A low odor, yellowing resistant liquid silicone coating and method of making the same

By deeply compounding refined and modified vinyl polysiloxane and modified hydrogen-containing silicone oil, combined with complexed modified platinum catalyst and ternary composite yellowing-resistant additive, the problems of odor residue, decreased transparency and insufficient yellowing resistance of existing liquid silicone rubber in high-end coating scenarios are solved, achieving a high-precision thin coating effect with low odor, environmental protection, high transparency and yellowing resistance.

CN123152297APending Publication Date: 2026-11-24ANHUI YUJIE NEW MATERIAL TECHNOLOGY CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202611566592.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-10
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing addition-type liquid silicone rubbers have problems such as residual odor, decreased transparency, insufficient resistance to yellowing, and mismatch between viscosity and crosslinking degree in high-end and high-precision coating scenarios. It is difficult to simultaneously achieve the comprehensive performance of low odor and environmental protection, high transparency, resistance to yellowing, and compatibility with multiple processes.

Method used

It employs refined modified vinyl polysiloxane, modified hydrogen-containing silicone oil, complexed modified platinum catalyst, and ternary composite anti-yellowing additive. Through deep refining and uniform compounding, a low-odor, anti-yellowing cross-linked network is formed. Combined with functional modification additives, it improves interfacial adhesion and leveling properties.

Benefits of technology

It achieves long-lasting low odor, excellent environmental performance, and strong resistance to yellowing, and is suitable for high-precision thin coating of new energy wire harnesses, ultra-thin protective sleeves, flexible silicone substrates, etc., improving the overall performance and service life of materials.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

This invention discloses a low-odor, yellowing-resistant liquid silicone rubber for coating and its preparation method, belonging to the field of liquid silicone rubber technology. The silicone rubber comprises, by weight, 40-60 parts of refined modified vinyl polysiloxane, 10-20 parts of modified hydrogen-containing silicone oil, 0.1-0.5 parts of complexed modified platinum catalyst, 1-3 parts of ternary composite yellowing-resistant additive, and 2-5 parts of functional modifying additive. The matrix raw materials are purified by vacuum distillation to remove small molecules and volatile impurities; the catalyst uses an alkynyl alcohol complexation system; the ternary yellowing-resistant additive is a compound of ultraviolet absorber, thermo-oxidative stabilizer, and metal ion passivator. This invention utilizes the synergistic effect of raw material refining and a composite anti-aging system to obtain a silicone rubber with low odor, yellowing resistance, high light transmittance, and good adhesion, while also possessing insulation, heat resistance, and waterproof properties. It is suitable for high-precision thin-coating of new energy wiring harnesses, ultra-thin sleeves, flexible substrates, and high-end sealed electronic devices.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of liquid silicone rubber technology, and in particular to a low-odor, yellowing-resistant liquid silicone rubber for coating and its preparation method. Background Technology

[0002] Addition-cure liquid silicone rubber possesses technical characteristics such as no curing byproducts, good moldability, resistance to high and low temperatures, electrical insulation, waterproofing, moisture resistance, and halogen-free flame retardancy. It is an important material in the field of precision coating protection and is widely used for surface protection of components such as new energy wiring harnesses, high-temperature protective sleeves, silicone cloth, transparent lampshades, and flexible substrates. With the technological iteration in the new energy, high-end electronics, and smart home fields, the market's requirements for the comprehensive performance indicators of coating silicone rubber continue to rise. In addition to meeting basic protective performance requirements such as insulation, flame retardancy, and high-temperature resistance, materials are also required to have low odor, high light transmittance, long-term resistance to yellowing, and the ability to adapt to high-precision coating under various working conditions.

[0003] Currently, various addition-type liquid silicone rubber formulations and preparation processes have been disclosed in this field. Conventional technologies in this field generally use vinyl polysiloxanes and hydrogen-containing silicone oils as the matrix, combined with conventional functional additives and platinum catalysts to form a crosslinking system, which can meet the basic coating and protection needs of conventional cables and conduits. However, existing conventional technologies have a simple system structure and limited performance matching, generally exhibiting performance shortcomings in high-end, high-precision coating scenarios, and failing to meet the application requirements of high precision, high environmental protection, and high weather resistance.

