Low dielectric loss polyphenylene sulfide polymer alloy, polyphenylene sulfide film and preparation method thereof
By introducing amorphous fluorinated polyarylate copolymers containing flexible segments and carboxyl-terminated groups into polyphenylene sulfide to form a block structure, the problem of high-frequency dielectric loss is solved, realizing a high-frequency, low-dielectric-loss polyphenylene sulfide polymer alloy suitable for 5G/6G communication.
Patent Information
- Application Number
- CN202611482562.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-22
- Publication Date
- 2026-11-24
AI Technical Summary
Existing technologies struggle to suppress the increase in dielectric loss under high-frequency millimeter-wave conditions without sacrificing the heat resistance and toughness of polyphenylene sulfide, thus limiting its application in 5G/6G communications.
By introducing amorphous fluorinated polyarylate copolymers with flexible segments and carboxyl-terminated ends into hydroxyl-terminated polyphenylene sulfide and forming a block structure through melt extrusion, in-situ reaction is promoted, and compatibility and toughness are improved.
The preparation of a low dielectric loss polyphenylene sulfide polymer alloy was achieved, which maintained the heat resistance and toughness of the material, while significantly reducing dielectric loss at high frequencies, making it suitable for 5G/6G communication.
Smart Images

Figure CN123152291A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of polymer alloy technology, specifically relating to low dielectric loss polyphenylene sulfide polymer alloys, polyphenylene sulfide films and their preparation methods. Background Technology
[0002] With the rapid iteration of 5G / 6G communication, high-speed integrated circuits, and aerospace technology, electronic and electrical equipment is developing towards miniaturization, high frequency, and high speed, placing stringent requirements on the dielectric constant, dielectric loss, heat resistance, and mechanical toughness of insulating polymer materials. Low-dielectric polymer insulating materials, with their advantages of low dielectric constant, low dielectric loss, light weight, and excellent processing performance, can suppress signal transmission delay, reduce signal crosstalk, and lower dielectric heat loss under high-frequency operating conditions, making them a core candidate material for high-frequency communication substrates, flexible copper-clad laminates, and radar components.
[0003] Polyphenylene sulfide (PPS), as a high-performance, low-dielectric aromatic polymer, has a molecular backbone composed of alternating benzene rings and thioether bonds. It possesses outstanding thermal stability, chemical resistance, and high flame retardancy, making it a promising candidate for applications in electronics, electrical engineering, and aerospace. However, in the millimeter-wave high-frequency band (≥10GHz), pure PPS suffers a significant increase in dielectric loss due to polarization relaxation hysteresis, making it difficult to meet the low-loss requirements of 5G / 6G millimeter-wave communication. Existing technologies introduce hollow microspheres and inorganic nanofillers to reduce the dielectric constant of PPS. However, inorganic fillers are prone to agglomeration, introducing significant interfacial polarization, which in turn increases high-frequency dielectric loss and further degrades the toughness of PPS. While blending with conventional elastomers can improve toughness, the high polarity and poor heat resistance of elastomers significantly compromise the dielectric properties and heat distortion temperature of the material.
[0004] In fluoropolymers, the electron clouds of the CF bonds are bound to the atomic nuclei, resulting in low electronic polarizability. Simultaneously, fluorine substitution increases the free volume of the molecular chain, effectively reducing the dielectric constant and dielectric loss. However, fluoropolymer molecular chains are highly inert and have poor compatibility with PPS. Physical blending of the two easily leads to phase separation, resulting in weak interfacial bonding and causing fluctuations in the material's dielectric properties and a decrease in strength.
[0005] Therefore, how to suppress the increase in dielectric loss under high-frequency millimeter wave conditions without sacrificing the inherent heat resistance and toughness of PPS, and thus achieve the preparation of high-frequency, low-dielectric-loss PPS-based polymer alloys, is a technical problem that urgently needs to be solved in this field. Summary of the Invention
[0006] To address the shortcomings of existing technologies in polyphenylene sulfide (PPS) under high-frequency millimeter-wave conditions, low-dielectric-loss PPS polymer alloys, PPS films, and their preparation methods are provided.
[0007] The objective of this invention is achieved through the following technical solution: In a first aspect, the present invention provides a low dielectric loss polyphenylene sulfide polymer alloy, comprising, by mass parts of raw materials: 55-85 parts of hydroxyl-terminated polyphenylene sulfide, 10-40 parts of toughening agent; The toughening agent is an amorphous fluorinated polyarylene copolymer containing flexible segments and carboxyl-terminated ends.
