Modified maleimide prepolymer, resin composition, cured product
By modifying maleimide compounds with a compound of diamino silicone resin and diamino indane compound, a modified maleimide prepolymer is formed, which solves the brittleness and dielectric properties of maleimide resin system and achieves a packaging substrate material with low CTE, low Dk/Df, low water absorption and high heat resistance.
Patent Information
- Application Number
- CN202611560011.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-09
- Publication Date
- 2026-11-24
AI Technical Summary
Existing maleimide resin systems struggle to simultaneously achieve excellent solvent solubility, good compatibility with other resins, low coefficient of thermal expansion (CTE), low dielectric constant (Dk) and dielectric loss tangent (Df), low water absorption, and high heat resistance.
Maleimide compounds were modified by compounding diamino silicone resin and diamino indane compound, and aminophenol was introduced to participate in the reaction to form modified maleimide prepolymer. The silicone unit and indane unit were introduced into the molecular chain to improve brittleness and dielectric properties, while the molecular weight and end group structure were adjusted to improve solubility and compatibility.
It effectively reduces the thermal expansion coefficient and dielectric constant of the substrate, improves heat resistance and peel strength, and is suitable for low dielectric packaging substrates to meet the performance requirements of high frequency signal transmission.
Smart Images

Figure SMS_36 
Figure SMS_42 
Figure SMS_48
Abstract
Description
Technical Field
[0001] This invention relates to the field of electronic materials technology, and more particularly to a modified maleimide prepolymer, a resin composition, and a cured product prepared from the resin composition. Background Technology
[0002] In recent years, with the rapid development of applications such as 5G communication, high-frequency and high-speed signal transmission, large-size chips and DDR5, the signal frequency of electronic devices has been increasing, which has put forward higher requirements for the performance of packaging substrate materials. The substrate materials are required to have a low coefficient of thermal expansion (CTE), as well as a lower dielectric constant (Dk) and dielectric loss tangent (Df) in order to minimize the loss and delay of high-frequency signals.
[0003] Bismaleimide resins are widely used in encapsulation substrate resin systems due to their excellent heat resistance, high modulus, and low CTE. However, maleimide resins also suffer from drawbacks such as high curing temperature, poor solvent solubility, high dielectric constant and dielectric loss, and high brittleness. To improve these shortcomings, diamines or allyl compounds are commonly used for modification. While products modified with aromatic diamines can improve solubility and toughness to some extent, aromatic diamines are highly toxic, and the modified products are typically only soluble in high-boiling-point polar solvents such as DMF and NMP. Furthermore, there is still significant room for improvement in toughness, heat resistance, dielectric properties, and water absorption.
[0004] Existing patent WO2025053233A1 discloses a mixed application technology of maleimide resin with an indmium skeleton, multifunctional maleimide resin and maleimide resin without an indmium skeleton. Although this solution can improve dielectric properties, the compatibility and solubility between the different bismaleimide components are poor, which can easily lead to incomplete curing of the final cured product. Unreacted maleimide groups are easily generated in the cured product, which has an adverse effect on the heat resistance, water absorption and dielectric properties of the substrate.
[0005] Therefore, existing maleimide resin systems still struggle to simultaneously achieve excellent solvent solubility, good compatibility with other resins, low CTE, low Dk / Df, low water absorption, and high heat resistance. Summary of the Invention
[0006] The purpose of this invention is to provide a modified maleimide prepolymer, a resin composition, and a cured product prepared from the resin composition.
[0007] To achieve the above-mentioned objectives, the present invention adopts the following technical solution: a modified maleimide prepolymer, which is obtained by reacting the following raw materials in parts by weight: Maleimide compound: 100 parts by weight; Diamino silicone resin: 20-60 parts by weight; Diaminoindene compound: 1-40 parts by weight; Aminophenol: 0.1-10 parts by weight.
[0008] As a further improvement of the present invention, the diamino organosilicon resin contains the structural formula (1). Structural formula (1); Where R is C1-C 20 Alkylene, where n is an integer from 1 to 20.
[0009] As a further improvement of the present invention, the diaminoindene compound contains structural formula (2). Structural formula (2); Where R1-R4 are the same or different, and are hydrogen or C1-C5 alkyl groups respectively, and m is an integer from 1 to 10.
[0010] As a further improvement of the present invention, the compound with m=1 accounts for more than 80% by mass of the total amount of diaminoindene compounds corresponding to structural formula (2).
[0011] As a further improvement of the present invention, R1-R4 in the structural formula (2) are the same, and are methyl, ethyl or tert-butyl.
[0012] As a further improvement of the present invention, the amino equivalent of the diaminoindane compound is 245-380 g / mol; and / or, the amino equivalent of the diamino organosilicon resin is 500-2500 g / mol; and / or, the amino equivalent ratio of the diamino organosilicon resin to the diaminoindane compound is 1.8-4.5.
[0013] As a further improvement of the present invention, the weight ratio of the diamino organosilicon resin and the diamino indane compound is 0.2-5.
[0014] As a further improvement of the present invention, the preparation steps of the modified maleimide prepolymer are as follows: first, the maleimide compound, diamino silicone resin and aminophenol are pre-reacted to obtain a pre-reactant; then, diamino indane compound is added to the pre-reactant to continue the reaction to obtain the modified maleimide prepolymer.
[0015] To achieve the above-mentioned objective, the present invention also provides a resin composition comprising, by weight: First component: 100 parts by weight, wherein the first component is the modified maleimide prepolymer according to any one of claims 1-8; The second component is selected from at least one of epoxy resin, double-bonded polyphenylene ether resin and cyanate ester compound; When the second component is epoxy resin, its dosage is 1-60 parts by weight; When the second component is a polyphenylene ether resin containing double bonds, its dosage is 10-200 parts by weight; When the second component is a cyanate ester compound, its dosage is 10-100 parts by weight.
[0016] As a further improvement of the present invention, the resin composition further includes: 20-260 parts by weight of inorganic filler, and / or 5-50 parts by weight of flame retardant, and / or 5-50 parts by weight of curing agent.