[0004] Chinese patent CN114058189B discloses an addition-type flame-retardant and high-temperature resistant silicone rubber and its preparation method. This technology uses vinyl polysiloxane and hydrogen-containing silicone oil as the matrix, combined with conventional additives and a platinum catalytic system, to achieve the basic properties of flame retardancy and high temperature resistance of the material, which is suitable for coating and protecting conventional cables and conduits. However, this technology has inherent technical defects: First, the raw materials do not include a low-molecular-weight removal and refining process, leaving small-molecule siloxanes and volatile impurities in the system. After curing, these small molecules continue to migrate and precipitate, resulting in residual odor in the finished product, which cannot meet the low-odor standards for use in sealed, home, and baby products. Second, the formula does not incorporate anti-yellowing and anti-thermal-oxidative aging systems. The residual metal ions in the catalytic system are prone to oxidation reactions under high-temperature conditions, causing the transparent adhesive layer to yellow, light transmittance to decrease, color difference to increase, and the material's long-term weather resistance to be insufficient. Third, the formula is optimized for flame retardancy and heat resistance, but the system has high rigidity and insufficient toughness. It does not adapt the viscosity and crosslinking degree for thin-walled components, ultra-fine wires, and flexible substrates for thin-coating processes, resulting in limited coating leveling and interfacial adhesion. The coating is prone to cracking and peeling after the substrate is bent, limiting the applicable working conditions.

[0005] Chinese patent CN120118522A discloses a high flame-retardant insulating liquid silicone rubber and its preparation method. This technology achieves high flame retardancy and high insulation performance by compounding inorganic flame-retardant fillers, which can meet the basic protection requirements of electrical equipment. However, the various performance indicators of this technology have the drawback of mutual constraints, making it difficult to achieve synergistic performance of multiple properties, and greatly limiting the applicable scenarios: First, the addition of a large amount of inorganic flame-retardant fillers to the system makes it easy for the fillers to adsorb volatile components of the system, aggravating the residual odor of the finished product and resulting in insufficient environmental performance. At the same time, inorganic fillers will reduce the light transmittance of the adhesive layer, making it unsuitable for highly transparent coated products. Second, the formula does not contain UV shielding and thermo-oxidative stabilizing functional components, and the material ages rapidly under light and high and low temperature alternating environments, resulting in significant yellowing and deterioration after long-term service and a short service life. Third, the curing parameters of the formula have poor adjustability, only suitable for conventional thick-layer coating processes, and cannot be adapted to the high-precision thin-layer coating production of ultra-fine wire harnesses, ultra-thin sleeves, and thin silicone cloths. It is prone to process defects such as uneven coating thickness, local missed coating, and brittle adhesive layer, limiting its mass production adaptability and overall practicality.

[0006] In summary, existing conventional addition-cure coated silicone rubbers have significant technical bottlenecks. Existing technologies often focus on flame retardancy, insulation, or heat resistance on one side only, resulting in obvious performance trade-offs. They cannot simultaneously achieve comprehensive performance characteristics such as low odor and environmental friendliness, high transparency, resistance to yellowing and aging, and compatibility with multiple processes. The overall performance balance of the material is insufficient, making it difficult to meet the application requirements of new energy, high-end electronics, and smart homes for refined, highly durable, and highly environmentally friendly coating materials. Summary of the Invention

[0007] In view of the problems existing in the background art, the purpose of the present invention is to provide a low-odor, yellowing-resistant liquid silicone rubber for coating and its preparation method.

[0008] To achieve the above-mentioned technical objectives, the present invention adopts the following technical solution:

[0009] The first aspect of the present invention provides a low-odor, yellowing-resistant liquid silicone rubber for coating, comprising the following raw materials in parts by weight: 40-60 parts of refined modified vinyl polysiloxane, 10-20 parts of modified hydrogen-containing silicone oil, 0.1-0.5 parts of complex-modified platinum catalyst, 1-3 parts of ternary composite yellowing-resistant additive, and 2-5 parts of functional modification additive.