[0008] In some specific embodiments of the present invention, the amorphous fluorinated polyarylate copolymer containing flexible segments and carboxyl-terminated groups is obtained by polycondensation of 2,3,5,6-tetrafluoroterephthaloyl chloride and bisphenol compounds.
[0009] In some specific embodiments of the present invention, the bisphenol compound is selected from one or more of bisphenol fluorene, phenolphthalein, 3,3-bis(4-hydroxyphenyl)-2-phenylprop-1-one, bisphenol A, and diether fluorene.
[0010] In some specific embodiments of the present invention, when the bisphenol compound is dietherfluorene and bisphenol compound B, wherein the bisphenol compound B is selected from one of bisphenolfluorene, phenolphthalein, 3,3-bis(4-hydroxyphenyl)-2-phenylprop-1-one, and bisphenol A, the molar ratio of the bisphenol compound B, dietherfluorene, and 2,3,5,6-tetrafluoroterephthaloyl chloride is (0.2-0.8):(0.8-0.2):1.05.
[0011] In some specific embodiments of the present invention, the bisphenol compound is bisphenol fluorene.
[0012] In some specific embodiments of the present invention, the structural formula of the amorphous fluorinated polyarylene copolymer containing flexible segments and carboxyl-terminated ends is shown in Formula I:
[0013] I In Formula I, 2 ≤ p ≤ 1000, 2 ≤ q ≤ 1000; R1 and R2 are each independently selected from one or more of the following groups obtained by dehydrogenation of bisphenols: bisphenol fluorene, phenolphthalein, 3,3-bis(4-hydroxyphenyl)-2-phenylprop-1-one, bisphenol A, and diether fluorene. R1 and R2 can be the same type of group or different types of groups.
[0014] In some specific embodiments of the present invention, the preparation method of the amorphous fluorinated polyarylene copolymer containing flexible segments and carboxyl-terminated ends is selected from one or more of the following: low-temperature solution polymerization, high-temperature solution polymerization, and melt polycondensation.
[0015] In some specific embodiments of the present invention, the hydroxyl-terminated polyphenylene sulfide has the structural formula shown in Formula II:
[0016] II In Equation II, 2 ≤ n ≤ 1500.
[0017] In some specific embodiments of the present invention, the preparation method of the hydroxyl-terminated polyphenylene sulfide includes the following steps: p-Hydroxybenzyl thiophenol was mixed with polyphenylene sulfide, and N-methylpyrrolidone was added. The mixture was reacted at 140-270°C for 4-36 hours under alkaline catalyst and in an inert atmosphere. After cooling and crystallization, the hydroxyl-terminated polyphenylene sulfide was obtained by filtration and acid washing.
[0018] In some specific embodiments of the present invention, the mass ratio of the polyphenylene sulfide to the p-hydroxythiophenol is 20-50:1; the reaction temperature is 200-240°C; the reaction time is 8-16 hours; and the acid washing is performed 5 times.
[0019] In a second aspect, the present invention provides a method for preparing the low dielectric loss polyphenylene sulfide polymer alloy described in the first aspect, comprising the following steps: According to the above ratio, hydroxyl-terminated polyphenylene sulfide and amorphous fluorinated polyarylate copolymer containing flexible segments and carboxyl-terminated groups are blended for 10-20 minutes and then melt-extruded at 300-350℃ to obtain a low dielectric loss polyphenylene sulfide polymer alloy.
[0020] In some specific embodiments of the present invention, blending hydroxyl-terminated polyphenylene sulfide and amorphous fluorinated polyarylene copolymer containing flexible segments and carboxyl-terminated groups for 10-20 minutes includes... First, melt and heat the hydroxyl-terminated polyphenylene sulfide for 5-10 minutes, then add the amorphous fluorinated polyarylate copolymer containing flexible segments and carboxyl-terminated groups and blend for 5-10 minutes.
[0021] Thirdly, the present invention provides a low dielectric loss polyphenylene sulfide film prepared from the low dielectric loss polyphenylene sulfide polymer alloy described in the first aspect.
[0022] Fourthly, the present invention provides a method for preparing the low dielectric loss polyphenylene sulfide film described in the third aspect, wherein the preparation method is selected from one or more of the pressing method and the blow molding method.
[0023] In some specific embodiments of the present invention, the preparation method is a pressure molding method, which specifically includes the following steps: Low dielectric loss polyphenylene sulfide polymer alloy is fed into a film press, and the film pressing temperature is 300-350℃ and the pressure is 5-10MPa to obtain a low dielectric loss polyphenylene sulfide film.