[0017] To achieve the above-mentioned objectives, the present invention also provides a cured product made from the above-mentioned resin composition, the cured product comprising a prepreg, a copper-clad laminate, or a circuit board.
[0018] Beneficial effects: Compared with the prior art, the present invention has the following advantages: Maleimide compounds were modified by compounding diamino silicone resin and diamino indane compounds, with aminophenol participating in the reaction. Both silicone and indane units were introduced into the molecular chain of the final modified maleimide prepolymer. The good flexibility of the long-chain silicone oxygen groups improved the brittleness of the maleimide resin curing and crosslinking system, effectively reducing the coefficient of thermal expansion of the substrate and decreasing water absorption. Meanwhile, the indane units effectively reduced the dielectric constant and dielectric loss of the maleimide crosslinking system. The participation of phenol in the reaction can also adjust the molecular weight and end group structure of the prepolymer, and provide phenolic hydroxyl groups to improve solubility, compatibility and subsequent curing reactivity; therefore, this modified maleimide prepolymer can effectively improve the low CTE and low Dk / Df performance of maleimide resin system, while taking into account low water absorption, high heat resistance and high peel strength. It is suitable for use in resin formulations for low dielectric packaging substrates and is well applied in the field of packaging substrates with high heat resistance, low CTE, low Dk / Df, low water absorption and high peel strength. Detailed Implementation
[0019] The following describes specific implementation methods of the embodiments of the present invention. It should be noted that those skilled in the art can make several improvements and modifications without departing from the principles of the embodiments of the present invention, and these improvements and modifications are also considered to be within the protection scope of the embodiments of the present invention.
[0020] In this specification, "comprising" or "containing" means that, in addition to the components described, the resin composition may contain other components that can impart different properties to the resin composition.
[0021] This invention provides a modified maleimide prepolymer, obtained by reacting the following raw materials in parts by weight: Maleimide compound: 100 parts by weight; Diamino silicone resin: 20-60 parts by weight; Diaminoindene compound: 1-40 parts by weight; Aminophenol: 0.1-10 parts by weight.
[0022] In this invention, a modified maleimide compound is prepared by compounding diamino silicone resin and diamino indane compound, and aminophenol is introduced to participate in the reaction. Both silicone units and indane units are introduced into the molecular chain of the final modified maleimide prepolymer. The good flexibility of the long-chain silicone oxygen groups improves the brittleness of the maleimide resin curing and crosslinking system, effectively reducing the coefficient of thermal expansion of the substrate and decreasing water absorption. Meanwhile, the indane units effectively reduce the dielectric constant and dielectric loss of the maleimide crosslinking system. The participation of aminophenol in the reaction can also adjust the molecular weight and end group structure of the prepolymer, and provide phenolic hydroxyl groups to improve solubility, compatibility and subsequent curing reactivity; therefore, this modified maleimide prepolymer can effectively improve the low CTE and low Dk / Df performance of maleimide resin system, while taking into account low water absorption, high heat resistance and high peel strength. It is suitable for use in resin formulations for low dielectric packaging substrates and is well applied in the field of packaging substrates with high heat resistance, low CTE, low Dk / Df, low water absorption and high peel strength.
[0023] In a preferred embodiment of the diamino silicone resin, the diamino silicone resin contains the structural formula (1). Structural formula (1); where R is C1-C 20 The alkylene group, n is an integer from 1 to 20. More preferably, the R group in the structural formula (1) is C2-C. 10 Alkylene.
[0024] In a preferred embodiment, the amino equivalent in the diamino silicone resin is 500-2500 g / mol.
[0025] In one specific embodiment, the diamino silicone resin is selected from Shin-Etsu Chemical's X-22-161A or X-22-161B.
[0026] In a preferred embodiment of the diaminoindane compound, the diaminoindane compound contains structural formula (2). Structural formula (2); Wherein, R1-R4 are the same or different, and are hydrogen or C1-C5 alkyl groups respectively, and m is an integer from 1 to 10. The diaminoindane compound containing structural formula (2) and maleimide resin have good compatibility, and the reaction between the two proceeds fully. Indane groups are well introduced into the curing and crosslinking system, which effectively reduces the dielectric constant and dielectric loss of the substrate, while maintaining excellent heat resistance.
[0027] More preferably, R1 to R4 are the same and are selected as methyl, ethyl or tert-butyl.
[0028] Furthermore, compounds with m=1 account for more than 80% by mass of the total number of diaminoindene compounds corresponding to structural formula (2).
[0029] When the content of low molecular weight diaminoindane compound with m=1 in the diaminoindane compound corresponding to structural formula (2) is greater than 80% by mass, the reactivity with maleimide resin is greatly improved, and the overall performance of the substrate is effectively improved.
[0030] In a preferred embodiment, the amino equivalent of the diaminoindane compound is 245~355 g / mol.
[0031] In a preferred embodiment, the amino equivalent ratio of the diamino silicone resin and the diamino indane compound is 1.8 to 4.5.
[0032] In a preferred embodiment, the weight ratio of the diamino silicone resin to the diamino indane compound is 0.2 to 5. When the weight ratio of the diamino silicone resin to the diamino indane compound is less than 0.2, the content of siloxy groups in the crosslinked cured product is low, resulting in no significant improvement in the coefficient of thermal expansion. At the same time, excessive indane group content in the system will reduce the heat resistance of the substrate. Conversely, when the weight ratio of the diamino silicone resin to the diamino indane compound is higher than 5, the content of siloxy groups in the crosslinked cured product is excessive, effectively reducing the coefficient of thermal expansion of the substrate, but the improvement in dielectric properties is not significant.
[0033] In one specific embodiment, the weight ratio of the diamino silicone resin to the diamino indane compound is 1 to 3.2. For example, the weight ratio can be selected as 1, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9, 2.0, 2.1, 2.2, 2.3, 2.4, 2.5, 2.6, 2.7, 2.8, 2.9, 3.0, 3.1, or 3.2, as well as specific values between the above values. Due to space limitations and for the sake of brevity, this invention will not exhaustively list all the specific values included in the range.
