A method for preparing surface static electricity dissipating PEEK modified particles
By using the crushing, mixing, and granulation process of PEEK material, combined with carbon nanotubes and fillers, a uniform conductive network is constructed, which solves the problem that the resistivity is difficult to reduce to 10⁶-10⁹Ω/sq in the existing technology. This achieves static dissipation, reduces costs, and improves the stability and protection capability of the conductive network.
Patent Information
- Application Number
- CN202611656153.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-26
- Publication Date
- 2026-11-24
AI Technical Summary
Existing technologies cannot stably reduce the surface resistivity of PEEK materials to the dissipation range of 10⁶-10⁹Ω/sq while simplifying the process, leading to the risk of electrostatic accumulation and discharge, especially in semiconductor manufacturing where there are potential risks of particulate contamination and electrical breakdown.
PEEK raw materials are ground into fine powder using cryogenic pulverization, air jet milling, or mechanical pulverization. Untreated carbon nanotubes are mixed with PEEK fine powder, and then a process of primary granulation, crushing, grinding, and secondary granulation is carried out. Combined with carbon fiber powder, kaolin, glass fiber powder, or fumed silica filler, a uniform conductive network is constructed to form PEEK modified particles with surface electrostatic dissipation.
It achieves a dissipation range of surface resistivity from 10⁶ to 10⁹ Ω/sq, reducing costs and improving the uniformity and stability of the conductive network. It provides controlled micro-current discharge protection, avoids violent discharge pulses, and meets the electrostatic dissipation requirements of semiconductor manufacturing.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] This invention relates to the field of special engineering plastic modification technology, specifically to a method for preparing PEEK modified particles with surface electrostatic dissipation. Background Technology
[0002] In ultra-clean and highly electrostatically sensitive industrial environments such as advanced semiconductor wafer fabrication, microelectronic packaging and testing, flat panel displays, and aerospace, static electricity accumulation can lead to two types of serious accidents: first, electrostatic attraction (ESA) of tiny particles, resulting in wafer surface contamination and micro / nano pattern defects; second, electrostatic discharge (ESD), which can break down the semiconductor gate oxide layer or sensitive components at the nanosecond level, causing irreversible electrical breakdown hard failures or potential latent soft failures. Furthermore, in environments with volatile flammable gases or dust, intense electrostatic sparks can also pose a safety hazard of combustion and explosion.
[0003] ESD PEEK profiles are a special semi-finished engineering plastic material developed to overcome the insulation defects of pure resin. Its electrostatic dissipation mechanism relies on the construction of uniformly interconnected three-dimensional conductive pathways within the insulating matrix, enabling the material to possess both the inherent high and low temperature resistance and high mechanical rigidity of PEEK, while also having controllable charge leakage capability.
[0004] Based on electrostatic discharge kinetics, the surface resistivity of the electrostatic dissipation profile was strictly adjusted to 10. 6 -10 9 Within the dissipation range of Ω / sq. This range is different from that of metals or perfectly conductive materials (resistivity <10). 5 There is a fundamental difference between the two: if the material's conductivity is too high, the accumulated charge will instantly form a huge surge current that can break down the microcircuit; if the material is in the electrostatic dissipation region, the discharge circuit will maintain a constant and controlled microcurrent discharge, which can quickly decay the residual charge to zero and prevent the formation of violent discharge pulses. According to the capacitor discharge model, when the material's equivalent impedance is at a reasonable dissipation level, it can release and degrade the initial static voltage to a safe residual voltage within tens of milliseconds, thus providing a passive protection mechanism for advanced chip manufacturing.
