicated. Thus, a feature defined as "first" or "second" may explicitly or implicitly include at least one of that feature. In the description of this invention, "a plurality of" means at least two, such as two, three, etc., unless otherwise explicitly specified.

[0034] In this invention, unless otherwise explicitly specified and limited, "above" or "below" the second feature can mean that the first feature is in direct contact with the second feature, or that the first feature is in indirect contact with the second feature through an intermediate medium. Furthermore, "above," "over," and "on top" of the second feature can mean that the first feature is directly above or diagonally above the second feature, or simply that the first feature is at a higher horizontal level than the second feature. "Below," "below," and "under" the second feature can mean that the first feature is directly below or diagonally below the second feature, or simply that the first feature is at a lower horizontal level than the second feature.

[0035] The present invention will now be described with reference to specific embodiments. It should be noted that these embodiments are merely descriptive and do not limit the present invention in any way.

[0036] The following abbreviations are used throughout this invention:

[0037] A schematic diagram of the process for modifying PEDOT using methanol-benzoic acid: PSS is shown below. Figure 1As shown. Commercially available PEDOT:PSS aqueous solution (pH 1000) was diluted with methanol to control the volume ratio of the original solution to methanol at 0.1:1 to 10:1 (e.g., 1:1). Benzoic acid powder was added and stirred overnight to achieve different concentrations of the precursor solution. In this study, the concentration of benzoic acid ranged from 0 to 500 mg / ml. The obtained precursor solution was spin-coated onto a substrate and heated at 120°C for 20 minutes. It was then rinsed with methanol and heated at 120°C for another 20 minutes to complete the preparation of the modified PEDOT:PSS thin film material. The thin film prepared from the original PEDOT:PSS aqueous solution served as a blank control group in this study.

[0038] A flexible supercapacitor was fabricated using PEDOT:PSS spin-coated onto Ti foil as the electrode and PVA soaked in 1M sulfuric acid as the dielectric material. When testing the capacitor's performance using a two-electrode method on an electrochemical workstation, the working electrode was connected to one terminal of the capacitor, while the reference and counter electrodes were connected together to the other terminal. The current density range for the galvanostatic charge-discharge (GCD) test was 0.5–20 mA / cm², and the voltage window was 0–1 V.

[0039] like Figure 2 As shown, when the benzoic acid concentration is 0%, this modification process is equivalent to using only methanol, and the resulting PEDOT:PSS conductivity is 650 S / cm, consistent with the results of many studies using only methanol for modification. With increasing benzoic acid concentration, the conductivity tends to reach saturation, which may be due to the chemical reaction between PSS and benzoic acid in the film reaching its reaction limit. At a benzoic acid concentration of 50 mg / ml, the conductivity reaches 3760 S / cm, which is the maximum conductivity achieved by modifying PEDOT:PSS using organic materials. Figure 2 It also demonstrated the transmittance in the visible light range. The improvement in visible conductivity did not sacrifice transmittance, with transmittance approaching 90%.

[0040] PEDOT:PSS (hereinafter referred to as PEDOT:PSS / BA) treated with 50 mg / ml BA was directly used as the positive and negative electrodes in the assembly of a supercapacitor. It absorbed 1.0 M PVA and Ti mesh distribution to act as the separator and current collector, such as... Figure 3 As shown in (a). Figure 3 As shown in (b), a symmetrical triangular GCD curve was obtained at current densities of 0.5-20 mA / cm², indicating excellent reversibility and negligible internal resistance. The device capacitance (C) is calculated using the following equation. d ):

[0041] Where I is the current, Δt is the discharge time, and ΔV is the voltage window.

[0042] Figure 3 (c) shows the area-based Rangeone plot of the device, further quantifying the relationship between energy density and power density. The formulas for calculating energy density and power density are: (4) (5) Where C d Here, ΔV is the device capacitance, ΔV is the voltage range, and Δt is the discharge time. The optimized supercapacitor exhibits excellent energy storage performance, achieving an areal energy density of 32.8 μWh / cm² at a power density of 1.2 mW / cm². Finally, this device can simultaneously charge multiple LEDs, demonstrating its enormous potential for practical applications, such as... Figure 3 As shown in (d).

[0043] Table 1 below compares the conductivity results of organic compounds modified with those reported in the prior art and the organic compound (methanol / benzoic acid) used in this invention. The prior art uses the following methods to test the conductivity of its modified compounds: First, a commercially available PEDOT:PSS aqueous solution was spin-coated onto the substrate surface and dried at 120°C for a certain period of time to prepare a PEDOT:PSS film. Then, this film was immersed in an organic material for a period of time, and then dried again at 120°C to obtain a modified sample. The conductivity of this sample was then tested.