[0034] In a preferred embodiment, the maleimide compound is selected from at least one of the following structures: Structural formula (3); Structural formula (4); Structural formula (5); Structural formula (6), where R2 is hydrogen, methyl, or ethyl, and R1 is methylene, ethylene, or... n is an integer from 1 to 10; Structure (7); The structure is (8), where n is an integer from 1 to 10; The structure is (9), where n is an integer from 1 to 10; Structural formula (10), where R is hydrogen, methyl or ethyl, and n is an integer from 1 to 10; In one specific embodiment, the maleimide compound may be selected from any one or more of the following grades of materials: BMI manufactured by Yamato Chemical Co., Ltd. 1000, BMI 1000H, BMI 1100, BMI 1100H, BMI 2000, BMI 2300, BMI 3000, BMI 3000H, BMI 4000H, BMI 5000, BMI 5100, BMI 7000, BMI 7000H; BMI, BMI manufactured by KI Chemical Co., Ltd. of Japan 70. BMI 80; MIR-3000 and MIR-5000 manufactured by Nippon Kayaku Co., Ltd.; X9-450 and X9-470 manufactured by DIC Co., Ltd. of Japan; D936, D937, D939, and D950 manufactured by Sichuan Dongcai Co., Ltd., etc.
[0035] The present invention does not impose any particular restrictions on the preparation method of the modified maleimide prepolymer, as long as the raw materials can react fully. Typically, the reaction temperature can be 45~175℃, and the reaction time can be 0.3~8.5h.
[0036] In a preferred embodiment, the preparation steps of the modified maleimide prepolymer are as follows: first, maleimide compound, diamino silicone resin and aminophenol are pre-reacted to obtain a pre-reactant; then, diamino indane compound is added to the pre-reactant for reaction to obtain the modified maleimide prepolymer.
[0037] Through the above stepwise reaction, long-chain siloxane groups are first introduced into the maleimide resin system, and then reacted with diaminoindane compounds. The overall reaction between maleimide groups and amino groups is more complete, effectively introducing siloxane groups and indane groups, and obtaining a final cured product with low dielectric properties, low CTE and high heat resistance.
[0038] Specifically, in order to promote the full cross-linking reaction between the components and improve the fluidity of the system during the reaction process, an organic solvent can be added appropriately, and the amount of the organic solvent can be 30 to 200 parts by weight.
[0039] In a preferred embodiment, the organic solvent is selected from at least one of acetone, butanone, methyl ethyl ketone, cyclohexanone, N,N-dimethylformamide and / or N,N-dimethylacetamide.
[0040] In one specific embodiment, the reaction temperature is 50–160°C, such as 50°C, 55°C, 60°C, 65°C, 70°C, 75°C, 80°C, 85°C, 90°C, 95°C, 100°C, 105°C, 110°C, 115°C, 120°C, 125°C, 130°C, 135°C, 140°C, 145°C, 150°C, or 160°C, as well as specific values between the above-mentioned values. Due to space limitations and for the sake of brevity, this invention will not exhaustively list all the specific values included in the range.
[0041] In one specific embodiment, the reaction time is 0.5 to 6.5 hours, for example, 0.5 hours, 0.6 hours, 0.8 hours, 1 hour, 1.2 hours, 1.5 hours, 1.8 hours, 2 hours, 2.2 hours, 2.5 hours, 2.8 hours, 3 hours, 3.2 hours, 3.5 hours, 3.8 hours, 4 hours, 4.2 hours, 4.5 hours, 4.8 hours, 5.0 hours, 5.5 hours, 6.0 hours, or 6.5 hours, as well as specific values between the above values. Due to space limitations and for the sake of brevity, this invention will not exhaustively list all the specific values included in the range.
[0042] Furthermore, the present invention also provides a resin composition comprising the above-mentioned modified maleimide prepolymer. Because the modified maleimide prepolymer simultaneously introduces organosilicon units and indane units into its molecular chain, and its end groups and reactivity can be adjusted by aminophenol, the modified maleimide prepolymer exhibits good compatibility and solvent solubility with other functional resins, and can be used as a base resin in resin compositions. Resin compositions containing the modified maleimide prepolymer can achieve a balance of low CTE, low Dk / Df, low water absorption, high heat resistance, and high peel strength, making them suitable for prepreg, copper-clad laminates, or circuit board encapsulation substrate materials.
[0043] In addition to the modified maleimide prepolymer described above, the resin composition may also include at least one of epoxy resin, double-bonded polyphenylene ether resin, and cyanate ester compound.
[0044] In one specific embodiment, the resin composition comprises, by weight: First component: 100 parts by weight, wherein the first component is the modified maleimide prepolymer described above; The second component is epoxy resin, and its dosage is 1-60 parts by weight.
[0045] Preferably, the epoxy resin is selected from any one or a combination of at least two of the following: bixylenol type epoxy resin, bisphenol A type epoxy resin, o-cresol formaldehyde type epoxy resin, bisphenol F type epoxy resin, bisphenol AF type epoxy resin, triphenol type epoxy resin, phosphorus-containing epoxy resin, isocyanate modified epoxy resin, phenolic epoxy resin, biphenyl type epoxy resin, dicyclopentadiene type epoxy resin, naphthalene type epoxy resin, alicyclic epoxy resin, glycidylamine type epoxy resin, glycidyl ester type epoxy resin, and aminophenol type epoxy resin.
[0046] More preferably, the epoxy resin is selected from at least one of o-cresol-type epoxy resin, naphthalene-type epoxy resin, dicyclopentadiene-type epoxy resin, or biphenyl-type epoxy resin.
[0047] In another specific embodiment, the resin composition comprises, by weight: First component: 100 parts by weight, wherein the first component is the modified maleimide prepolymer described above; The second component is a polyphenylene ether resin containing double bonds, and its dosage is 10-200 parts by weight.
[0048] Preferably, the polyphenylene ether resin has styrene or methacrylate groups at its ends.
