Nylon alloy for metal insulation extrusion and preparation method thereof

By combining amorphous copolymer nylon, polyphenylene ether, and modified styrene-glycidyl methacrylate copolymer, the problems of uneven coating and interface instability of existing metal insulating materials at low temperatures are solved, and continuous and uniform coating and long-term electrical insulation performance of complex metal components are achieved.

CN123152284APending Publication Date: 2026-11-24SHANDONG DONGCHEN ENG PLASTIC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611539288.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-30
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing metal insulating extruded materials are difficult to achieve good coating integrity, interface stability and long-term moisture resistance and thermal and electrical insulation performance at low temperatures. In particular, they are prone to insufficient adhesion, local gaps or uneven coating thickness on complex metal components, and are prone to cracking and delamination in high and low temperature cycles and salt water environments.

Method used

A combination of amorphous copolymer nylon, polyphenylene ether, maleic anhydride-grafted ethylene-octene copolymer elastomer, and protocatechuic acid-modified styrene-glycidyl methacrylate copolymer is used for melt mixing through segmented feeding to form a continuous and uniform metal insulating coating layer, reducing interfacial residual stress, improving interfacial bonding strength and electrical insulation stability in salt water environments.

Benefits of technology

At a lower extrusion temperature, continuous and uniform coating of complex metal components was achieved, which improved the material's resistance to thermal cycling cracking and electrical insulation stability in long-term salt water environment, reduced interface defects and moisture penetration, and enhanced the interaction between the material and the metal substrate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123152284A_ABST
    Figure CN123152284A_ABST
Patent Text Reader

Abstract

This application discloses a nylon alloy for metal insulation extrusion and its preparation method, belonging to the field of engineering plastics technology. The nylon alloy for metal insulation extrusion, by weight, comprises the following components: 65-90 parts of amorphous copolymer nylon; 5-15 parts of polyphenylene ether; 5-10 parts of maleic anhydride-grafted ethylene-octene copolymer elastomer; and 0.5-10 parts of additives; wherein the glass transition temperature of the amorphous copolymer nylon is 105-128℃. This nylon alloy for metal insulation extrusion enables low-temperature continuous single-layer extrusion coating of metal components, improves the wetting and adhesion of the insulation layer, reduces interfacial residual stress, and inhibits cracking, delamination, and pressure resistance attenuation under aging and thermal cycling.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to a nylon alloy for metal insulation extrusion and its preparation method, belonging to the field of engineering plastics technology. Background Technology

[0002] Metal conductors, aluminum busbars, copper busbars, and other metal components are widely used in rail transit traction converters, new energy power battery control systems, and energy storage equipment. To ensure safe operation, an insulating protective layer is typically formed integrally on the surface of these metal components through extrusion. These components are exposed to environments such as humid heat, alternating high and low temperatures, DC high voltage, and salt spray for extended periods, and some components have thin walls, sharp edges, bends, or complex irregular shapes. Therefore, the insulating material must not only maintain stable insulation resistance and withstand voltage performance but also adhere stably to the metal substrate, possess low molding shrinkage, good crack resistance, and adaptability to extrusion processing.

[0003] Currently, crystalline nylon is the main material used for metal insulation extrusion. Crystalline nylon has good mechanical strength and chemical resistance, but it is prone to crystallization shrinkage during molding. Amorphous nylon has a lower tendency to crystallize and a relatively smaller molding shrinkage rate, which can improve the shrinkage and cracking problems that easily occur during the extrusion of crystalline nylon. However, in long-term humid and hot, salt spray, and high-pressure environments, moisture can penetrate into the insulation material of pure amorphous nylon, leading to a decrease in the material's electrical insulation performance. At the same time, interface defects between the insulation layer and the metal substrate will gradually expand during high and low temperature cycling or long-term aging, resulting in delamination, cracking, or a decrease in the withstand voltage of the insulation layer.

[0004] Alicyclic amorphous nylon combined with functionalized polyolefins can improve the toughness and processing properties of materials, but its melt processing temperature is relatively high, limiting melt flow and interfacial wetting ability at relatively low extrusion temperatures. This is especially problematic when thin-walling flat busbars, bent metal parts, or metal components with angular or abrupt thickness changes, easily leading to insufficient adhesion, localized gaps, or uneven coating thickness. Furthermore, the significant temperature difference between the high-temperature melt and the metal component can cause residual interfacial stress during the cooling and solidification of the insulating layer due to the mismatch in thermal shrinkage between the resin and the metal.

[0005] Therefore, existing metal-insulating extruded materials still struggle to simultaneously achieve good coating integrity, interfacial stability, and long-term moisture resistance and thermoelectric insulation properties at relatively low extrusion temperatures. Summary of the Invention

[0006] To address the aforementioned issues, a nylon alloy for metal insulation extrusion and its preparation method are provided. This enables low-temperature continuous single-layer extrusion coating of metal components, improves the wetting and adhesion of the insulation layer, reduces interfacial residual stress, and inhibits cracking, delamination, and pressure resistance attenuation under aging and thermal cycling.

