Polyurethane structural resin for composite material pole towers and preparation method and application thereof

By using a two-component system of polytetrahydrofuran ether diol isocyanate prepolymer and long-suspended chain vegetable oil polyol, along with the synergistic effect of latent curing agent and silane coupling agent modified nano-silica, the problems of curing bubble defects and difficulty in simultaneously achieving strength modulus, water resistance and interfacial properties in composite towers were solved, achieving the effects of bubble-free curing, high strength and high modulus, low water absorption and water resistance and high interfacial strength.

CN123152276APending Publication Date: 2026-11-24BEIJING UNIV OF CHEM TECH +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611602237.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-16
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing polyurethane structural resins have problems in composite material tower winding or pultrusion molding, such as numerous curing bubble defects and difficulty in simultaneously achieving strength modulus, water resistance and interface properties.

Method used

A two-component system is constructed using polytetrahydrofuran ether diol isocyanate prepolymer and long-suspension-chain vegetable oil polyol. A latent curing agent and a compound defoamer are introduced to work synergistically. Silane coupling agent is used to modify nano-silica to improve the interfacial bonding performance between the resin matrix and glass fiber. Through synergistic reinforcement of soft and hard segments in micro-regions, graded defoaming by latent curing agent, and interfacial chemical bonding of nano-silica, bubble-free curing, high strength and high modulus, low water absorption and water resistance, and high interfacial strength are achieved.

Benefits of technology

It achieves bubble-free curing of composite material towers, improves strength modulus, water resistance and interfacial strength, and is suitable for winding or pultrusion molding of composite material towers, with broad application prospects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure REF-OBJ-1790653798425-000001
    Figure REF-OBJ-1790653798425-000001
Patent Text Reader

Abstract

This invention belongs to the field of specialty polyurethane resins, specifically relating to a polyurethane structural resin for composite towers, its preparation method, and its application. The resin consists of component A and component B: component A is an isocyanate prepolymer obtained by reacting aromatic or aliphatic isocyanate with polytetrahydrofuran ether diol, with an isocyanate group content of 10-18 wt%; component B consists of long-chain plant oil polyol, polyether polyol, chain extender, latent curing agent, coupling agent, silane coupling agent-modified nano-silica, leveling agent, compounded defoamer, and catalyst. This invention achieves a bubble-free curing process through the synergistic effect of the latent curing agent and compounded defoamer; achieves high strength and high modulus through the microphase separation of soft and hard segments of polytetrahydrofuran ether diol and the crosslinking of trifunctional polyether polyol; constructs a molecular-level hydrophobic barrier through the suspended chains of the long-chain plant oil polyol; and constructs a three-level interfacial chemical bonding network of "matrix-nano-silica-glass fiber" through silane coupling agent-modified nano-silica. The resulting resin combines bubble-free curing, high strength and high modulus, low water absorption and water resistance with high interfacial strength, making it suitable for the winding or pultrusion molding of composite material towers.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a polyurethane structural resin for composite material towers, its preparation method, and its applications. This invention belongs to the field of specialty polyurethane resins. Background Technology

[0002] Transmission line towers and communication towers are crucial infrastructure for power grids and communication networks. Traditional wooden towers are prone to decay and have poor fire resistance, concrete towers are heavy and difficult to transport and install, and steel towers are susceptible to corrosion and require regular anti-corrosion maintenance. As power grids develop towards larger capacity, longer distances, higher altitudes, and coastal high-salt-fog environments, higher demands are placed on the lightweight, weather-resistant, and insulating performance of towers. Glass fiber reinforced composite material towers offer advantages such as lightweight, high strength, corrosion resistance, good insulation, and maintenance-free operation, leading to their increasingly widespread application in power transmission, distribution, and communication. Among these, polyurethane, due to its excellent mechanical properties, high design flexibility, good wettability with glass fiber, and flexible curing process, has become an important matrix resin for spiral wound or pultruded composite material towers.

[0003] Polyurethane structural resins typically employ a two-component system consisting of an isocyanate component and a polyol component. To balance high strength, high modulus, and water resistance and durability, the polyol component often incorporates polyether polyols, vegetable oil polyols, chain extenders, latent curing agents, coupling agents, nanofillers, and various additives, forming a multi-component composite system. However, during the preparation and molding of two-component polyurethanes, trace amounts of moisture in the raw materials and environment can react with the isocyanate groups to generate carbon dioxide, forming bubbles and micropores in thick-section wound or pultruded products. Simultaneously, different polyols and fillers differ in polarity, hydroxyl value, functionality, and interfacial characteristics. If the ratio or compatibility is insufficient, problems such as inadequate microphase separation, filler agglomeration, interfacial debonding, and stress concentration can easily occur, leading to a decrease in product strength, modulus, elongation at break, and interfacial properties, as well as defects such as bubbles and pinholes. This affects molding stability and shortens the service life of the tower.

[0004] Existing polyurethane structural resins generally suffer from the problem of balancing strength, modulus, water resistance, and interfacial properties. To achieve high strength and high modulus, it is usually necessary to increase the isocyanate content and hard segment ratio. However, excessive hard segment content can make the resin brittle and significantly reduce its elongation at break. Using ordinary polyether polyols results in high water absorption and significant performance degradation after hygrothermal aging. The relationship between the resin and glass fiber is mainly based on physical adsorption, leading to insufficient interlaminar shear strength and axial mechanical properties. Simply increasing the crosslinking density can improve the modulus, but may exacerbate brittleness. Directly introducing ordinary nanofillers may result in uneven dispersion and stress concentration due to insufficient interfacial bonding, making it difficult to simultaneously meet the requirements of bubble-free curing, high strength and high modulus, low water absorption and water resistance, and high interfacial strength.

[0005] Therefore, it is necessary to develop a polyurethane structural resin for composite towers that combines non-foaming curing, high strength and high modulus, low water absorption and water resistance, and high interfacial strength. Summary of the Invention

[0006] The purpose of this invention is to address the problems of numerous curing bubble defects and the difficulty in simultaneously achieving high strength, modulus, water resistance, and interfacial properties in the winding or pultrusion molding of composite material towers using existing two-component polyurethane resins. This invention provides a polyurethane structural resin for composite material towers and its preparation method. Through formulation design, a two-component system is constructed using a polytetrahydrofuran ether diol isocyanate prepolymer and a long-chain vegetable oil polyol. A latent curing agent and a compounded defoamer are introduced to synergistically improve the interfacial bonding performance between the resin matrix and glass fiber, as well as the strength, modulus, and water resistance of the cured product. This resin can be used for winding or pultrusion molding of composite material towers in power transmission, communication, and other fields, and has wide applications. The technical solution adopted by this invention to solve its technical problems is as follows: This invention provides a polyurethane structural resin for composite material towers, which is composed of component A and component B; Component A is an isocyanate prepolymer obtained by reacting aromatic isocyanates and / or aliphatic isocyanates with polytetrahydrofuran ether diol, wherein the -NCO content in the prepolymer is 10-18 wt%. Component B, by weight, is composed of the following raw materials: 40-70 parts of long-suspension chain plant oil polyols; 20-40 parts of polyether polyol; Chain extender 2-10 parts; Latent curing agent 1.0-5.0 parts; 0.5-3.0 parts of coupling agent; 0.5-3.0 parts of silane coupling agent modified nano-silica; Leveling agent 0.1-1.0 parts; Compound defoamer 0.1-1.0 parts; Catalyst 0.1-0.5 parts; The long-suspension-chain plant oil polyol has a hydroxyl value of 50-600 mg KOH / g.