[0049] Further preferably, the polyphenylene ether resin contains the structural formula (11). Structural formula (11); Among them, a, b, and c may be the same or different, and each is an independent integer from 1 to 50; X is at least one of the following structures: , , where R 11 R 12 R 13 R 14 R 15 R 16 R 17 R 18 Whether the two are the same or different, each is independently selected from hydrogen, C1-C5 alkyl, and B is an oxygen or C1-C 20 Alkylene; Y is R 21 R 22 R 23 R 24 They may be the same or different, and are each independently selected from hydrogen and C1-C5 alkyl groups.
[0050] In yet another embodiment, the resin composition comprises, by weight: First component: 100 parts by weight, wherein the first component is the modified maleimide prepolymer described above; The second component is a cyanate ester compound, and its dosage is 10-100 parts by weight.
[0051] Preferably, the cyanate compound is selected from any one or a mixture of at least two of bisphenol A cyanate resin, bisphenol F cyanate resin, bisphenol M cyanate, dicyclopentadiene cyanate resin, or phenolic cyanate resin.
[0052] Examples of the mixtures mentioned above include: mixtures of bisphenol A cyanate resin and bisphenol F cyanate resin, mixtures of bisphenol M cyanate, dicyclopentadiene cyanate resin and phenolic cyanate resin, and mixtures of bisphenol A cyanate resin, bisphenol F cyanate resin, bisphenol M cyanate and dicyclopentadiene cyanate resin, etc.
[0053] It should be noted that, in addition to epoxy resin, polyphenylene ether resin containing double bonds and cyanate ester compound, other functional resins may be further mixed into the above resin composition according to actual performance requirements without departing from the purpose of this invention. This invention does not impose any particular limitation on this. Those skilled in the art can select and adjust the dosage within the conventional range according to the target application scenario, as long as the comprehensive performance such as low CTE, low Dk / Df, low water absorption, high heat resistance and high peel strength desired by this invention can be achieved.
[0054] Furthermore, the resin composition also contains 5-50 parts by weight of curing agent. The addition of curing agent can promote the crosslinking reaction between the modified maleimide prepolymer and components such as epoxy resin, double-bonded polyphenylene ether resin, or cyanate ester compound in the resin composition, so that the resin system can be fully cured at a suitable temperature to form a dense and uniform crosslinked network. The amount of curing agent is controlled within the range of 5-50 parts by weight, which can ensure that the curing reaction is fully carried out, while avoiding incomplete curing, decreased heat resistance and mechanical properties due to insufficient curing agent, or excessive curing agent leading to excessive crosslinking density, increased brittleness of the system, and deterioration of dielectric properties and process applicability. This is beneficial to balance the comprehensive properties such as degree of curing, processing window, heat resistance, low CTE, low Dk / Df, low water absorption and high peel strength.
[0055] Specifically, the curing agent is selected from phenolic resin, aromatic amine compound, acid anhydride compound, active ester compound or dicyandiamide.
[0056] Furthermore, the resin composition also contains 20-260 parts by weight of inorganic filler. The addition of inorganic filler can effectively reduce the coefficient of thermal expansion of the resin composition, improve the dimensional stability, rigidity, and heat resistance of the cured product, and also help reduce water absorption and improve dielectric properties. Controlling the amount of inorganic filler within the range of 20-260 parts by weight can ensure the above-mentioned improvement effects while avoiding insufficient improvement in low CTE and dimensional stability due to insufficient filler, or excessive filler leading to increased viscosity of the resin composition, poor processing fluidity, decreased wettability with reinforcing materials, and reduced mechanical properties and peel strength of the cured product. This is beneficial for achieving a balance of low CTE, low Dk / Df, low water absorption, high heat resistance, high peel strength, and good processability.
[0057] Further preferably, the content of the inorganic filler is 60-180 parts by weight.
[0058] Specifically, the inorganic filler includes any one or a combination of at least two of the following: non-metallic oxides, metal oxides, metal hydroxides, metal nitrides, non-metallic nitrides, inorganic hydrates, inorganic salts, metal hydrates, and inorganic phosphorus. Preferably, the inorganic filler includes any one or a combination of at least two of the following: silicon dioxide, titanium dioxide, zinc oxide, aluminum hydroxide, aluminum oxide, magnesium oxide, magnesium hydroxide, calcium carbonate, aluminum nitride, boron nitride, silicon aluminum carbide, silicon carbide, zirconium oxide, mica, boehmite, calcined talc, talc, silicon nitride, strontium titanate, barium titanate, and calcined kaolin. The silicon dioxide can be any one or a combination of at least two of the following: fused silica, crystalline silica, spherical silica, and hollow silica.
[0059] In a preferred embodiment, the median particle size (D50) of the inorganic filler is 0.01-10 μm, for example, it can be 0.05 μm, 0.1 μm, 0.3 μm, 0.5 μm, 0.8 μm, 1 μm, 3 μm, 5 μm, 8 μm or 9 μm, as well as specific values between the above values. Due to space limitations and for the sake of brevity, the present invention will not exhaustively list the specific values included in the range. Controlling the median particle size of the inorganic filler within the above range is beneficial to achieving good dispersibility and filling effect in the resin composition, avoiding uneven filling and increased interface defects due to excessively large particle size, or excessively small particle size leading to increased specific surface area, difficulty in dispersion, and increased system viscosity.
[0060] In a further preferred embodiment, the inorganic filler is surface-treated with an aminosilane coupling agent, an epoxysilane coupling agent, or a double-bond silane coupling agent. This improves the compatibility between the inorganic filler and the organic resin, enhances the dispersibility of the filler, and increases the interfacial bonding force with the resin, thereby improving the mechanical properties, heat resistance, low water absorption, and dimensional stability of the cured product.
[0061] Furthermore, the resin composition also contains 5-50 parts by weight of a flame retardant. Without significantly affecting the original dielectric and mechanical properties of the resin system, the fire safety level of the cured product is significantly improved through the synergistic mechanism of the flame retardant. This provides crucial safety assurance for the final substrate and other components operating in high-voltage, high-current environments such as charging piles, greatly reducing the risk of fires caused by electrical faults.
