High-strength wear-resistant nylon / basalt fiber biomimetic structure composite material and preparation method thereof
By using a multi-level interlocking laminated structure of modified basalt fiber and nylon 66 matrix and a microencapsulated polytetrafluoroethylene self-lubricating phase, the problems of insufficient strength and high wear of nylon composite materials under heavy load and high speed conditions are solved, achieving the effects of high strength, low friction, high modulus and high temperature creep resistance.
Patent Information
- Application Number
- CN202611095296.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-22
- Publication Date
- 2026-11-24
AI Technical Summary
Existing nylon composite materials suffer from insufficient strength, high wear, and significant damage to mating pairs under heavy loads, high speeds, or alternating dry and wet conditions. In particular, the poor interfacial compatibility between basalt fibers and the nylon matrix leads to fiber pull-out and insufficient interlaminar shear strength.
Low melt viscosity nylon 66 is used as the continuous phase and short-cut basalt fiber as the reinforcing phase. The fiber surface is modified by biopolysaccharide-silane coupling to form a multi-level interlocking layered structure. Combined with microencapsulated polytetrafluoroethylene as a solid lubricating phase, a nacreous layered biomimetic structure is constructed to achieve strong interfacial bonding and self-lubricating effect between the fiber and the matrix.
It significantly improves the specific strength, specific modulus, and high-temperature creep resistance of composite materials, reduces the coefficient of friction and volumetric wear rate, extends the life of the wear pair, and increases the heat distortion temperature.
Smart Images

Figure CN123152279A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of high-performance thermoplastic composite materials technology, specifically relating to a high-strength, wear-resistant nylon / basalt fiber biomimetic structural composite material and its preparation method. Background Technology
[0002] Nylon (PA) series engineering plastics have become important candidate materials for replacing metals in the manufacture of wear-resistant structural components such as bearings, gears, and pulleys due to their advantages such as lightweight, chemical resistance, self-lubrication, and ease of molding. However, pure nylon suffers from defects such as easy creep, low heat distortion temperature, and high wear rate under heavy load, high speed, or dry-wet alternating conditions, which seriously limit its service life and reliability in high-end equipment. Traditional reinforcement methods often use chopped glass fibers (GF) or carbon fibers (CF), which can improve strength and modulus, but bring new problems such as high cost, poor interfacial wetting, large scratches on the surface of the wear pair, and difficulty in recycling.
[0003] Basalt fiber (BF), a high-performance inorganic fiber made from the melting and drawing of natural volcanic rock, has higher tensile strength, elastic modulus, temperature resistance and chemical stability than alkali-free glass fiber (E-GF). It also has a wide range of raw material sources and a low carbon footprint, and is hailed as a "new green industrial material for the 21st century".
[0004] For example, in patent CN116426120A, it is pointed out that basalt fibers have problems such as fiber pull-out and insufficient interlaminar shear strength due to their high surface polarity and poor compatibility with the nylon matrix interface.
[0005] However, the high surface polarity of basalt fibers and their poor interfacial compatibility with the nylon matrix lead to severe fiber pull-out, low interlaminar shear strength of the composite material, and easy formation of brittle wear debris during wear, which accelerates damage to the mating pairs.
[0006] Therefore, how to fully utilize the reinforcing potential of basalt fiber and simultaneously improve the friction reduction and wear resistance of nylon matrix without damaging the wear pair has become a technical bottleneck that urgently needs to be overcome in this field. Summary of the Invention
[0007] To overcome the problems existing in the prior art, the present invention aims to provide a high-strength, wear-resistant nylon / basalt fiber biomimetic structural composite material and its preparation method. The composite material prepared by this method exhibits improved specific strength and specific modulus, high-temperature creep resistance, reduced friction coefficient and volumetric wear rate, and extended wear life of mating pairs. This solves the problems of insufficient strength, high wear, and significant damage to mating pairs in traditional nylon composite materials under heavy-load, high-speed, dry / wet alternating operating conditions.
