Composite aerogel microspheres, preparation method thereof and application thereof in uranium extraction from seawater
By preparing composite aerogel microspheres with aramid nanofibers/carboxymethyl chitosan framework and anchoring phosphoric acid-functionalized porous organic cages, the problems of pore collapse, swelling, biofouling, and poor adsorption selectivity in seawater uranium extraction materials were solved, achieving efficient and stable uranium adsorption performance and long-term recycling.
Patent Information
- Application Number
- CN202611180005.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-05
- Publication Date
- 2026-11-24
AI Technical Summary
Existing seawater uranium extraction adsorbents are prone to pore collapse during freeze-drying, swelling and dissociation under long-term immersion, poor adsorption selectivity, slow kinetics, and are susceptible to biofouling, making them difficult to prepare on a large scale and use stably for a long time.
Composite aerogel microspheres, employing an aramid nanofiber/carboxymethyl chitosan dual-network framework and anchored with phosphoric acid-functionalized porous organic cages, form a stable structure through physical entanglement and chemical cross-linking. Combined with the strong coordination ability of phosphate groups, a synergistic coordination microenvironment is constructed.
The material achieves structural stability and ultralight properties, excellent uranium adsorption performance, high-capacity extraction from natural seawater, good stability during recycling, an adsorption capacity of 22.5 mg·g⁻¹, and a capacity retention rate of over 90% after cycling.
Smart Images

Figure CN123152285A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of functional composite materials and nuclear fuel resource extraction technology, specifically relating to a composite aerogel microsphere based on an aramid nanofiber / carboxymethyl chitosan dual network framework and anchored phosphoric acid functionalized porous organic cage, its large-scale preparation method, and the application of this material in the selective adsorption and extraction of uranyl ions from seawater. Background Technology
[0002] With the growth of global energy demand and the advancement of zero-carbon emission strategies, nuclear energy is increasingly prominent as a highly efficient and clean energy source. However, terrestrial uranium resources are becoming increasingly depleted, while seawater reserves are approximately 4.5 billion tons, nearly a thousand times the terrestrial reserves. Uranium extraction from seawater (UES) is of great strategic significance for ensuring the sustainable development of nuclear energy. Seawater has extremely low uranium concentrations (approximately 3.3 ppb) and contains numerous competing ions (such as V, Ca, and Mg) and complex biological systems, placing extremely high demands on adsorption materials. Three-dimensional composite aerogel microspheres, due to their high specific surface area, high porosity, and open interpenetrating network structure, show promising potential in the field of UES.
[0003] Aramid nanofibers (ANFs), prepared from poly(p-phenylene terephthalamide) (PPTA) fibers through deprotonation exfoliation, possess ultra-high tensile strength, excellent chemical inertness, and thermal stability, making them an ideal matrix for constructing high-performance porous frameworks. Carboxymethyl chitosans (CMCs), a natural polysaccharide rich in amino, hydroxyl, and carboxyl groups, can significantly improve the hydrophilicity of the framework and provide additional chelating sites. Phosphate groups have a strong coordination ability for uranyl ions, but introducing them into the three-dimensional framework in an ordered manner and constructing a synergistic coordination microenvironment remains a technical challenge.
