A composite material for use in multilayer tubing and a method of making the same

By using COC and MXD6 or MXD10 alloys to replace EVOH or ETFE, combined with compatibilizers and antioxidants, the problems of decreased barrier performance and limited raw material supply in multilayer tubing were solved, achieving material stability and ease of processing, and reducing costs.

CN123152283APending Publication Date: 2026-11-24JIANGSU HAIJU NEW MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611472087.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-21
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

In existing automotive multilayer oil pipes, EVOH's barrier properties decrease after absorbing moisture, and the supply of raw materials is limited. ETFE is difficult to process and has poor compatibility, resulting in a narrow processing window and large cost fluctuations.

Method used

A multilayer tubing material is prepared by melt blending extrusion using cyclic olefin copolymer COC and m-phenylenediamine-based semi-aromatic nylon MXD6 or MXD10 as the barrier layer material, combined with maleic anhydride graft polymer as a compatibilizer, toughening agent and antioxidant, to form a COC/MXD6 or COC/MXD10 alloy to replace EVOH or ETFE.

Benefits of technology

It achieves stable barrier properties, has a wide range of raw material sources, reduces costs, has a wide processing window, high interlayer bonding strength, is not prone to delamination, and is suitable for processing with conventional equipment.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

This invention discloses a composite material for multilayer oil pipes and its preparation method, relating to the technical field of multilayer composite pipeline materials for automobiles. By weight, it comprises the following components: cyclic olefin copolymer (COC): 10-40 parts; m-phenylenediamine-based semi-aromatic nylon, selected from one or a mixture of two of poly(m-phenylenediamine adipamide) MXD6 and poly(m-phenylenediamine sebacate) MXD10: 40-80 parts; compatibilizer: 2-10 parts, wherein the compatibilizer is maleic anhydride-grafted polyolefin or maleic anhydride-grafted nylon; toughening agent: 1-8 parts; antioxidant: 0.1-1 part; lubricant: 0.1-0.5 parts. This composite material for multilayer oil pipes and its preparation method use a COC / MXD6 or COC / MXD10 composite alloy to replace EVOH or ETFE as the main raw material for the barrier layer. COC and MXD6 are commercial products from multiple domestic and international manufacturers, ensuring a wide range of raw material sources and reducing costs by not being limited by a single supplier.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of multilayer composite pipeline materials for automobiles, specifically a composite material for use in multilayer oil pipes and its preparation method. Background Technology

[0002] Existing automotive fuel lines or fuel delivery lines mostly employ multi-layered composite structures. The barrier layer often uses ethylene-vinyl alcohol copolymer (EVOH) or ethylene-tetrafluoroethylene copolymer (ETFE) combined with aliphatic nylon (such as PA6) and high-temperature nylon (such as PA9T / PPA9T). However, this technology has the following drawbacks: EVOH's barrier properties deteriorate significantly after absorbing moisture, and the raw materials are monopolized by a few foreign manufacturers, resulting in limited supply and large price fluctuations. ETFE has high processing temperature and poor compatibility with nylon layers, requiring a special bonding layer. Co-extrusion is difficult and the processing window is narrow. Therefore, we propose a composite material for multilayer tubing and its preparation method. Summary of the Invention

[0003] The purpose of this invention is to provide a composite material for multilayer tubing and its preparation method, in order to solve the problems mentioned in the background art where the barrier properties of EVOH in the composite material for multilayer tubing are severely reduced after moisture absorption, and the raw materials are monopolized by a few foreign manufacturers, resulting in limited supply and large price fluctuations.

[0004] To achieve the above objectives, the present invention provides the following technical solution: a composite material for use in multilayer tubing, comprising the following components by weight: cyclic olefin copolymer COC: 10-40 parts; m-Phenylenediamine is a semi-aromatic nylon selected from one or a mixture of two of poly(m-phenylenediamine adipate) MXD6 and poly(m-phenylenediamine sebacate) MXD10: 40-80 parts; Compatibilizer: 2-10 parts, wherein the compatibilizer is maleic anhydride-grafted polyolefin or maleic anhydride-grafted nylon; Toughening agent: 1-8 parts; Antioxidant: 0.1 to 1 part; Lubricant: 0.1–0.5 parts; The glass transition temperature (Tg) of the COC is 100–170°C, and the melting point of the MXD6 is 230–245°C.

[0005] Furthermore, the mass ratio of COC to m-phenylenediamine-based semi-aromatic nylon is (15-30):(55-70).

[0006] Furthermore, the maleic anhydride-grafted polyolefin is selected from one or more of maleic anhydride-grafted ethylene-octene copolymer POE-g-MAH and maleic anhydride-grafted low-density polyethylene LDPE-g-MAH; the maleic anhydride-grafted nylon is selected from one or more of maleic anhydride-grafted PA6 and maleic anhydride-grafted PA66.

