Flame retardant composition comprising a recycled polycarbonate and polybutylene terephthalate blend
By combining polycarbonate, PCR polybutylene terephthalate and polycarbonate-siloxane copolymer in specific proportions, and adding phosphazene flame retardant and silicone oil, the balance between flame retardancy, impact strength and heat distortion temperature of thermoplastic compositions in consumer electronics has been solved, achieving efficient and sustainable material applications.
Patent Information
- Application Number
- CN202611358391.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2020-07-24
- Filing Date
- 2021-07-22
- Publication Date
- 2026-11-24
AI Technical Summary
Existing thermoplastic compositions struggle to achieve a good balance of flame retardancy, impact strength, and heat distortion temperature in consumer electronics. Furthermore, their properties are limited when using recycled polymer materials, and flame retardant additives can be detrimental to these properties.
A thermoplastic composition is formed by combining approximately 10-65% virgin polycarbonate, 10-40% PCR polybutylene terephthalate, 25-65% PCR polycarbonate, 10-40% polycarbonate-siloxane copolymer, 0.1-10% phosphazene flame retardant, and 0.1-2% silicone oil.
A composition exhibiting good flame retardancy and high notched cantilever beam impact strength at -10°C was achieved, with an increased heat distortion temperature to meet the sustainability requirements of consumer electronics products.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
[0001] This application is a divisional application of the patent application filed on July 22, 2021, with application number 202180064178.0 and invention title: "Flame-retardant composition comprising a blend of recycled polycarbonate and polybutylene terephthalate". Technical Field
[0002] This disclosure relates to thermoplastic compositions comprising resins derived from at least two post-consumer recycled (PCR) polymers, having improved impact and flame retardant properties. Background Technology
[0003] Thermoplastic compositions comprising polycarbonate and polyester blends are popular in the consumer electronics market because they offer a balance of impact resistance, chemical resistance, and flowability. Polycarbonate copolymers can be added to further enhance the chemical resistance and improve the ductility of the compositions. Flame retardant additives can also be incorporated to improve flame retardancy for consumer electronics applications. Unfortunately, these additional additives, especially flame retardants, have been found to have detrimental effects on certain properties, such as impact strength and heat distortion temperature (HDT). Identifying compositions that achieve a good balance of all these properties is a challenge.
[0004] Furthermore, it is increasingly important for consumer electronics to be formed from more sustainable or “greener” materials to reduce their environmental impact. One way to reduce the footprint of thermoplastic compositions used in such applications is to use post-consumer recycled (PCR) polymers as raw materials for the thermoplastic compounds in said compositions. For example, polybutylene terephthalate (PBT) can be made from post-consumer recycled polyethylene terephthalate (PET). Examples of such PBT plastics are available from SABIC and are known as “iQ PBT” resin. Further, PCR-polycarbonate (PC) can be used in such compositions. Unfortunately, PCR resins such as iQ PBT and PCR-PC have limitations, making it even more challenging to identify compositions with a good balance of properties such as flame retardancy / flame toughness, impact resistance, and thermal properties.
[0005] These and other shortcomings are addressed through the aspects of this disclosure. Summary of the Invention
[0006] Aspects of this disclosure relate to thermoplastic compositions comprising: (a) about 10% to about 65% by weight of at least one virgin polycarbonate; (b) about 10% to about 40% by weight of a polybutylene terephthalate (PBT) component derived from a post-consumption recycled (PCR) polymer; (c) about 25% to about 65% by weight of at least one PCR polycarbonate; (d) about 10% to about 40% by weight of a polycarbonate-siloxane (PC-Si) copolymer; (e) 0.1% to about 10% by weight of a phosphazene flame retardant; and (f) 0.1% to about 2% by weight of a silicone oil.
[0007] This disclosure further relates to articles comprising the thermoplastic composition, the thermoplastic composition including components of consumer electronics products.
[0008] This invention includes the following: 1. A thermoplastic composition comprising: (a) about 10% by weight to about 65% by weight of at least one virgin polycarbonate; (b) About 10% by weight to about 40% by weight of polybutylene terephthalate (PBT) component derived from post-consumption recycled (PCR) polymers; (c) about 25% by weight to about 65% by weight of at least one PCR polycarbonate; (d) about 10% by weight to about 40% by weight of polycarbonate-siloxane (PC-Si) copolymer; (e) 0.1% by weight to about 10% by weight of phosphazene flame retardant; and (f) 0.1% by weight to about 2% by weight of silicone oil.
[0009] The combined weight percentage of all components does not exceed 100% by weight, and all weight percentages are based on the total weight of the complex.
[0010] 2. The thermoplastic composition according to Embodiment 1, wherein the PBT component is obtained from PCR polyethylene terephthalate (PET).
[0011] 3. The thermoplastic composition according to embodiment 1 or 2, wherein the PC-Si copolymer has a siloxane content of about 5% to about 45% by weight.
[0012] 4. The thermoplastic composition according to any one of embodiments 1 to 3, wherein the PC-Si copolymer has a siloxane content of about 15% to about 25% by weight.
[0013] 5. The thermoplastic composition according to any one of embodiments 1 to 4, wherein the PC-Si copolymer has a siloxane content of about 20% by weight.
[0014] 6. The thermoplastic composition according to any one of embodiments 1 to 5, wherein the composition further comprises more than 0% by weight to about 2% by weight of an anti-drip agent, wherein the anti-drip agent comprises polytetrafluoroethylene (PTFE) encapsulated in styrene-acrylonitrile (SAN).