[0008] To achieve the above objectives, the technical solution adopted by the present invention is as follows: A high-strength and wear-resistant nylon / basalt fiber biomimetic structural composite material uses nylon 66 (PA66) with low melt viscosity and fast crystallization rate as the continuous phase, short-cut basalt fiber (BF) with surface modification by biopolysaccharide-silane coupling as the reinforcing phase, and microencapsulated polytetrafluoroethylene (m-PTFE) as the solid lubricating phase. Furthermore, the modified BF and m-PTFE form a nacreous layer in the PA66 matrix. The material interior consists of a hard reinforcing thin layer (brick phase) composed of modified basalt fiber and a soft matrix thin layer (mortar phase) composed of PA66 nylon resin. The two thin layers are stacked alternately along the thickness direction, and the fiber layers are arranged in a 0° / 90° orthogonal orientation. The microencapsulated polytetrafluoroethylene m-PTFE is uniformly dispersed in the nylon matrix thin layer. The layers are tightly bonded by strong interfaces constructed by biopolysaccharides and silanes, forming a multi-level interlocking layered biomimetic structure. Unlike ordinary hybrid composite materials with randomly dispersed fibers, it achieves a synergistic improvement in high strength, high modulus, creep resistance, and wear resistance and lubrication by alternating stacking of soft and hard layers.
[0009] The modified short-cut basalt fiber is a continuous fiber segment of 50–100 mm, with a single filament diameter of 7–13 μm and a shear strength at the interface between the surface and the PA66 matrix ≥45 MPa. The m-PTFE has an average particle size of 20–80 μm, a core material of pure PTFE, a wall material of thermoplastic polyimide (TPI), a wall thickness of 0.5–2 μm, and a mass percentage of 3–8% in the PA66 matrix. It can controllably release PTFE under frictional heat to form an in-situ transfer lubricating film. The total fiber volume fraction of the composite material is controlled at 25–40% (referring to the proportion of modified basalt fiber in the total volume of the composite material, achieved through step 4.2) and oriented to the designed number of 25–40 layers. The fiber direction of each layer is orthogonally alternated at 0° / 90°. The interlaminar shear strength is ≥70MPa, the dry / wet friction coefficient is reduced by more than 50% compared with pure PA66, and the volume wear rate is reduced by more than 70%.
[0010] A method for preparing a high-strength, wear-resistant nylon / basalt fiber biomimetic structural composite material includes the following steps: Step 1): Basalt fiber precursor is calcined to remove the surface wetting agent, and then subjected to low-temperature oxygen plasma treatment to obtain surface-active hydroxylated BF; Step 2): Immediately immerse the BF obtained in Step 1) in a chitosan-lactic acid solution for ultrasonic impregnation, rinse with deionized water, and then vacuum dry to complete the grafting of biopolysaccharides and obtain BF; Step 3): Immerse the BF obtained in Step 2) in 1~3wt% KH-560 anhydrous ethanol solution, adjust the pH with acetic acid, reflux the reaction, remove and vacuum solidify to obtain the final modified BF; Step 4): The modified BF is solution pre-impregnated and oriented lay-up to obtain a pre-impregnated preform; Step 5): The pre-impregnated blank obtained in Step 4) is placed into a mold preheated to 270~290℃ and subjected to two-step hot pressing to obtain a high-strength wear-resistant nylon / basalt fiber biomimetic structural composite material.
[0011] In step 1), the basalt fiber precursor is calcined at 350~450℃ for 3~8min to remove the surface wetting agent. The conditions for low-temperature oxygen plasma treatment are: power 200~400W, atmosphere O2 150~250sccm, time 200~400s.
[0012] Step 2) specifically refers to: The chitosan-lactic acid solution is 0.3~0.8wt%, pH 4.5~5.5, temperature 40~60℃, ultrasonically impregnated for 20~40min, rinsed with deionized water and then vacuum dried at 70~90℃ for 1.5~3h.
[0013] Step 3) specifically involves: adjusting the pH to 4.0-5.0 with acetic acid, refluxing at 50-70°C for 1-3 hours, and then vacuum curing at 100-120°C for 0.5-2 hours.