[0004] Traditional ANF-based composite gels are prone to pore collapse during freeze-drying, and physical hydrogen bonds or single covalent crosslinking alone are insufficient to resist the swelling and shear forces caused by long-term immersion in seawater. The shear stress generated by ice crystal growth easily leads to network shrinkage and pore collapse, resulting in framework disintegration. Single phosphate groups or single carboxyl groups are difficult to effectively adsorb highly stable UO2 in seawater. 2+ Ions, lacking sufficient electron donation capacity and spatial configuration matching, result in slow adsorption kinetics and insufficient selectivity. Existing aerogel materials lack effective antibacterial functional groups on their surfaces, easily forming biofilms in natural seawater, physically masking active sites and blocking mass transfer channels. Therefore, developing composite aerogel materials that combine structural stability, synergistic coordination ability, anti-biofouling properties, and scalable fabrication is a key requirement in the current UES field. Summary of the Invention
[0005] Technical problems to be solved: The purpose of this invention is to solve the following technical problems faced by existing seawater uranium extraction adsorbents: 1. Traditional aerogels and composite gels are prone to macroscopic shrinkage and pore collapse during the preparation process (especially the freeze-drying stage), resulting in a sharp reduction in specific surface area and blockage of mass transfer channels; 2. Single physical entanglements or single chemical cross-linked networks are prone to swelling and dissociation of coordination sites under long-term immersion in seawater; 3. Existing adsorbent materials have a single surface functional group, making it difficult to overcome the stable presence of UO2 in seawater. 2+ 4. The high dissociation energy barrier of the complex leads to poor adsorption selectivity and slow kinetics; 5. The material is susceptible to biofouling in natural seawater, and the microbial film blocks the mass transfer channels and masks the active sites, causing the adsorption capacity to decay rapidly; 6. Existing high-performance adsorption materials are difficult to balance scalable preparation, size control, and long-term cycle stability.
[0006] Technical solution: A composite aerogel microsphere, wherein the composite aerogel microsphere is composed of ternary composite aerogel microspheres with ANFs as the backbone, CMCs as the crosslinking matrix and phosphoric acid functionalized porous organic cages as functional active components.
[0007] Preferably, the preparation method of the above-mentioned composite aerogel microspheres includes the following steps: S1. Mix PPTA, KOH, deionized water and DMSO by stirring and magnetically stirring at room temperature. The PPTA is converted into a uniform and stable ANFs / DMSO dispersion through a deprotonation-stripping process and set aside. S2. Dissolve CMCs in deionized water to prepare an aqueous solution of CMCs; disperse phosphoric acid-functionalized porous organic cages in DMSO to form a suspension for later use; S3. Add the CMCs aqueous solution and the phosphoric acid-functionalized porous organic cage suspension to the ANFs / DMSO dispersion in step S1 above, and stir continuously to obtain a homogeneous precursor solution. S4. The precursor solution was continuously added dropwise to the coagulation bath using a peristaltic pump. During the dropwise addition, DMSO underwent rapid solvent exchange with the coagulation bath. At the same time, the protonation of acetic acid triggered the desolvation of ANFs and physical entanglement, which encapsulated CMCs and PhosCage in situ, initially forming spherical hydrogel microspheres, which were then incubated in the coagulation bath for 2 hours. S5. The hydrogel microspheres obtained in step S4 are transferred to an aqueous solution of glutaraldehyde to carry out a chemical cross-linking reaction; the aldehyde group of glutaraldehyde reacts with the primary amine group on the CMCs chain segment via a Schiff base reaction to generate a stable covalent imine bond (C=N), which, together with the physical hydrogen bond network in step S3, forms a double cross-linking network. S6. The cross-linked microspheres were placed in an aqueous solution of tert-butanol for solvent exchange to replace the water in the pores and reduce damage from ice crystal growth; then freeze-drying was performed to obtain composite aerogel microspheres.
[0008] Preferably, the solid-liquid ratio of PPTA, KOH, deionized water and DMSO in step S1 is (0.20-0.50)g:(0.10-0.15)g:(0.40-0.80)ml:20ml; the magnetic stirring speed is 500-800rpm, and the time is 3-5 days; Preferably, the preparation method of the phosphoric acid functionalized porous organic cage includes the following steps: dissolving 2,5-dihydroxyterephthalaldehyde in anhydrous 1,4-dioxane, sonicating, then adding tris(2-aminoethyl)amine, stirring the reaction at room temperature, washing the resulting yellow solid sequentially with 1,4-dioxane and ethanol, and drying under vacuum to obtain the hydroxyl-functionalized organic cage precursor; subsequently, under nitrogen protection, dispersing the precursor in dry acetonitrile, sonicating, cooling, adding triethylamine, then adding phosphorus oxychloride dropwise, heating and stirring the reaction, collecting the solid by centrifugation after the reaction is completed, washing sequentially with acetonitrile and deionized water, and freeze-drying to obtain the phosphoric acid functionalized porous organic cage.