[0015] 7. The thermoplastic composition according to any one of embodiments 1 to 6, wherein the composition further comprises more than 0% by weight to about 2% by weight of an epoxy impact modifier.
[0016] 8. The thermoplastic composition according to Embodiment 7, wherein the epoxy impact modifier comprises a terpolymer containing ethylene, acrylate and glycidyl methacrylate.
[0017] 9. The thermoplastic composition according to any one of embodiments 1 to 8, wherein the composition further comprises more than 0% by weight to about 5% by weight of at least one stabilizer, wherein the at least one stabilizer includes a UV stabilizer, a zinc phosphate stabilizer, or a combination thereof.
[0018] 10. The thermoplastic composition according to any one of embodiments 1 to 9, wherein the at least one PCR polycarbonate contains at least 10 mol% of -OH end groups.
[0019] 11. The thermoplastic composition according to embodiment 10, wherein the at least one PCR polycarbonate comprises 10 mol% to about 35 mol% of -OH end groups.
[0020] 12. The thermoplastic composition according to any one of embodiments 1 to 11, wherein the composition has a flame retardancy of V0 at a thickness of 1.5 mm or less when measured according to UL94.
[0021] 13. The thermoplastic composition according to any one of embodiments 1 to 12, wherein the composition has: (1) flame retardancy of V0 at a thickness of at least 1.5 mm as determined according to UL94, and (2) a notched cantilever beam impact strength of at least 690 joules / meter and 100% ductility at a temperature of -10°C or lower, as determined according to ASTM D256.
[0022] 14. The thermoplastic composition according to any one of embodiments 1 to 13, wherein the composition has: (1) flame retardancy of V0 at a thickness of at least 1.5 mm, and (2) a heat distortion temperature of at least 85°C, which is determined according to ASTM D648 at 1.82 MPa for a sample with a thickness of 3.2 mm.
[0023] 15. An article comprising the composition according to any one of embodiments 1 to 14, wherein the article is a component of a consumer electronic product. Detailed Implementation
[0024] This disclosure relates to thermoplastic compositions of impact-modified flame-retardant PC / PBT compounds, comprising iQ PBT formed from PCR-PET. The compositions offer a good balance of chemical resistance, flame retardancy, and impact properties, and also meet market expectations regarding sustainability.
[0025] This disclosure can be more readily understood by referring to the following detailed description and examples included in this disclosure. In several aspects, this disclosure relates to thermoplastic compositions comprising: (a) about 10% to about 65% by weight of at least one virgin polycarbonate; (b) about 10% to about 40% by weight of a polybutylene terephthalate (PBT) component derived from a post-consumption recycled (PCR) polymer; (c) about 25% to about 65% by weight of at least one PCR polycarbonate; (d) about 10% to about 40% by weight of a polycarbonate-siloxane (PC-Si) copolymer; (e) 0.1% to about 10% by weight of a phosphazene flame retardant; and (f) 0.1% to about 2% by weight of a silicone oil.
[0026] Before disclosing and describing the compounds, compositions, articles, systems, devices, and / or methods of the present invention, it should be understood that, unless otherwise stated, they are not limited to specific synthetic methods, or, unless otherwise stated, are not limited to specific reagents, as these can certainly vary. It should also be understood that the terminology used herein is for descriptive purposes only and is not intended to be limiting.
[0027] This disclosure covers various combinations of elements of this disclosure, such as combinations of elements from dependent claims that are subordinate to the same independent claim.
[0028] Furthermore, it should be understood that, unless expressly stated otherwise, no method described herein is intended to be construed as requiring its steps to be performed in a particular order. Therefore, no order is intended to be inferred in any respect where a method claim does not actually describe the order in which its steps are to be followed, or where the claims or specification do not otherwise specifically state that the steps are limited to a particular order. This applies to any possible non-express basis of interpretation, including: logical questions concerning the arrangement of steps or procedures; general meanings derived from grammatical organization or punctuation; and the number or type of aspects described in the specification.
[0029] All publications mentioned in this article are incorporated herein by reference to disclose and describe the methods and / or materials described in the cited publications.
[0030] definition
[0031] It should also be understood that the terminology used herein is for descriptive purposes only and is not intended to be limiting. As used in the specification and claims, the term "comprising" may include aspects "consisting of" and "substantially consisting of". Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this disclosure pertains. Many terms defined herein will be referenced in this specification and in the appended claims.
[0032] As used in the specification and appended claims, the singular forms “(indefinite article) an (a, an)” and “the” include a plural indicator unless the context clearly specifies otherwise. Thus, for example, reference to “silicone oil” includes a mixture of two or more silicone oils.
[0033] As used herein, the term "composite" includes blends, mixtures, alloys, reaction products, etc.
[0034] A range may be expressed herein as a range from one value (first value) to another value (second value). When expressing such a range, the range includes, in some respects, one or both of the first value and the second value. Similarly, when a value is expressed as an approximation using the antecedent “about,” it will be understood that the specific value forms another aspect. It will be further understood that the endpoints of each range are significant relative to and independent of the other endpoints. It is also understood that many values are disclosed herein, and each value is also disclosed herein as “about” that specific value, in addition to being the value itself. For example, if the value “10” is disclosed, then “about 10” is also disclosed. It is also understood that each unit between two specific units is also disclosed. For example, if 10 and 15 are disclosed, then 11, 12, 13, and 14 are also disclosed.