[0010] Preferably, the refined modified vinyl polysiloxane is a vinyl-terminated polydimethylsiloxane with a kinematic viscosity of 8000-20000 mPa·s at 25°C, and the molecular chain ends with vinyl groups to provide crosslinking reaction sites.

[0011] Preferably, the modified hydrogen-containing silicone oil is a side-hydrogen type polymethylhydrosiloxane with a kinematic viscosity of 100-500 mPa·s at 25°C and a hydrogen mass fraction of 0.4%-1.2%. As a crosslinking agent, it undergoes a hydrosilylation reaction with vinyl polysiloxane to form a crosslinked network.

[0012] Preferably, the complex-modified platinum catalyst is an alkynyl alcohol complex-modified chloroplatinic acid complex, used to reduce the residual free metal ions in the system and effectively avoid the yellowing and aging problems of materials caused by the residual free metal ions; more preferably, it is 1-ethynyl-1-cyclohexanol; the mass content of platinum in the catalyst is 1000-3000 ppm; the alkynyl alcohol complex-modified chloroplatinic acid complex can complex and capture platinum ions, reduce the content of free metal ions in the system, and inhibit the oxidative yellowing of silicone rubber catalyzed by free platinum ions under high temperature and light conditions.

[0013] Preferably, the ternary composite anti-yellowing agent is composed of a UV absorber, a thermo-oxidative stabilizer, and a metal ion passivator.

[0014] Preferably, the ultraviolet absorber is a benzotriazole-based ultraviolet absorber, such as 2-(2H-benzotriazole-2-yl)-4,6-di-tert-butylphenol; the thermo-oxidative stabilizer is a hindered phenolic antioxidant, such as pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate]; and the metal ion passivator is an acylhydrazine-based metal ion passivator, such as N,N'-bis(3-salicylic acid)malonylhydrazine; the three are compounded in a mass ratio of 1:0.8-1.2:0.5-0.8 to synergistically block ultraviolet degradation, thermo-oxidative aging, and metal ion catalytic oxidation pathways.

[0015] Preferably, the functional modifying agent is used to improve the interfacial adhesion of liquid silicone rubber on PET and copper substrate surfaces, improve the leveling properties of the rubber compound during thin coating, eliminate pinholes and craters in the thin coating process, and adapt to high-precision thin coating processes; the functional modifying agent is selected from one or more of silane coupling agents and polyether leveling and wetting agents; the silane coupling agent can be vinyltrimethoxysilane; the polyether leveling and wetting agent is used to improve the wetting and spreading properties of the rubber compound on flexible substrate surfaces.

[0016] A second aspect of the present invention provides a method for preparing a low-odor, yellowing-resistant liquid silicone rubber for coating, comprising the following steps: S1. Deep refining and pretreatment of raw materials: Vinyl polysiloxane and hydrogen-containing silicone oil are subjected to vacuum distillation to remove small molecule siloxanes and volatile organic impurities from the system. S2. Uniform compounding of base adhesive: The refined vinyl polysiloxane is mixed with the modified hydrogen-containing silicone oil and stirred at high speed to obtain the composite base adhesive. S3. Functional additive modification: Add ternary composite anti-yellowing additive and functional modification additive to the composite base adhesive, stir and disperse to ensure that the additives are completely and uniformly dispersed; S4. Catalytic curing and molding: Add complexed modified platinum catalyst to the system, stir thoroughly, degas under vacuum, and cure at a constant temperature to obtain low-odor, yellowing-resistant liquid silicone rubber for coating.

[0017] Preferably, in step S1, the conditions for vacuum distillation are: temperature 80-120℃, vacuum degree -0.08--0.1MPa for 2-4 hours.

[0018] Preferably, in step S2, the stirring speed is 300-500 r / min and the stirring time is 20-40 min.

[0019] Preferably, in step S3, the order of adding materials is as follows: first add the ternary composite anti-yellowing additive, stir and pre-disperse for 10-20 minutes, and then add the functional modification additive to continue dispersing. This can effectively prevent the additive from agglomerating and improve the uniformity of the system.