[0007] Furthermore, The hard segment content in the cured resin product is 25-40 wt%; the hard segment is a rigid segment formed by the reaction of isocyanate and chain extender.

[0008] Furthermore, The long-suspension-chain plant oil polyol has long fatty suspension chains of C15-C20, which extend laterally in the solidified network to form a comb-shaped / brush-shaped molecular structure.

[0009] Furthermore, The long-suspension chain vegetable oil polyol is at least one of cashew nut shell oil polyol and castor oil polyol.

[0010] Furthermore, The latent curing agent is an oxazolidine latent curing agent and / or an imine latent curing agent; The oxazolidine latent curing agent is a monooxazolidine and / or a bisoxazolidine, and the imine latent curing agent is an aldehydeimine and / or a ketimine.

[0011] Furthermore, The amount of the latent curing agent used is such that the amount of active hydrogen released after complete hydrolysis is not less than the amount of isocyanate groups in component A that can participate in the side reaction with water.

[0012] Furthermore, The polyether polyols comprise more than 60 wt% of the total mass of the polyether polyols, with a number average molecular weight of 300-6000; the remainder comprises difunctional polyether polyols with a number average molecular weight of 500-2000.

[0013] Furthermore, The compound defoamer is a mixture of organosilicon polysiloxane defoamer and fluorine-modified organosilicon defoamer in a mass ratio of (1-3):1.

[0014] Another object of the present invention is to provide a method for preparing the above-mentioned composite material tower polyurethane structural resin, comprising the following steps: S1, react aromatic isocyanate and / or aliphatic isocyanate with polytetrahydrofuran ether diol at 60-120℃ to obtain component A with a -NCO content of 10-18wt%. S2, long suspended chain vegetable oil polyol, polyether polyol, chain extender, latent curing agent, coupling agent, silane coupling agent modified nano silica, leveling agent, compound defoamer and catalyst are vacuum degassed and mixed at 20-50℃ to obtain component B; S3, Component A and Component B are mixed at an isocyanate index R = 0.90-1.10 to obtain the polyurethane structural resin for the composite tower.

[0015] Another object of the present invention is to provide an application of the above-mentioned resin in the preparation of glass fiber reinforced polyurethane composite towers by winding or pultrusion molding, wherein the curing temperature of the winding molding is 60-120°C.

[0016] The beneficial effects of this invention are: (1) This invention uses polytetrahydrofuran ether diol isocyanate prepolymer as the linear soft segment continuous phase, and the hard segment generated by the reaction of isocyanate and chain extender as the rigid reinforcing phase. Trifunctional polyether polyol and long-suspended-chain vegetable oil polyol are introduced to synergistically regulate the crosslinking density. Specifically, the difunctional polytetrahydrofuran ether diol soft segment molecular chains are regular and flexible, forming an ordered micro-region structure with the hard segments. The hard segment micro-regions act as physical crosslinking points to bear the load. The trifunctional polyether polyol provides appropriate chemical crosslinking points, and the flexible suspended chains of the long-suspended-chain vegetable oil polyol buffer the stress of the chain segments. Based on this synergistic effect of soft and hard segments, the high strength and high modulus of the cured resin product are improved.

[0017] (2) This invention employs a latent curing agent and a compound defoamer to construct a graded defoaming system. The latent curing agent remains stable during storage and mixing, and upon entering the curing stage, it preferentially undergoes a hydrolysis reaction with trace amounts of moisture in the system, blocking the path of moisture reacting with isocyanate groups to generate carbon dioxide from the source. The organosilicon polysiloxane component in the compound defoamer eliminates macroscopic bubbles that have already been incorporated, while the fluorinated modified component inhibits the retention of microbubbles during fiber impregnation. This achieves full-process defoaming through "source blocking - process elimination - interface inhibition," resulting in a cured product cross-section free of visible bubbles and micropore defects, thus improving the uniformity and durability of the product's mechanical properties.

[0018] (3) This invention uses a silane coupling agent to modify nano-silica to construct a chemically bonded network at the resin matrix-nano-silica interface. One end of the silane coupling agent forms a Si-O-Si chemical bond with the surface of the nano-silica, while the other end connects to the polyurethane crosslinking network and bonds with the hydroxyl groups on the glass fiber surface, replacing traditional physical adsorption with chemical bonding. This reduces interfacial debonding and stress concentration, improves interlaminar shear strength, and thus enhances the axial mechanical properties of the composite material tower.

[0019] (4) The present invention uses long-suspension chain vegetable oil polyol, which is renewable and partially replaces petroleum-based polyether polyol, thus reducing raw material costs and being low-carbon and environmentally friendly. At the same time, its long fatty suspension chains extend laterally in the solidified network to form a molecular-level hydrophobic barrier, reducing the water absorption rate of the solidified product and improving water resistance and durability.

[0020] (5) The present invention achieves moderate viscosity and a pot life that meets the requirements of continuous winding or pultrusion operations by synergistically adjusting the isocyanate index and ratio of component A and component B. The curing temperature matches the process window of existing winding / pultrusion equipment, and can be implemented without modifying existing production lines, with strong process adaptability.

[0021] In summary, this invention achieves a continuous mechanism of action through micro-regional synergistic enhancement of soft and hard segments, hierarchical defoaming of latent curing agents, interfacial chemical bonding of nano-silica, hydrophobic barrier of long suspended chains, and matching of process windows. This enables the material to simultaneously achieve bubble-free curing, high strength and high modulus, low water absorption and water resistance, and high interfacial strength. It is suitable for composite material poles and towers with high requirements for mechanical properties and durability through winding or pultrusion molding. Detailed Implementation

[0022] The present invention will be described in detail below with reference to embodiments. However, it should be understood that the following embodiments are merely illustrative examples of implementation of the present invention and are not intended to limit the scope of the present invention.