[0044] Table 1

[0045] This invention presents a mild yet efficient strategy to enhance the conductivity of PEDOT:PSS through methanol-benzoic acid co-modification. The optimized PEDOT:PSS film achieved a record-high conductivity of 3760 S / cm in its organically modified counterpart, and the mechanism of this conductivity enhancement was elucidated through comprehensive spectroscopic analysis. Crucially, this modification preserves the material's mechanical flexibility while significantly improving its electrochemical performance.

[0046] The flexible supercapacitor fabricated using the modified PEDOT:PSS electrode also exhibits excellent energy-power characteristics, with a maximum energy density of 32.8 μWh / cm2 at a power density of 1.2 mW / cm2, which is superior to most reported PEDOT-based supercapacitors.

[0047] In the description of this specification, the references to terms such as "one embodiment," "some embodiments," "example," "specific example," or "some examples," etc., indicate that a specific feature, structure, material, or characteristic described in connection with that embodiment or example is included in at least one embodiment or example of the present invention. In this specification, the illustrative expressions of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments or examples. Moreover, without contradiction, those skilled in the art can combine and integrate the different embodiments or examples described in this specification, as well as the features of different embodiments or examples.

[0048] Although embodiments of the present invention have been shown and described above, it is understood that the above embodiments are exemplary and should not be construed as limiting the present invention. Those skilled in the art can make changes, modifications, substitutions and variations to the above embodiments within the scope of the present invention.

Claims

1. A modified PEDOT:PSS film, characterized by, The modified PEDOT:PSS film is obtained by co-treatment of PEDOT:PSS with methanol and benzoic acid.

2. The modified PEDOT:PSS film according to claim 1, characterized in that, The modified PEDOT:PSS film has a reduced PSS content and PEDOT exhibits a highly conductive extended quinone structure. Optionally, the electrical conductivity of the modified PEDOT:PSS film is ≥3000 S / cm; Preferably, the electrical conductivity of the modified PEDOT:PSS film is 3760 S / cm; Optionally, the modified PEDOT:PSS film has a visible light transmittance of ≥88% at 550 nm.

3. A method for preparing a modified PEDOT:PSS film, characterized by, include: S1: PEDOT:PSS aqueous solution was diluted with methanol and benzoic acid was added to form a mixed precursor solution; S2: The mixed precursor solution is formed into a film and dried, then soaked and washed with methanol, and finally dried a second time to obtain the modified PEDOT:PSS film.

4. The production method according to claim 3, characterized by, In step S1, the volume ratio of PEDOT:PSS aqueous solution to methanol is 0.1:1-10:1; Optionally, the concentration of benzoic acid in the mixed precursor solution is greater than 0 mg / mL; Optionally, the concentration of benzoic acid in the mixed precursor solution is greater than 0 mg / mL and less than or equal to 500 mg / mL; Preferably, the concentration of benzoic acid in the mixed precursor solution is 50 mg / mL.

5. The preparation method according to claim 3, characterized in that, In step S2, the film formation method is spin coating, blade coating, or spray coating; Optionally, the film formation in step S2 is performed by spin-coating the mixed precursor liquid onto a substrate; Optionally, the substrate is a glass substrate, a polyethylene terephthalate (PET) substrate, a polyurethane (PUR) substrate, or a titanium foil (Ti) substrate; Optionally, the drying is carried out at a temperature of 80–160°C for 5–60 minutes. Preferably, the drying is carried out at a temperature of 120°C for 20 minutes; Optionally, the methanol soaking and cleaning time in step S2 is 1 to 60 minutes.

6. The preparation method according to claim 3, characterized in that, The electrical conductivity of the modified PEDOT:PSS film is ≥3000 S / cm; Preferably, the electrical conductivity of the modified PEDOT:PSS film is 3760 S / cm; Optionally, the modified PEDOT:PSS film has a visible light transmittance of ≥88% at 550 nm.

7. A flexible electrode, characterized in that, The modified PEDOT:PSS film according to any one of claims 1 or 2, or the modified PEDOT:PSS film prepared by the preparation method according to any one of claims 3-6.

8. A flexible supercapacitor, characterized in that, The flexible supercapacitor includes the flexible electrode as described in claim 7.

9. The flexible supercapacitor according to claim 8, characterized in that, The flexible supercapacitor has an area energy density of 32.8 μWh / cm² at a power density of 1.2 mW / cm².

10. The application of the modified PEDOT:PSS film according to any one of claims 1 or 2, or the modified PEDOT:PSS film prepared by the preparation method according to any one of claims 3-6, in flexible electronics, wearable devices, flexible energy storage devices, and foldable screen terminals.