[0009] Preferably, in step S2, the solid-liquid ratio of CMCs to water is 80-120 mg: 2 ml; and the solid-liquid ratio of phosphoric acid functionalized porous organic cages to DMSO is (5-100) mg: 8 ml.
[0010] Preferably, the stirring speed in step S3 is 500-800 rpm; the time is 12-24 h.
[0011] Preferably, the coagulation bath in step S4 consists of an aqueous solution of 4-6 v% acetic acid and 20-40 v% ethanol; the incubation time is 2-4 h.
[0012] Preferably, the concentration of the glutaraldehyde aqueous solution in step S5 is 1-3 wt%; the temperature for chemical crosslinking is 30-40℃, and the time is 12-24 h.
[0013] Preferably, the concentration of the tert-butanol aqueous solution in step S6 is 30-50 vt%, the solvent exchange time is 12-24 h, and the freeze-drying temperature is -50 to -30 °C for 12-24 h.
[0014] Preferably, the above-mentioned composite aerogel microspheres are used for the selective adsorption of uranyl ions in uranium-containing aqueous solutions and seawater.
[0015] Beneficial effects: The composite aerogel microspheres of the present invention have the following advantages: 1. Structural Stability and Ultralight Properties: These microspheres utilize ANFs as the framework and CMCs as the crosslinking matrix. Covalent imine bonds are formed through glutaraldehyde chemical crosslinking, synergistically constructing a double-crosslinked network with physical hydrogen bonds. This endows the material with excellent mechanical strength and an ultralight apparent density (capable of supporting dandelion fluff without deformation). Thermogravimetric analysis shows that the material is mass-stable below 300°C, with a maximum decomposition temperature of 540-550°C, meeting the deployment requirements of harsh conditions such as complex marine environments.
[0016] 2. Excellent uranium adsorption performance: thanks to the abundant active recognition sites provided by the phosphoric acid functionalized porous organic cage and the mass transfer efficiency promoted by the three-dimensional porous structure of the aerogel; under the conditions of pH 6.0 and 25 °C, the adsorption equilibrium of the uranium solution with an initial concentration of 20 mg·L⁻¹ can be reached within 180 minutes.
[0017] 3. High-capacity extraction from natural seawater: After continuous dynamic adsorption in 25 L of natural seawater for 15 days, the uranium extraction capacity reached 22.5 mg·g⁻¹, which is about 3.8 times the large-scale economic feasibility benchmark (6 mg·g⁻¹) set by the U.S. Department of Energy (DOE), and no additional energy input is required.