[0023] The purpose of this invention is to develop a polyurethane structural resin for composite towers, addressing the problems of existing polyurethane structural resins in curing bubble defects and the difficulty in simultaneously achieving strength modulus and water resistance interfacial properties during winding or pultrusion molding. The design concept is as follows: Firstly, from the perspective of defoaming and interfacial synergy, a latent curing agent and a compounded defoamer are introduced. The latent curing agent preferentially hydrolyzes with trace amounts of water during the curing stage, blocking carbon dioxide generation at the source, and its hydrolysis products serve as additional crosslinking points to reinforce the network. The compounded defoamer contains organosilicon and fluorine-modified components that progressively eliminate macro and micro bubbles. Furthermore, a silane coupling agent is used to modify nano-silica, anchoring one end of the nano-silica and connecting the other end to the polyurethane crosslinking network, bonding with hydroxyl groups on the glass fiber surface, thus constructing a three-level interfacial chemical bonding network of "matrix-nano-silica-glass fiber". On the other hand, from the perspective of soft and hard segment structure design, a polytetrahydrofuran ether diol-based isocyanate prepolymer provides linear soft segments, which form microphase separation with the isocyanate-chain extender hard segments. Trifunctional polyether polyols provide chemical crosslinking points, and the C15-C20 suspended chains of long-chain vegetable oil polyols extend laterally to form a molecular-level hydrophobic barrier and buffer chain segment stress. The theoretical basis is that the hard segment microregions act as physical crosslinking points to bear the load, the linear soft segments ensure flexibility and orderly microphase separation, the latent curing agent and compounded defoamer work together to achieve a completely bubble-free process, modified nano-silica strengthens the interface by replacing physical adsorption with chemical bonding, and the long-chain vegetable oil polyols combine hydrophobic toughening with bio-based low carbon content. After stepwise modification and mixing, winding, or pultrusion molding, the components work synergistically to achieve bubble-free curing, high strength and high modulus, low water absorption and water resistance, and high interfacial strength. This is suitable for the winding or pultrusion molding of composite material towers and is conducive to promoting the large-scale application of composite materials in power infrastructure. Examples of this invention are as follows: This invention provides a polyurethane structural resin for composite material towers, composed of component A and component B; Component A is an isocyanate prepolymer obtained by reacting aromatic isocyanates and / or aliphatic isocyanates with polytetrahydrofuran ether diol, wherein the -NCO content in the prepolymer is 10-18 wt%. The aromatic isocyanate is diphenylmethane diisocyanate; the aliphatic isocyanate is hexamethylene diisocyanate or isophorone diisocyanate.

[0024] The polytetrahydrofuran ether diol has a number average molecular weight of 650-3000, preferably 1000-2000, a functionality of 2, and a primary hydroxyl group at the end; BASF's PolyTHF 1000 or PolyTHF 2000 can be used, with corresponding hydroxyl values ​​of approximately 112 mg KOH / g and 56 mg KOH / g, respectively.

[0025] Component B, by weight, is composed of the following raw materials: 40-70 parts of long-suspension chain plant oil polyols; 20-40 parts of polyether polyol; Chain extender 2-10 parts; Latent curing agent 1.0-5.0 parts; 0.5-3.0 parts of coupling agent; 0.5-3.0 parts of silane coupling agent modified nano-silica; Leveling agent 0.1-1.0 parts; Compound defoamer 0.1-1.0 parts; Catalyst 0.1-0.5 parts; The long-suspension-chain plant oil polyol has a hydroxyl value of 50-600 mg KOH / g.

[0026] The hard segment content in the cured resin product is 25-40 wt%; the hard segment is a rigid chain segment formed by the reaction of isocyanate and chain extender. The hard segment content is calculated as (mass of isocyanate + mass of chain extender) / total mass of cured product, and can be determined from the formulation.

[0027] The long-chain plant oil polyol has long fatty suspension chains of C15-C20, which extend laterally in the solidified network to form a comb / brush-shaped molecular structure; it can be at least one of cashew nut shell oil polyol and castor oil polyol. The cashew nut shell oil polyol has C15 long fatty suspension chains with a hydroxyl value of 120-250 mgKOH / g, and can be selected from Cardlä's NX-9001 (hydroxyl value of about 175 mgKOH / g) or GX-9005, GX-9007 series. The castor oil polyol has C18 long fatty suspension chains with a hydroxyl value of 100-200 mgKOH / g, and can be selected from Vertellus's Polycin GR-110 (hydroxyl value of about 109 mgKOH / g) or Polycin GR-160 (hydroxyl value of about 164 mgKOH / g).

[0028] The latent curing agent is an oxazolidine latent curing agent and / or an imine latent curing agent; the oxazolidine latent curing agent is a monooxazolidine and / or a bisoxazolidine, such as Incorez's Incozol 2 (monoxazolidine) or Incozol LV, Incozol 4 (bisoxazolidine); the imine latent curing agent is an aldehydeimine and / or a ketimine, such as Evonik's Vestamin A139 (a blocked aldehydeimine crosslinking agent based on alicyclic diamines, which releases a diamine upon contact with water and reacts with isocyanate groups to form urea bonds).

[0029] The amount of the latent curing agent used is such that the amount of active hydrogen released after complete hydrolysis is not less than the amount of isocyanate groups in component A that can participate in the side reaction with water.

[0030] The polyether polyol comprises at least 60 wt% trifunctional polyether polyol with a number average molecular weight of 300-6000; the remainder is difunctional polyether polyol with a number average molecular weight of 500-2000. The trifunctional polyether polyol can be a glycerol-based propylene oxide polyether triol, such as Dow's VORANOL CP4701 or CP6001; the difunctional polyether polyol can be a propylene oxide polyether diol, such as PPG-1000 or PPG-2000.

[0031] The chain extender is at least one of 1,4-butanediol, ethylene glycol, diethylene glycol, and neopentyl glycol, preferably 1,4-butanediol.

[0032] The coupling agent is a silane coupling agent, preferably at least one of γ-aminopropyltriethoxysilane (KH-550), γ-glycidoxypropyltrimethoxysilane (KH-560), and γ-methacryloyloxypropyltrimethoxysilane (KH-570); the coupling agent is added independently of the silane coupling agent-modified nano-silica and is used for glass fiber surface treatment and interface wetting.