[0007] According to one aspect of this application, a nylon alloy for metal insulation extrusion is provided, comprising the following components by weight: 65-90 parts of amorphous copolymer nylon; 5-15 parts of polyphenylene ether; 5-10 parts of maleic anhydride-grafted ethylene-octene copolymer elastomer; Additives: 0.5–10 parts; The glass transition temperature of the amorphous copolymer nylon is 105–128°C.

[0008] Optionally, the amorphous copolymer nylon is copolymerized from bis(3-methyl-4-aminocyclohexyl)methane, decanediamine, dodecanoic acid and tetradecanoic acid in a molar ratio of (8-10):1:1:(9-11).

[0009] Optionally, the weight ratio of the polyphenylene ether to the maleic anhydride-grafted ethylene-octene copolymer elastomer is (1.4-2.0):1.

[0010] Optionally, the maleic anhydride grafting rate of the maleic anhydride-grafted ethylene-octene copolymer elastomer is 0.7 to 1.2 wt%.

[0011] Optionally, it also includes 0.8 to 1.2 parts by weight of an interface agent, wherein the interface agent is a protocatechuic acid-modified styrene-glycidyl methacrylate copolymer.

[0012] Optionally, the additives include antioxidants and lubricants; The antioxidant is selected from at least one of hindered phenolic antioxidants, hindered amine antioxidants, phosphite antioxidants, and thiolated antioxidants; The lubricant is selected from at least one of stearic acid, stearate, butyl stearate, and ethylene bis-stearamide.

[0013] According to another aspect of this application, a method for preparing the nylon alloy for metal insulation extrusion as described in any of the above claims is provided, comprising the following steps: Step 1: Add bis(3-methyl-4-aminocyclohexyl)methane, decanediamine, dodecanoic acid and tetradecanoic acid to a salt-forming kettle, add deionized water, and stir the reaction at 60-100℃ for 1-3 hours under nitrogen protection to obtain a mixed nylon salt aqueous solution. Step 2: Transfer the mixed nylon salt aqueous solution to a polymerization reactor, heat it to 200-250℃ under a nitrogen atmosphere, maintain the pressure at 1.5-2.0MPa for 2-3 hours, then release the pressure to atmospheric pressure, heat it to 260-290℃, and continue the polycondensation reaction for 2-4 hours to obtain the copolymerized nylon melt. After water cooling, stretching, pelletizing, and drying, the amorphous copolymerized nylon is obtained. Step 3: Weigh amorphous copolymer nylon, polyphenylene ether, maleic anhydride grafted ethylene-octene copolymer elastomer and additives, add them to a high speed mixer with a speed of 300-800 r / min and mix for 5-15 min to obtain a premix. Step 4: Feed the premixed material into the twin-screw extruder through the main feed port. After the components are melted and dispersed, add the protocatechuic acid-modified styrene-glycidyl methacrylate copolymer through the middle and rear side feed port. Continue to melt-mix, homogenize and extrude granulate to obtain the nylon alloy for metal insulation extrusion.

[0014] Optionally, in step three, the high-speed mixer rotates at a speed of 300–800 r / min.

[0015] Optionally, in step four, the screw speed is 200–350 r / min.

[0016] Optionally, in step four, the melting temperature from the main feed port to the side feed port of the twin-screw extruder is 230–260°C, and the melting temperature from the side feed port to the extrusion port is 235–255°C.

[0017] Optionally, the preparation method of the protocatechuic acid-modified styrene-glycidyl methacrylate copolymer includes: Styrene-glycidyl methacrylate copolymer was dissolved in anhydrous N,N-dimethylformamide, protocatechuic acid and catalyst were added, and the reaction was carried out at 90-100℃ for 4-8 h under nitrogen protection. After the reaction solution was cooled to room temperature, it was added to methanol to precipitate the precipitate, filtered, and the precipitate was collected. The precipitate was washed with methanol until no free protocatechuic acid was detected in the washing solution, and then dried under vacuum at 50-70℃ for 8-12 h to obtain protocatechuic acid modified styrene-glycidyl methacrylate copolymer.

[0018] Optionally, the molar ratio of the carboxyl group of the protocatechuic acid to the epoxy group of the styrene-glycidyl methacrylate copolymer is (0.1-0.3):1; And / or, the amount of catalyst used is 1 to 3% of the weight of the styrene-glycidyl methacrylate copolymer.

[0019] Optionally, the catalyst is tetrabutylammonium bromide.

[0020] In this application, "room temperature" refers to 20-30℃.