[0018] 4. Outstanding stability during repeated use: After seven adsorption-desorption cycles, the capacity retention rate exceeds 90%; after cycling, the microsphere micropores do not collapse significantly, the characteristic peaks of phosphate groups remain unchanged, and there is no loss of active sites. Attached Figure Description
[0019] Figure 1 A schematic diagram of the dual-network formation mechanism of composite aerogel microspheres; Figure 2 A schematic diagram showing composite aerogel microspheres falling onto dandelion seeds; Figure 3 The microstructure and elemental distribution of the composite aerogel microspheres; Figure 4 Here is the FT-IR characterization image of the composite aerogel microspheres; Figure 5 Figure showing the optimization of the loading of phosphate organic cages in composite aerogel microspheres; Figure 6 Analysis of the pH effect on composite aerogel microspheres; Figure 7 A diagram showing the continuous flow dynamic adsorption platform for the construction of composite aerogel microspheres; Figure 8 The diagram shows the cyclic regeneration performance of the composite aerogel microspheres. Figure 9 The adsorption equilibrium time and adsorption saturation amount of the composite aerogels in the examples and comparative examples are shown. Detailed Implementation
[0020] The present invention will be further described below with reference to embodiments. These embodiments are illustrative of the present invention, but the present invention is not limited to these embodiments: Example 1
[0021] The preparation of phosphoric acid-functionalized porous organic cages includes the following steps: Step 1: Synthesis of hydroxyl-functionalized organic cage precursor: 50 mg of 2,5-dihydroxyterephthalaldehyde (2,5-DHA) was dissolved in 10 mL of anhydrous 1,4-dioxane and sonicated for 5 minutes; 50 µL of tris(2-aminoethyl)amine (TAEA) was added, and the mixture was stirred at room temperature (25 °C) for 5 days; the resulting yellow solid was washed successively with 1,4-dioxane and ethanol; and dried under vacuum at 70 °C for 24 hours to obtain the hydroxyl-functionalized organic cage precursor. Step 2: Synthesis of Phosphoric Acid Porous Organic Cages: Under nitrogen protection, 68.3 mg of the above cage precursor was dispersed in 10 mL of dry acetonitrile (MeCN) and sonicated for 5 minutes; cooled to 0 °C, and 1 mL of triethylamine (Et3N) was added in one go; then 578 µL of phosphorus oxychloride (POCl3) was added dropwise; the mixture was stirred and reacted at 65 °C under nitrogen atmosphere for 5 hours; after the reaction was completed, the solid was collected by centrifugation and washed successively with acetonitrile and deionized water; lyophilized at −40 °C for 24 hours to obtain phosphoric acid functionalized porous organic cages (PhosCage).
[0022] Example 2
[0023] The preparation method of the above-mentioned composite aerogel microspheres includes the following steps: S1. Mix 0.3 g PPTA fiber, 0.15 g KOH, 0.4 mL deionized water with 20 mL DMSO, stir at room temperature for 4 days to obtain ANFs / DMSO dispersion, and set aside for later use; S2. Dissolve 100 mg CMCs in 2 mL of water and disperse 5 mg PhosCage in 8 mL of DMSO for later use; S3. Add the CMCs aqueous solution and the phosphoric acid-functionalized porous organic cage suspension to the ANFs / DMSO dispersion in step S1 above, and stir at 25°C for 12 h to obtain a homogeneous precursor solution. S4. The precursor solution was continuously added dropwise to a 5 v% acetic acid / 30 v% ethanol coagulation bath using a peristaltic pump and incubated in the coagulation bath for 2 hours. S5. The hydrogel microspheres obtained in step S4 were transferred to a 2 wt% glutaraldehyde aqueous solution and crosslinked at 37 °C for 12 h to carry out a chemical crosslinking reaction; S6. The cross-linked microspheres were placed in a 40 v% tert-butanol aqueous solution for solvent exchange for 12 h, followed by freeze drying to obtain composite aerogel microspheres.
[0024] Example 3
[0025] The preparation method of the above-mentioned composite aerogel microspheres includes the following steps: S1. Mix 0.3 g PPTA fiber, 0.15 g KOH, 0.4 mL deionized water with 20 mL DMSO, stir at room temperature for 4 days to obtain ANFs / DMSO dispersion, and set aside for later use; S2. Dissolve 100 mg CMCs in 2 mL of water and disperse 25 mg PhosCage in 8 mL of DMSO for later use; S3. Add the CMCs aqueous solution and the phosphoric acid-functionalized porous organic cage suspension to the ANFs / DMSO dispersion in step S1 above, and stir at 25°C for 12 h to obtain a homogeneous precursor solution. S4. The precursor solution was continuously added dropwise to a 5 v% acetic acid / 30 v% ethanol coagulation bath using a peristaltic pump and incubated in the coagulation bath for 2 hours. S5. The hydrogel microspheres obtained in step S4 were transferred to a 2 wt% glutaraldehyde aqueous solution and crosslinked at 37 °C for 12 h to carry out a chemical crosslinking reaction; S6. The cross-linked microspheres were placed in a 40 v% tert-butanol aqueous solution for solvent exchange for 12 h, followed by freeze drying to obtain composite aerogel microspheres.