[0033] The silane coupling agent modified nano-silica is silane coupling agent KH-550 modified nano-silica. The nano-silica is obtained by fumed silica or precipitation method, with a specific surface area of ​​150-380 m². 2 / g, with an average particle size of 7-40nm, Evonik's hydrophilic Aerosil 200 can be used. The preparation method of the silane coupling agent KH-550 modified nano-silica is as follows: A11. Nano-silica was added to a 1.0 mol / L hydrochloric acid solution and stirred at 60 °C for 3 h. After acid washing, the mixture was filtered, and the filter cake was repeatedly washed with deionized water until the pH of the filtrate was 6.5-7.0. The filter cake was then dried in a vacuum drying oven at 100 °C for 6 h to obtain acid-washed activated nano-silica. After acid washing and activation, the hydroxyl content on the surface of the nano-silica was 2.0 mmol / g (determined by acetic anhydride / pyridine acetylation-reverse titration). The mass-to-volume ratio of the nano-silica to the hydrochloric acid solution was 1 g:20 mL.

[0034] A12, acid-washed and activated nano-silica was added to an ethanol / water (V / V=90 / 10) mixture, and the pH of the system was adjusted to 4.5; then, silane coupling agent KH-550 was added, and the mixture was stirred at 60℃ for 3 hours; after the reaction, the mixture was filtered, washed 2-3 times with ethanol and deionized water, and then dried at 100℃ for 6 hours to obtain silane coupling agent modified nano-silica. The amount of silane coupling agent KH-550 added was 3 wt% of the mass of the acid-washed and activated nano-silica.

[0035] The leveling agent is a silicone or acrylate leveling agent, such as BYK-306 or BYK-333.

[0036] The compound defoamer is a mixture of organosilicon polysiloxane defoamer and fluorine-modified organosilicon defoamer in a mass ratio of (1-3):1; the organosilicon polysiloxane defoamer can be BYK-066N, and the fluorine-modified organosilicon defoamer is a commercially available fluorosilicone defoamer.

[0037] The catalyst is an organotin catalyst and / or a tertiary amine catalyst, preferably dibutyltin dilaurate, but stannous octoate or dimorpholine diethyl ether can also be used.

[0038] Another objective of this invention is to provide a method for preparing the above-mentioned composite material tower polyurethane structural resin, comprising the following steps: S1, Preparation of component A: S11, dehydrate polytetrahydrofuran ether diol at 100-120℃ and a vacuum degree not exceeding -0.09MPa for 2-3 hours to achieve a water content not exceeding 0.05wt%. S12, add aromatic isocyanate and / or aliphatic isocyanate to the reactor, heat to 60-90℃ under nitrogen protection (90-120℃ when using aliphatic isocyanate), add dehydrated polytetrahydrofuran ether diol in batches under stirring, keep the reaction at the temperature for 2-3 hours, until the -NCO content of the system reaches 10-18wt% (determined by di-n-butylamine back titration), cool and discharge the material and seal it for storage to obtain component A; when using aliphatic isocyanate, a catalyst can be added at the same time to ensure that the reaction is complete.

[0039] S2, Preparation of component B: S21, dehydrate long-suspension chain vegetable oil polyols and polyether polyols at 100-120℃ and a vacuum degree not higher than -0.09MPa for 1-2 hours; S22, weigh out the dehydrated long-suspension chain vegetable oil polyol, polyether polyol, chain extender, latent curing agent, coupling agent, silane coupling agent modified nano silica, leveling agent, compound defoamer and catalyst according to the weight parts, and vacuum defoam and stir at 20-50℃ for 0.5-1.5h until uniformly mixed to obtain component B; wherein, the latent curing agent and catalyst are added just before use.

[0040] S3. Resin preparation: Component A and component B are mixed at an isocyanate index R = 0.90-1.10 to obtain the polyurethane structural resin for the composite tower; wherein, the isocyanate index R is the ratio of the isocyanate group equivalent in component A to the sum of the hydroxyl equivalent in component B and the active hydrogen equivalent released by the complete hydrolysis of the latent curing agent.

[0041] Another objective of this invention is to provide an application of the above-mentioned polyurethane structural resin for composite towers in the preparation of glass fiber reinforced polyurethane composite towers by winding or pultrusion molding: The above components A and B are mixed at an isocyanate index R = 0.90-1.10 and then used for winding or pultrusion molding of glass fiber reinforced polyurethane composite towers.

[0042] During the winding process, the temperature of the impregnation tank is 20-40℃, the resin gel time is 15-60min, and the curing regime is a segmented temperature increase of 60-120℃ (e.g., curing at 80℃ for 2h, curing at 120℃ for 2h).

[0043] During pultrusion molding, the die is temperature controlled in three sections along the traction direction: 80-100℃, 120-140℃ and 140-160℃ respectively, and the traction speed is 0.2-0.8m / min.

[0044] The glass fiber content is 55%-70% by volume.

[0045] The technical mechanism of this invention is as follows: A latent curing agent and a compound defoamer constitute a graded defoaming system. During the storage and mixing stages of components A and B, the latent curing agent does not react with isocyanate groups, maintaining system stability. Upon entering the curing stage, it preferentially hydrolyzes upon encountering trace amounts of moisture in the system, consuming the moisture and blocking the pathway of water reacting with isocyanate groups to generate carbon dioxide, thus inhibiting chemical foaming at its source. In the compound defoamer, the polysiloxane component has low surface tension and can quickly migrate to the gas-liquid interface, eliminating macroscopic bubbles entrained during mixing and impregnation. The fluorinated modified component further reduces interfacial tension, inhibiting the retention of microbubbles between glass fiber bundles. The three components work synergistically to achieve comprehensive defoaming through "source blocking - process elimination - interfacial inhibition."

[0046] The enhancement, interfacial bonding, and hydrophobicity of the cured product are synergistically achieved by the soft and hard segment structure, nano-silica, and vegetable oil polyol. Polytetrahydrofuran ether diol is a linear, difunctional soft segment with a regular and flexible molecular chain. It undergoes microphase separation with the hard segments formed by isocyanate and chain extenders. The hard segment micro-regions act as physical crosslinking points, while the trifunctional polyether polyol provides chemical crosslinking points. The flexible suspended chains of the long-chain vegetable oil polyol extend laterally within the crosslinking network, forming a molecular-level hydrophobic barrier and buffering chain segment stress. Silane coupling agent-modified nano-silica is anchored at one end to the nano-silica and connected to the polyurethane crosslinking network at the other end, bonding with the hydroxyl groups on the glass fiber surface, forming a three-level interfacial chemical bonding network of "resin matrix-nano-silica-glass fiber".

[0047] The synergistic effect of the above components gives the structural resin properties such as being bubble-free, having high strength and modulus, low water absorption, and high interfacial strength.

[0048] To further understand the present invention, the following detailed description of a polyurethane structural resin for composite material towers provided by the present invention is provided in conjunction with specific embodiments. The scope of protection of the present invention is not limited by the following embodiments.