[0014] Step 4) specifically refers to: Step 4.1) Preparation of nylon matrix solution: Dissolve 100 parts of PA66 resin in a mixed solvent of formic acid and dichloromethane (volume ratio 1:1, solid content 10~25wt%), stir at 50~70℃ until completely dissolved; add 2~10 parts of m-PTFE, 0.3~0.8 parts of antioxidant 1098, and 0.1~0.5 parts of lubricant EBS, and ultrasonically disperse for 20~40 min to obtain a uniform casting solution; Step 4.2) Oriented Fiber Layup: Using an oriented fiber layup device (a comb plate with parallel grooves, groove width 300~600μm, groove depth 100~300μm, and adjustable interlayer spacing), the modified BF (continuous fiber segments with a length of 50~100mm) obtained in Step 3) is oriented layer by layer: The fiber bundles are inserted parallel to the grooves of the comb plate, and a pre-tightening force of 3~15N is applied to keep the fibers taut; the fiber directions of each layer are alternately laid at 0° / 90° orthogonal; after each layer is laid, the casting solution is evenly coated on the surface of the fiber layer to fully impregnate the resin. Repeat the layup until the designed number of layers (20~40 layers, fiber volume fraction 20~40%); cover with release film, vacuum dry at 50~80℃ for 2~6h to remove solvent, and obtain pre-impregnated preform; Step 5) involves two hot pressing steps: Pre-compression stage: 270~290℃, 3~10MPa, 5~15min, to allow the resin to melt and flow and remove residual solvent; Molding stage: 285~310℃, 10~20MPa, vacuum degree ≤–0.05MPa~–0.10MPa, 15~30min, to ensure tight bonding between layers; cold pressing and shaping: holding pressure 5~20MPa, cooling to 60~100℃ for demolding, to obtain the high-strength wear-resistant nylon / basalt fiber biomimetic structural composite material plate.
[0015] In step 5, a high-temperature release agent is sprayed onto the mold surface, and the vacuum degree is ≤–0.03MPa~–0.10MPa to ensure that there are no air bubbles between layers and that the fiber volume fraction is accurately controllable.
[0016] The above-mentioned high-strength wear-resistant nylon / basalt fiber biomimetic structural composite material is used in the manufacture of high-end bearings, gears, worm gears, slide plates, guide rails and underwater friction pair components.
[0017] The beneficial effects of this invention are: This invention employs a synergistic interface modification process using "biopolysaccharide-silane" (Step 1) oxygen plasma treatment to generate active hydroxyl groups on the BF surface; Step 2) chitosan-biopolysaccharide grafting to introduce amino and hydroxyl groups; and Step 3) KH-560 silane coupling secondary treatment to chemically bond the silane ends to the PA66 matrix. This creates a dual network of chemical bonds and hydrogen bonds between the basalt fiber and the PA66 matrix, increasing the interlaminar shear strength by more than 50% compared to unmodified basalt fiber and resolving fiber pull-out issues. The introduction of hot-melt m-PTFE microcapsules, triggered by frictional heat, continuously releases PTFE, forming a uniform transfer film on the friction pair surface, achieving a synergistic "self-lubrication-self-repair" effect. The dry / wet friction coefficient is consistently ≤0.18, and the volumetric wear rate is ≤1.5×10⁻⁶. -6 mm³ / N·m; Through a three-step process of "solution pre-impregnation - directional layup - hot pressing", (step 4.2 uses a comb-plate directional layup device to lay 25-40 layers of modified BF in alternating 0° / 90° directions; step 5 hot pressing melts PA66 resin to fill the fiber gaps, forming a multi-level nacreous biomimetic structure of brick-mortar with modified BF as the hard "brick" phase and PA66 matrix as the soft "mortar" phase), this invention achieves a fiber arrangement regularity of more than 90% by directional layup of basalt fibers modified with biopolysaccharides and silanes through comb-plate directional layup, and constructs a nacreous brick-mortar laminated structure by alternating 0° / 90° directions. On the one hand, the highly regular directional arrangement of basalt fibers itself has high specific strength and high specific modulus. The orthogonal layup allows for uniform in-plane load-bearing in both directions. Combined with the strong interface of chemical bonds and hydrogen bonds between the fiber and the PA66 matrix, it can efficiently transfer stress and prevent fiber pull-out. At the same time, the rigid fiber layer bears the load, while the soft nylon matrix layer passes off cracks. The multi-layered structure can deflect and dissipate crack energy. These multiple effects result in a 110% increase in specific strength and a 130% increase in specific modulus of the composite material. On the other hand, the regular and continuous high-rigidity fiber skeleton can restrain the high-temperature slippage of nylon polymer chains. The dense orthogonal layup forms a physical barrier to inhibit resin melt flow. The strong interface can also prevent interfacial slippage between the fiber and the matrix at high temperatures, significantly improving the material's high-temperature creep resistance and deformation resistance. Ultimately, the heat distortion temperature is increased by 70°C compared to pure nylon.