[0021] The beneficial effects of this application include, but are not limited to: 1. This application uses amorphous copolymer nylon with a glass transition temperature of 105-128℃ as the matrix, combined with polyphenylene ether, maleic anhydride-grafted ethylene-octene copolymer elastomer and protocatechuic acid-modified styrene-glycidyl methacrylate copolymer, to adjust melt flow, moisture heat resistance, insulation, toughness and interfacial interaction, and to perform melt mixing through segmented feeding; the components and preparation process complement each other, which is conducive to forming a continuous and uniform metal insulation coating layer at a lower extrusion temperature, taking into account the molding adaptability of complex metal components, resistance to cracking under thermal cycling and electrical insulation stability in long-term salt water environment.

[0022] 2. This application uses a low-Tg amorphous copolymer nylon prepared from bis(3-methyl-4-aminocyclohexyl)methane, decanediamine, dodecanoic acid and tetradecanoic acid; the copolymer nylon has a low crystallization tendency, which reduces the crystallization shrinkage of the insulation layer during cooling; its melt flow at a lower processing temperature is beneficial for covering flat busbars, corners and abrupt thickness changes, reducing local insufficient bonding and mitigating the interfacial stress caused by the mismatch between the cooling shrinkage of the resin and the metal.

[0023] 3. The polyphenylene ether and amorphous copolymer nylon of this application are compounded to compensate for the deficiencies of low Tg copolymer nylon in terms of heat resistance and long-term damp heat insulation; the maleic anhydride-grafted ethylene-octene copolymer elastomer provides a flexible dispersed phase, which helps to buffer the local stress borne by the insulation layer during bending and thermal cycling; the combination of the two allows the material to maintain its adaptability to extrusion at lower temperatures while improving its insulation stability in long-term salt water environments.

[0024] 4. The catechin-modified styrene-glycidyl methacrylate copolymer of this application simultaneously possesses styrene segments, a catechol structure, and residual epoxy groups. The styrene segments facilitate its distribution near the polyphenylene ether, the residual epoxy groups can undergo interfacial reactions with the active end groups of the amorphous copolymer nylon, and the catechol structure can enhance the interaction between the material and the oxide layer on the metal surface. The synergistic effect of these different functional structures helps improve the interfacial bonding between nylon and polyphenylene ether, reducing defects at the metal contact interface and the moisture penetration channels caused by these defects.

[0025] 5. In this application, the amorphous copolymer nylon, polyphenylene ether, and maleic anhydride-grafted ethylene-octene copolymer elastomer are first melt-mixed. After they are melt-dispersed, the protocatechuic acid modified copolymer is added from the side feed port for a second melt-mixing. This feeding sequence allows the basic components to form a relatively uniform melt system first, shortens the residence time of the modified copolymer in the high-temperature barrel, and helps to control the thermal history of its residual epoxy groups and catechol structure. At the same time, it preserves the mixing process for its participation in subsequent interfacial interactions. Attached Figure Description

[0026] The accompanying drawings, which are included to provide a further understanding of this application and form part of this application, illustrate exemplary embodiments and are used to explain this application, but do not constitute an undue limitation of this application. In the drawings: Figure 1 This is a photograph of a nylon alloy for metal insulation extrusion, as per this application. Detailed Implementation

[0027] The endpoints and any values ​​of the ranges disclosed herein are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of the various ranges, the endpoint values ​​of the various ranges and individual point values, and individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed herein.

[0028] Unless otherwise specified in the examples, the procedures shall be performed under standard conditions or conditions recommended by the manufacturer. Raw materials or instruments whose manufacturers are not specified are all commercially available products.