[0007] Furthermore, the toughening agent is selected from one or more of ethylene-octene copolymer (POE), ethylene propylene diene monomer (EPDM), or acrylate toughening agent (MBS); the antioxidant is a compound of hindered phenolic antioxidant and phosphite antioxidant.

[0008] A method for preparing a composite material for multilayer tubing, comprising the following steps: S1. Premix: According to the formula, COC, m-phenylenediamine-based semi-aromatic nylon, compatibilizer, toughening agent, antioxidant and lubricant are added to a high-speed mixer and mixed evenly to obtain a premix; S2. Melt blending extrusion: The premixed material is added to a twin-screw extruder for melt blending extrusion. The screw length-to-diameter ratio L / D is 36-48:1, and the vacuum degree is ≤-0.06MPa. S3. Cooling, pelletizing, and drying yield the composite material.

[0009] Furthermore, in step S1, the m-phenylenediamine-based semi-aromatic nylon is first dried in a forced-air dryer at 80-100°C for 4-6 hours until the moisture content is <0.05%, and then the COC is dried at 60-80°C for 2-3 hours before being mixed with other additives.

[0010] This invention provides a composite material for use in multilayer tubing and its preparation method, which has the following advantages: This invention uses COC / MXD6 or COC / MXD10 composite alloy to replace EVOH or ETFE as the main raw material for the barrier layer. COC and MXD6 are commercial products from multiple domestic and foreign manufacturers, with a wide range of raw material sources, not limited by a single supplier, thus reducing costs; the alloy material has a moderate melt flow rate and can be processed at conventional nylon extrusion temperatures without the need for special high-temperature equipment, resulting in a wide processing window; after modification with a compatibilizer, the alloy and inner and outer layers such as PA12 / PA612 can achieve good interlayer peel strength through conventional bonding resins, resulting in good interlayer bonding and preventing delamination. Detailed Implementation

[0011] The embodiments of the present invention will be described in further detail below with reference to examples. These examples are for illustrative purposes only and should not be construed as limiting the scope of the invention.

[0012] In the specific implementation of this invention, the composite materials used in multilayer tubing are typically proportioned according to the following approach: First, cyclic olefin copolymer COC is selected as one of the matrix resins. COC has excellent chemical corrosion resistance and low permeability. Its glass transition temperature is controlled in the range of 100 to 170°C to ensure that the material maintains good dimensional stability and barrier performance in high-temperature fuel environments. The content of COC is generally controlled in the range of 10 to 40 parts by weight to ensure that it plays a sufficient oil-blocking role in the alloy system, while also taking into account the processing fluidity. Secondly, a semi-aromatic nylon based on m-phenylenediamine is selected as another main matrix component. Specifically, one or a mixture of poly(m-phenylenediamine adipamide) MXD6, poly(m-phenylenediamine sebacamide) MXD10, or both can be selected. MXD6 typically has a melting point of 230–245°C and exhibits good thermal compatibility with COC during melt blending. This component is generally used in amounts of 40–80 parts by weight, primarily serving to provide mechanical strength and high gas barrier properties. Due to the significant polarity difference between COC and MXD6 / MXD10, a compatibilizer is added to the system to improve the interfacial bonding between them. The compatibilizer is selected from maleic anhydride-grafted polyolefin or maleic anhydride-grafted nylon, preferably one or more of maleic anhydride-grafted ethylene-octene copolymer, maleic anhydride-grafted low-density polyethylene, maleic anhydride-grafted PA6 or maleic anhydride-grafted PA66. The amount of compatibilizer added is usually 2 to 10 parts by weight, which can form chemical or physical bonds between COC and nylon phases, reduce interfacial defects, and improve the overall performance of the alloy. To improve the toughness and impact resistance of composite materials, toughening agents are also introduced into the formulation. Specifically, one or more of the following can be selected: ethylene-octene copolymer (POE), ethylene propylene diene monomer (EPDM) rubber, or acrylate toughening agent (MBS). The dosage is 1 to 8 parts by weight. The toughening agent usually exists in the matrix in the form of a dispersed phase to absorb external impact energy and prevent the material from brittle fracture under low temperature or dynamic load. In addition, to prevent the material from degrading due to thermo-oxidative aging during processing and use, antioxidants are added to the system. Antioxidants are generally composed of hindered phenolic main antioxidants and phosphite auxiliary antioxidants, with a total dosage of 0.1 to 1 part by weight, which can effectively extend the service life of the material. To reduce the frictional resistance of the melt during extrusion and improve processing performance, the formulation also includes a lubricant, commonly calcium stearate or other fatty acid salts, in an amount of 0.1 to 0.5 parts by weight. In actual production, the content of each component can be adjusted appropriately within the above range according to the specific usage environment and performance requirements. For example, in applications requiring high barrier performance, the proportion of COC can be appropriately increased; in applications requiring higher mechanical performance, the amount of MXD6 or MXD10 can be appropriately increased.