[0018] This invention constructs a nacreous layered biomimetic structure with fiber orientation and alignment of >90%, resulting in a 110% increase in specific strength, a 130% increase in specific modulus, and a 70°C increase in heat distortion temperature of the composite material. It also achieves lightweight, high strength, wear resistance, and high-temperature creep resistance. Basalt fiber is widely available, low in cost, and environmentally friendly. The composite material is recyclable and reprocessable, meeting multiple development needs for resource conservation, energy saving and emission reduction, circular economy, and lightweighting of high-end equipment, thus possessing significant social and economic benefits. (See attached figures.) Figure 1 This is a schematic diagram of the biomimetic "pearl-like" layered structure described in this invention.
[0019] Figure 2 This is a schematic diagram of the cross-sectional morphology of m-PTFE microcapsules.
[0020] Figure 3 This is a schematic diagram of the controlled release mechanism of PTFE according to the present invention.
[0021] Figure 4 This is a flowchart of the composite material preparation process described in this invention. Detailed Implementation
[0022] The present invention will now be described in further detail with reference to the accompanying drawings.
[0023] Example 1 1) Basalt fiber short filaments (4.5 mm in length) were calcined at 400°C for 5 min → oxygen plasma at 300W for 300 s → ultrasonicated at 50°C for 30 min with 0.5 wt% chitosan solution → vacuum dried at 80°C for 2 h → refluxed at 60°C with 2 wt% KH-560 ethanol solution for 2 h → cured at 110°C for 1 h to obtain modified BF; 2) m-PTFE was prepared by solvent evaporation method: PTFE to TPI mass ratio 70:30, NMP concentration 15%, emulsification speed 12000 rpm, spray drying inlet temperature 180°C, thermal imidization 220°C / 2h, to obtain microcapsules with an average particle size of 45 μm and a wall thickness of 1.2 μm. 3) Dissolve 100 parts of PA66 in a mixed solvent of formic acid / dichloromethane (1:1, solid content 18wt%), stir at 60°C to dissolve, then add 5 parts of m-PTFE, 0.5 parts of antioxidant 1098, and 0.3 parts of EBS, and ultrasonically disperse for 30 min to obtain a casting solution; use a directional comb plate device (groove width 450μm) to lay modified BF (length 80mm) in 0° / 90° orthogonal layers, coat each layer with the casting solution, lay 30 layers in total, and vacuum dry at 60° for 4 h to obtain a prepreg blank; 4) The pre-impregnated blank is placed into a preheated mold at 280°C, pre-pressed at 280°C / 5MPa for 10 minutes, vacuum-pressed at 295°C / 15MPa (vacuum degree -0.08MPa) for 20 minutes, and then cooled to 80°C to demold to obtain a 4mm thick composite board. 5) Process tensile, bending, and friction specimens according to ISO 527, ISO 178, and ASTM D3702 standards, and conduct mechanical and tribological tests.
[0024] Example 2 Prepared by steps 1)–5) of Example 1, wherein the mass fraction of modified BF in step 3) is adjusted to 35.
[0025] Example 3 Prepared by steps 1)–5) of Example 1, wherein the mass fraction of m-PTFE in step 3) is adjusted to 7.
[0026] Comparative Example 1 Using pure PA66 resin as raw material, a comparative sample was obtained by hot pressing in step 4).
[0027] Comparative Example 2 Comparative samples were prepared using 30 parts of unmodified basalt fiber (80 mm in length), 100 parts of PA66, and 5 parts of m-PTFE, and the same method (solution pre-impregnation-directional lay-up-hot pressing) was used.
[0028] Comparative Example 3 A comparative sample was prepared by replacing the modified BF with 30 parts of E-glass fiber (80 mm in length, treated with coupling agent A-1100), with the rest being the same as in Example 1.
[0029] Comparative Example 4 A comparative sample was prepared using 30 parts of modified BF, 100 parts of pure PA66, without the addition of m-PTFE, and the rest was the same as in Example 1.