[0024] In this invention, the term "flexible segment" refers to a movable molecular segment in a polymer that can freely curl, absorb stress, and improve the flexibility of the material. The flexible segment includes -CH2-CH2-, -O-, and -CO-.
[0025] In this invention, the term "hydroxyl-terminated" refers to the fact that the molecular chain of polyphenylene sulfide has a hydroxyl functional group at its end.
[0026] In this invention, the term "carboxyl-terminated" refers to the fact that the molecular chain of an amorphous fluorinated polyarylate copolymer has a carboxyl functional group at its end.
[0027] In this invention, the term "amorphous fluorinated polyarylate copolymer" refers to its aggregated structure. Due to its twisted and non-planar nature, its molecular chains cannot achieve long-range ordered stacking. XRD tests show that it has obvious diffuse peaks near 2θ=20°, and no crystalline peaks appear at any angle, which makes it compatible with polyphenylene sulfide resin.
[0028] The beneficial effects achieved by this invention are as follows: (1) The low dielectric loss polyphenylene sulfide polymer alloy provided by the present invention is formed by end-group activation and extrusion processing reaction to form a block structure, which solves the problem that fluorinated polyarylate and hydroxyl-terminated polyphenylene sulfide are prone to phase separation under high toughening agent conditions in the prior art, and realizes the preparation of low dielectric loss PPS polymer alloy. At the same time, it can improve the toughness of PPS and maintain its inherent heat resistance. This amorphous fluorinated polyarylate copolymer contains flexible segments in its molecular backbone. When subjected to external forces, the numerous flexible molecular structures in its molecular chain can absorb impact energy, thereby effectively increasing toughness. More importantly, the carboxyl groups of the amorphous fluorinated polyarylate copolymer and the highly active phenolic hydroxyl groups introduced at the ends of the PPS molecular chain work synergistically to react in situ and generate block copolymers. This effectively improves the compatibility of PPS with fluorinated polymers, while the ester bonds of the block copolymers further enhance the toughness of the PPS material.
[0029] (2) The preparation method of the low dielectric loss polyphenylene sulfide polymer alloy provided by the present invention is a one-step melt extrusion. The high temperature and high shear force of melt extrusion promote the in-situ compatibilization reaction between the hydroxyl groups of PPS and the functional groups of the toughening agent, and the alloying is completed in one step. The process is efficient and easy to industrialize. Attached Figure Description
[0030] To more clearly illustrate the technical solution of this application, the drawings used in the embodiments will be briefly introduced below. Obviously, for those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0031] Figure 1 The fluorinated polyarylene copolymer (CPAR-F) and the non-fluorinated polyarylene copolymer (CPAR) prepared in Example 1 of this invention. 1 H NMR spectrum.
[0032] Figure 2 The infrared spectra of the fluorinated polyarylene copolymer (CPAR-F) and the non-fluorinated polyarylene copolymer (CPAR) prepared in Example 1 of this invention are shown. Detailed Implementation
[0033] The present invention will be further described in detail below with reference to specific embodiments. The following embodiments are not intended to limit the present invention, but only to illustrate the present invention. Unless otherwise specified, the experimental methods used in the following embodiments are generally performed under conventional conditions. Unless otherwise specified, the materials and reagents used in the following embodiments are commercially available.
[0034] Unless otherwise specified, the raw materials used in the embodiments and comparative examples of this invention are all commercially available.
[0035] In this invention, the unnotched impact strength of the polyphenylene sulfide polymer alloy was tested according to the GB / T 1043.1-2008 standard. The testing instrument was a simply supported beam impact testing machine. During the test, the span was set to 62 mm, the impact energy to 15 J, the effective length of the specimen to be 80 mm, the width to be 10 mm, and the thickness to be 4 mm.
[0036] In this invention, the heat distortion temperature of the polyphenylene sulfide polymer alloy was tested according to GB / T 1634.2-2019 standard. The testing instrument was a Vicat heat distortion tester (SS-3900HV6) with a computer system, manufactured by Songshu Testing Instruments Co., Ltd. During the test, the load was 1.8 MPa, the sample was placed flat, the span was 64 mm, the effective length of the sample was 80 mm, the width was 10 mm, and the thickness was 4 mm.