[0035] As used herein, the terms “about” and “in (for) or about” mean that the quantity or value in question may be a specified value, approximately the specified value, or approximately the same as the specified value. As used herein, it is generally understood that, unless otherwise indicated or inferred, nominal values represent ±10% variation. This term is intended to convey that similar values promote equivalent results or effects enumerated in the claims. That is, it is understood that quantities, dimensions, formulations, parameters, and other quantities and characteristics are not and do not need to be precise, but may be approximate and / or larger or smaller as required, reflecting tolerances, conversion factors, rounding, measurement errors, and other factors known to those skilled in the art. Generally, quantities, dimensions, formulations, parameters, or other quantities or characteristics are “about” or “approximate”, whether or not explicitly stated so. It is understood that where “about” is used before a quantity value, unless otherwise specifically stated, the parameter also includes the specific quantity value itself.
[0036] The components to be used in preparing the compositions disclosed herein, as well as the compositions themselves to be used in the methods disclosed herein, are disclosed herein. These and other materials are disclosed herein, and it is understood that when combinations, subsets, interactions, groups, etc., of these materials are disclosed, each is specifically considered and described herein, although not explicitly mentioned in detail, as every different individual and collective combination and arrangement of these compounds is not explicitly disclosed. For example, if a particular compound is disclosed and discussed, and many modifications that can be made to a number of molecules including said compound are discussed, then every combination and arrangement of said compounds and possible modifications are specifically considered, unless explicitly stated otherwise. Thus, if a class of molecules A, B, and C and a class of molecules D, E, and F are disclosed, and an example of a combination of molecules AD is disclosed, then each is considered individually and collectively, even if not individually enumerated, meaning that combinations AE, AF, BD, BE, BF, CD, CE, and CF are considered disclosed. Similarly, any subset or combination of these is also disclosed. Thus, for example, subgroups of AE, BF, and CE would be considered disclosed. This concept applies to all aspects of this application, including but not limited to the steps in methods for preparing and using the compositions disclosed herein. Therefore, if there are various additional steps that can be performed, it is understood that each of these additional steps can be performed using any particular aspect or combination of aspects of the methods of this disclosure.
[0037] The reference to parts by weight of a specific element or component in the composition or article, as mentioned in the specification and the final claims, indicates the weight relationship between that element or component and any other element or component, expressed in parts by weight. Therefore, in a compound containing 2 parts by weight of component X and 5 parts by weight of component Y, X and Y are present in a 2:5 weight ratio, and in this ratio regardless of whether the compound contains any other components.
[0038] Unless otherwise stated, the weight percentages of components are based on the total weight of formulations or compositions that include said components.
[0039] As used in this article, the terms "number-average molecular weight" or "M" are used in conjunction with other terms. n "These terms are interchangeable and refer to the statistical average molecular weight of all polymer chains in the sample, defined by the following formula:"
[0040] Where M i It is the molecular weight of the chain, and N i This refers to the number of chains at that molecular weight. The M of a polymer, such as a polycarbonate polymer, can be determined using methods well known to those skilled in the art, using molecular weight standards, such as polycarbonate standards or polystyrene standards, preferably certified or traceable molecular weight standards. n .
[0041] As used herein, the interchangeable terms “BisA,” “BPA,” or “bisphenol A” refer to compounds having a structure represented by the following formula:
[0042] BisA can also be referred to as 4,4'-(propane-2,2-diyl)diphenol, p,p'-isopropylidene bisphenol, or 2,2-bis(4-hydroxyphenyl)propane. BisA has CAS # 80-05-7.
[0043] As used herein, “polycarbonate” refers to an oligomer or polymer comprising residues of one or more dihydroxy compounds, such as dihydroxy aromatic compounds, linked by carbonate bonds; it also encompasses homopolymers, copolymers, and (co)polyesters.
[0044] The terms “residue” and “structural unit” used in relation to the components of the polymer are synonymous throughout this specification.
[0045] As used herein, unless otherwise stated, the terms "weight percentage," "weight % (wt.%)," and "weight % (wt.%)" are interchangeable and represent the weight percentage of a given component based on the total weight of the composition. That is, unless otherwise stated, all weight % values are based on the total weight of the composition. It should be understood that the sum of the weight % values of all components in the disclosed compositions or formulations equals 100.
[0046] Unless otherwise stated herein, all testing standards are current and valid at the time of filing of this application.
[0047] Each material disclosed herein is available and / or the method of preparing it is known to those skilled in the art.
[0048] It is understood that the compositions disclosed herein have certain functions. Certain structural requirements for performing the disclosed functions are disclosed herein, and it is understood that various structures exist that can perform the same functions associated with the disclosed structures, and these structures will generally achieve the same results.
[0049] thermoplastic composition
[0050] Aspects of this disclosure relate to thermoplastic compositions comprising: (a) about 10% to about 65% by weight of at least one virgin polycarbonate; (b) about 10% to about 40% by weight of a polybutylene terephthalate (PBT) component derived from a post-consumption recycled (PCR) polymer; (c) about 25% to about 65% by weight of at least one PCR polycarbonate; (d) about 10% to about 40% by weight of a polycarbonate-siloxane (PC-Si) copolymer; (e) 0.1% to about 10% by weight of a phosphazene flame retardant; and (f) 0.1% to about 2% by weight of a silicone oil.
[0051] As used herein, virgin polycarbonate is polycarbonate derived from petrochemical sources; virgin polycarbonate does not include recycled polycarbonate content. Polycarbonate may include polycarbonate copolymers.
[0052] The polybutylene terephthalate (PBT) component is derived from a PCR polymer. In some aspects, the PBT component is derived from PCR polyethylene terephthalate (PET). The PBT component derived from the PCR polymer (e.g., PCR PET) can be formed according to conventional methods and may include iQ PBT plastic available from SABIC. In some aspects, the composition comprises about 10% to about 20% by weight of the PBT component derived from the PCR polymer. The PBT component may include a PBT copolymer.