[0005] The existing methods for implementing electrostatic dissipation / antistatic PEEK mainly include: First, partially carbonized carbon fiber type, such as the one disclosed in publication number CN110591329A, which uses a volume resistivity of 10 2 -10 5Compositions using partially carbonized carbon fiber powder or chopped carbon fibers to construct semiconductive networks (Ω·cm) rely on special carbonized fiber raw materials, limiting the source and batch consistency. Secondly, the two-step method for carbon nanotube masterbatch, such as the process disclosed in publications CN115558236A and CN121610054A (first preparing the masterbatch and then secondary blending), typically requires surface treatment of the carbon nanotubes, such as acidification, making the process complex. Thirdly, the single-stage granulation + side-feeding fiber process, such as publication CN121343349A, aims for an antistatic window rather than a lower resistivity dissipation window. None of these approaches can stably reduce the surface resistivity to 10 Ω·cm while simplifying the process. 6 -10 9 Ω / sq dissipation range. Summary of the Invention
[0006] In view of the shortcomings of the existing technology, the purpose of this invention is to provide a method for preparing PEEK modified particles with surface electrostatic dissipation.
[0007] To achieve the above objectives, the present invention provides a method for preparing PEEK modified particles with surface electrostatic dissipation, comprising the following steps: S1. Coarse powder processing: Using one of cryogenic milling, air jet milling or mechanical milling, the coarse powder of PEEK raw material is ground to a D90 of 200-500 mesh with a mesh tolerance of ±10% to obtain fine PEEK powder. S2, One-time mixing: The untreated carbon nanotubes are mixed with the PEEK fine powder obtained in step S1 using a high-speed mixing device. The amount of carbon nanotubes added is 2%-5% of the mass of PEEK fine powder. The stirring paddle linear speed is 10-50m / min and the mixing time is 10-20min. S3. Primary granulation: The mixture obtained in step S2 is fed into the feed port of a twin-screw extruder for extrusion granulation. The processing temperature is 350-400℃, the particle diameter is 1-3mm, the extrusion speed is 5-20m / min, and the screw speed is 200rpm. S4. Particle crushing: Use a crusher to mechanically crush the particles obtained in step S3; S5. Secondary grinding: The product obtained in step S4 is ground to a D90 of 300-500 mesh using one of cryogenic grinding, air jet milling or mechanical grinding, with a mesh tolerance of ±20%. S6. Filler mixing: Use a high-speed mixer to mix the filler with the powder obtained in step S5. The filler addition amount is 10%-30%wt, the stirring paddle linear speed is 10-50m / min, and the mixing time is 30-90min. S7. Secondary granulation: The mixture obtained in step S6 is fed into the feed port of a twin-screw extruder for extrusion granulation. The processing temperature is 350-400℃, the particle diameter is 1-3mm, and the extrusion speed is 5-20m / min to obtain PEEK modified particles with surface static dissipation.
[0008] Preferably, the carbon nanotubes in step S2 are either multi-walled carbon nanotubes or single-walled carbon nanotubes, and are used directly without any surface treatment. The amount of carbon nanotubes added is 3%-4% of the mass of the PEEK fine powder.
[0009] Preferably, the filler in step S6 is one or a mixture of carbon fiber powder, kaolin, glass fiber powder, and fumed silica.
[0010] Preferably, the filler material in step S6 is kaolin.
[0011] Preferably, the kaolin has a mesh size of 2000 mesh; in step S6, the stirring paddle linear speed is 50 m / min and the mixing time is 60 min.
[0012] Preferably, the filler addition amount in step S6 is 15%-30%wt.
[0013] Preferably, the surface resistivity of the 10mm thick sheet material extruded from the surface electrostatic dissipation PEEK modified particles in step S7 is 10. 6 -10 9 Ω / sq.
[0014] A surface electrostatic dissipation PEEK modified particle, by mass percentage, consists of 68%-88% polyetheretherketone, 2%-5% untreated carbon nanotubes, and 10%-30% filler, wherein the amount of carbon nanotubes is calculated based on the mass of polyetheretherketone, and the amount of filler is calculated based on the total mass of polyetheretherketone and carbon nanotubes.
[0015] A static dissipation PEEK profile is made by extruding surface static dissipation PEEK modified particles into plates, rods or tubes, and is used for semiconductor wafer processing carriers, chip packaging and testing fixtures or flat panel display equipment components.