[0026] Example 4
[0027] The preparation method of the above-mentioned composite aerogel microspheres includes the following steps: S1. Mix 0.3 g PPTA fiber, 0.15 g KOH, 0.4 mL deionized water with 20 mL DMSO, stir at room temperature for 4 days to obtain ANFs / DMSO dispersion, and set aside for later use; S2. Dissolve 100 mg CMCs in 2 mL of water and disperse 50 mg PhosCage in 8 mL of DMSO for later use; S3. Add the CMCs aqueous solution and the phosphoric acid-functionalized porous organic cage suspension to the ANFs / DMSO dispersion in step S1 above, and stir at 25°C for 12 h to obtain a homogeneous precursor solution. S4. The precursor solution was continuously added dropwise to a 5 v% acetic acid / 30 v% ethanol coagulation bath using a peristaltic pump and incubated in the coagulation bath for 2 hours. S5. The hydrogel microspheres obtained in step S4 were transferred to a 2 wt% glutaraldehyde aqueous solution and crosslinked at 37 °C for 12 h to carry out a chemical crosslinking reaction; S6. The cross-linked microspheres were placed in a 40 v% tert-butanol aqueous solution for solvent exchange for 12 h, followed by freeze drying to obtain composite aerogel microspheres.
[0028] Example 5
[0029] The preparation method of the above-mentioned composite aerogel microspheres includes the following steps: S1. Mix 0.3 g PPTA fiber, 0.15 g KOH, 0.4 mL deionized water with 20 mL DMSO, stir at room temperature for 4 days to obtain ANFs / DMSO dispersion, and set aside for later use; S2. Dissolve 100 mg CMCs in 2 mL of water and disperse 75 mg PhosCage in 8 mL of DMSO for later use; S3. Add the CMCs aqueous solution and the phosphoric acid-functionalized porous organic cage suspension to the ANFs / DMSO dispersion in step S1 above, and stir at 25°C for 12 h to obtain a homogeneous precursor solution. S4. The precursor solution was continuously added dropwise to a 5 v% acetic acid / 30 v% ethanol coagulation bath using a peristaltic pump and incubated in the coagulation bath for 2 hours. S5. The hydrogel microspheres obtained in step S4 were transferred to a 2 wt% glutaraldehyde aqueous solution and crosslinked at 37 °C for 12 h to carry out a chemical crosslinking reaction; S6. The cross-linked microspheres were placed in a 40 v% tert-butanol aqueous solution for solvent exchange for 12 h, followed by freeze drying to obtain composite aerogel microspheres.
[0030] Example 6
[0031] The preparation method of the above-mentioned composite aerogel microspheres includes the following steps: S1. Mix 0.3 g PPTA fiber, 0.15 g KOH, 0.4 mL deionized water with 20 mL DMSO, stir at room temperature for 4 days to obtain ANFs / DMSO dispersion, and set aside for later use; S2. Dissolve 100 mg CMCs in 2 mL of water and disperse 100 mg PhosCage in 8 mL of DMSO for later use; S3. Add the CMCs aqueous solution and the phosphoric acid-functionalized porous organic cage suspension to the ANFs / DMSO dispersion in step S1 above, and stir at 25°C for 12 h to obtain a homogeneous precursor solution. S4. The precursor solution was continuously added dropwise to a 5 v% acetic acid / 30 v% ethanol coagulation bath using a peristaltic pump and incubated in the coagulation bath for 2 hours. S5. The hydrogel microspheres obtained in step S4 were transferred to a 2 wt% glutaraldehyde aqueous solution and crosslinked at 37 °C for 12 h to carry out a chemical crosslinking reaction; S6. The cross-linked microspheres were placed in a 40 v% tert-butanol aqueous solution for solvent exchange for 12 h, followed by freeze drying to obtain composite aerogel microspheres.