[0053] The composition further includes about 25% to about 65% by weight of at least one PCR polycarbonate. The PCR polycarbonate may be formed according to conventional methods and may include PCR-PC available from SABIC. The PCR-PC component may include copolymers containing PCR-PC. Recycled (e.g., PCR) polycarbonate can be distinguished from virgin polycarbonate by including at least 10 mol% of -OH end groups in the polycarbonate. In some aspects, the PCR polycarbonate includes 10 mol% to about 35 mol% of -OH end groups in the polycarbonate. The -OH end group content of the PCR PC can be determined according to conventional methods known to those skilled in the art. The recycled PC may be clear or colored. Clear recycled PC may be derived from, for example, water bottles, recycled PC sheets, automotive headlights, and optical discs (e.g., one or more of compact discs (CDs), digital universal discs (DVDs), and Blu-ray discs). An exemplary source of colored PC is a water bottle.
[0054] PC-Si copolymers may include, but are not limited to, PC-Si copolymers with a siloxane content of about 5% to about 45% by weight. In a further aspect, the PC-Si copolymer has a siloxane content of about 15% to about 25% by weight, or about 20% by weight. Exemplary PC-Si copolymers include SABIC EXL copolymers.
[0055] The phosphazene used in the flame retardant composition is an organic compound having a —P═N— bond in its molecule. In one embodiment, the phosphazene is a cyclic phenoxyphosphazene represented by the following formula:
[0056] In the formula, m represents an integer from 3 to 25, P represents phenyl, R1 and R2 are the same or different, and are independently hydrogen, hydroxyl, C 1-12 Alkoxy or C 1-12 Alkyl group. In some respects, m is an integer from 2 to 10, or in certain respects, an integer from 3 to 8.
[0057] The composition comprises 0.1% by weight to about 2% by weight of silicone oil. An exemplary silicone oil is SFR100, which is available from Momentive Performance Materials.
[0058] In some aspects, the composition further comprises greater than 0% by weight to about 2% by weight of an anti-drip agent. A purely exemplary anti-drip agent is polytetrafluoroethylene (PTFE) encapsulated in styrene-acrylonitrile (SAN).
[0059] In one aspect, the composition comprises greater than 0% to about 2% by weight of an epoxy impact modifier. The epoxy impact modifier may include, but is not limited to, a terpolymer comprising ethylene, acrylate, and glycidyl methacrylate. In other aspects, the composition comprises greater than 0% to about 5% by weight of at least one stabilizer. The at least one stabilizer may include, but is not limited to, a UV stabilizer, a zinc phosphate stabilizer, or a combination thereof.
[0060] Properties of thermoplastic compositions
[0061] The thermoplastic compositions according to aspects of this disclosure have improved properties compared to comparative / reference compositions that do not include phosphazene flame retardants or silicone oils. Specifically, in some aspects, the compositions have improved notched cantilever beam (Izod) impact strength, as determined according to ASTM D256 and ASTM D4812, compared to comparative compositions that do not include phosphazene flame retardants. In some aspects, the notched cantilever beam impact strength is improved by at least 50%, or at least 75%, or at least 100%, or at least 150%, or at least 200%, or at least 250%, or at least 500%, or at least 600%, or at least 700%, or at least 800%, or up to 1500%, or 50-1500%, or 75-1500%. The comparative compositions described in aspects of this disclosure may include bisphenol A bis(diphenyl phosphate) (BPADP) instead of phosphazene flame retardants. BPADP has the following chemical formula:
[0062] In a further aspect, compared to a comparative composition excluding phosphazene flame retardants, the composition exhibits improved notched cantilever beam impact strength at 0°C or -10°C (low temperature), as determined according to ASTM D256 and ASTM D4812. In a specific aspect, compared to a comparative composition excluding phosphazene flame retardants, the composition exhibits a low-temperature notched cantilever beam impact strength that is improved by at least 50%, or at least 100%, or at least 250%, or at least 500%, or at least 600%, or at least 700%, or at least 1000%, or up to 1500%, or 50-1500%, or 100-1500%, or 250-1500%, or 500-1500%.
[0063] In some aspects, the composition has an improved heat distortion temperature (HDT) compared to a comparative composition that does not contain phosphazene flame retardants, as determined according to ASTM D648. In a further aspect, the HDT is improved by at least 10%, or at least 12%, or at least 14%, or at least 16%, or at least 18%, or at least 20%, or at least 25%, or up to 50%, or 10-50%, or 12-50%, compared to a comparative composition that does not contain phosphazene flame retardants.
[0064] In a specific aspect, the composition exhibits improved flame retardancy, as determined according to UL94, compared to a comparative composition excluding phosphazene flame retardants. Specifically, compared to a comparative composition excluding phosphazene flame retardants, the flame retardancy (V1 or V2 burning time, in seconds) is reduced by at least 8%, or at least 10%, or at least 15%, or at least 20%, or at least 30%, or at least 40%, or up to 50%, or 8-50%, or 10-50%. In a further aspect, the composition exhibits a V0 flame retardancy at a thickness of 1.5 mm or less, or at a thickness of 3.0 mm or less, as determined according to UL94.0.