[0037] The pendulum impact energy resistance of the polyphenylene sulfide film prepared by the pressure film method in this invention was tested according to GB / T 8809-2015 standard. The testing instrument was a film impact tester (PARAM FIT-01) from Jinan Langguang Electromechanical Technology Co., Ltd. Before testing, the sample was placed in a standard laboratory environment (23℃, 50%RH) for 48 hours for conditioning. During the test, the impact energy was 3J, the resolution was 0.001J, the punch size was Φ25.4mm, the sample clamp diameter was Φ89mm, and the film thickness was 100±10μm.
[0038] The elastic modulus of the polyphenylene sulfide film prepared by the pressure molding method in this invention was tested according to the standard GB / T1040.3-2006. The testing instrument was an electronic universal testing machine (INSTRON 3366, US). Before testing, the samples were placed in a standard laboratory environment (23℃, 50%RH) for 48 hours for conditioning. During the test, the tensile rate was 2 mm / min, and the total length of the film sample was ≥150 mm, the effective length was 50 mm, the width was 10 mm, and the thickness was 100 ± 10 μm.
[0039] In this invention, the dielectric loss of the polyphenylene sulfide (PPS) film prepared by blow molding was tested using the quasi-optical cavity method according to the T / CSTM 00990-2023 standard. Before testing, the film sample was cut into circular sheet-like specimens with a diameter of not less than 60 mm and placed in a standard laboratory environment (23℃, 50%RH) for 48 hours for conditioning. During the test, the test temperature was 25℃, and tests were conducted at frequencies of 20 GHz, 30 GHz, 40 GHz, and 50 GHz. The resonant frequency and quality factor (Q value) at each frequency were recorded, and the dielectric loss tangent was calculated according to the calculation formula in the standard (see Chapter 10 of the standard).
[0040] The polyphenylene sulfide resin (brand name Q508) used in this invention was purchased from Shandong Binhua Binyang Fuel Chemical Co., Ltd., and is a linear PPS powder resin with chlorine-terminated groups and a number-average molecular weight of 125,000.
[0041] Example 1 This embodiment provides a method for preparing a low dielectric loss polyphenylene sulfide polymer alloy, which specifically includes the following steps: (1) Hydroxyl-terminated polyphenylene sulfide: Take 25g of Q508 polyphenylene sulfide resin (PPS), 1g of p-hydroxybenzylthiophenol, and 5g of NaOH catalyst, and place them in 1L of N-methylpyrrolidone (NMP) solution. React at 200℃ for 10h under nitrogen protection. After the reaction is completed, precipitate in methanol solution, filter, and wash 5 times with acetic acid, adding 20mL of acetic acid each time. Finally, dry to obtain hydroxyl-terminated polyphenylene sulfide. The reaction process is as follows:
[0042] ; (2) Preparation of toughening agent: Using phenolphthalein and 2,3,5,6-tetrafluoroterephthaloyl chloride as raw materials, an amorphous fluorinated polyarylene copolymer containing flexible segments and carboxyl-terminated ends was prepared by low-temperature solution polymerization. The specific preparation process is as follows: Add 6.62 g (20.8 mmol) phenolphthalein, 3 mL triethylamine (TEA), and 70 mL dichloromethane to a three-necked flask equipped with a mechanical stirrer, and stir at 10 °C for about 40 min to obtain a mixture; A 60 mL solution of dichloromethane containing 5.49 g (20 mmol) of 2,3,5,6-tetrafluoroterephthaloyl chloride was slowly added dropwise to the above mixture. The viscosity gradually increased. After the addition was completed in about 30 minutes, the reaction was continued for 5 hours. After the reaction was completed, the mixture was placed in a methanol solution to precipitate the precipitate, and then dried under vacuum at 60 °C for 12 hours to obtain a fluorinated amorphous polyarylate containing flexible segments. The reaction process is as follows:
[0043] (3) Preparation of PPS polymer alloy: Based on the mass fraction of raw materials, take 56 parts of hydroxyl-terminated polyphenylene sulfide obtained in step (1) and 30 parts of fluorine-containing and flexible segment-containing amorphous polyarylate obtained in step (2), blend them for 20 min, and then melt extrude them at 330°C to obtain the polyphenylene sulfide polymer alloy of this embodiment.