[0016] The present invention has the following beneficial effects: 1. Carbon nanotubes are directly mixed with PEEK fine powder at a high loading (2%-5%wt). A dense and uniform conductive network is constructed through a two-stage powder recycling process of "primary granulation—crushing—secondary grinding—filler mixing—secondary granulation," further reducing the surface resistivity to 10. 6 -10 9Compared to existing routes that require surface modification of carbon nanotubes, the Ω / sq dissipation range significantly simplifies the process and reduces costs. 2. Compared with antistatic PEEK materials, this invention lowers the resistivity window by using a higher carbon nanotube loading and adjusts the conductivity balance and mechanical properties of the system with powder fillers, which is beneficial to improving dimensional stability and reducing costs; 3. The material is in the electrostatic dissipation region, and the discharge circuit maintains a constant and controlled microcurrent discharge, which can quickly discharge residual charge and prevent violent discharge pulses, providing passive protection for sensitive devices. Detailed Implementation
[0017] To make the technical means and beneficial effects of the present invention clearer, the present invention will be further described below in conjunction with specific embodiments.
[0018] Example 1: This example provides a method for preparing PEEK modified particles with surface electrostatic dissipation, including the following steps: S1. Coarse powder processing: PEEK raw material coarse powder is ground to D90 of 350 mesh (tolerance ±10%) using cryogenic grinding. S2, One-time mixing: High-speed mixing of untreated multi-walled carbon nanotubes with PEEK fine powder, CNT addition amount is 4%wt, stirring paddle linear speed is 30m / min, mixing time is 15min; S3, Single-stage granulation: Granulation using a twin-screw extruder, processing temperature 375℃ (10-zone temperature settings: 350 / 365 / 370 / 370 / 370 / 375 / 375 / 375 / 380 / 385℃, with vacuum pump applied in zones 5 and 8 of the extruder barrel), particle diameter 2mm, extrusion speed 10m / min, screw speed 200rpm, screw diameter 35mm; S4. Particle crushing: Mechanical crushing by a crusher; S5. Secondary grinding: freeze grinding to D90 of 400 mesh (tolerance ±20%). S6. Filler mixing: Mix 2000 mesh kaolin with the powder obtained in step S5 at high speed, with an addition amount of 30%wt, a stirring paddle linear speed of 50m / min, and a mixing time of 60min. S7. Secondary granulation: Processing temperature 375℃, particle diameter 2mm, extrusion speed 10m / min.
[0019] Example 2 The process is basically the same as in Example 1, except that the filler in step S6 is replaced with carbon fiber powder (1000 mesh), the addition amount is 20%wt, the stirring paddle linear speed is 30m / min, and the mixing time is 60min.
[0020] Example 3 The process is basically the same as in Example 1, except that the filler in step S6 is replaced with glass fiber powder (1000 mesh), the addition amount is 20%wt, the stirring paddle linear speed is 30m / min, and the mixing time is 60min.
[0021] Example 4 The process is basically the same as in Example 1, except that the filler in step S6 is replaced with fumed silica, the addition amount is 15%wt, the stirring paddle linear speed is 30m / min, and the mixing time is 60min.
[0022] Example 5 The process is basically the same as in Example 1, except that the filler in step S6 is replaced with a mixture of 2000 mesh kaolin and carbon fiber powder in a 1:1 mass ratio, with a total addition amount of 25%wt.
[0023] Test Example 1 The PEEK modified particles obtained in Example 1, which have surface electrostatic dissipation, were extruded into 10mm thick sheets. The surface resistance was tested using an ACL 800 surface resistance meter under the following conditions: RH=55%, T=27℃, and ESD STM11.11 standard. The testing method was the electrode pen method: with the center of the upper surface of the sheet as the origin, test points were taken every 1mm along the diagonal direction from the edge inwards (i.e., 5 circles at distances of 5mm, 6mm, 7mm, 8mm, and 9mm from the edge). Six test points were evenly distributed along the circumference of each circle. The test voltage was 10V, and the unit was Ω / sq, as shown in Table 1. With surface resistivity falling into 10 6 -10 9 Ω / sq is the pass / fail criterion. The above results show that the surface resistivity of the 10mm plate at each measuring point is consistently within 10 Ω / sq. 6 -10 9 Within the Ω / sq electrostatic dissipation range, the resistance values at each measuring point are consistent, indicating that the conductive network is uniformly distributed in the substrate and can dissipate residual static charge in a controlled microcurrent manner, meeting the electrostatic dissipation requirements of advanced semiconductor manufacturing scenarios.