[0065] In some respects, the composition exhibits improved flame retardancy compared to a comparative composition excluding silicone oil, as determined according to UL94. In a further respect, the flame retardancy (V1 or V2 burning time, in seconds) is reduced by at least 20%, or at least 25%, or at least 30%, or at least 35%, or at least 50%, or up to 100%, or 20-100%, or 20-50%, compared to a comparative composition excluding silicone oil.
[0066] In some aspects, the thermoplastic composition has: (1) a flame retardancy of V0 at a thickness of at least 1.5 mm, as determined according to UL94, and (2) a notched cantilever beam impact strength of at least 690 J / m at a temperature of -10°C or lower, and 100% ductility, as determined according to ASTM D256. In a further aspect, the composition has: (1) a flame retardancy of V0 at a thickness of at least 1.5 mm, and (2) a heat distortion temperature of at least 85°C, as determined according to ASTM D648 at 1.82 MPa for a sample with a thickness of 3.2 mm.
[0067] Manufacturing method
[0068] One or any of the aforementioned components described herein may first be dry-mixed with each other, or with any combination of the aforementioned components, and then fed into the extruder from one or more feeders, or fed into the extruder individually from one or more feeders. Fillers (if included) used in the composition may also be first processed into a masterbatch and then fed into the extruder. Components may be fed into the extruder from a throat hopper or any side feeder.
[0069] The extruder used in this disclosure may be a single screw, a multi-screw, intermeshing screws rotating in the same or opposite directions, non-intermeshing screws rotating in the same or opposite directions, a reciprocating screw, screws with pins, screws with screens, pinned cylinders, rollers, rams, helical rotors, co-kneaders, disc-pack processors, various other types of extrusion equipment, or combinations including at least one of the foregoing.
[0070] The components may also be mixed together and then melt-blended to form the thermoplastic composition. Melt blending of the components involves the use of shear force, tensile force, compressive force, ultrasonic energy, electromagnetic energy, thermal energy, or a combination including at least one of the foregoing forms of force or energy.
[0071] If the resin is a semi-crystalline organic polymer, the barrel temperature on the extruder during compounding can be set at a temperature at which at least a portion of the polymer has reached a temperature greater than or equal to approximately the melt temperature; or if the resin is an amorphous resin, the barrel temperature on the extruder during compounding can be set at the flow point (e.g., the glass transition temperature).
[0072] If desired, the mixture comprising the aforementioned components can undergo multiple blending and forming steps. For example, the thermoplastic composition can first be extruded and formed into pellets. The pellets can then be fed into a molding machine, where they can be formed into any desired shape or product. Alternatively, the thermoplastic composition emitted from a single melt blender can be formed into sheets or strips and subjected to post-extrusion processes such as annealing, uniaxial or biaxial orientation.
[0073] In some respects, the melt temperature in this method is kept as low as possible to avoid excessive thermal degradation of the components. In some respects, the melt temperature is maintained between about 230°C and about 350°C, although higher temperatures may be used, provided the residence time of the resin in the processing equipment remains relatively short. In some respects, the melt-processed composition exits the processing equipment, such as an extruder, through a small outlet orifice in the die. The resulting strand of molten resin can be cooled by passing it through a water bath. The cooled strand can be cut into granules for packaging and further handling.
[0074] Manufacturing of products
[0075] In some aspects, this disclosure relates to articles comprising the thermoplastic composition that have been shaped, molded, or molded. The thermoplastic composition can be molded into useful tangible articles by various means such as injection molding, extrusion, rotational molding, blow molding, and thermoforming to form articles and structural components such as: personal or commercial electronic devices, including but not limited to cellular phones, tablet computers, personal computers, laptops, and portable computers, and other such devices; medical applications; RFID applications; automotive applications; etc. In a further aspect, the article is extruded. In yet another further aspect, the article is injection molded.
[0076] In certain respects, the article is a component of a consumer electronics product.
[0077] This disclosure covers various combinations of elements of this disclosure, such as combinations of elements from dependent claims that are subordinate to the same independent claim.
[0078] Aspects of publicly disclosed content
[0079] In several respects, this disclosure relates to and includes at least the following aspects.
[0080] Aspect 1. A thermoplastic composition comprising, consisting of, or substantially consisting of the following: (a) about 10% by weight to about 65% by weight of at least one virgin polycarbonate; (b) About 10% by weight to about 40% by weight of polybutylene terephthalate (PBT) component derived from post-consumption recycled (PCR) polymers; (c) about 25% by weight to about 65% by weight of at least one PCR polycarbonate; (d) about 10% by weight to about 40% by weight of polycarbonate-siloxane (PC-Si) copolymer; (e) 0.1% by weight to about 10% by weight of phosphazene flame retardant; and (f) 0.1% by weight to about 2% by weight of silicone oil, The combined weight percentage of all components does not exceed 100% by weight, and all weight percentages are based on the total weight of the complex.
[0081] Aspect 2. The thermoplastic composition according to aspect 1, wherein the PBT component is derived from PCR polyethylene terephthalate (PET).
[0082] Aspect 3. The thermoplastic composition according to aspect 1 or 2, wherein the PC-Si copolymer has a siloxane content of about 5% to about 45% by weight.
[0083] Aspect 4. The thermoplastic composition according to any one of aspects 1 to 3, wherein the PC-Si copolymer has a siloxane content of about 15% to about 25% by weight.
[0084] Aspect 5. The thermoplastic composition according to any one of Aspects 1 to 4, wherein the PC-Si copolymer has a siloxane content of about 20% by weight.
[0085] Aspect 6. The thermoplastic composition according to any one of aspects 1 to 5, wherein the silicone oil comprises organosilicon.