[0044] Figure 1 The fluorinated polyarylate copolymers (CPAR) and the fluorinated polyarylate copolymers (CPAR-F) prepared in Example 1 are examples of non-fluorinated polyarylate copolymers (CPAR). 1 ¹H NMR spectrum. The fluorine-free polyarylate copolymer (CPAR) was prepared by replacing 2,3,5,6-tetrafluoroterephthaloyl chloride with 20 mmol of terephthaloyl chloride. The specific preparation method is as follows: 6.62 g (20.8 mmol) of phenolphthalein, 3 mL of triethylamine (TEA), and 70 mL of dichloromethane were added to a three-necked flask equipped with a mechanical stirrer and stirred at 10 °C for about 40 min to obtain a mixture. 60 mL of a dichloromethane solution containing 4.06 g (20 mmol) of terephthaloyl chloride (TPC) was slowly added dropwise to the above mixture, and the viscosity gradually increased. After the addition was completed for about 30 min, the reaction was continued for 5 h. After the reaction was completed, the mixture was placed in methanol to precipitate and then dried under vacuum at 60 °C for 12 h to obtain a fluorine-free polyarylate copolymer (CPAR).
[0045] Figure 1 The peak signals at chemical shifts of 7.26, 7.47, 7.62, 7.76, and 7.99 ppm correspond to hydrogen atoms (2, 1, 4, 6, 5, 3) on the phenolphthalein structure, respectively. The signal at chemical shift 8.32 ppm is attributed to the hydrogen atom of the benzene ring on the terephthaloyl chloride (TPC) structural unit in the CPAR structure. The complete disappearance of the signal peak at the same chemical shift for CPAR-F indicates that the hydrogen atom has been completely replaced by fluorine, thus proving the successful synthesis of a semi-fluorinated phenolphthalein-based polyarylate.
[0046] Figure 2 The infrared spectra of CPAR and CPAR-F prepared in Example 1 are shown, with 3037 cm⁻¹. -1 The characteristic infrared absorption peak at this location is attributed to the CH stretching vibration in the benzene ring skeleton. Because the hydrogen atom on the benzene ring of the TPC structural unit in the molecular chain is replaced by fluorine, the absorption peak intensity of CPAR-F at this location is significantly weaker than that of CPAR. At 1772 cm⁻¹ -1 The tensile vibration at 1737 cm⁻¹ is attributed to the phenolphthalein ring (C=O). -1 The absorption peaks at these positions are attributed to the stretching vibration of the ester bond in the main chain. Due to the strong electron-withdrawing inductive effect of the fluorine atom, the absorption peaks of CPAR-F at these two positions shift and partially overlap. 1242 cm⁻¹ -1 The peak at 998 cm⁻¹ represents the stretching vibration of the aryl ether bond (Ar–O–Ar). -1 The absorption peak at that point is attributed to the carbon-fluorine bond (Ar-F) on the benzene ring. Infrared spectroscopy further confirmed the successful preparation of a fluorinated polyarylate copolymer.
[0047] Example 2 This embodiment provides a method for preparing a low dielectric loss polyphenylene sulfide polymer alloy, which specifically includes the following steps: (1) Hydroxyl-terminated polyphenylene sulfide: Take 100g of Q508 polyphenylene sulfide resin (PPS), 2g of p-hydroxybenzylthiophenol, and 5g of KOH catalyst, place them in 2L of NMP solution, and react at 200℃ for 10h under nitrogen protection. After the reaction, precipitate in methanol solution, filter, wash 5 times with hydrochloric acid, and add 20mL of HCl aqueous solution with pH 3.0 each time. Finally, dry to obtain hydroxyl-terminated polyphenylene sulfide. The reaction process is as follows:
[0048] ; (2) Preparation of toughening agent: Amorphous polyarylate containing fluorine and flexible segments was prepared by high-temperature solution polymerization using bisphenol A, bisetherfluorene (BPEF) and 2,3,5,6-tetrafluoroterephthaloyl chloride as raw materials. The specific preparation process is as follows: Add 2.28 g (10 mmol) of bisphenol A, 3.73 g (8.5 mmol) of BPEF and 70 mL of diphenyl ether to a three-necked flask equipped with a mechanical stirrer, and stir at 150 °C for about 40 min to obtain a mixture; 4.01 g (14.6 mmol) of 2,3,5,6-tetrafluoroterephthaloyl chloride was added to the above mixture, and the mixture was heated to 170 °C and reacted for 5 h. After the reaction was completed, the mixture was placed in a methanol solution to precipitate the precipitate, and then dried under vacuum at 60 °C for 12 h to obtain a fluorinated amorphous polyarylate containing flexible segments. The reaction process is as follows: ; (3) Preparation of PPS polymer alloy: Based on the mass fraction of raw materials, take 76 parts of hydroxyl-terminated polyphenylene sulfide obtained in step (1) and 24 parts of fluorine-containing and flexible segment-containing amorphous polyarylate obtained in step (2), blend them for 20 min, and then melt extrude them at 330°C to obtain the polyphenylene sulfide polymer alloy of this embodiment.