[0032] Comparative Example 1 The main difference between Comparative Example 1 and Example 4 is that the chemical cross-linking step S5 is omitted, glutaraldehyde is not added, and physical entanglement is relied upon alone.
[0033] Comparative Example 2 The main difference between Comparative Example 2 and Example 4 is that the fiber morphology does not include ANFs, and only CMCs are crosslinked with glutaraldehyde.
[0034] Comparative Example 3 The main difference between Comparative Example 3 and Example 4 is that an equimolar amount of free small molecule phosphate ligands replaces the phosphoric acid-functionalized porous organic cage.
[0035] Comparative Example 4 The main difference between Comparative Example 4 and Example 4 is that the carboxymethyl chitosan component is omitted, and it is constructed only from ANFs and phosphoric acid-functionalized porous organic cages.
[0036] Comparative Example 5 The main difference between Comparative Example 5 and Example 4 is that no phosphoric acid functionalized porous organic cage was added, and only a blank ANF / CMC dual network framework was prepared.
[0037] Performance Test 1: Microstructure and elemental distribution: Scanning electron microscopy (SEM) combined with energy-dispersive X-ray spectroscopy (EDX); Chemical structure: Fourier transform infrared spectroscopy (FT-IR); Macroscopic aramid fibers were deprotonated in a DMSO / KOH system to form a stable purple-red aramid nanofiber dispersion. Simultaneously, CMCs were dissolved in deionized water to allow their hydrophilic polymer chains to fully extend. Subsequently, PhosCage was mixed into the CMCs and ANFs / DMSO co-solvent matrix under high-speed shearing to form a homogeneous viscous mixture. After the mixture was uniformly extruded into a coagulation bath using a peristaltic pump, the intense solvent exchange and protonation during phase inversion promoted the rapid self-assembly and physical entanglement of ANFs, effectively embedding and locking CMCs and PhosCage into a spherical structure. Subsequently, glutaraldehyde was used for covalent post-crosslinking via a Schiff base reaction to further enhance its network stability. On one hand, the abundant hydroxyl and carboxyl groups on the CMC chains formed dense intermolecular hydrogen bonds with the amide groups on the ANF backbone, constructing a highly entangled physical crosslinked network; on the other hand, the aldehyde groups of glutaraldehyde covalently linked with the primary amine groups on the CMC chains to form stable imine bonds. Figure 1 This chemical cross-linking effectively prevents the swelling or dissociation of polysaccharide chains in an aqueous environment, fixing the ANF / CMCs matrix into a stable three-dimensional framework. The resulting microspheres are uniformly spherical with a diameter of approximately 2-3 mm. After gold sputtering, the microstructure and composition of the AC-POC aerogel microspheres were observed using a scanning electron microscope (S-4800) and energy-dispersive X-ray spectroscopy. Thanks to the high-openness hierarchical porous network preserved by the freeze-drying process, the AC-POC aerogel microspheres exhibit extremely low apparent density and can stably support dandelion fluff. Figure 2 SEM revealed a continuous 3D nanofiber network. Figure 3 EDX mapping confirmed the uniform distribution of C, N, O, and P elements. Fourier transform infrared spectroscopy was performed on a PerkinElmer 100 spectrometer using the KBr pellet method at 4000-500 cm⁻¹. -1 Analyzing chemical groups within the wavelength range. FT-IR revealed new absorption peaks for P=O and COP at 1260 cm⁻¹ and 1081 cm⁻¹. Figure 4 This confirms the formation of the dual network and the successful introduction of PhosCage.