[0029] Example 1 A method for preparing a nylon alloy for metal insulation extrusion includes the following steps: Step 1: Add bis(3-methyl-4-aminocyclohexyl)methane, decanediamine, dodecanoic acid and tetradecanoic acid in a molar ratio of 9:1:1:10 to a salt-forming vessel, add deionized water, and stir the mixture at 80°C for 2 hours under nitrogen protection to obtain a mixed nylon salt aqueous solution. Step 2: Transfer the mixed nylon salt aqueous solution to the polymerization reactor, heat it to 230°C under a nitrogen atmosphere, maintain the pressure at 1.8 MPa for 2.5 h, then release the pressure to atmospheric pressure, heat it to 280°C, and continue the polycondensation reaction for 3 h to obtain the copolymerized nylon melt. After water cooling, drawing, pelletizing and drying, the amorphous copolymerized nylon is obtained. The glass transition temperature is 125°C as determined by DSC. Step 3: Weigh 80 parts by weight of amorphous copolymer nylon, 12 parts by weight of polyphenylene ether, 7 parts by weight of maleic anhydride-grafted ethylene-octene copolymer elastomer (maleic anhydride grafting rate of 1 wt%), 1 part by weight of hindered phenolic antioxidant and 1 part by weight of butyl stearate, add them to a high speed mixer at 500 r / min and mix for 10 min to obtain a premix. Step 4: Feed the premixed material into a twin-screw extruder through the main feed port at a screw speed of 300 r / min. After melting and dispersing at 240℃, add 1 part by weight of protocatechuic acid-modified styrene-glycidyl methacrylate copolymer through the middle and rear side feed port. All components are then melt-mixed, homogenized, and extruded and granulated at 240℃ to obtain a nylon alloy for metal insulation extrusion. Figure 1 As shown; The preparation method of the protocatechuic acid-modified styrene-glycidyl methacrylate copolymer includes: 100 parts by weight of styrene-glycidyl methacrylate copolymer (SG) were dissolved in 500 parts by weight of anhydrous N,N-dimethylformamide. Protocatechuic acid and tetrabutylammonium bromide (TBAB) were added. The molar ratio of the carboxyl group of protocatechuic acid to the epoxy group of SG was 0.2:1, and the amount of TBAB was 2% of the weight of SG. The reaction was carried out at 95°C for 6 hours under nitrogen protection. During the reaction, samples were taken at regular intervals, and the mixture was rapidly precipitated with cold methanol. After thoroughly washing to remove free protocatechuic acid, the residual epoxy groups were immediately measured. The theoretical residual epoxy group content was calculated based on the feed ratio. When the measured residual epoxy group content was close to the theoretical value and the reaction solution remained transparent without visible gel or precipitation, heating was stopped. After cooling the reaction solution to room temperature, 8 times the volume of methanol was slowly added to precipitate the mixture. The precipitate was filtered, collected, and washed with fresh methanol until no free protocatechuic acid was detected in the washing solution. Finally, the mixture was vacuum dried at 60°C for 10 hours to obtain protocatechuic acid modified styrene-glycidyl methacrylate copolymer.

[0030] Example 2 A method for preparing a nylon alloy for metal insulation extrusion includes the following steps: Step 1: Add bis(3-methyl-4-aminocyclohexyl)methane, decanediamine, dodecanoic acid and tetradecanoic acid in a molar ratio of 8:1:1:9 to a salt-forming vessel, add deionized water, and stir the mixture at 60°C for 3 hours under nitrogen protection to obtain a mixed nylon salt aqueous solution. Step 2: Transfer the mixed nylon salt aqueous solution to the polymerization reactor, heat it to 200°C under a nitrogen atmosphere, maintain the pressure at 1.5 MPa for 3 hours, then release the pressure to atmospheric pressure, heat it to 260°C, and continue the polycondensation reaction for 4 hours to obtain the copolymerized nylon melt. After water cooling, drawing, pelletizing and drying, the amorphous copolymerized nylon is obtained. The glass transition temperature is 105°C as determined by DSC. Step 3: Weigh 65 parts by weight of amorphous copolymer nylon, 7 parts by weight of polyphenylene ether, 5 parts by weight of maleic anhydride-grafted ethylene-octene copolymer elastomer (maleic anhydride grafting rate of 1 wt%), 0.25 parts by weight of hindered amine antioxidant and 0.25 parts by weight of stearic acid, add them to a high-speed mixer at 300 r / min and mix for 15 min to obtain a premix. Step 4: Feed the premixed material into the twin-screw extruder through the main feed port. The screw speed is 200 r / min. After melting and dispersing at 230℃, add 0.8 parts by weight of protocatechuic acid modified styrene-glycidyl methacrylate copolymer through the middle and rear side feed port. After melting, mixing, homogenizing and extruding granulation of each component at 235℃, the nylon alloy for metal insulation extrusion is obtained. The preparation method of the protocatechuic acid-modified styrene-glycidyl methacrylate copolymer includes: 100 parts by weight of SG were dissolved in 400 parts by weight of anhydrous N,N-dimethylformamide. Protocatechuic acid and TBAB were added. The molar ratio of the carboxyl group of protocatechuic acid to the epoxy group of SG was 0.1:1, and the amount of TBAB was 1% of the weight of SG. The reaction was carried out at 90°C for 8 hours under nitrogen protection. During the reaction, samples were taken at regular intervals, and the mixture was rapidly precipitated with cold methanol. After thoroughly washing to remove free protocatechuic acid, the residual epoxy groups were immediately measured. The theoretical residual epoxy group content was calculated based on the feed ratio. When the measured residual epoxy group content was close to the theoretical value and the reaction solution remained transparent without any visible gel or precipitate, heating was stopped. After cooling the reaction solution to room temperature, 5 times the volume of methanol was slowly added to precipitate the mixture. The precipitate was filtered, collected, and washed with fresh methanol until no free protocatechuic acid was detected in the washing solution. Finally, the mixture was vacuum dried at 50°C for 12 hours to obtain the protocatechuic acid modified styrene-glycidyl methacrylate copolymer.