[0030] Following the above method, the tensile strength, flexural strength, interlaminar shear strength, heat distortion temperature (HDT), dry / wet friction coefficient, and volumetric wear rate of Examples 1–3 and Comparative Examples 1–4 were tested respectively. The friction pair was a Ø10mm GCr15 steel ball-polymer disk, with a load of 20N, a linear velocity of 0.3m / s, and dry friction for 2 hours followed by adding deionized water for another 2 hours. The test temperature was 23°C, and the average of 5 tests was taken for each group. The results are shown in Tables 1 and 2.
[0031] Table 1 Mechanical and thermal properties of different materials Group Tensile strength MPa Flexural strength MPa Interlaminar shear rate (MPa) HDT℃ Example 1 210 280 72 210 Example 2 225 295 75 215 Example 3 205 275 70 208 Comparative Example 1 75 110 — 140 Comparative Example 2 165 220 48 190 Comparative Example 3 180 240 55 195 Comparative Example 4 200 265 68 205 Table 2 Tribological properties of different materials (dry → wet continuous test) Group dry friction coefficient wet friction coefficient Volumetric wear rate Example 1 0.16 0.14 1.35 Example 2 0.17 0.15 1.48 Example 3 0.15 0.13 1.28 Comparative Example 1 0.35 0.31 6.20 Comparative Example 2 0.28 0.25 3.90 Comparative Example 3 0.26 0.23 3.10 Comparative Example 4 0.22 0.19 2.50 As shown in Tables 1 and 2, compared with pure PA66, Examples 1–3 of the present invention, while maintaining the advantage of lightweight, exhibit tensile strength increased by 180–200%, flexural strength increased by 150–170%, interlaminar shear strength ≥70MPa, and HDT increased by 70℃; the dry / wet friction coefficient decreased by more than 50%, and the volumetric wear rate decreased by more than 70%; among them, Example 3 (m-PTFE 7%) showed the best overall performance. Comparative Examples 2 and 3 show that unmodified BF or GF, due to weak interfaces and large damage to the friction pairs, have significantly inferior friction performance compared to the present invention; Comparative Example 4 confirms that the wear rate is still higher than that of the examples even without m-PTFE, indicating that the synergy of "interface enhancement + self-lubrication" is the key to the performance breakthrough of the present invention.
[0032] Figure 1 The invention demonstrates the multi-scale structural features of the high-strength, wear-resistant nylon / basalt fiber biomimetic composite material, including: (a) Schematic diagram of pearl-like layered structure: It shows a brick-and-mortar biomimetic structure with alternating layers of modified basalt fiber as the hard brick phase (green layered structure) and PA66 matrix as the soft mortar phase (transparent layer). m-PTFE microspheres (gold spheres) are uniformly dispersed in the matrix layer to form a multi-scale biomimetic interlocking structure.
[0033] (b) Nylon / basalt fiber composite material: The three-dimensional macroscopic structure of the composite material is shown. PA66 continuous phase (white cube) is the matrix, m-PTFE microsphere capsules (gold spheres) are the solid lubricating phase, and modified basalt fiber (green layered structure) is the reinforcing phase. The three work together to form a pearl-like layered composite material.
[0034] (c) Schematic diagram of m-PTFE microsphere capsule structure: It shows the microcapsule structure with pure PTFE (white spheres) as the core material and thermoplastic polyimide (TPI) (gold shell) as the wall material. The spheres have a particle size of 20~80μm and the TPI wall thickness is 0.5~2μm. Under the action of frictional heat, the TPI wall material breaks and the core material PTFE is released in a controlled manner to form an in-situ transfer lubricating film.
[0035] (d) Modified basalt fiber: The structure of basalt fiber after synergistic surface modification by biopolysaccharide-silane is shown. Biopolysaccharide is grafted onto the fiber surface and formed a chemical bond + hydrogen bond dual network interface with PA66 matrix through a three-step process of step 1) low temperature oxygen plasma pretreatment, step 2) chitosan grafting, and step 3) KH-560 secondary coupling.
[0036] Figure 2 The core-shell structure of the microencapsulated polytetrafluoroethylene (m-PTFE) microspheres described in this invention is shown: Core material: Pure PTFE (white spheres), providing solid lubrication; Wall material: Thermoplastic polyimide (TPI) (gold shell), wall thickness 0.5~2μm, protects the core material PTFE from premature release at room temperature, softens and cracks under frictional heat, and achieves controlled release of PTFE; The sphere size is 20~80μm, which matches the processing flowability of PA66 matrix and facilitates uniform dispersion.