[0038] Performance Test 2: Uranium concentration determination: Inductively coupled plasma mass spectrometry (ICP-MS) The experimental sample solution was filtered through a 0.22-micron filter and then diluted with 2% nitric acid. The concentration of uranyl ions in the solution was measured using a Shimadzu ICP-MS-2030, and then converted into adsorption capacity. Figure 5 As can be seen from Examples 2-6, the adsorption capacity first increases and then decreases with increasing PhosCage loading in AC-POC. 1.0The maximum value is reached at this point. Excessive loading (>1.0) leads to PhosCage buildup, creating steric hindrance that shields active sites and blocks pores, increasing interfacial mass transfer resistance. Therefore, AC-POC is determined to be the optimal choice. 1.0 This is the optimal formula.
[0039] from Figure 6 As can be seen, tests in Example 4 within different pH ranges of 2.0-8.0 showed that the adsorption capacity first increased and then decreased with increasing pH, reaching its maximum at pH ≈ 6.0. The zero charge point (pH_PZC) of the material was determined to be approximately 3.2; when pH < 3.2, surface protonation caused electrostatic repulsion, and when pH > 7.0, uranium formed anionic complexes, leading to increased repulsion.
[0040] from Figure 7 As can be seen from the results, in order to construct a continuous flow dynamic adsorption platform using the composite aerogel prepared in Example 4, 25 L of physically filtered natural seawater (from the Wanggezhuang sea area of Qingdao) was used without adjusting the pH or ionic composition. AC-POC1.0 was packed into the adsorption column and continuously circulated at a certain flow rate. Uranium concentration was measured at regular intervals over 15 days. The results showed that the extraction capacity continued to increase in the first 6 days, and adsorption equilibrium was reached from day 12 to day 15, with a maximum uranium extraction capacity of 22.5 mg·g⁻¹.
[0041] from Figure 8 As can be seen from the results, the composite aerogel microspheres prepared in Example 4 underwent a cycle regeneration performance evaluation. The AC-POC microspheres, saturated with adsorption, were desorbed using 0.1 MHNO3 or a suitable eluent, washed with deionized water, and regenerated. This process was repeated seven times. The results showed that after seven cycles, the capacity retention rate was 92.7%, and the elution efficiency remained stable at approximately 90%, confirming that the dual-network structure effectively inhibited molecular chain degradation and loss of active sites during repeated acid washing.
[0042] like Figure 9As shown, the adsorption equilibrium time of the embodiment is shorter than that of all comparative examples, and the saturated adsorption capacity is higher than that of all comparative examples. The novel composite aerogel microsphere (AC-POC) constructed in this invention, which is reconstructed from an aramid nanofiber / carboxymethyl chitosan framework and integrates a phosphoric acid functionalized porous organic cage (PhosCage), benefits from the multi-group synergistic chelation center formed by phosphate groups and carboxyl groups. AC-POC exhibits ultrafast adsorption kinetics and high capacity. Comparative Example 1 omits the chemical cross-linking step of glutaraldehyde and relies only on physical cross-linking. The stability of the gel microsphere is poor, and the shear force generated by stirring compresses the internal network structure, resulting in hindered ion transport. Therefore, the adsorption equilibrium time is significantly longer than that of Example 4, and the saturated adsorption capacity is also much lower than that of Example 4. Comparative Example 2 does not add rigid ANF fibers and relies only on soft CMC chain molecules to anchor the phosphoric acid organic cage. The anchoring force is poor, and the stability is weak. During the adsorption process, the phosphoric acid organic cage molecules gradually fall out of the mesh, resulting in a sharp reduction in active sites and extremely low adsorption capacity. Comparative Example 3 uses a small-molecule phosphate ligand, whose phosphate adsorption sites are located within the nodes of the framework. Due to steric hindrance, the phosphate groups cannot effectively contact uranyl ions in the solution, resulting in adsorption rates and capacities far lower than in Example 4. Comparative Example 4 uses only rigid ANF fibers, where the phosphate organic cage molecules lack sufficient anchoring sites, leading to the gradual detachment of the phosphate organic cage molecules from the mesh during adsorption, a sharp reduction in active sites, and extremely low adsorption capacity. Comparative Example 5 lacks phosphate-selective adsorption sites and relies solely on negatively charged carboxyl groups on the framework for adsorption. This results in low adsorption energy and the absence of a multidentate anchoring adsorption structure, making it easy for uranyl ions to detach, leading to low adsorption equilibrium time and saturation adsorption capacity.