[0049] Example 1

[0050] A polyurethane structural resin for composite material towers, composed of component A and component B; Component A is an isocyanate prepolymer obtained by reacting diphenylmethane diisocyanate with PolyTHF 1000, and the -NCO content in the prepolymer is 14wt%.

[0051] Component B, by weight, is composed of the following raw materials: 55 parts of long-suspension chain plant oil polyols; 30 parts of polyether polyol; 6 parts of 1,4-butanediol; 3.0 parts of latent curing agent; 1.5 parts of γ-aminopropyltriethoxysilane (KH-550); 1.5 parts of KH-550 modified nano-silica; Leveling agent BYK-333, 0.5 parts; 0.6 parts of compound defoamer; 0.3 parts of dibutyltin dilaurate; The long-suspension-chain vegetable oil polyol is castor oil polyol (C18 long fatty suspension chain), model Polycin GR-160 (hydroxyl value approximately 164 mg KOH / g).

[0052] The hard segment content in the cured resin product is 31 wt%; the hard segment is a rigid segment formed by the reaction of isocyanate and chain extender.

[0053] The polyether polyol comprises 80 wt% trifunctional polyether polyol, specifically Dow's VORANOL CP4701 (number average molecular weight 4800); the balance is PPG-1000.

[0054] The latent curing agent Incozol LV.

[0055] The compound defoamer is a mixture of BYK-066N and fluorine-modified organosilicon defoamer at a mass ratio of 2:1.

[0056] A method for preparing the above-mentioned composite material pole tower polyurethane structural resin includes the following steps: S1, Preparation of component A: S11, polytetrahydrofuran ether diol is dehydrated at 110℃ and under a vacuum degree not exceeding -0.09MPa for 2.5h to achieve a water content not exceeding 0.05wt%; S12, add aromatic isocyanate to the reactor, heat to 80°C under nitrogen protection, add dehydrated polytetrahydrofuran ether diol in batches under stirring, keep the reaction at the temperature for 2.5 h, until the -NCO content of the system reaches 14 wt% (determined by di-n-butylamine back titration), cool and discharge the material and seal it for storage to obtain component A.

[0057] S2, Preparation of component B: S21, long-suspension chain vegetable oil polyols and polyether polyols are dehydrated for 1.5 h at 110 °C and a vacuum degree not higher than -0.09 MPa; S22, weigh out the dehydrated long-suspension chain vegetable oil polyol, polyether polyol, chain extender, latent curing agent, coupling agent, silane coupling agent modified nano silica, leveling agent, compound defoamer and catalyst according to the weight parts, and vacuum degas and stir at 40℃ for 1 hour until the mixture is uniform to obtain component B; wherein, the latent curing agent and catalyst are added before use.

[0058] S3. Resin preparation: Component A and component B are mixed at an isocyanate index R = 1.05 to obtain the polyurethane structural resin for the composite tower; wherein, the isocyanate index R is the ratio of the isocyanate group equivalent in component A to the sum of the hydroxyl equivalent in component B and the active hydrogen equivalent released by the complete hydrolysis of the latent curing agent.

[0059] An application of the above-mentioned polyurethane structural resin for composite towers in the preparation of glass fiber reinforced polyurethane composite towers by winding: After mixing the above components A and B according to the isocyanate index R, they are used for winding or pultrusion molding of glass fiber reinforced polyurethane composite towers.

[0060] During the winding process, the temperature of the impregnation tank is 30℃, the resin gel time is 30min, and the curing regime is such as curing at 80℃ for 2h or curing at 120℃ for 2h.

[0061] The glass fiber content is 65% by volume.

[0062] Example 2

[0063] A polyurethane structural resin for composite material towers, composed of component A and component B; Component A is an isocyanate prepolymer obtained by reacting diphenylmethane diisocyanate with PolyTHF 1000, and the -NCO content in the prepolymer is 10wt%.

[0064] Component B, by weight, is composed of the following raw materials: 40 parts of long-suspension chain plant oil polyols; 40 parts of polyether polyol; 2 parts of 1,4-butanediol; 5.0 parts of latent curing agent; 0.5 parts of γ-aminopropyltriethoxysilane (KH-550); 3.0 parts of KH-550 modified nano-silica; Leveling agent BYK-333 1.0 part; 0.1 parts of compound defoamer; 0.1 parts of dibutyltin dilaurate; The long-suspension-chain vegetable oil polyol is castor oil polyol (C18 long fatty suspension chain), model Polycin GR-160 (hydroxyl value approximately 164 mg KOH / g).

[0065] The hard segment content in the cured resin product is 25 wt%; the hard segment is a rigid segment formed by the reaction of isocyanate and chain extender.

[0066] The polyether polyol comprises 80 wt% trifunctional polyether polyol, specifically Dow's VORANOL CP4701 (number average molecular weight 4800); the balance is PPG-1000.

[0067] The latent curing agent Incozol LV.

[0068] The compound defoamer is a mixture of BYK-066N and fluorine-modified organosilicon defoamer at a mass ratio of 2:1.

[0069] A method for preparing the above-mentioned composite material pole tower polyurethane structural resin includes the following steps: S1, Preparation of component A: S11, polytetrahydrofuran ether diol is dehydrated at 120℃ and under a vacuum degree not exceeding -0.09MPa for 2 hours to achieve a water content not exceeding 0.05wt%; S12, add aromatic isocyanate to the reactor, heat to 90°C under nitrogen protection, add dehydrated polytetrahydrofuran ether diol in batches under stirring, keep the reaction at the temperature for 2 hours until the -NCO content of the system reaches 10wt% (determined by di-n-butylamine back titration), cool and discharge the material and seal it for storage to obtain component A.

[0070] S2, Preparation of component B: S21, dehydrate long-suspension chain vegetable oil polyols and polyether polyols at 120℃ and a vacuum degree not higher than -0.09MPa for 1 hour; S22, weigh out the dehydrated long-suspension chain vegetable oil polyol, polyether polyol, chain extender, latent curing agent, coupling agent, silane coupling agent modified nano silica, leveling agent, compound defoamer and catalyst according to the weight parts, and vacuum degas and stir at 50°C for 0.5h until the mixture is uniform to obtain component B; wherein, the latent curing agent and catalyst are added before use.

[0071] S3. Resin preparation: Component A and component B are mixed at an isocyanate index R = 1.05 to obtain the polyurethane structural resin for the composite tower; wherein, the isocyanate index R is the ratio of the isocyanate group equivalent in component A to the sum of the hydroxyl equivalent in component B and the active hydrogen equivalent released by the complete hydrolysis of the latent curing agent.