[0020] Preferably, in step S3, the stirring temperature is 40-60℃, the stirring speed is 300-500 r / min, the stirring and dispersion time is 30-50 min, and the system is kept under slight negative pressure during the stirring process to reduce the introduction of air bubbles during the dispersion of the additives.

[0021] Preferably, in step S4, the vacuum degassing time is 15-30 min, the curing temperature is 100-150℃, and the curing time is 30-60 min.

[0022] The third aspect of the present invention also provides the application of the low-odor, yellowing-resistant liquid silicone rubber prepared by the above-mentioned preparation method in high-precision thin-coating protection scenarios such as new energy wiring harnesses, ultra-thin protective sleeves, flexible silicone substrates, high-end electronic sealing devices, and smart home interior decoration.

[0023] Beneficial effects (1) Long-lasting low odor and high environmental protection level: This invention thoroughly removes the volatile components of small molecules in the matrix through deep refining and pretreatment of raw materials, and eliminates the problem of small molecule migration and odor return after long-term use of finished products. No need for post-baking deodorization, the process is simple and the energy consumption is lower. It can be stably adapted to high environmental protection application scenarios such as sealed devices, home interior decoration, and mother and baby products. Its environmental protection performance far exceeds that of existing conventional products.

[0024] (2) Excellent resistance to yellowing and weathering, and long service life: This invention uses a low-residue complexation catalytic system combined with a ternary composite anti-aging system to inhibit material oxidation, ultraviolet aging and metal catalytic degradation reaction in multiple dimensions, effectively avoiding problems such as yellowing, devitrification and cracking of the coating layer after long-term use, and greatly improving the appearance stability and service life of high-end coated products.

[0025] (3) This invention improves odor by refining raw materials to remove small molecules, inhibits catalytic aging caused by metal ions by alkynol complexing platinum, and blocks the light, heat and metal-induced aging pathways simultaneously by ternary additives. The three factors work together to overcome the technical bottleneck of traditional silicone rubber, which is difficult to achieve low odor, high transparency, yellowing resistance and high adhesion at the same time. While retaining the basic protective properties of silicone rubber such as insulation, heat resistance and waterproofing, it also takes into account the high precision thin coating adaptability. It is suitable for mass production applications of new energy wire harnesses, ultra-thin protective sleeves, flexible substrates and high-end sealed electronic devices, and has high market value. Detailed Implementation

[0026] The technical solutions of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments.

[0027] The vinyl polysiloxane used in the following embodiments of the present invention is a vinyl-terminated polydimethylsiloxane with a kinematic viscosity of 8000-20000 mPa·s at 25°C; the modified hydrogen-containing silicone oil used is a side-hydrogen type polymethylhydrosiloxane with a kinematic viscosity of 100-500 mPa·s at 25°C and a hydrogen mass fraction of 1.0%. The ternary composite anti-yellowing additive used is composed of a UV absorber, a thermo-oxidative stabilizer, and a metal ion passivator, with a ratio of UV absorber:thermothermal stabilizer:metal ion passivator = 1:1:0.6. Among them, the UV absorber is 2-(2H-benzotriazol-2-yl)-4,6-di-tert-butylphenol; the thermo-oxidative stabilizer is pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate]; and the metal ion passivator is N,N'-bis(3-salicylic acid)malonylhydrazine. The three types of additives work synergistically to block the pathways of UV degradation, thermo-oxidative aging, and metal ion catalytic oxidation.

[0028] The functional modification additives used are a compound system of vinyltrimethoxysilane and polyether leveling and wetting agent (1:1, v / v), which can effectively improve the interfacial adhesion of liquid silicone rubber on PET and copper substrates, improve the leveling properties of the rubber compound during thin coating, eliminate pinholes and craters in the thin coating process, and adapt to high-precision thin coating processes.

[0029] The complex-modified platinum catalyst used is a 1-ethynyl-1-cyclohexanol complex-modified chloroplatinic acid complex, and the mass content of metallic platinum in the catalyst is 2000 ppm. The alkynol ligand can complex and capture platinum ions, reduce the residual free metal ions in the system, and inhibit the oxidative yellowing of silicone rubber catalyzed by free platinum ions under high temperature and light conditions.