[0024] Test Example 2 The surface electrostatic dissipation PEEK modified particles obtained in Example 2 were used to extrude 10mm plates. The testing instruments, testing conditions and testing standards were the same as in Example 1.
[0025] The test results of Example 2 are shown in Table 2 (unit: Ω / sq): In Example 2, the mass fraction of carbon fiber powder was increased by approximately 1.1 percentage points compared to Example 1. Furthermore, the resistivity of the carbon fiber powder itself was significantly lower than that of the PEEK matrix, and it possessed a good aspect ratio. The conductive network within the particles was provided by carbon nanotubes, and the carbon fiber powder formed oriented auxiliary conductive bridges at the particle scale. Simultaneously, the addition of carbon fiber powder increased the system viscosity and shear strength, and the agglomeration degree of the carbon nanotubes was further reduced compared to Example 1. Therefore, the surface resistivity at each measuring point in Example 2 was further reduced compared to Example 1, and the dispersion within the single plate was narrowed. The surface resistivity of the 10mm plate was within 1×10⁻⁶. 7 -2×10 8 Ω / sq, still at 10 6 -10 9 Within the Ω / sq electrostatic dissipation range.
[0026] The above results indicate that when carbon fiber powder is used as the powder filler, the surface resistivity at all measuring points of the 10mm plate is within 10%. 6 -10 9 Within the Ω / sq electrostatic dissipation range, the conductive network is uniformly distributed.
[0027] Test Example 3 The surface electrostatic dissipation PEEK modified particles obtained in Example 3 were used to extrude 10mm plates. The testing instruments, testing conditions and testing standards were the same as in Example 1.
[0028] The test results of Example 3 are shown in Table 3 (unit: Ω / sq): In Example 3, the glass fiber powder has a volume resistivity of approximately 1×10⁻⁶. 13 -1×10 14 The insulating filler with an Ω·cm content does not participate in the formation of the conductive network. Its function is to increase the melt viscosity and crystallization density during the cooling process, allowing the carbon nanotubes to be more fully dispersed in the shear field during secondary granulation and inhibiting their secondary migration and agglomeration in the amorphous region. Simultaneously, the addition of glass fiber powder slightly dilutes the effective concentration of the conductive phase in the particles. These two effects partially offset each other, resulting in a surface resistivity of 2 × 10⁻⁶ for the 10mm plate in Example 3. 8 -2×10 9 Ω / sq, which is about an order of magnitude higher than in Example 1, but still within 10 6 -10 9 Within the Ω / sq electrostatic dissipation range.
[0029] The above results indicate that when glass fiber powder is used as the powder filler, the surface resistivity of the 10mm plate remains stable at 10. 6 -10 9 Within the Ω / sq electrostatic dissipation range, it did not fail due to the dilution effect of the insulating filler.
[0030] Test Example 4 The surface electrostatic dissipation PEEK modified particles obtained in Example 4 were used to extrude 10mm plates. The testing instruments, testing conditions and testing standards were the same as in Example 1.
[0031] The test results of Example 4 are shown in Table 4 (unit: Ω / sq): In Example 4, fumed silica has a large specific surface area (150-200m²). 2 The surface is rich in silanol groups ( / g), exhibiting strong interfacial interactions with both PEEK molecular chains and carbon nanotubes. At an addition of 15%wt, it effectively increases melt viscosity and inhibits secondary agglomeration of carbon nanotubes under high-temperature shear conditions during secondary granulation. However, it is also insulating and has low density, thus diluting the conductive phase. Considering both factors, the surface resistivity of the 10mm plate in Example 4 is 6×10⁻⁶. 7 -6×10 8 The resistance value is Ω / sq, which is on the same order of magnitude as in Example 1, and the resistance distribution within the single board is more concentrated.