[0086] Aspect 7. The thermoplastic composition according to any one of Aspects 1 to 6, wherein the phosphazene is a cyclic phenoxyphosphazene represented by the following formula:
[0087] Where m represents an integer from 3 to 25, P represents phenyl, R1 and R2 are the same or different, and are independently hydrogen, hydroxyl, or C. 1-12 Alkoxy or C 1-12 alkyl.
[0088] Aspect 8. The thermoplastic composition according to any one of aspects 1 to 7, wherein the composition further comprises more than 0% by weight to about 2% by weight of an anti-drip agent.
[0089] Aspect 9. The thermoplastic composition according to aspect 8, wherein the anti-drip agent comprises polytetrafluoroethylene (PTFE) encapsulated in styrene-acrylonitrile (SAN).
[0090] Aspect 10. The thermoplastic composition according to any one of aspects 1 to 9, wherein the composition further comprises more than 0% by weight to about 2% by weight of an epoxy impact modifier.
[0091] Aspect 11. The thermoplastic composition according to aspect 10, wherein the epoxy impact modifier comprises a terpolymer comprising ethylene, acrylate and glycidyl methacrylate.
[0092] Aspect 12. The thermoplastic composition according to any one of aspects 1 to 11, wherein the composition further comprises at least one stabilizer of more than 0% by weight to about 5% by weight.
[0093] Aspect 13. The thermoplastic composition according to aspect 12, wherein the at least one stabilizer comprises a UV stabilizer, a zinc phosphate stabilizer, or a combination thereof.
[0094] Aspect 14. The thermoplastic composition according to any one of Aspects 1 to 13, wherein the composition has improved notched cantilever beam impact strength, as determined according to ASTM D256 and ASTM D4812, compared to a comparative composition excluding phosphazene flame retardants.
[0095] Aspect 15. The thermoplastic composition according to any one of Aspects 1 to 14, wherein the composition has improved notched cantilever beam impact strength at 0°C or -10°C, as determined according to ASTM D256 and ASTM D4812, compared to a comparative composition excluding phosphazene flame retardants.
[0096] Aspect 16. The thermoplastic composition according to any one of Aspects 1 to 15, wherein the composition has an improved heat distortion temperature (HDT) as determined according to ASTM D648, compared with a comparative composition excluding a phosphazene flame retardant.
[0097] Aspect 17. The thermoplastic composition according to any one of Aspects 1 to 16, wherein the composition has improved flame retardancy, as determined according to UL94, compared with a comparative composition excluding phosphazene flame retardants.
[0098] Aspect 18. The thermoplastic composition according to any one of aspects 1 to 17, wherein the composition has improved flame retardancy, as determined according to UL94, compared with a comparative composition excluding silicone oil.
[0099] Aspect 19. Article comprising the composition according to any one of aspects 1 to 18.
[0100] Aspect 20. The article of manufacture according to aspect 19, wherein the article of manufacture is a component of a consumer electronic product.
[0101] Aspect 21. A thermoplastic composition comprising: (a) about 10% by weight to about 65% by weight of at least one virgin polycarbonate; (b) About 10% by weight to about 40% by weight of polybutylene terephthalate (PBT) component derived from post-consumption recycled (PCR) polymers; (c) about 25% by weight to about 65% by weight of at least one PCR polycarbonate; (d) about 10% by weight to about 40% by weight of polycarbonate-siloxane (PC-Si) copolymer; (e) 0.1% by weight to about 10% by weight of phosphazene flame retardant; and (f) 0.1% by weight to about 2% by weight of silicone oil, The combined weight percentage of all components does not exceed 100% by weight, and all weight percentages are based on the total weight of the complex.
[0102] Aspect 22. The thermoplastic composition according to aspect 21, wherein the PBT component is derived from PCR polyethylene terephthalate (PET).
[0103] Aspect 23. The thermoplastic composition according to aspect 21 or 22, wherein the PC-Si copolymer has a siloxane content of about 5% to about 45% by weight.
[0104] Aspect 24. The thermoplastic composition according to any one of aspects 21 to 23, wherein the PC-Si copolymer has a siloxane content of about 15% to about 25% by weight.
[0105] Aspect 25. The thermoplastic composition according to any one of aspects 21 to 24, wherein the PC-Si copolymer has a siloxane content of about 20% by weight.
[0106] Aspect 26. The thermoplastic composition according to any one of aspects 21 to 25, wherein the composition further comprises more than 0% by weight to about 2% by weight of an anti-drip agent, wherein the anti-drip agent comprises polytetrafluoroethylene (PTFE) encapsulated in styrene-acrylonitrile (SAN).
[0107] Aspect 27. The thermoplastic composition according to any one of aspects 21 to 26, wherein the composition further comprises more than 0% by weight to about 2% by weight of an epoxy impact modifier.
[0108] Aspect 28. The thermoplastic composition according to aspect 27, wherein the epoxy impact modifier comprises a terpolymer comprising ethylene, acrylate and glycidyl methacrylate.
[0109] Aspect 29. The thermoplastic composition according to any one of aspects 21 to 28, wherein the composition further comprises more than 0% by weight to about 5% by weight of at least one stabilizer, wherein the at least one stabilizer comprises a UV stabilizer, a zinc phosphate stabilizer, or a combination thereof.
[0110] Aspect 30. The thermoplastic composition according to any one of aspects 21 to 29, wherein the at least one PCR polycarbonate contains at least 10 mol% of -OH end groups.
[0111] Aspect 31. The thermoplastic composition according to aspect 30, wherein the at least one PCR polycarbonate comprises 10 mol% to about 35 mol% of -OH end groups.