[0062] The flame retardant is selected from bromine-based flame retardants, phosphorus-based flame retardants, nitrogen-based flame retardants, etc.
[0063] Specifically, the brominated flame retardant is selected from decabromodiphenyl ether, decabromodiphenyl ethane, styrene bromide, or tetrabromophthalamide.
[0064] The phosphorus-based flame retardant is selected from inorganic phosphorus, phosphate esters, phosphoric acid, hypophosphoric acid, phosphorus oxide, 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide (DOPO), and 10-(2,5-dihydroxyphenyl)-9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide (DOPO-HQ). (m is an integer from 1 to 5) Organophosphorus compounds including 10-phenyl-9,10-dihydro-9-oxa-10-phenanthroline-10-oxide, tris(2,6-dimethylphenyl)phosphine, phosphazenes, and modified phosphazenes. The DOPO group is... .
[0065] The nitrogen-based flame retardant is selected from triazine compounds, cyanuric acid compounds, isocyanate compounds, phenothiazine, etc.
[0066] In one specific embodiment, the flame retardant is selected from the following: phosphazene esters manufactured by Otsuka Chemicals of Japan, with grades SPB-10, BP-PZ, PP-PZ, SPCN-100, SPV-100 and SPB-100L; phosphazene esters manufactured by Fushimi Pharmaceuticals, with grades FP-100, FP-300B and FP-390; phosphate esters manufactured by Daihachi Chemicals, with grades PX-200, PX-201 and PX-202; phosphate esters manufactured by FRX of the United States, with grades OL3001 and OL5000; phosphate esters manufactured by Clariant, with grades OP-935 and OP-945; and brominated flame retardants manufactured by Albemarle, with grade SAYTEX8010.
[0067] Furthermore, the resin composition also contains 0.05-10 parts by weight of a catalyst.
[0068] Specifically, the catalyst is selected from 2-methylimidazole, 2-ethyl-4-methylimidazole, 2-phenylimidazole, 2-undecylimidazole, 1-benzyl-2-methylimidazole, 2-heptadecylimidazole, 2-isopropylimidazole, 2-phenyl-4-methylimidazole, 2-dodecylimidazole, isocyanate-modified imidazole, or 1-cyanoethyl-2-methylimidazole.
[0069] Furthermore, the present invention also provides a cured product prepared from the above-described resin composition, wherein the cured product includes, but is not limited to, a prepreg, a copper-clad laminate, or a circuit board. The prepreg is prepared from the resin composition, the copper-clad laminate is prepared from the prepreg, and the circuit board is prepared from the prepreg and / or the copper-clad laminate.
[0070] Specifically, the prepreg includes a reinforcing material and the aforementioned resin composition attached to the reinforcing material, wherein the resin composition is specifically attached to the reinforcing material by impregnation and drying.
[0071] The reinforcing material is selected from at least one of natural fibers, organic synthetic fibers, organic fabrics, and inorganic fabrics.
[0072] Preferably, the reinforcing material is glass fiber cloth, and the glass fiber cloth preferably uses open fiber cloth or flat cloth. More preferably, the glass fiber cloth is E glass fiber cloth, T glass fiber cloth, S glass fiber cloth or Q glass fiber cloth.
[0073] Specifically, when the reinforcing material is glass fiber cloth, the glass fiber cloth generally needs to undergo chemical treatment to improve the bonding between the resin composition and the glass fiber cloth interface. The main method of chemical treatment is coupling agent treatment, and the coupling agent used is preferably a silane coupling agent containing double bonds or an aminosilane coupling agent to provide good adhesion and heat resistance.
[0074] The method for preparing the prepreg is as follows: The aforementioned resin composition was dissolved in a solvent to prepare a gel solution, which was then mechanically stirred at room temperature for 3-6 hours to dissolve and mature. The adhesive is applied to the reinforcing material by impregnation. The impregnated reinforcing material is then removed and baked at 100~180℃ for 1~15 minutes. After drying, the semi-cured sheet is obtained.
[0075] Specifically, the solvent may be selected from at least one of acetone, butanone, methyl isobutyl ketone, N,N-dimethylformamide, N,N-dimethylacetamide, ethylene glycol methyl ether, propylene glycol methyl ether, benzene, toluene, xylene, and cyclohexane. The amount of solvent added is not specifically limited in this invention. The amount of solvent added shall be selected by those skilled in the art based on their experience, as long as the resulting adhesive reaches a suitable viscosity for use.
[0076] The amount of solvent added is not specifically limited in this invention. The amount of solvent added is selected by those skilled in the art based on their experience, as long as the resulting adhesive solution reaches a suitable viscosity for use.
[0077] In one optional embodiment of the copper-clad laminate, the copper-clad laminate includes a prepreg as described above and copper foil covering one or both sides of the prepreg. In this case, the preparation method of the copper-clad laminate specifically involves covering one or both surfaces of the prepreg with copper foil.
[0078] In another optional embodiment of the copper-clad laminate, the copper-clad laminate includes a laminated prepreg formed by stacking at least two of the aforementioned prepreg sheets, and copper foil covering one or both sides of the laminated prepreg sheet. In this case, the specific method for preparing the copper-clad laminate is as follows: at least two prepreg sheets are stacked to form a laminated prepreg sheet; copper foil is then applied to one or both surfaces of the laminated prepreg sheet; and the laminate is obtained by hot pressing. The hot pressing conditions are: pressure of 0.2~3.5 MPa, temperature of 100~250℃, and pressing time of 2~6 h.
[0079] In a preferred embodiment, the thickness of the copper foil is 5μm, 8μm, 12μm, 18μm, 35μm or 70μm.
[0080] The present invention will be described in detail below with reference to specific embodiments 1 to 7 and comparative examples 1 to 6; of course, it is understood that the embodiments in the present invention are not limited to these embodiments.