[0031] Example 3 A method for preparing a nylon alloy for metal insulation extrusion includes the following steps: Step 1: Add bis(3-methyl-4-aminocyclohexyl)methane, decanediamine, dodecanoic acid and tetradecanoic acid in a molar ratio of 10:1:1:11 to a salt-forming vessel, add deionized water, and stir the mixture at 100°C for 1 hour under nitrogen protection to obtain a mixed nylon salt aqueous solution. Step 2: Transfer the mixed nylon salt aqueous solution to the polymerization reactor, heat it to 250°C under a nitrogen atmosphere, maintain the pressure at 2.0 MPa for 2 hours, then release the pressure to atmospheric pressure, heat it to 290°C, and continue the polycondensation reaction for 2 hours to obtain the copolymerized nylon melt. After water cooling, drawing, pelletizing and drying, the amorphous copolymerized nylon is obtained. The glass transition temperature is 128°C as determined by DSC. Step 3: Weigh 90 parts by weight of amorphous copolymer nylon, 15 parts by weight of polyphenylene ether, 7.5 parts by weight of maleic anhydride-grafted ethylene-octene copolymer elastomer (maleic anhydride grafting rate of 1 wt%), 5 parts by weight of phosphite antioxidant and 5 parts by weight of ethylene bis-stearamide, add them to a high-speed mixer at 800 r / min and mix for 5 min to obtain a premix. Step 4: Feed the premixed material into the twin-screw extruder through the main feed port. The screw speed is 350 r / min. After melting and dispersing at 260℃, add 1.2 parts by weight of protocatechuic acid modified styrene-glycidyl methacrylate copolymer through the middle and rear side feed port. After melting, mixing, homogenizing and extruding granulation of each component at 255℃, the nylon alloy for metal insulation extrusion is obtained. The preparation method of the protocatechuic acid-modified styrene-glycidyl methacrylate copolymer includes: 100 parts by weight of SG were dissolved in 600 parts by weight of anhydrous N,N-dimethylformamide. Protocatechuic acid and TBAB were added. The molar ratio of the carboxyl group of protocatechuic acid to the epoxy group of SG was 0.3:1, and the amount of TBAB was 3% of the weight of SG. The reaction was carried out at 100℃ for 4 hours under nitrogen protection. During the reaction, samples were taken at regular intervals, and the mixture was rapidly precipitated with cold methanol. After thoroughly washing to remove free protocatechuic acid, the residual epoxy groups were immediately measured. The theoretical residual epoxy group content was calculated based on the feed ratio. When the measured residual epoxy group content was close to the theoretical value and the reaction solution remained transparent without visible gel or precipitate, heating was stopped. After cooling the reaction solution to room temperature, 10 times the volume of methanol was slowly added to precipitate the mixture. The precipitate was filtered, collected, and washed with fresh methanol until no free protocatechuic acid was detected in the washing solution. Finally, the mixture was vacuum dried at 70℃ for 8 hours to obtain the protocatechuic acid modified styrene-glycidyl methacrylate copolymer.

[0032] Example 4 The difference from Example 1 is that the preparation method of the protocatechuic acid modified styrene-glycidyl methacrylate copolymer is not disclosed; the protocatechuic acid modified styrene-glycidyl methacrylate copolymer is replaced with styrene-glycidyl methacrylate copolymer.

[0033] Example 5 The difference from Example 1 is that the preparation method of protocatechuic acid modified styrene-glycidyl methacrylate copolymer is not disclosed; step four is: the premix is ​​fed into the twin-screw extruder through the main feed port, the screw speed is 300 r / min, and after melting and mixing, homogenization and extrusion granulation at 240℃, the nylon alloy for metal insulation extrusion is obtained.

[0034] Example 6 The difference from Example 1 is that step four is as follows: the premix and 1 part by weight of protocatechuic acid modified styrene-glycidyl methacrylate copolymer are fed into a twin-screw extruder through the main feed port. The screw speed is 300 r / min. After melt mixing, homogenization and extrusion granulation at 240°C, the nylon alloy for metal insulation extrusion is obtained.

[0035] Comparative Example 1 The difference from Example 1 is that: Step 1 is: adding bis(3-methyl-4-aminocyclohexyl)methane, decanediamine and tetradecanoic acid in a molar ratio of 9:1:10 into a salt-forming vessel, adding deionized water, and stirring the mixture at 80°C for 2 hours under nitrogen protection to obtain a mixed nylon salt aqueous solution. According to DSC measurement, the glass transition temperature of amorphous copolymer nylon is 150℃.

[0036] Comparative Example 2 The difference from Example 1 is that step three is as follows: Weigh 80 parts by weight of amorphous copolymer nylon, 7 parts by weight of maleic anhydride-grafted ethylene-octene copolymer elastomer (maleic anhydride grafting rate of 1 wt%), 1 part by weight of hindered phenolic antioxidant and 1 part by weight of butyl stearate, add them to a high-speed mixer with a rotation speed of 500 r / min and mix for 10 min to obtain a premix.