[0037] Figure 3 The invention demonstrates the controllable release and lubrication mechanism of m-PTFE microcapsules in a GCr15 steel ball-polymer disk friction pair, which is divided into three stages: (a) Initial contact stage: Under load, the GCr15 steel ball-polymer disk friction pair comes into contact with the surface of the PA66 / basalt fiber composite material. At this time, the m-PTFE microcapsules are dispersed in the PA66 matrix, the TPI wall material is intact, and an effective lubricating film has not yet formed on the surface of the composite material.
[0038] (b) Frictional heat-triggered release stage: As friction proceeds, frictional heat softens and melts the TPI wall material of the m-PTFE microcapsule, causing the wall material to rupture and the core material PTFE to be released from the microcapsule in a controlled manner, forming an initial lubricating substance at the friction interface.
[0039] (c) In-situ transfer lubricating film formation stage: The released PTFE is deposited and spread on the surface of the GCr15 steel ball-polymer disk friction pair to form a uniform friction-induced PTFE transfer film. This transfer film covers the surface of the friction pair, realizing a "self-lubricating-self-repairing" synergistic effect, and steadily reducing the dry / wet friction coefficient.
[0040] Figure 4 This is a flowchart of the composite material preparation process described in the embodiment. The embodiment includes three parallel modules: (a) Preparation of modified basalt fibers: pretreatment activation → chitosan grafting (0.5wt% chitosan solution, pH 5.0, 50℃, 30min) → silane coupling (2wt% KH-560, pH 4.5, 60℃, 2h); (b) Preparation of m-PTFE microsphere capsules: solvent evaporation method → high-speed emulsification → spray drying → thermal imidization (220℃ / 2h); (c) Preparation of nylon / basalt fiber composite material: casting solution preparation (PA66 dissolved in formic acid / dichloromethane, m-PTFE, antioxidant 1098, EBS added) → prepreg preparation (25~40 layers of 0° / 90° orthogonal layup) → compression molding (280℃ / 5MPa pre-compression for 10min → 295℃ / 15MPa vacuum compression for 20min → cooling and demolding).
Claims
1. A high-strength, wear-resistant nylon / basalt fiber biomimetic structural composite material, characterized in that, Nylon 66 (PA66) was used as the continuous phase, short-cut basalt fiber (BF) with synergistic surface modification via biopolysaccharide-silane coupling was used as the reinforcing phase, and microencapsulated polytetrafluoroethylene (m-PTFE) was used as the solid lubricating phase. Furthermore, the modified BF and m-PTFE are in the form of nacreous layers in the PA66 matrix. The material is composed of a hard reinforcing thin layer of modified basalt fiber and a soft matrix thin layer of PA66 nylon resin. The two thin layers are stacked alternately along the thickness direction. The fiber layers are arranged in a 0° / 90° orthogonal orientation. The microencapsulated polytetrafluoroethylene m-PTFE is uniformly dispersed in the nylon matrix thin layer. The layers are tightly bound together by strong interfaces constructed from biopolysaccharides and silanes, forming a multi-level interlocking layered biomimetic structure.
2. The high-strength, wear-resistant nylon / basalt fiber biomimetic structural composite material according to claim 1, characterized in that, The modified short-cut basalt fiber is a continuous fiber segment of 50–100 mm, with a single filament diameter of 7–13 μm and a shear strength at the interface between the surface and the PA66 matrix ≥45 MPa. The m-PTFE has an average particle size of 20–80 μm, a core material of pure PTFE, a wall material of thermoplastic polyimide with a wall thickness of 0.5–2 μm, and a mass percentage of 3–8% in the PA66 matrix.
3. The high-strength, wear-resistant nylon / basalt fiber biomimetic structural composite material according to claim 1, characterized in that, The total fiber volume fraction of the composite material is controlled at 25-40% and oriented to achieve the designed number of 25-40 layers. The fiber directions of each layer are orthogonally alternated at 0° / 90°, and the interlayer shear strength is ≥70MPa.