[0043] Obviously, the above embodiments are merely illustrative examples for clear explanation and are not intended to limit the implementation. Those skilled in the art will recognize that other variations or modifications can be made based on the above description. It is neither necessary nor possible to exhaustively list all possible implementations here. However, obvious variations or modifications derived therefrom are still within the scope of protection of this invention.
Claims
1. A composite aerogel microsphere, characterized in that: The composite aerogel microspheres are composed of ternary composite aerogel microspheres with ANFs as the framework, CMCs as the crosslinking matrix, and phosphoric acid-functionalized porous organic cages as the functional active components.
2. The method for preparing composite aerogel microspheres according to claim 1, characterized in that, Includes the following steps: S1. Mix PPTA, KOH, deionized water and DMSO by stirring and magnetically stirring at room temperature. The PPTA is converted into a uniform and stable ANFs / DMSO dispersion through a deprotonation-stripping process and set aside. S2. Dissolve CMCs in deionized water to prepare an aqueous solution of CMCs; disperse phosphoric acid-functionalized porous organic cages in DMSO to form a suspension for later use; S3. Add the CMCs aqueous solution and the phosphoric acid-functionalized porous organic cage suspension to the ANFs / DMSO dispersion in step S1 above, and stir continuously to obtain a homogeneous precursor solution. S4. The precursor solution is continuously added dropwise to the coagulation bath using a peristaltic pump. During the dropwise addition, spherical hydrogel microspheres are initially formed and incubated in the coagulation bath. S5. (The steps are...) S 4. The obtained hydrogel microspheres were transferred to an aqueous solution of glutaraldehyde for chemical cross-linking reaction; S6. The cross-linked microspheres were placed in an aqueous solution of tert-butanol for solvent exchange to replace the water in the pores and reduce damage from ice crystal growth; then freeze-drying was performed to obtain composite aerogel microspheres.
3. The method for preparing composite aerogel microspheres according to claim 2, characterized in that: In step S1, the solid-liquid ratio of PPTA, KOH, deionized water and DMSO is (0.20-0.50)g:(0.10-0.15)g:(0.40-0.80)ml:20ml; the magnetic stirring speed is 500-800 rpm, and the time is 3-5 days.
4. The method for preparing composite aerogel microspheres according to claim 2, characterized in that: In step S2, the solid-liquid ratio of CMCs to water is 80-120 mg: 2 ml; the solid-liquid ratio of phosphoric acid functionalized porous organic cages to DMSO is (5-100) mg: 8 ml.
5. The method for preparing composite aerogel microspheres according to claim 2, characterized in that: The stirring speed in step S3 is 500-800 rpm; the stirring time is 12-24 h.
6. The method for preparing composite aerogel microspheres according to claim 2, characterized in that: The coagulation bath in step S4 consists of an aqueous solution of 4-6 v% acetic acid and 20-40 v% ethanol; the incubation time is 2-4 h.
7. The method for preparing composite aerogel microspheres according to claim 2, characterized in that: In step S5, the concentration of the glutaraldehyde aqueous solution is 1-3 wt%; the temperature for chemical cross-linking is 30-40℃, and the time is 12-24 h.
8. The method for preparing composite aerogel microspheres according to claim 2, characterized in that: The concentration of the tert-butanol aqueous solution in step S6 is 30-50 wt%, the solvent exchange time is 12-24 h, and the freeze-drying temperature is -50~-30℃ for 24-48 h.
9. The application of the composite aerogel microspheres according to claim 1 in the selective adsorption of uranyl ions in uranium-containing aqueous solutions and seawater.