[0112] Aspect 32. The thermoplastic composition according to any one of aspects 21 to 31, wherein the composition has a flame retardancy of V0 at a thickness of 1.5 mm or less when measured according to UL94.
[0113] Aspect 33. The thermoplastic composition according to any one of Aspects 21 to 32, wherein the composition has: (1) flame retardancy of V0 at a thickness of at least 1.5 mm as determined according to UL94, and (2) a notched cantilever beam impact strength of at least 690 joules / meter and 100% ductility at a temperature of -10°C or lower, as determined according to ASTM D256.
[0114] Aspect 34. The thermoplastic composition according to any one of aspects 21 to 33, wherein the composition has: (1) flame retardancy of V0 at a thickness of at least 1.5 mm, and (2) a heat distortion temperature of at least 85°C, which is determined according to ASTM D648 at 1.82 MPa for a sample having a thickness of 3.2 mm.
[0115] Aspect 35. Article comprising the composition according to any one of aspects 21 to 34, wherein the article is a component of a consumer electronic product.
[0116] Example
[0117] The following examples are provided to provide those skilled in the art with a complete disclosure and description of how to prepare and evaluate the compounds, compositions, articles, apparatus, and / or methods claimed herein, and are intended to be purely exemplary and not to limit the scope of this disclosure. Efforts have been made to ensure the accuracy of figures (e.g., amounts, temperatures, etc.), but some errors and deviations should be taken into account. Unless otherwise stated, parts are parts by weight, temperatures are in °C or ambient temperature, and pressures are at or near atmospheric pressure. Unless otherwise stated, percentages relating to compositions are expressed as % by weight.
[0118] Reaction conditions, such as component concentrations, desired solvents, solvent mixtures, temperature, pressure, and other reaction ranges and conditions that can be used to optimize the purity and yield of the product obtained from the described method, have many variations and combinations. Only reasonable and routine experiments will be needed to optimize such process conditions.
[0119] The materials used in the comparative and example compositions described in this article are listed in Table 1: Table 1 – Materials
[0120] The composition was formulated into granules using conventional methods. The resin and all additives except BPADP were premixed and fed through the main throat; BPADP (if included) was fed downstream of the extruder. The composition was formulated using an output of 40 kg / hr, a screw speed of 350 rpm, a vacuum of 0.08 MPa, 50-65% torque, a barrel temperature of 250-255°C, and a die temperature of 255°C.
[0121] Inject the granules according to the conditions given in Table 2: Table 2 - Injection Molding Parameters
[0122] Tensile properties were measured using the ASTM D638 method at a test speed of 5 mm / min. Impact strength was evaluated at room temperature using a pendulum energy (PE) of 5 lbf / ft, according to ASTM D256 and ASTM D4812. Flexural properties were measured using the ASTM D790 method at a test speed of 1.27 mm / min with a part thickness of 3.2 mm. Density was measured using the immersion method for solid plastic parts according to ASTM D792. Melt volumetric rate (MVR) was measured using granular samples dried at 90°C for 4 hours, according to ASTM D1238. Heat deflection temperature (HDT) was measured using the ASTM D648 method at a stress of 1.82 MPa or 0.45 MPa with a part thickness of 3.2 mm. Water absorption of the plastic was tested using the GEP method by immersing the part in water at room temperature for 48 hours.
[0123] Table 3 lists the comparative and example compositions developed to evaluate the effect of replacing virgin PBT (C1) with recycled PBT (iQ PBT). Different FR components (PPZ and BPADP) were also evaluated. All values provided in this table and other tables listing the compositions and their components are provided as weight percentages (wt%). Table 3 – Comparative and Example Compositions
[0124] The various properties of the compositions in Table 3 were evaluated; the results are provided in Table 4: Tables 4-3 Properties of the Compositions
[0125] From the results in Table 4, by comparing C1 and Ex1, it was observed that replacing the original PBT with iQ PBT resulted in a decrease in notched impact strength and a reduction in average elongation from 88% to 60%. The results indicate that compositions including recycled resin components are more sensitive to notched impact strength than those including virgin resin.
[0126] To address this issue, potential solutions were evaluated, including the use of epoxy-based impact modifiers and / or more neutral FR additives (e.g., phosphazenes). These compositions were evaluated in Ex2 and Ex3. Ex2 included 1% Lotader® AX8900 (which contains epoxy functional groups) as an impact modifier. As observed, a slight increase in impact strength was observed without adversely affecting FR performance. Other properties were comparable. Ex3 included PPZ as an FR additive; a significant increase in cantilever beam impact strength—over 50%—was found compared to Ex1. After aging at room temperature for 1 month, the cantilever beam impact strength of the Ex1 composition decreased by 12%, while the cantilever beam impact strength of Ex3 remained unchanged. Overall, the impact performance (both notched cantilever beam impact strength and aging stability) was significantly improved when the composition included PPZ. Simultaneously, the thermal properties (HDT) of the Ex3 composition were also improved; the HDT of the Ex3 composition at 1.82 MPa was approximately 5°C higher than that of the Ex1 composition. Furthermore, the Ex3's FR robustness also improves with a shorter combustion time.
[0127] To further investigate the compositions, PCR-PC was included in the compositions shown in Table 5. Comparative composition C2 comprises PC and iQ PBT, with BPADP as the FR component; the formulation is similar to that of Ex1. Ex4 comprises PC and iQ PBT, with PPZ as the FR component; the formulation is similar to that of Ex3 but with a lower PPZ loading. Ex5 comprises two types of recycled resin – iQ PBT and PCR-PC. Ex6 is a PPZ-based formulation containing two types of recycled resin (iQ PBT) and PCR-PC.