[0049] Example 3 This embodiment provides a method for preparing a low dielectric loss polyphenylene sulfide polymer alloy, which specifically includes the following steps: (1) Hydroxyl-terminated polyphenylene sulfide: Take 50g of Q508 polyphenylene sulfide resin (PPS), 1g of p-hydroxythiophenol, and 5g of sodium carbonate, place them in 1L of NMP solution, and react at 220℃ for 10h under nitrogen protection. After the reaction is completed, precipitate in methanol solution, filter, and wash the precipitate 5 times with acetic acid, adding 20mL of acetic acid each time. Finally, dry to obtain hydroxyl-terminated polyphenylene sulfide. The reaction process is as follows:
[0050] ; (2) Preparation of toughening agent: Amorphous polyarylate containing fluorine and flexible segments was prepared by low-temperature solution polymerization using bisphenol fluorene, bisether fluorene (BPEF) and 2,3,5,6-tetrafluoroterephthaloyl chloride as raw materials. The specific preparation process is as follows: Add 3.68 g (10.5 mmol) of bisphenol fluorene, 3.73 g (8.5 mmol) of BPEF, 3 mL of triethylamine, and 70 mL of dichloromethane to a three-necked flask equipped with a mechanical stirrer, and stir at 10 °C for about 40 min to obtain a mixture; A 100 mL solution of dichloromethane containing 4.01 g (14.6 mmol) of 2,3,5,6-tetrafluoroterephthaloyl chloride was slowly added dropwise to the above mixture. The viscosity gradually increased. After the addition was completed in about 30 minutes, the reaction was continued for 5 hours. After the reaction was completed, the mixture was placed in methanol to precipitate the product, and then dried under vacuum at 60 °C for 12 hours to obtain an amorphous polyarylate containing fluorine and flexible segments. The reaction process is as follows: ;
[0051] (3) Preparation of PPS polymer alloy: Based on the mass fraction of raw materials, take 56 parts of hydroxyl-terminated polyphenylene sulfide obtained in step (1) and 30 parts of fluorine-containing and flexible segment-containing amorphous polyarylate obtained in step (2), blend them for 20 min, and then melt extrude them at 330°C to obtain the polyphenylene sulfide polymer alloy of this embodiment.
[0052] Example 4 This embodiment provides a method for preparing a low dielectric loss polyphenylene sulfide polymer alloy, which specifically includes the following steps: (1) Hydroxyl-terminated polyphenylene sulfide: Take 50g of Q508 polyphenylene sulfide resin (PPS), 15g of liquid alkali (20% sodium hydroxide aqueous solution), and 2L of NMP solution and add them to a 5L reactor. Heat to 200℃ and react for 5h. Then cool down to crystallize. The filtered cake is washed with water and dried to obtain hydroxyl-terminated polyphenylene sulfide. The reaction process is as follows: ; (2) Preparation of toughening agent: Amorphous polyarylate containing fluorine and flexible segments was prepared by low-temperature solution polymerization using phenolphthalein, bis(ether)fluorene (BPEF) and 2,3,5,6-tetrafluoroterephthaloyl chloride as raw materials. The specific preparation process is as follows: Add 3.02 g (9.5 mmol) phenolphthalein, 3.73 g (8.5 mmol) BPEF, 3 mL triethylamine, and 70 mL dichloromethane to a three-necked flask equipped with a mechanical stirrer, and stir at 10 °C for about 40 min to obtain a mixture; A 100 mL solution of dichloromethane containing 4.95 g (18 mmol) of 2,3,5,6-tetrafluoroterephthaloyl chloride was slowly added dropwise to the above mixture. The viscosity gradually increased. After the addition was completed in about 30 minutes, the reaction was continued for 5 hours. After the reaction was completed, the mixture was placed in a methanol solution to precipitate the precipitate, and then dried under vacuum at 90 °C for 12 hours to obtain a fluorinated amorphous polyarylate containing flexible segments. The reaction process is as follows: ; (3) Preparation of PPS polymer alloy: Based on the mass fraction of raw materials, take 75 parts of hydroxyl-terminated polyphenylene sulfide obtained in step (1) and 20 parts of fluorine-containing and flexible segment-containing amorphous polyarylate obtained in step (2), blend them for 20 min, and then melt extrude them at 310℃ to obtain the polyphenylene sulfide polymer alloy of this embodiment.