[0081] The components and contents of the resin compositions in Examples 1-8 are shown in Table 1 below: Table 1: Ingredient list of resin compositions in Examples 1-7
[0082] The preparation methods for modified maleimide prepolymers A to C are as follows: Modified maleimide prepolymer A: Add 2,6 Dimethylaniline 48.5g (0.4mol), α,α' dihydroxy 1,3 272.0 g (1.4 mol) of diisopropylbenzene, 280 g of xylene, and 70 g of activated clay were heated to 120 °C while stirring. The distillate water was then removed, and the temperature was raised to 210 °C for 3 hours. The mixture was then cooled to 140 °C, and 2,6-dimethylbenzene was added. 145.4 g (1.2 mol) of dimethylaniline was added, and the mixture was heated to 220 °C and reacted for 3 hours. After the reaction, the mixture was cooled to 100 °C and diluted with 300 g of toluene. Activated clay was removed by filtration, and the solvent and unreacted low molecular weight substances were removed by distillation under reduced pressure. This yielded diaminoindane compound A, with an amine equivalent of 298 g / mol and a monomeric structure of n=1 comprising more than 85% of the composition.
[0083]
[0084] 25g of diamino silicone resin (Shin-Etsu Chemical, X-22-161A), 100g of maleimide compound (structural formula (9), Nippon Kayaku Corporation MIR-3000), 25g of the above-mentioned diamino indane compound A, 1.5g of 4-aminophenol, and 170g of propylene glycol monomethyl ether were added to a reaction flask and reacted at 125°C for 4.5h to obtain modified maleimide prepolymer A.
[0085] Modified maleimide prepolymer B: Add 2,6 Diethylaniline 59.7g (0.4mol), α,α' dihydroxy 1,3 272.0 g (1.4 mol) of diisopropylbenzene, 350 g of xylene, and 94 g of activated clay were heated to 120 °C while stirring. The distillate water was then removed, and the temperature was raised to 210 °C for 3 hours. The mixture was then cooled to 140 °C, and 2,6-dimethylbenzene was added. After adding 179.1 g (1.2 mol) of diethylaniline, the mixture was heated to 220 °C and reacted for 3 hours. Following the reaction, the mixture was cooled to 100 °C and diluted with 500 g of toluene. Activated clay was removed by filtration, and the solvent and unreacted low-molecular-weight substances were removed by distillation under reduced pressure. This yielded the diaminoindene compound B, with an amine equivalent of 364 g / mol and a monomeric structure containing more than 85% n=1.
[0086] 35g of diamino silicone resin (Shin-Etsu Chemical, X-22-161A), 100g of maleimide compound (structural formula (5), BMI-80 prepared by KI synthesis), 10g of diamino indane compound B, 1.5g of 4-aminophenol, and 170g of propylene glycol monomethyl ether were added to a reaction flask and reacted at 125°C for 4.5h to obtain modified maleimide prepolymer B.
[0087] Modified maleimide prepolymer C: Add 2,6 Dimethylaniline 48.5g (0.4mol), α,α' dihydroxy 1,3 272.0 g (1.4 mol) of diisopropylbenzene, 280 g of xylene, and 70 g of activated clay were heated to 120 °C while stirring. The distillate water was then removed, and the temperature was raised to 210 °C for 3 hours. The mixture was then cooled to 140 °C, and 2,6-dimethylbenzene was added. 145.4 g (1.2 mol) of dimethylaniline was added, and the mixture was heated to 220 °C and reacted for 3 hours. After the reaction, the mixture was cooled to 100 °C and diluted with 300 g of toluene. Activated clay was removed by filtration, and the solvent and unreacted low molecular weight substances were removed by distillation under reduced pressure. This yielded diaminoindane compound A, with an amine equivalent of 298 g / mol and a monomeric structure of n=1 comprising more than 85% of the composition.
[0088]
[0089] 25g of diamino silicone resin (Shin-Etsu Chemical, X-22-161A), 100g of maleimide compound (structural formula (9), Nippon Kayaku Corporation MIR-3000), 1.5g of 4-aminophenol, and 170g of propylene glycol monomethyl ether were added to a reaction flask. After reacting at 125°C for 2.5h, 25g of diamino indane compound A was added, and the reaction was continued for 2h at the same temperature to obtain modified maleimide prepolymer C.
[0090] The components and contents of the resin compositions of Comparative Examples 1 to 6 are shown in Table 1 below: Table 2: Ingredient list of resin compositions for Comparative Examples 1-6
[0091] The preparation methods for modified maleimide prepolymers A', B', and C' are as follows: Modified maleimide prepolymer A': 50g of diamino silicone resin (Shin-Etsu Chemical, X-22-161A), 100g of maleimide compound (structural formula (9), Nippon Kayaku Corporation MIR-3000), 1.5g of 4-aminophenol, and 170g of propylene glycol monomethyl ether were added to a reaction flask and reacted at 125°C for 4.5h to obtain modified maleimide prepolymer A'.
[0092] Modified maleimide prepolymer B': 100g of maleimide compound (structural formula (9), Nippon Kayakusei MIR-3000), 40g of diaminoindane compound A, 1.5g of 4-aminophenol, and 170g of propylene glycol monomethyl ether were added to a reaction flask and reacted at 125°C for 4.5h to obtain modified maleimide prepolymer B'.
[0093] In addition, the flame retardant in Examples 1-8 and Comparative Examples 1-5 above is selected as phosphate ester PX-200, the filler is selected as spherical silica, the epoxy resin is selected as biphenyl type epoxy resin, the cyanate is selected as bisphenol A type cyanate, the polyphenylene ether is selected as styrene-terminated polyphenylene ether, and the unmodified maleimide is selected as MIR-3000.