[0128] Table 5 - Comparative and Example Compositions
[0129] The properties of the compositions in Table 5 are provided in Table 6: Tables 6-5 Properties of the Compositions
[0130] As confirmed in Table 6, a comparison of C2 and Ex4 shows that replacing BPADP with PPZ significantly improves notched impact strength, especially at lower temperatures. HDT also increases substantially (approximately 20%). Furthermore, the FR robustness of the Ex4 composition (a PPZ-based formulation) is improved, exhibiting a shorter burning time.
[0131] Comparing C2 with Ex5, as expected, a significant negative impact was observed on the cantilever beam impact strength, including the inclusion of recycled resin (PCR-PC). Even at room temperature, the impact strength decreased from 452 J / m to 86 J / m, completely losing its ductility. HDT also showed a decrease of approximately 3 °C.
[0132] For the PCR-PC and iQ PBT blends, PPZ was used in the Ex6 composition. It was observed that using PPZ as a FR additive resulted in improved robustness of the notched cantilever beam properties compared to the Ex5 composition, with both impact strength and HDT significantly improved. The notched cantilever beam impact robustness of the Ex6 PCR-PC and iQ PBT blends increased to the same level as Ex4 without PCR-PC.
[0133] Other exemplary compositions and their properties are shown in Table 7: Table 7 - Examples of Compositions
[0134] Comparing Ex7 with 6 wt% PPZ to Ex5 with 5 wt% PPZ, Ex7 exhibited more robust FR performance with a shorter ignition time (15 seconds). However, the thermal properties of this composition were reduced. Another approach (which included silicone oil) (Ex8) showed improved FR robustness and higher notched cantilever beam strength. Ex8 also had a slightly higher HDT. Furthermore, as shown in Ex9, using silicone oil as an FR synergist allowed for lower PPZ loading and EXL loading, thus permitting higher PCR-PC content loading (55 wt%), thereby providing improved sustainability benefits for the environment.
[0135] The foregoing description is intended to be illustrative and not restrictive. For example, the embodiments (or one or more aspects thereof) described above may be used in combination with each other. Other aspects may be used by one of ordinary skill in the art upon reading the foregoing description. An abstract is provided to conform to 37 CFR §1.72(b) to allow the reader to quickly determine the nature of the technical disclosure. By this understanding, it is considered that it will not be used to interpret or limit the scope or meaning of the claims. Furthermore, in the foregoing detailed description, various features may be grouped together to simplify the disclosure. This should not be construed as an intention that unclaimed features are essential to any claim. Rather, the subject matter of the invention may lie in fewer than all features of a specific disclosed aspect. Therefore, the appended claims are thus incorporated into the detailed description as examples or aspects, wherein each claim is an independent, separate aspect, and such aspects are contemplated to be combined with each other in various combinations or arrangements. The scope of this disclosure should be determined by reference to the appended claims and the full scope of their equivalents.
Claims
1. A thermoplastic composition comprising: (a) 10% to 65% by weight of a polycarbonate component, said polycarbonate component comprising at least one virgin polycarbonate and 25% to 65% by weight of at least one post-consumption recycled (PCR) polycarbonate. (b) 10% to 40% by weight of polybutylene terephthalate (PBT) component derived from PCR polymer; (c) 10% to 40% by weight of polycarbonate-siloxane (PC-Si) copolymer; (d) 0.1% to 10% by weight of phosphazene flame retardant; and (e) 0% to 2% by weight silicone oil, The composition described herein possesses: (1) a flame retardancy of V0 at a thickness of 1.5 mm, as determined according to UL94; and (2) a notched cantilever beam impact strength of at least 690 joules / m at a temperature of -10°C, as determined according to ASTM D256. The combined weight percentage of all components does not exceed 100% by weight, and all weight percentages are based on the total weight of the composition.
2. The thermoplastic composition according to claim 1, wherein the composition comprises 0.1% to 2% by weight of the silicone oil.
3. The thermoplastic composition according to claim 1, wherein the composition has 100% extensibility at a temperature of -10°C or lower, as determined according to ASTM D256.
4. The thermoplastic composition according to claim 1, wherein the PBT component is derived from PCR polyethylene terephthalate (PET).
5. The thermoplastic composition according to claim 1, wherein the PC-Si copolymer has a siloxane content of 15% to 25% by weight.
6. The thermoplastic composition according to any one of claims 1 to 5, wherein the composition further comprises more than 0% to 2% by weight of an anti-drip agent, wherein the anti-drip agent comprises polytetrafluoroethylene (PTFE) encapsulated in styrene-acrylonitrile (SAN).
7. The thermoplastic composition according to any one of claims 1 to 5, wherein the composition further comprises more than 0% to 2% by weight of an epoxy impact modifier, said epoxy impact modifier comprising a terpolymer comprising ethylene, acrylate and glycidyl methacrylate.
8. The thermoplastic composition according to any one of claims 1 to 5, wherein the composition further comprises more than 0% to 5% by weight of at least one stabilizer, wherein the at least one stabilizer includes a UV stabilizer, a zinc phosphate stabilizer, or a combination thereof.
9. The thermoplastic composition according to any one of claims 1 to 5, wherein the composition has a heat distortion temperature of at least 85°C, determined according to ASTM D648 at 1.82 MPa for a sample having a thickness of 3.2 mm.
10. An article comprising the composition according to any one of claims 1 to 5, wherein the article is a component of a consumer electronics product.