[0053] Example 5 This embodiment utilizes the polyphenylene sulfide polymer alloys prepared in Examples 1 to 4 to provide a method for preparing a low dielectric loss polyphenylene sulfide film, specifically including the following steps: Polyphenylene sulfide polymer alloys obtained in Examples 1 to 4 were used to prepare polyphenylene sulfide films by a pressing method. Specifically, the polyphenylene sulfide polymer alloys obtained in Examples 1 to 4 were put into a pressing machine and pressed into shape. The pressing temperature was 320°C, the pressure was 10 MPa, and the gas was released four times to obtain four kinds of polyphenylene sulfide films.
[0054] Example 6 This embodiment utilizes the polyphenylene sulfide polymer alloys prepared in Examples 1 to 4 to provide a method for preparing a low dielectric loss polyphenylene sulfide film, specifically including the following steps: Polyphenylene sulfide polymer alloys obtained in Examples 1 to 4 were used to prepare polyphenylene sulfide films by blow molding. Specifically, the polyphenylene sulfide polymer alloys obtained in Examples 1 to 4 were dried in an oven at 120°C for 5 hours, and then put into an extrusion blow molding device to prepare films. The blow ratio was set to 1 and the stretching ratio was set to 3, resulting in 4 kinds of polyphenylene sulfide films.
[0055] Comparative Example 1 This comparative example provides a commercially available polyphenylene sulfide resin (PPS) with the grade Q508.
[0056] Comparative Example 2 This comparative example provides a method for preparing a polyphenylene sulfide film using the polyphenylene sulfide resin of Comparative Example 1, specifically including the following steps: A polyphenylene sulfide film was prepared from commercially available polyphenylene sulfide resin of Comparative Example 1, grade Q508, by a molding process. Specifically, the commercially available polyphenylene sulfide resin of Comparative Example 1, grade Q508, was put into a molding machine and molded. The molding temperature was 320℃, the pressure was 10MPa, and the film was vented four times to obtain the polyphenylene sulfide film of this comparative example.
[0057] Comparative Example 3 This comparative example provides a method for preparing a polyphenylene sulfide film using the polyphenylene sulfide resin of Comparative Example 1, specifically including the following steps: A polyphenylene sulfide film was prepared by blow molding using commercially available polyphenylene sulfide resin of Comparative Example 1 with the grade Q508. Specifically, the commercially available polyphenylene sulfide resin of Comparative Example 1 with the grade Q508 was dried in an oven at 120°C for 5 hours, and then fed into an extrusion blow molding device to form a film. The blow ratio was set to 1 and the stretch ratio to 3 to obtain a polyphenylene sulfide film.
[0058] The unnotched impact strength and heat distortion temperature of the polyphenylene sulfide polymer alloys prepared in Examples 1 to 4 and the polyphenylene sulfide resin of Comparative Example 1 were tested, and the results are shown in Table 1.
[0059] Table 1 Properties of polyphenylene sulfide polymer alloys and polyphenylene sulfide resins
[0060] The pendulum impact energy and elastic modulus of the polyphenylene sulfide films prepared by the pressing method in Example 5 and Comparative Example 2 were tested, and the dielectric loss of the films prepared by the blow molding method in Example 6 and Comparative Example 3 were tested. The results are shown in Table 2.
[0061] Table 2 Mechanical and insulating properties of polyphenylene sulfide films
[0062] As can be seen from Table 1, the unnotched impact strength of the polyphenylene sulfide polymer alloys prepared in Examples 1-4 is more than 4 times higher than that of Comparative Example 1, and the heat distortion temperature is also significantly improved. It can be seen that the polyphenylene sulfide polymer alloys prepared by the present invention are significantly better than pure PPS in terms of toughness and heat resistance. This indicates that the in-situ reaction between the fluorinated polyarylene toughening agent and the hydroxyl-terminated PPS effectively improves the compatibility and synergistically enhances the toughness and thermal properties of PPS.
[0063] As can be seen from Table 2, the dielectric loss of the polyphenylene sulfide films prepared in Examples 1-4 decreased significantly across the entire test frequency band (20-50 GHz), achieving high frequency and low dielectric loss. At the same time, the films still outperformed pure PPS in terms of impact toughness, and the elastic modulus did not show serious deterioration, or even increased. This shows that the rigidity of the polyphenylene sulfide films remained good.