[0094] Modified maleimide prepolymer C': Add 2,6 Diethylaniline 59.7g (0.4mol), α,α' dihydroxy 1,3 272.0 g (1.4 mol) of diisopropylbenzene, 350 g of xylene, and 94 g of activated clay were heated to 120 °C while stirring. The distillate water was then removed, and the temperature was raised to 210 °C for 3 hours. The mixture was then cooled to 140 °C, and 2,6-dimethylbenzene was added. After adding 179.1 g (1.2 mol) of diethylaniline, the mixture was heated to 220 °C and reacted for 3 hours. Following the reaction, the mixture was cooled to 100 °C and diluted with 500 g of toluene. Activated clay was removed by filtration, and the solvent and unreacted low-molecular-weight substances were removed by distillation under reduced pressure. This yielded the diaminoindene compound B, with an amine equivalent of 364 g / mol and a monomeric structure containing more than 85% n=1.
[0095] 7g of diamino silicone resin (Shin-Etsu Chemical, X-22-161A), 100g of maleimide compound (structural formula (5), BMI-80 prepared by KI synthesis), 40g of diaminoindane compound B (synthesis example 2), 1.5g of 4-aminophenol, and 170g of propylene glycol monomethyl ether were added to a reaction flask and reacted at 125°C for 4.5h to obtain modified maleimide prepolymer C'.
[0096] The preparation methods for the prepregs corresponding to Examples 1-7 and Comparative Examples 1-6 are as follows: The E-glass fiber cloth 2116, which is used as a reinforcing material, is pretreated with an aminosilane coupling agent. The resin compositions of Examples 1-7 (according to Table 1) and Comparative Examples 1-6 (according to Table 2) were dissolved in methyl ethyl ketone to prepare a glue solution, and mechanically stirred at room temperature for 3-6 hours to dissolve and mature, thereby obtaining the glue solution. E-glass fiber cloth was sequentially immersed in the adhesive solutions obtained in Examples 1-7 and Comparative Examples 1-6. After immersion, the cloth was removed and placed in a forced-air drying oven at 155°C. After baking for 3-6 minutes, semi-cured sheets corresponding to Examples 1-7 and Comparative Examples 1-6 were obtained respectively.
[0097] Preparation of copper-clad laminates for performance evaluation: Two prepregs prepared in Examples 1-7 and Comparative Examples 1-6 were cut to 300×300mm. These prepregs were stacked to form a composite prepreg with a certain structure. Then, an electrolytic copper foil with a thickness of 18μm was placed on each side of the composite prepreg. The prepreg was then placed in a vacuum hot press and hot-pressed for 3.5h at a pressure of 2.2MPa and a temperature of 150-220℃ to obtain a copper-clad laminate.
[0098] For performance evaluation, the copper-clad laminates prepared above, corresponding to Examples 1-7 and Comparative Examples 1-6 respectively, were used for performance testing. Specifically, the performance evaluation method is as follows: (1) Glass transition temperature (Tg): According to IPC-TM-650 2.4.24.4, it was tested with a dynamic thermomechanical analyzer (DMA) at a heating rate of 10℃ / min and a frequency of 10Hz. (2) Dk and Df: Dielectric properties were measured at 10 GHz according to IPC-TM-650 2.5.5.5, SPDR; (3) Coefficient of thermal expansion (CTE) along the X-axis: The TMA method was used to determine the CTE according to the IPC-TM-650 method. The heating rate was 10℃ / min and the test temperature range was 30~100℃. (4) Water absorption rate: The water absorption rate was determined according to the method of IPC-TM-6502.6.2.1. Specifically, three samples with a length × width of 10cm × 10cm and a thickness of 0.4mm were taken and the electrolytic copper foil was removed from both sides. They were dried at 100℃ for 2 hours, weighed, and the weight was recorded as W1. Then they were placed in a pressure cooker and treated at 121℃ and 2 atmospheres for 6 hours. The weight was recorded as W2. The water absorption rate was determined to be (W2-W1) / W1×100%. (5) Peel strength: The peel strength of the copper foil layer was tested according to the "post-thermal stress" test conditions in the IPC-TM-650 method.
[0099] The properties of copper-clad laminates obtained using the prepregs in Examples 1-7 and Comparative Examples 1-6 are shown in Tables 3 and 4 below.
[0100] Table 3 (Examples 1-7)
[0101] Table 4 (Comparative Examples 1-6)
[0102] A parallel comparison was made between Examples 3 and 7. The modified maleimide prepolymer C used in the resin composition of Example 3 was prepared by a stepwise method, while the modified maleimide prepolymer A in Example 7 was prepared by a one-step method. Comparing the performance of the copper-clad laminates prepared by the two methods, it can be seen that, compared with Example 7, the copper-clad laminate prepared by the resin composition of Example 3 has a higher glass transition temperature, higher peel strength, lower Dk and Df, lower CTE value, and lower water absorption rate. It can be better applied in the field of packaging substrates with high heat resistance, low CTE, low Dk / Df, low water absorption rate, and high peel strength.
[0103] Example 1 and Comparative Example 1 were compared in parallel. The modified maleimide prepolymer A used in the resin composition of Example 1 contained diamino silicone resin, diamino indane compound A, and aminophenol; while the modified maleimide prepolymer A' in Comparative Example 1 was not modified with diamino indane compound. Comparing the performance of the copper-clad laminates prepared by the two, it can be seen that, compared with Comparative Example 1, the copper-clad laminate prepared by the resin composition of Example 1 has a higher glass transition temperature, higher peel strength, lower Dk and Df, lower CTE value, and lower water absorption rate. It can be well applied in the field of packaging substrates with high heat resistance, low CTE, low Dk / Df, low water absorption rate, and high peel strength.
[0104] Example 1 and Comparative Example 5 were compared in parallel. The modified maleimide prepolymer A used in the resin composition of Example 1 was modified with diamino silicone resin, diamino indane compound A, and aminophenol; while Comparative Example 5 used unmodified maleimide resin. Comparing the performance of the copper-clad laminates prepared by the two, it can be seen that the unmodified maleimide resin used in Comparative Example 5 resulted in uneven dissolution of the adhesive and could not be prepared. The copper-clad laminate prepared by the resin composition of Example 1 can be well applied in the field of packaging substrates with high heat resistance, low CTE, low Dk / Df, low water absorption and high peel strength.