[0072] An application of the above-mentioned polyurethane structural resin for composite towers in the preparation of glass fiber reinforced polyurethane composite towers by winding: After mixing the above components A and B according to the isocyanate index R, they are used for winding or pultrusion molding of glass fiber reinforced polyurethane composite towers.

[0073] During the winding process, the temperature of the impregnation tank is 40℃, the resin gel time is 15min, and the curing regime is such as curing at 80℃ for 2h or curing at 120℃ for 2h.

[0074] The glass fiber content is 55% by volume.

[0075] Example 3

[0076] A polyurethane structural resin for composite material towers, composed of component A and component B; Component A is an isocyanate prepolymer obtained by reacting diphenylmethane diisocyanate with PolyTHF 1000, and the -NCO content in the prepolymer is 18wt%.

[0077] Component B, by weight, is composed of the following raw materials: 70 parts of long-suspension chain plant oil polyols; 20 parts of polyether polyol; 10 parts of 1,4-butanediol; Latent curing agent 1.0 part; γ-aminopropyltriethoxysilane (KH-550) 3.0 parts; 0.5 parts of KH-550 modified nano-silica; Leveling agent BYK-333, 0.1 parts; 1.0 part of compound defoamer; 0.5 parts of dibutyltin dilaurate; The long-suspension-chain vegetable oil polyol is castor oil polyol (C18 long fatty suspension chain), model Polycin GR-160 (hydroxyl value approximately 164 mg KOH / g).

[0078] The hard segment content in the cured resin product is 37 wt%; the hard segment is a rigid segment formed by the reaction of isocyanate and chain extender.

[0079] The polyether polyol comprises 80 wt% trifunctional polyether polyol, specifically Dow's VORANOL CP4701 (number average molecular weight 4800); the balance is PPG-1000.

[0080] The latent curing agent Incozol LV.

[0081] The compound defoamer is a mixture of BYK-066N and fluorine-modified organosilicon defoamer at a mass ratio of 2:1.

[0082] A method for preparing the above-mentioned composite material pole tower polyurethane structural resin includes the following steps: S1, Preparation of component A: S11, polytetrahydrofuran ether diol is dehydrated at 100℃ and under a vacuum degree not exceeding -0.09MPa for 3 hours to achieve a water content not exceeding 0.05wt%; S12, add aromatic isocyanate to the reactor, heat to 60°C under nitrogen protection, add dehydrated polytetrahydrofuran ether diol in batches under stirring, keep the reaction at the temperature for 3 hours until the -NCO content of the system reaches 18wt% (determined by di-n-butylamine back titration), cool and discharge the material and seal it for storage to obtain component A.

[0083] S2, Preparation of component B: S21, long-hanging chain vegetable oil polyols and polyether polyols are dehydrated for 2 hours at 100℃ and under a vacuum degree not higher than -0.09MPa; S22, weigh out the dehydrated long-suspension chain vegetable oil polyol, polyether polyol, chain extender, latent curing agent, coupling agent, silane coupling agent modified nano silica, leveling agent, compound defoamer and catalyst according to the weight parts, and vacuum defoam and stir at 20°C for 1.5h until the mixture is uniform to obtain component B; wherein, the latent curing agent and catalyst are added just before use.

[0084] S3. Resin preparation: Component A and component B are mixed at an isocyanate index R = 1.05 to obtain the polyurethane structural resin for the composite tower; wherein, the isocyanate index R is the ratio of the isocyanate group equivalent in component A to the sum of the hydroxyl equivalent in component B and the active hydrogen equivalent released by the complete hydrolysis of the latent curing agent.

[0085] An application of the above-mentioned polyurethane structural resin for composite towers in the preparation of glass fiber reinforced polyurethane composite towers by winding: After mixing the above components A and B according to the isocyanate index R, they are used for winding or pultrusion molding of glass fiber reinforced polyurethane composite towers.

[0086] During the winding process, the temperature of the impregnation tank is 20℃, the resin gel time is 60min, and the curing regime is such as curing at 80℃ for 2h or curing at 120℃ for 2h.

[0087] The glass fiber content is 70% by volume.

[0088] Example 4

[0089] Everything else is the same as in Example 1, except that: In component A, diphenylmethane diisocyanate was replaced with isophorone diisocyanate, and the reaction temperature of S12 was adjusted from 80℃ to 100℃. At the same time, during the prepolymer reaction of component A, dibutyltin dilaurate, accounting for 0.05wt% of the isocyanate prepolymer mass, was added as a catalyst to ensure complete reaction.

[0090] Example 5

[0091] Everything else is the same as in Example 1, except that: Replace PolyTHF 1000 in component A with PolyTHF 2000 (and adjust the isocyanate feed amount accordingly to keep the -NCO content at 14wt%).

[0092] Example 6

[0093] Everything else is the same as in Example 1, except that: The long-suspension chain vegetable oil polyol is cashew nut shell oil polyol (C15 long fatty suspension chain), model number Cardläne NX-9001 (hydroxyl value approximately 175 mg KOH / g).

[0094] Example 7

[0095] Everything else is the same as in Example 1, except that: The long-suspension chain vegetable oil polyol is castor oil polyol (C18 long fatty suspension chain), model PolycinGR-50 (hydroxyl value approximately 52 mg KOH / g).

[0096] Example 8

[0097] Everything else is the same as in Example 1, except that: The long-suspension-chain vegetable oil polyol is castor oil polyol (C18 long fatty suspension chain), specifically a high-hydroxyl-value polyol (hydroxyl value 584 mg KOH / g) modified by alcoholysis of castor oil and glycerol under alkaline catalysis. The preparation steps are as follows: Castor oil and glycerol are added to a reaction vessel at a mass ratio of 1:0.6, heated to 200°C under nitrogen protection, and an alkaline catalyst (lithium hydroxide, 0.2% of the total material mass) is added. The mixture is then stirred and subjected to alcoholysis (ester exchange) for 3 hours. Byproducts are removed under reduced pressure, and after cooling, the mixture is neutralized with acid and dehydrated to obtain a high-hydroxyl-value castor oil polyol (C18 long fatty suspension chain) with a hydroxyl value of 584 mg KOH / g.

[0098] Example 9

[0099] Everything else is the same as in Example 1, except that: The long-suspension-chain vegetable oil polyol is arachidonic acid glyceride polyol (C20 long fatty acid suspension chain). Its preparation method is as follows: arachidic acid (eicosanoic acid) and glycerol are added to a reaction vessel at a molar ratio of 1.5:1, along with an esterification catalyst (lithium hydroxide). The reaction is carried out at 180°C for 4 hours under nitrogen protection. The generated water is removed under reduced pressure, and after cooling, arachidonic acid glyceride polyol with a hydroxyl value of approximately 172 mgKOH / g is obtained.