[0032] The above results indicate that fumed silica can maintain 10% concentration even at low addition levels. 6 -10 9 Ω / sq electrostatic dissipation window, and improves the on-board consistency of resistance values.
[0033] Test Example 5 The surface electrostatic dissipation PEEK modified particles obtained in Example 5 were used to extrude 10mm plates. The testing instruments, testing conditions and testing standards were the same as in Example 1.
[0034] The test results of Example 5 are shown in Table 5 (unit: Ω / sq): Example 5 uses a mixed filler composed of 2000-mesh kaolin and carbon fiber powder in a 1:1 mass ratio, with a total addition of 25% wt. The flaky kaolin readily oriented in the melt flow direction, forming a layered barrier structure within the particles and extending the circuitous path of the conductive pathway; the carbon fiber powder provides bridging across the layers; the synergy of both results in a surface resistivity of 1×10⁻⁶ for the 10mm thick sheet of Example 5. 8 -8×10 8 Ω / sq, which is about half an order of magnitude higher than that of single kaolin filler (Example 1), but still within the range of 10. 6 -10 9 Within the Ω / sq electrostatic dissipation range.
[0035] The above results indicate that using a mixed filler of kaolin and carbon fiber powder can achieve a 106 -10 9 A balance between resistance and cost is achieved within the Ω / sq electrostatic dissipation window.
[0036] Comparative Example 1: Pure PEEK resin was extruded using the same process to produce 10mm thick sheets with a surface resistivity greater than 1.0 × 10⁻⁶. 15 Ω / sq, which is in the insulating range, does not have the ability to dissipate static electricity, and there is a risk of electrostatic adsorption and electrostatic discharge during wafer processing.
[0037] Comparative Example 2: Except for step S2, where the amount of carbon nanotubes added was 1.5% wt (lower than the 2%-5 wt% limit specified in this invention), the remaining steps were the same as in Example 1. The resulting 10 mm thick plate had a surface resistivity of approximately 3.0 × 10⁻⁶. 10 Ω / sq, falling into the anti-static range instead of 10. 6 -10 9 The Ω / sq electrostatic dissipation range indicates that when the amount of carbon nanotubes added is less than 2%wt, it is impossible to build a sufficiently dense conductive network and thus insufficient to shift the resistivity down to the dissipation range.
[0038] Comparative Example 3: Except for omitting steps S4-S5 (i.e., directly mixing fillers and secondary granulation after primary granulation, without crushing and secondary grinding), the remaining steps are the same as in Example 1. The obtained 10mm plate was tested according to the method in Test Example 1, and the test results are shown in Table 6 (unit: Ω / sq): In Comparative Example 3, after the first granulation, no crushing or secondary grinding was performed. The carbon nanotubes only underwent one extrusion shearing, and their dispersion remained in a state where "agglomerates were mechanically broken up but not fully exfoliated." During the secondary granulation, the mixing of filler and powder only occurred at the agglomerate scale. The connectivity of the conductive network was determined by the local CNT enrichment region. Macroscopically, this manifested as a resistivity difference of 2-3 orders of magnitude at different measuring points on the same plate: some measuring points were still in the dissipation range, while others had jumped to 1×10⁻⁶. 9 Ω / sq or higher, even 1×10 10 The resistance is on the order of Ω / sq, with some measuring points approaching insulation. This indicates that the two-stage powder circulation (crushing + secondary grinding) deagglomerates the carbon nanotubes before secondary granulation and uniformly coats them, which is a necessary condition for obtaining a narrow resistance window.
[0039] The foregoing has shown and described the basic principles, main features, and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments. The embodiments and descriptions in the specification are merely illustrative of the principles of the invention. Various changes and modifications can be made to the invention without departing from its spirit and scope, and all such changes and modifications fall within the scope of the present invention as claimed. The scope of protection of this invention is defined by the appended claims and their equivalents.