[0105] Example 3 and Comparative Example 2 were compared in parallel. The modified maleimide prepolymer C used in the resin composition of Example 3 was modified with diamino silicone resin, diamino indane compound A, and aminophenol; while the modified maleimide prepolymer B' used in the resin composition of Comparative Example 2 was not modified with diamino silicone resin. Comparing the performance of the copper-clad laminates prepared by the two, it can be seen that, compared with Comparative Example 2, the copper-clad laminate prepared by the resin composition of Example 3 has a higher glass transition temperature, higher peel strength, lower Dk and Df, lower CTE value, and lower water absorption rate. It can be well applied in the field of packaging substrates with high heat resistance, low CTE, low Dk / Df, low water absorption rate, and high peel strength.
[0106] A parallel comparison was made between Example 5 and Comparative Example 6. The content of each raw material in the modified maleimide prepolymer C used in the resin composition of Example 5 conforms to the scheme protected by this application. However, the content of each raw material in the modified maleimide prepolymer C' used in the resin composition of Comparative Example 6 does not conform to the scheme to be protected by this application. For example, the content of diamino silicone resin is 7g, which does not conform to the range of 20-60 parts by weight, and the weight ratio of diamino silicone resin to diamino indane compound does not conform to 0.2-5. Comparing the performance of the copper-clad laminates prepared by the two, it can be seen that, compared with Comparative Example 6, the copper-clad laminate prepared by the resin composition of Example 5 has a higher glass transition temperature, higher peel strength, lower Dk and Df, lower CTE value, and lower water absorption rate. It can be well applied in the field of packaging substrates with high heat resistance, low CTE, low Dk / Df, low water absorption rate and high peel strength.
[0107] Example 6 and Comparative Example 4 were compared in parallel. In Example 6, the modified maleimide prepolymers A and C used in the resin composition were modified with diamino silicone resin and diamino indane compound A. In contrast, in Comparative Example 4, the modified maleimide prepolymer A' used in the resin composition was not modified with diamino indane compound, and the modified maleimide prepolymer B' used was not modified with diamino silicone resin. Comparing the performance of the copper-clad laminates prepared by the two examples, it can be seen that, compared with Comparative Example 4, the copper-clad laminate prepared by the resin composition of Example 6 has a higher glass transition temperature, higher peel strength, lower Dk and Df, lower CTE value, and lower water absorption rate. It can be well applied in the field of packaging substrates with high heat resistance, low CTE, low Dk / Df, low water absorption rate, and high peel strength.
[0108] It should be understood that although this specification describes embodiments, not every embodiment contains only one independent technical solution. This way of describing the specification is only for clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment can also be appropriately combined to form other embodiments that can be understood by those skilled in the art.
[0109] The detailed descriptions listed above are merely specific descriptions of feasible embodiments of the present invention, and are not intended to limit the scope of protection of the present invention. All equivalent embodiments or modifications made without departing from the spirit of the present invention should be included within the scope of protection of the present invention.
Claims
1. A modified maleimide prepolymer characterized in that, It is obtained by reacting the following raw materials in parts by weight: Maleimide compound: 100 parts by weight; Diamino silicone resin: 20-60 parts by weight; Diaminoindene compound: 1-40 parts by weight; Aminophenol: 0.1-10 parts by weight.
2. The modified maleimide prepolymer according to claim 1, wherein The diamino organosilicon resin contains the structural formula (1). Formula (1); wherein R is a C1-C 20 alkylene group, and n is an integer from 1 to 20.
3. The modified maleimide prepolymer of claim 1, wherein, The diaminoindene compound contains structural formula (2). Formula (2); Where R1-R4 are the same or different, and are hydrogen or C1-C5 alkyl groups respectively, and m is an integer from 1 to 10.
4. The modified maleimide prepolymer according to claim 3, characterized in that, Compounds with m=1 account for more than 80% by mass of the total number of diaminoindene compounds corresponding to structural formula (2).
5. The modified maleimide prepolymer according to claim 3, characterized in that, The R1-R4 in the structural formula (2) are the same, and are methyl, ethyl or tert-butyl.
6. The modified maleimide prepolymer according to claim 1, characterized in that, The amino equivalent of the diaminoindane compound is 245-380 g / mol; and / or, the amino equivalent of the diamino organosilicon resin is 500-2500 g / mol; and / or, the amino equivalent ratio of the diamino organosilicon resin to the diaminoindane compound is 1.8-4.
5.
7. The modified maleimide prepolymer according to claim 1, characterized in that, The weight ratio of the diamino organosilicon resin to the diamino indane compound is 0.2-5.
8. The modified maleimide prepolymer according to claim 1, characterized in that, The preparation steps of the modified maleimide prepolymer are as follows: first, the maleimide compound, diamino silicone resin and aminophenol are pre-reacted to obtain a pre-reactant; then, diamino indane compound is added to the pre-reactant to continue the reaction to obtain the modified maleimide prepolymer.
9. A resin composition, characterized in that, By weight, it includes: First component: 100 parts by weight, wherein the first component is the modified maleimide prepolymer according to any one of claims 1-8; The second component is selected from at least one of epoxy resin, double-bonded polyphenylene ether resin and cyanate ester compound; When the second component is epoxy resin, its dosage is 1-60 parts by weight; When the second component is a polyphenylene ether resin containing double bonds, its dosage is 10-200 parts by weight; When the second component is a cyanate ester compound, its dosage is 10-100 parts by weight.
10. The resin composition according to claim 9, characterized in that, The resin composition further includes: 20-260 parts by weight of inorganic filler, and / or 5-50 parts by weight of flame retardant, and / or 5-50 parts by weight of curing agent.
11. A cured product made from the resin composition of claim 9 or 10, characterized in that, The cured material includes a prepreg, copper-clad laminate, or circuit board.
Citation Information
Patent Citations
Thermosetting resin composition, prepreg, resin film, laminate, printed wiring board, and semiconductor package
WO2025053233A1