[0037] Comparative Example 3 The difference from Example 1 is that step three is as follows: 80 parts by weight of amorphous copolymer nylon, 12 parts by weight of polyphenylene ether, 1 part by weight of hindered phenolic antioxidant and 1 part by weight of butyl stearate are weighed and added to a high-speed mixer with a rotation speed of 500 r / min and mixed for 10 min to obtain a premix.

[0038] Comparative Example 4 The difference from Example 1 is that polyphenylene ether is replaced with polyphenylene sulfide.

[0039] Comparative Example 5 The difference from Example 1 is that the maleic anhydride-grafted ethylene-octene copolymer elastomer is replaced with maleic anhydride-grafted polyphenylene ether.

[0040] Experimental Example 1 Volume resistivity test: Nylon alloy samples were injection molded into 50mm diameter, 4mm thick discs, with at least 5 discs per group. The volume resistivity of the insulating material was measured using a three-electrode and guard ring structure. The resistivity measurement method followed IEC 62631-3-1:2023. The discs were immersed in a 1% (w / w) NaCl aqueous solution at 85℃ for 0, 168, 504, and 1000 hours, respectively. When measuring the wet resistivity, the discs were removed, and the surface free liquid was quickly removed with absorbent paper without drying. The test was completed within 5 minutes of removal at (23±2)℃. The electrode area, sample thickness, applied voltage, and pressurization time were recorded. The groups were compared using the same measurement conditions. The appearance of the insulation layer was also inspected on the aluminum busbar specimens. Volume resistivity is expressed in Ω·m; 1 Ω·m = 10⁻⁶. 3 Ω·mm.

[0041] Withstand voltage test: Each metal-coated aluminum busbar was 1m long, 15mm wide, and 5mm thick, with an insulation layer thickness of 0.5-1mm. Five pieces were prepared for each group. 50mm of insulation layer was peeled off from each end, and the junction between the metal and insulation layer was sealed to prevent leakage at the ends. The entire coated section, approximately 600mm in length, was immersed in a 1% (w / w) NaCl aqueous solution and placed at 85±5℃ for 1000h. The metal busbar was connected to the positive terminal of a 48V DC power supply, and the copper electrode in the solution was connected to the negative terminal. After the test, the busbar was removed, and an AC voltage of 1kV was applied between the metal busbar and a water bath electrode placed outside the insulation layer for 1min. Breakdown, flashover, and obvious leakage were recorded. Any occurrence of any of these was considered a failure. The number of passed pieces / total number of pieces was reported.

[0042] Peel strength test: Prepare aluminum strips with a length of 500 mm, a width of 15 mm, and a thickness of 5 mm using the same process, with at least 5 pieces per group; cut a peel strip 15 mm wide from the insulation layer, pre-peel about 20 mm from the end, fix the aluminum strip to a 90° floating platform, clamp the free end of the insulation layer in a tensile testing machine, speed 50 mm / min, stroke 100 mm; exclude the initial and end fluctuation zones, report the average peel strength and inter-sample standard deviation of the middle stable zone, in N / 15 mm, and record the interface or internal material failure morphology.

[0043] Metal insulation extrusion sample preparation process: Aluminum busbars are rinsed with clean water, dried at 80-100℃, and preheated to 150℃; each group of nylon alloy granules must be pre-dried and extruded under the same conditions, with the machine body set at 200-240℃, traction speed at 10m / min, and insulation layer thickness at 0.5-1mm; pre-cooled with 40-60℃ warm water, followed by room temperature air cooling. Record the actual temperature increase when stable plasticization fails.

[0044] The results are detailed in Table 1.

[0045] Table 1

[0046] As shown in Table 1, after soaking in 1% NaCl aqueous solution at 85℃ for 1000 h, the wet volume resistivity of Examples 1-3 was still 7.60 × 10⁻⁶. 9 ~1.30×10 10 The AC withstand voltage test results for the aluminum-coated busbars were all 5 / 5, with a peel strength of 151-166 N / 15 mm and no obvious cracks were observed.

[0047] Experimental Example 2 The modified styrene-glycidyl methacrylate copolymer (SG) prepared in Examples 1-3 and the unmodified SG were used.

[0048] Free protocatechuic acid was determined by ultraviolet absorption spectrometry. 1.000 g of the dried product was weighed and washed several times with methanol via shaking. The washings were combined and diluted to volume. The absorption spectrum of a protocatechuic acid standard solution was scanned in the same methanol system. A standard curve was established by selecting a characteristic wavelength confirmed by scanning and with minimal interference from the sample blank. The washings obtained from unmodified SG using the same procedure were used as a matrix blank. After necessary dilution of the washings, the absorbance was measured, and the percentage of free protocatechuic acid in the product mass was calculated.