[0013] The preparation of the above-mentioned composite materials is typically carried out using the following steps: Step S1: Premixing: First, the m-phenylenediamine-based semi-aromatic nylon is dried in a forced-air environment at 80–100°C for 4–6 hours to reduce its moisture content to below 0.05% to prevent hydrolysis during high-temperature processing; simultaneously, the COC is dried at 60–80°C for 2–3 hours. Then, the dried COC, m-phenylenediamine-based semi-aromatic nylon, compatibilizer, toughening agent, antioxidant, and lubricant are added to a high-speed mixer and mixed thoroughly to obtain a premix. The mixing time should be controlled during the premixing process to ensure uniform dispersion of all components and to prevent significant localized overheating.

[0014] Step S2: Melt Blending Extrusion: The premixed material is added to a twin-screw extruder for melt blending extrusion. The length-to-diameter ratio (L / D) of the twin-screw extruder is controlled between 36 and 48:1 to ensure sufficient residence time and shearing action of the material within the barrel, achieving thorough dispersion and interfacial bonding of the components. During extrusion, a vacuum of ≤-0.06 MPa is maintained to remove moisture and low-molecular-weight volatiles from the material, preventing bubbles or silver streaks in the final product. The temperature of each heating zone is set according to the characteristics of the raw material, ensuring that the material is blended in a stable molten state.

[0015] Step S3: Cooling, pelletizing, and drying: The molten strip extruded from the extruder die is cooled by water or air, then cut into pellets by a pelletizer. The pellets are then subjected to post-drying at 60–80°C to further remove residual moisture, yielding the composite material. The resulting pellets can be directly used for co-extrusion molding of multilayer tubing.

[0016] The composite material prepared above is particularly suitable for the barrier layer of multilayer oil pipes. In practical applications, this composite material can be used as an intermediate barrier layer, co-extruded with the inner layer, outer layer, and adhesive layer using multiple extruders. The inner and outer layers are typically made of long-chain nylon or high-temperature nylon, while the adhesive layer is made of modified polyolefin or copolyamide adhesive resin, thus forming a multilayer composite oil pipe with stable structure and low fuel permeability.

[0017] The above embodiments are merely preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, or improvements made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.

[0018] The embodiments of the present invention are given for illustrative and descriptive purposes only, and are not intended to be exhaustive or to limit the invention to the forms disclosed. Many modifications and variations will be apparent to those skilled in the art. The embodiments were chosen and described in order to better illustrate the principles and practical application of the invention, and to enable those skilled in the art to understand the invention and to design various embodiments with various modifications suitable for a particular purpose.

Claims

1. A composite material for use in multilayer tubing, characterized in that, By weight, it consists of the following components: cyclic olefin copolymer COC: 10-40 parts; m-Phenylenediamine is a semi-aromatic nylon selected from one or a mixture of two of poly(m-phenylenediamine adipate) MXD6 and poly(m-phenylenediamine sebacate) MXD10: 40-80 parts; Compatibilizer: 2-10 parts, wherein the compatibilizer is maleic anhydride-grafted polyolefin or maleic anhydride-grafted nylon; Toughening agent: 1-8 parts; Antioxidant: 0.1 to 1 part; Lubricant: 0.1 to 0.5 parts.

2. The composite material for use in multilayer tubing according to claim 1, characterized in that, The mass ratio of COC to m-phenylenediamine-based semi-aromatic nylon is (15-30):(55-70).

3. The composite material for use in multilayer tubing according to claim 1, characterized in that, The maleic anhydride-grafted polyolefin is selected from one or more of maleic anhydride-grafted ethylene-octene copolymer POE-g-MAH and maleic anhydride-grafted low-density polyethylene LDPE-g-MAH; the maleic anhydride-grafted nylon is selected from one or more of maleic anhydride-grafted PA6 and maleic anhydride-grafted PA66.

4. The composite material for use in multilayer tubing according to claim 1, characterized in that, The toughening agent is selected from one or more of ethylene-octene copolymer (POE), ethylene propylene diene monomer (EPDM), or acrylate toughening agent (MBS); the antioxidant is a compound of hindered phenolic antioxidant and phosphite antioxidant.

5. A method for preparing a composite material for multilayer tubing, used to prepare the composite material for multilayer tubing as described in claim 4, characterized in that, Includes the following steps: S1. Premix: According to the formula, COC, m-phenylenediamine-based semi-aromatic nylon, compatibilizer, toughening agent, antioxidant and lubricant are added to a high-speed mixer and mixed evenly to obtain a premix; S2. Melt blending extrusion: The premixed material is added to a twin-screw extruder for melt blending extrusion. The screw length-to-diameter ratio L / D is 36-48:1, and the vacuum degree is ≤-0.06MPa. S3. Cooling, pelletizing, and drying yield the composite material.

6. A method for preparing a composite material for multilayer tubing according to claim 5, characterized in that, In step S1, the m-phenylenediamine-based semi-aromatic nylon is first dried in a forced-air dryer at 80-100°C for 4-6 hours until the moisture content is <0.05%. Then, the COC is dried at 60-80°C for 2-3 hours and then mixed with other additives.