[0064] In summary, the polyphenylene sulfide (PPS) polymer alloy provided by this invention successfully overcomes the challenge of low compatibility between PPS and fluoropolymers by introducing a fluorinated flexible segment copolymer and utilizing in-situ reaction compatibilization. This achieves the preparation of a low-dielectric-loss PPS polymer alloy, which also possesses high toughness, high heat resistance, and maintains the inherent rigidity of PPS. This low-dielectric-loss PPS polymer alloy maintains a dielectric loss consistently below 0.002 in the millimeter-wave band (≥20GHz), significantly outperforming pure PPS, and is suitable for high-frequency applications such as 5G / 6G communications.
[0065] It should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and are not intended to limit it. Although the present invention has been described in detail with reference to preferred embodiments, those skilled in the art should understand that modifications or equivalent substitutions can be made to the technical solutions of the present invention without departing from the spirit and scope of the technical solutions of the present invention, and all such modifications or substitutions should be covered within the scope of the claims of the present invention.
Claims
1. A low dielectric loss polyphenylene sulfide high molecular alloy characterized by: Based on the mass fractions of raw materials, it includes: 55-85 parts of hydroxyl-terminated polyphenylene sulfide, 10-40 parts of toughening agent; The toughening agent is an amorphous fluorinated polyarylene copolymer containing flexible segments and carboxyl-terminated ends.
2. The low dielectric loss polyphenylene sulfide high molecular alloy of claim 1, wherein: The amorphous fluorinated polyarylate copolymer containing flexible segments and carboxyl-terminated groups is obtained by polycondensation of 2,3,5,6-tetrafluoroterephthaloyl chloride and bisphenol compounds.
3. The low dielectric loss polyphenylene sulfide polymer alloy according to claim 2, characterized in that: The bisphenol compounds are selected from one or more of bisphenol fluorene, phenolphthalein, 3,3-bis(4-hydroxyphenyl)-2-phenylprop-1-one, bisphenol A, and diether fluorene.
4. The low dielectric loss polyphenylene sulfide polymer alloy according to claim 3, characterized in that: The structural formula of the amorphous fluorinated polyarylene copolymer containing flexible segments and carboxyl-terminated ends is shown in Formula I: ; I In Formula I, 2≤p≤1000, 2≤q≤1000; R1 and R2 are each independently selected from one or more of the following groups obtained by dehydrogenation of bisphenol: bisphenol fluorene, phenolphthalein, 3,3-bis(4-hydroxyphenyl)-2-phenylprop-1-one, bisphenol A, and diether fluorene.
5. The low dielectric loss polyphenylene sulfide polymer alloy according to claim 4, characterized in that: The preparation method of the amorphous fluorinated polyarylene copolymer containing flexible segments and carboxyl-terminated groups is selected from one or more of the following: low-temperature solution polymerization, high-temperature solution polymerization, and melt polycondensation.
6. The low dielectric loss polyphenylene sulfide polymer alloy according to any one of claims 1 to 5, characterized in that: The structural formula of the hydroxyl-terminated polyphenylene sulfide is shown in Formula II: ; II In Equation II, 2 ≤ n ≤ 1500.
7. The low dielectric loss polyphenylene sulfide polymer alloy according to claim 6, characterized in that: The preparation method of the hydroxyl-terminated polyphenylene sulfide includes the following steps: p-Hydroxybenzyl thiophenol and polyphenylene sulfide were reacted at 140-270℃ for 4-36 hours under alkaline catalyst and in an inert atmosphere. After cooling and crystallization, hydroxyl-terminated polyphenylene sulfide was obtained by filtration and acid washing.
8. A method for preparing a low dielectric loss polyphenylene sulfide polymer alloy according to any one of claims 1 to 7, characterized in that: Includes the following steps: According to any one of the proportions described in claims 1 to 7, hydroxyl-terminated polyphenylene sulfide and amorphous fluorinated polyarylate copolymer containing flexible segments and carboxyl-terminated groups are blended for 10-20 minutes and then melt-extruded at 300-350°C to obtain a low dielectric loss polyphenylene sulfide polymer alloy.
9. A low dielectric loss polyphenylene sulfide film, characterized in that: It is prepared from the low dielectric loss polyphenylene sulfide polymer alloy as described in any one of claims 1 to 7.
10. A method for preparing a low dielectric loss polyphenylene sulfide film according to claim 9, characterized in that: The preparation method is selected from one or more of the compression molding method and blow molding method.