[0049] Residual epoxy groups were characterized using a hydrochloric acid-acetone reaction and alkaline back titration. A dry sample was accurately weighed, and an excess of standardized hydrochloric acid-acetone solution was added. The epoxy groups were allowed to open at the same temperature and reaction time. The remaining hydrochloric acid was then titrated with standard sodium hydroxide solution. A reagent blank was set up, and acid group correction was performed using the same sample with fully opened epoxy groups. The residual epoxy group content was calculated (mmol / g) based on the difference in alkaline solution volume between the blank and the sample, after deducting the deviation caused by acid groups. Each group was measured in parallel at least three times.

[0050] Catechol structure uses ultraviolet absorption and Fe 3+ Colorimetric reaction combined examination. The thoroughly washed modified copolymer and original SG were prepared into solutions of the same concentration, and their UV absorption spectra were scanned, subtracting the background absorption of the original SG. An equal volume of sample was added to freshly prepared FeCl3 solution, and the colorimetric state was recorded and the visible light region was scanned. A blank sample of original SG, a positive control of free protocatechuic acid, and a control of original SG and protocatechuic acid physically mixed and then thoroughly washed under the same conditions were set up.

[0051] The results are detailed in Table 2.

[0052] Table 2

[0053] Table 2 shows that the residual epoxy groups in Examples 1-3 decreased with increasing protocatechuic acid feed ratio, while all retained a certain amount of epoxy groups; the modified products after thorough washing exhibited UV and Fe chromatographic properties. 3+ The product exhibits a colorimetric response, while the physical mixture control does not show the same response, indicating that some epoxy groups are involved in the modification, while others are retained, and that the product contains a catechol structure.

[0054] Experimental Example 3 Using the same aluminum busbars, preheating conditions, traction speed, and cooling process as in Example 1, extrusion was performed on Examples 1-6 and Comparative Examples 1-5. Starting from a lower machine temperature, the lowest machine set temperature for each group to achieve stable extrusion was recorded, based on the criteria of continuous and stable plasticization, no visible melt fracture in the coating layer, and no significant thickness fluctuation after 30 minutes of continuous production. At least 5 aluminum busbars were produced for each group, and at least three cross-sections were taken from the straight section, the corner section, and the section with thickness changes. The insulation layer thickness was measured using an optical microscope, and the presence of exposed substrate, gaps, material accumulation, and corner cracks was recorded.

[0055] The results are detailed in Table 3.

[0056] Table 3

[0057] As shown in Table 3, the minimum set temperature for stable extrusion in Examples 1-3 is 230-240℃, the thinnest insulation layer thickness at the corners is 0.59-0.64mm, the thickness variation coefficient is 6.1%-7.3%, and no substrate exposure occurs during continuous production. This indicates that the nylon alloy of this application can be stably extruded at lower temperatures and form a relatively continuous and uniform insulating coating layer at the metal corners.

[0058] Test Example 4 Take at least 5 coated aluminum busbars produced according to the stable process of each group. First, in... The specimen was kept at 40℃ for 2 hours, then at 85℃ for 2 hours, constituting one cycle, for a total of 100 cycles. The transfer time, specimen placement method, and observation position remained consistent. After the cycle, cracks and delamination were inspected at straight edges, corners, and areas of abrupt thickness changes, and the peel force was measured according to the method in Test Example 1. The number of cycles in which the first visible crack appeared was also recorded; those in which no crack appeared were recorded as 100 cycles without cracks.

[0059] The results are detailed in Table 4.

[0060] Table 4

[0061] As shown in Table 4, no obvious cracking or delamination was observed in Examples 1-3 after 100 cycles of thermal cycling, with a peel strength retention rate of 89.4%–90.4%. Examples 4-6 and Comparative Examples 1-5 showed varying degrees of cracking or delamination during the cycling process, with a peel strength retention rate of 66.7%–80.7%. This indicates that the material composition and side-feeding process are beneficial in mitigating the localized stress generated by thermal cycling and maintaining the interfacial bonding between the insulation layer and the metal.

[0062] Experimental Example 5 In Experiment 1, the wet volume resistivity of the material disc was measured, but the disc cannot directly reflect the moisture intrusion between the metal and the insulating layer. Therefore, another coated aluminum busbar with sealed ends was used and immersed in the same 85°C, 1% NaCl aqueous solution as in Experiment 1 for 1000 hours. After removal, the 90° peel force of the immersed section was measured; after peeling, the continuous wet area on the metal surface was observed, and the maximum moisture intrusion length extending inward from the defect initiation point along the interface was recorded. At least 5 pieces were used in each group, and the sample dispersion of peel force and intrusion length was reported.

[0063] The results are detailed in Table 5.