[0100] Example 10

[0101] Everything else is the same as in Example 1, except that: The trifunctional polyether polyol accounts for 60 wt% of the total mass of the polyether polyol.

[0102] Example 11

[0103] Everything else is the same as in Example 1, except that: The trifunctional polyether polyol accounts for 100 wt% of the total mass of the polyether polyol.

[0104] Example 12

[0105] Everything else is the same as in Example 1, except that: The latent curing agent is a mixture of Incozol 2, Incozol LV and Evonik's Vestamin A139 in a mass ratio of 1:1:1.

[0106] Example 13

[0107] Everything else is the same as in Example 1, except that: The compound defoamer is a mixture of BYK-066N and fluorine-modified organosilicon defoamer at a mass ratio of 1:1.

[0108] Example 14

[0109] Everything else is the same as in Example 1, except that: The compound defoamer is a mixture of BYK-066N and fluorine-modified organosilicon defoamer at a mass ratio of 3:1.

[0110] Example 15

[0111] Everything else is the same as in Example 1, except that: Component A and component B are mixed at an isocyanate index R = 0.9.

[0112] Example 16

[0113] Everything else is the same as in Example 1, except that: Mix component A and component B at an isocyanate index R = 1.10.

[0114] The following comparative examples are all compared with specific embodiment 1: Comparative Example 1 Everything else is the same as in Example 1, except that: The hard segment content in the cured resin product is 20 wt%. Specifically, the amount of 1,4-butanediol is reduced from 6 parts to 1 part, and the -NCO content of component A is adjusted from 14 wt% to 9 wt%.

[0115] Comparative Example 2 Everything else is the same as in Example 1, except that: The hard segment content in the cured resin product is 45 wt%. Specifically, the amount of 1,4-butanediol is increased from 6 parts to 12 parts, and the -NCO content of component A is adjusted from 14 wt% to 18 wt%.

[0116] Comparative Example 3 Everything else is the same as in Example 1, except that: The long-suspension chain vegetable oil polyol is replaced with methyl oleate (hydroxyl value of approximately 0 mg KOH / g, no hydroxyl function).

[0117] Comparative Example 4 Everything else is the same as in Example 1, except that: The long-suspension-chain vegetable oil polyol is an ultra-high hydroxyl value polyol (hydroxyl value 711 mg KOH / g) modified by deep alcoholysis of castor oil and pentaerythritol. Its preparation method is as follows: Castor oil and pentaerythritol are added to a reaction vessel at a mass ratio of 1:0.4, heated to 220°C under nitrogen protection, and an alkaline catalyst (lithium hydroxide, 0.2%) is added. The alcoholysis reaction is stirred for 4 hours, followed by cooling, acid neutralization, and dehydration to obtain an ultra-high hydroxyl value castor oil polyol with a hydroxyl value of approximately 711 mg KOH / g.

[0118] Comparative Example 5 Everything else is the same as in Example 1, except that: The long-suspension-chain vegetable oil polyol is decanoic acid glyceride polyol (C10 suspended chain). Its preparation method is as follows: Decanoic acid and glycerol are added to a reaction vessel at a molar ratio of 1.5:1, an esterification catalyst is added, and the reaction is carried out at 180℃ for 4 hours under nitrogen protection. The generated water is removed under reduced pressure, and after cooling, decanoic acid glyceride polyol with a hydroxyl value of approximately 202 mgKOH / g is obtained.

[0119] Comparative Example 6 Everything else is the same as in Example 1, except that: The long-suspension-chain vegetable oil polyol is behenic acid glyceride polyol (C22 suspension chain). Its preparation method is as follows: behenic acid and glycerol are added to a reaction vessel at a molar ratio of 1.5:1, an esterification catalyst is added, and the reaction is carried out at 190℃ for 4 hours under nitrogen protection. The generated water is removed under reduced pressure, and after cooling, behenic acid glyceride polyol with a hydroxyl value of approximately 187 mgKOH / g is obtained.

[0120] Comparative Example 7 Everything else is the same as in Example 1, except that: The trifunctional polyether polyol accounts for 50 wt% of the total mass of the polyether polyol.

[0121] Comparative Example 8 Everything else is the same as in Example 1, except that: The amount of latent curing agent added is 0 parts; that is, no latent curing agent was added.

[0122] Comparative Example 9 Everything else is the same as in Example 1, except that: Replace the compound defoamer with BYK-066N single defoamer.

[0123] Comparative Example 10 Everything else is the same as in Example 1, except that: The compound defoamer was replaced with a single fluorinated modified silicone defoamer.

[0124] Comparative Example 11 Everything else is the same as in Example 1, except that: The amount of KH-550 modified nano silica added was 0 parts; that is, no KH-550 modified nano silica was added.

[0125] Comparative Example 12 Everything else is the same as in Example 1, except that: The KH-550 modified nano silica was replaced with unmodified nano silica.

[0126] The physical properties of the polyurethane structural resin and glass fiber reinforced polyurethane composite material used in the embodiments and comparative examples of this invention are shown in Table 1.

[0127] Table 1 Physical performance tests of each embodiment

[0128] First, Table 1 shows that Examples 1-16 of the present invention have tensile strength > 60 MPa, tensile modulus ≥ 2.5 GPa, elongation at break > 3.0%, heat distortion temperature > 70℃, axial tensile strength > 330 MPa, axial compression > 290 MPa, and axial bending > 310 MPa; simultaneously, the bubble porosity is 0.31%-0.71% and the water absorption rate is 0.48%-0.92%. This indicates that the resin of the present invention possesses high strength and high modulus, bubble-free curing, low water absorption and water resistance, and high interfacial strength.

[0129] Examples 1 and Comparative Examples 1-2 show that the hard segment content must be controlled between 25% and 40%. In Comparative Example 1, when the hard segment content was reduced to 20%, the modulus and heat distortion temperature decreased significantly; in Comparative Example 2, when the hard segment content was increased to 45%, the elongation at break plummeted to 1.59%, resulting in brittle fracture. This is because the hard segment micro-regions act as physical cross-linking points, bearing the load; too low a content leads to insufficient cross-linking, while too high a content results in loss of toughness.

[0130] Examples 1 and Comparative Examples 3-6 demonstrate that long-chain plant oil polyols must possess both hydroxyl activity and an appropriate chain length. Comparative Example 3, after replacing methyl oleate with a non-hydroxyl-containing compound, showed severely incomplete curing, with a tensile strength of only 25.6 MPa and a porosity as high as 8.52%. Comparative Example 4, when the hydroxyl value increased to 711 mg KOH / g, experienced over-crosslinking, resulting in an elongation at break of only 1.04%. Comparative Example 5, when the chain lengthened to C10, saw its water absorption increase to 1.69%. Comparative Example 6, when the chain lengthened to C22, crystallization reduced the elongation at break to 2.52%. Therefore, a C15-C20 chain length and a hydroxyl value of 50-600 mg KOH / g are crucial for achieving a balance between curing properties, hydrophobicity, and toughness.