Claims
1. A method of making surface static dissipative PEEK modified particles, characterized in that, Includes the following steps: (S1) Coarse powder processing: Using one of cryogenic milling, air jet milling or mechanical milling, the coarse powder of PEEK raw material is ground to a D90 of 200-500 mesh with a mesh tolerance of ±10% to obtain fine PEEK powder. (S2) First mixing: The untreated carbon nanotubes are mixed with the PEEK fine powder obtained in step (S1) using a high-speed mixing device. The amount of carbon nanotubes added is 2%-5% of the mass of PEEK fine powder. The stirring paddle linear speed is 10-50m / min and the mixing time is 10-20min. (S3) Primary granulation: The mixture obtained in step (S2) is fed into the feed port of a twin-screw extruder for extrusion granulation. The processing temperature is 350-400℃, the particle diameter is 1-3mm, the extrusion speed is 5-20m / min, and the screw speed is 200rpm. (S4) Particle crushing: The particles obtained in step (S3) are mechanically crushed using a crusher; (S5) Secondary grinding: The product obtained in step (S4) is ground to a D90 of 300-500 mesh using one of cryogenic grinding, air jet milling or mechanical grinding, with a mesh tolerance of ±20%; (S6) Filler mixing: Use a high-speed mixing device to mix the filler with the powder obtained in step (S5). The filler addition amount is 10%-30%wt, the stirring paddle linear speed is 10-50m / min, and the mixing time is 30-90min. (S7) Secondary granulation: The mixture obtained in step (S6) is fed into the feed port of a twin-screw extruder for extrusion granulation. The processing temperature is 350-400℃, the particle diameter is 1-3mm, and the extrusion speed is 5-20m / min to obtain PEEK modified particles with surface static dissipation.
2. The method for preparing surface electrostatic dissipation PEEK modified particles according to claim 1, characterized in that, The carbon nanotubes in step (S2) are either multi-walled carbon nanotubes or single-walled carbon nanotubes, and the amount of carbon nanotubes added is 3%-4% of the mass of PEEK fine powder.
3. The method for preparing surface electrostatic dissipation PEEK modified particles according to claim 1, characterized in that, The filler in step (S6) is one or a mixture of carbon fiber powder, kaolin, glass fiber powder, and fumed silica.
4. The method for preparing surface electrostatic dissipation PEEK modified particles according to claim 1, characterized in that, The filler material used in step (S6) is kaolin.
5. The method for preparing surface electrostatic dissipation PEEK modified particles according to claim 4, characterized in that, The kaolin has a mesh size of 2000; in step (S6), the stirring paddle linear speed is 50 m / min and the mixing time is 60 min.
6. The method for preparing surface electrostatic dissipation PEEK modified particles according to claim 1, characterized in that, In step (S6), the amount of filler added is 15%-30%wt.
7. A PEEK-modified particle with surface electrostatic dissipation, characterized in that, The material is composed of 68%-88% polyetheretherketone (PEEK), 2%-5% untreated carbon nanotubes, and 10%-30% filler by mass percentage. The amount of carbon nanotubes is calculated based on the mass of PEEK, and the amount of filler is calculated based on the total mass of PEEK and carbon nanotubes. The surface electrostatic dissipation PEEK modified particles are prepared by the preparation method described in any one of claims 1-6.
8. The surface electrostatic dissipation PEEK modified particles according to claim 7, characterized in that, The surface resistivity of a 10 mm thick plate extruded from the particles is 10 6 -10 9 Ω / sq.
9. A static dissipation PEEK profile, characterized in that, The surface electrostatic dissipation PEEK modified particles as described in claim 7 or 8 are extruded into plates, rods or tubes for use in semiconductor wafer processing carriers, chip packaging and testing fixtures or flat panel display equipment components.
Citation Information
Patent Citations
Polyaryletherketone composition for static dissipative plate with highly uniform resistivity and preparation method of polyaryletherketone composition
CN110591329A
Antistatic polyether-ether-ketone composite material and preparation method thereof
CN115558236A
Anti-static polyether-ether-ketone composite material and preparation method thereof
CN121343349A
Polyaryletherketone composite material and preparation method thereof
CN121610054A