[0064] Table 5

[0065] As shown in Table 5, the metal-coated interfaces formed in Examples 1 to 3 have good binding and retention capabilities after immersion in salt water, which can reduce the intrusion of water along the interface.

[0066] The above description is merely an embodiment of this application, and the scope of protection of this application is not limited to these specific embodiments, but is determined by the claims of this application. Various modifications and variations can be made to this application by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the technical concept and principles of this application should be included within the scope of protection of this application.

Claims

1. A nylon alloy for metal insulation extrusion, characterized in that, By weight, it includes the following components: 65-90 parts of amorphous copolymer nylon; 5-15 parts of polyphenylene ether; 5-10 parts of maleic anhydride-grafted ethylene-octene copolymer elastomer; Additives: 0.5–10 parts; The glass transition temperature of the amorphous copolymer nylon is 105–128°C.

2. The nylon alloy for metal insulation extrusion according to claim 1, characterized in that, The amorphous copolymer nylon is copolymerized from bis(3-methyl-4-aminocyclohexyl)methane, decanediamine, dodecanoic acid and tetradecanoic acid in a molar ratio of (8-10):1:1:(9-11).

3. The nylon alloy for metal insulation extrusion according to claim 1, characterized in that, The weight ratio of the polyphenylene ether to the maleic anhydride-grafted ethylene-octene copolymer elastomer is (1.4-2.0):

1.

4. The nylon alloy for metal insulation extrusion according to claim 1, characterized in that, It also includes 0.8 to 1.2 parts by weight of an interface agent, wherein the interface agent is a protocatechuic acid-modified styrene-glycidyl methacrylate copolymer.

5. The nylon alloy for metal insulation extrusion according to claim 1, characterized in that, The additives include antioxidants and lubricants; The antioxidant is selected from at least one of hindered phenolic antioxidants, hindered amine antioxidants, phosphite antioxidants, and thiolated antioxidants; The lubricant is selected from at least one of stearic acid, stearate, butyl stearate, and ethylene bis-stearamide.

6. A method for preparing a nylon alloy for metal insulation extrusion according to any one of claims 1 to 5, characterized in that, Includes the following steps: Step 1: Add bis(3-methyl-4-aminocyclohexyl)methane, decanediamine, dodecanoic acid and tetradecanoic acid to a salt-forming kettle, add deionized water, and stir the reaction at 60-100℃ for 1-3 hours under nitrogen protection to obtain a mixed nylon salt aqueous solution. Step 2: Transfer the mixed nylon salt aqueous solution to a polymerization reactor, heat it to 200-250℃ under a nitrogen atmosphere, maintain the pressure at 1.5-2.0MPa for 2-3 hours, then release the pressure to atmospheric pressure, heat it to 260-290℃, and continue the polycondensation reaction for 2-4 hours to obtain the copolymerized nylon melt. After water cooling, stretching, pelletizing, and drying, the amorphous copolymerized nylon is obtained. Step 3: Weigh amorphous copolymer nylon, polyphenylene ether, maleic anhydride grafted ethylene-octene copolymer elastomer and additives, add them to a high-speed mixer and mix for 5-15 minutes to obtain a premix. Step 4: Feed the premixed material into the twin-screw extruder through the main feed port. After the components are melted and dispersed, add the protocatechuic acid-modified styrene-glycidyl methacrylate copolymer through the middle and rear side feed port. Continue to melt-mix, homogenize and extrude granulate to obtain the nylon alloy for metal insulation extrusion.

7. The preparation method according to claim 6, characterized in that, In step four, the melt temperature from the main feed port to the side feed port of the twin-screw extruder is 230–260°C, and the melt temperature from the side feed port to the extrusion port is 235–255°C.

8. The preparation method according to claim 6, characterized in that, The preparation method of the protocatechuic acid modified styrene-glycidyl methacrylate copolymer includes: Styrene-glycidyl methacrylate copolymer was dissolved in anhydrous N,N-dimethylformamide, protocatechuic acid and catalyst were added, and the reaction was carried out at 90-100℃ for 4-8 h under nitrogen protection. After the reaction solution was cooled to room temperature, it was added to methanol to precipitate the precipitate, filtered, and the precipitate was collected. The precipitate was washed with methanol until no free protocatechuic acid was detected in the washing solution, and then dried under vacuum at 50-70℃ for 8-12 h to obtain protocatechuic acid modified styrene-glycidyl methacrylate copolymer.

9. The preparation method according to claim 8, characterized in that, The molar ratio of the carboxyl group of the protocatechuic acid to the epoxy group of the styrene-glycidyl methacrylate copolymer is (0.1-0.3):1; And / or, the amount of catalyst used is 1 to 3% of the weight of the styrene-glycidyl methacrylate copolymer.

10. The preparation method according to claim 8, characterized in that, The catalyst is tetrabutylammonium bromide.