4. A method for preparing a high-strength, wear-resistant nylon / basalt fiber biomimetic structural composite material according to any one of claims 1-3, characterized in that, Includes the following steps: Step 1): Basalt fiber precursor is calcined to remove the surface wetting agent, and then subjected to low-temperature oxygen plasma treatment to obtain surface-active hydroxylated BF; Step 2): Immediately immerse the BF obtained in Step 1) in a chitosan-lactic acid solution for ultrasonic impregnation, rinse with deionized water, and then vacuum dry to complete the grafting of biopolysaccharides and obtain BF; Step 3): Immerse the BF obtained in Step 2) in 1~3wt% KH-560 anhydrous ethanol solution, adjust the pH with acetic acid, reflux the reaction, remove and vacuum solidify to obtain the final modified BF; Step 4): The modified BF is solution pre-impregnated and oriented lay-up to obtain a pre-impregnated preform; Step 5): The pre-impregnated blank obtained in Step 4) is loaded into a preheated mold and subjected to two-step hot pressing to obtain a high-strength wear-resistant nylon / basalt fiber biomimetic structural composite material.
5. The preparation method of a high-strength, wear-resistant nylon / basalt fiber biomimetic structural composite material according to claim 4, characterized in that, In step 1), the basalt fiber precursor is calcined at 350~450℃ for 3~8min to remove the surface wetting agent. The conditions for low-temperature oxygen plasma treatment are: power 200~400W, atmosphere O2 150~250sccm, time 200~400s.
6. The preparation method of a high-strength, wear-resistant nylon / basalt fiber biomimetic structural composite material according to claim 4, characterized in that, Step 2) specifically refers to: The chitosan-lactic acid solution is 0.3~0.8wt%, pH 4.5~5.5, temperature 40~60℃, ultrasonically impregnated for 20~40min, rinsed with deionized water and then vacuum dried at 70~90℃ for 1.5~3h.
7. The preparation method of a high-strength, wear-resistant nylon / basalt fiber biomimetic structural composite material according to claim 4, characterized in that, Step 3) specifically involves: adjusting the pH to 4.0-5.0 with acetic acid, refluxing at 50-70°C for 1-3 hours, and then vacuum curing at 100-120°C for 0.5-2 hours.
8. The preparation method of a high-strength, wear-resistant nylon / basalt fiber biomimetic structural composite material according to claim 4, characterized in that, Step 4) specifically refers to: Step 4.1): Dissolve 100 parts of PA66 resin in a mixed solvent of formic acid and dichloromethane at a volume ratio of 1:1 and a solid content of 10-25 wt%. Stir at 50-70°C until completely dissolved. Add 2-10 parts of m-PTFE, 0.3-0.8 parts of antioxidant 1098, and 0.1-0.5 parts of lubricant EBS. Disperse the solution ultrasonically for 20-40 minutes to obtain a uniform casting solution. Step 4.2): Using an oriented fiber layup device, the modified BF obtained in step 3) is oriented layer by layer: The fiber bundles are inserted parallel to the grooves of the comb plate, and a pre-tightening force of 3~15N is applied to keep the fibers taut; the fiber directions of each layer are alternately laid at 0° / 90° orthogonal; after each layer is laid, the casting solution is evenly coated on the surface of the fiber layer to fully impregnate the resin. Repeat the layup until the designed number of layers is reached; cover with release film, and vacuum dry at 50~80℃ for 2~6 hours to remove solvent, thus obtaining the pre-impregnated blank.
9. The method for preparing a high-strength, wear-resistant nylon / basalt fiber biomimetic structural composite material according to claim 4, characterized in that, Step 5) involves two hot pressing steps: Pre-compression stage: 270~290℃, 3~10MPa, 5~15min, to allow the resin to melt and flow and remove residual solvent; Molding stage: 285~310℃, 10~20MPa, vacuum degree ≤–0.05MPa~–0.10MPa, 15~30min, to ensure tight bonding between layers; cold pressing and shaping: holding pressure 5~20MPa, cooling to 60~100℃ for demolding, to obtain the high-strength wear-resistant nylon / basalt fiber biomimetic structural composite material plate.
10. The method for preparing a high-strength, wear-resistant nylon / basalt fiber biomimetic structural composite material according to claim 4, characterized in that, In step 5, a high-temperature release agent is sprayed onto the mold surface, and the vacuum degree is ≤–0.03MPa~–0.10MPa.
Citation Information
Patent Citations
Basalt fiber reinforced nylon 66 composite material and preparation method thereof
CN116426120A