[0131] Example 1 and Comparative Example 7 show that the proportion of trifunctional polyether polyol must be above 60 wt%; when the proportion of Comparative Example 7 is reduced to 50 wt%, the modulus and heat distortion temperature both deteriorate, indicating that insufficient chemical crosslinking points make it difficult to form a high-strength, high-modulus network.

[0132] Example 1 and Comparative Example 8 show that the latent curing agent is the key to suppressing foam throughout the process; after the removal of the latent curing agent in Comparative Example 8, the bubble porosity increased to 4.84% and the tensile strength decreased to 48.8 MPa, indicating that if the carbon dioxide generated by moisture is not blocked, bubble defects will be formed and the mechanical properties will be significantly weakened.

[0133] Examples 1 and Comparative Examples 9-10 show that compound defoamers are superior to single defoamers; when only a single component was used in Comparative Examples 9 and 10, the porosity increased significantly, confirming the hierarchical defoaming synergy of organosilicon and fluorine-modified components.

[0134] Examples 1 and Comparative Examples 11-12 show that silane coupling agent modification of nano-silica is the key to interfacial bonding; when no addition was made in Comparative Example 11 and no modification was made in Comparative Example 12, the axial tensile strength was significantly deteriorated, indicating that the construction of a three-level interfacial network of "matrix-nano-silica-glass fiber" through chemical bonding has a positive effect on improving the axial strength of the composite material.

[0135] In summary, this invention achieves a combination of high strength and high modulus, bubble-free curing, low water absorption and water resistance, and high interfacial strength through multiple synergistic processes, including hard segment microphase separation enhancement, long suspended chain hydrophobic barrier, latent curing agent graded defoaming, and modified nano silica interfacial bonding. This makes the resin suitable for the winding or pultrusion molding of composite material towers.

[0136] The testing method is as follows: (1) Tensile strength, tensile modulus of elasticity and elongation at break: tested according to the methods described in GB / T 1040.2-2022.

[0137] (2) Heat distortion temperature: Tested according to the method described in GB / T 1634.2-2019.

[0138] (3) Axial tension: Tested according to the method described in GB / T 1447-2005.

[0139] (4) Axial compression: Tested according to the method described in GB / T 1448-2005.

[0140] (5) Axial bending: Tested according to the method described in GB / T 1449-2005.

[0141] (6) Bubble porosity: The porosity of the solidified product was statistically analyzed by image method after polishing the cross-section using a metallographic microscope.

[0142] (7) Water absorption rate: Tested according to the method described in GB / T 1034-2008.

[0143] Based on the above-described preferred embodiments of the present invention, and through the foregoing description, those skilled in the art can make various changes and modifications without departing from the inventive concept. The technical scope of this invention is not limited to the contents of the specification, but must be determined according to the scope of the claims.

Claims

1. A polyurethane structural resin for composite material towers, characterized in that, It consists of component A and component B; Component A is an isocyanate prepolymer obtained by reacting aromatic isocyanates and / or aliphatic isocyanates with polytetrahydrofuran ether diol, wherein the -NCO content in the prepolymer is 10-18 wt%. Component B, by weight, is composed of the following raw materials: 40-70 parts of long-suspension chain plant oil polyols; 20-40 parts of polyether polyol; Chain extender 2-10 parts; Latent curing agent 1.0-5.0 parts; 0.5-3.0 parts of coupling agent; 0.5-3.0 parts of silane coupling agent modified nano-silica; Leveling agent 0.1-1.0 parts; Compound defoamer 0.1-1.0 parts; Catalyst 0.1-0.5 parts; The long-suspension-chain plant oil polyol has a hydroxyl value of 50-600 mg KOH / g.

2. The polyurethane structural resin for composite material towers according to claim 1, characterized in that, The hard segment content in the cured resin product is 25-40 wt%; the hard segment is a rigid segment formed by the reaction of isocyanate and chain extender.

3. The polyurethane structural resin for composite material towers according to claim 1, characterized in that, The long-suspension-chain plant oil polyol has long fatty suspension chains of C15-C20, which extend laterally in the solidified network to form a comb-shaped / brush-shaped molecular structure.

4. The polyurethane structural resin for composite material towers according to claim 3, characterized in that, The long-suspension chain vegetable oil polyol is at least one of cashew nut shell oil polyol and castor oil polyol.

5. The polyurethane structural resin for composite material towers according to claim 1, characterized in that, The latent curing agent is an oxazolidine latent curing agent and / or an imine latent curing agent; The oxazolidine latent curing agent is a monooxazolidine and / or a bisoxazolidine, and the imine latent curing agent is an aldehydeimine and / or a ketimine.

6. The polyurethane structural resin for composite material towers according to claim 1, characterized in that, The amount of the latent curing agent used is such that the amount of active hydrogen released after complete hydrolysis is not less than the amount of isocyanate groups in component A that can participate in the side reaction with water.

7. The polyurethane structural resin for composite material towers according to claim 1, characterized in that, The polyether polyols comprise more than 60 wt% of the total mass of the polyether polyols, with a number average molecular weight of 300-6000; the remainder comprises difunctional polyether polyols with a number average molecular weight of 500-2000.

8. The polyurethane structural resin for composite material towers according to claim 1, characterized in that, The compound defoamer is a mixture of organosilicon polysiloxane defoamer and fluorine-modified organosilicon defoamer in a mass ratio of (1-3):

1.

9. A method for preparing a polyurethane structural resin for composite material towers according to any one of claims 1-8, characterized in that, Includes the following steps: S1, react aromatic isocyanate and / or aliphatic isocyanate with polytetrahydrofuran ether diol at 60-120℃ to obtain component A with a -NCO content of 10-18wt%. S2, long suspended chain vegetable oil polyol, polyether polyol, chain extender, latent curing agent, coupling agent, silane coupling agent modified nano silica, leveling agent, compound defoamer and catalyst are vacuum degassed and mixed at 20-50℃ to obtain component B; S3, Component A and Component B are mixed at an isocyanate index R = 0.90-1.10 to obtain the polyurethane structural resin for the composite tower.

10. The application of the resin according to any one of claims 1-8 in the preparation of glass fiber reinforced polyurethane composite towers by winding or pultrusion molding, characterized in that, The curing temperature for the winding process is 60-120℃.