[0030] The following embodiments of the present invention use a unified raw material pretreatment process: vinyl polysiloxane and hydrogen-containing silicone oil are distilled under reduced pressure for 3 hours at 100°C and -0.09MPa to remove small molecule impurities; a unified preparation process is used: the base adhesive is stirred at 400r / min for 30 minutes, the additive is stirred at 50°C and 400r / min for 40 minutes, vacuum degassing is performed for 20 minutes, and constant temperature curing is carried out at 120°C for 45 minutes; the ternary composite anti-yellowing additive has a unified ratio: UV absorber: thermal oxygen stabilizer: metal ion passivator = 1:1:0.6.

[0031] Example 1 A low-odor, yellowing-resistant liquid silicone rubber for coating, by weight, comprises the following raw material formula: 50 parts refined modified vinyl polysiloxane, 15 parts modified hydrogen-containing silicone oil, 0.3 parts alkynyl alcohol complexed platinum catalyst, 2 parts ternary composite yellowing-resistant additive, and 3 parts functional modifying additive.

[0032] Example 2 A low-odor, yellowing-resistant liquid silicone rubber for coating, by weight, comprises the following raw material formula: 45 parts refined modified vinyl polysiloxane, 12 parts modified hydrogen-containing silicone oil, 0.2 parts alkynyl alcohol complexed platinum catalyst, 1.5 parts ternary composite yellowing-resistant additive, and 2.5 parts functional modifying additive.

[0033] Example 3 A low-odor, yellowing-resistant liquid silicone rubber for coating, by weight, comprises the following raw material formula: 55 parts refined modified vinyl polysiloxane, 18 parts modified hydrogen-containing silicone oil, 0.4 parts alkynyl alcohol complexed platinum catalyst, 2.5 parts ternary composite yellowing-resistant additive, and 4 parts functional modifying additive.

[0034] Example 4 A low-odor, yellowing-resistant liquid silicone rubber for coating, by weight, comprises the following raw material formula: 40 parts refined modified vinyl polysiloxane, 10 parts modified hydrogen-containing silicone oil, 0.1 parts alkynyl alcohol complexed platinum catalyst, 1 part ternary composite yellowing-resistant additive, and 2 parts functional modifying additive.

[0035] Example 5 A low-odor, yellowing-resistant liquid silicone rubber for coating, by weight, comprises the following raw material formula: 60 parts refined modified vinyl polysiloxane, 20 parts modified hydrogen-containing silicone oil, 0.5 parts alkynyl alcohol complexed platinum catalyst, 3 parts ternary composite yellowing-resistant additive, and 5 parts functional modifying additive.

[0036] Comparative Example 1 The matrix is ​​made from ordinary vinyl polysiloxane and ordinary hydrogen-containing silicone oil that have not undergone vacuum distillation. No low-molecular-weight removal process is performed on the raw materials. A conventional chloroplatinic acid platinum catalyst is used, and no ternary composite anti-yellowing additive is added. All other basic additives and preparation processes are completely consistent with Example 1. The formulation by weight is: 50 parts vinyl polysiloxane, 15 parts ordinary hydrogen-containing silicone oil, 0.3 parts general-purpose platinum catalyst, and 3 parts conventional functional additives.

[0037] Comparative Example 2 This formulation uses unrefined common matrix raw materials and is compounded with a large amount of inorganic flame-retardant fillers (aluminum hydroxide and silica). It lacks a ternary yellowing-resistant system and requires no raw material refining process, making it a mainstream high-flame-retardant, low-transparency silicone rubber formulation in the industry. The preparation process is consistent with Example 1. The formulation by weight is: 50 parts of common vinyl polysiloxane, 15 parts of common hydrogen-containing silicone oil, 0.3 parts of general-purpose platinum catalyst, 8 parts of inorganic flame-retardant filler, and 3 parts of conventional functional additives.

[0038] Performance testing A uniform 1mm thick transparent adhesive film was prepared, cured to standard, and allowed to stand at room temperature for 24 hours before testing. The testing environment was a constant temperature and humidity environment of 25℃ and 50%. The specific test items are as follows: (1) Odor level and long-term odor return test: According to the PV3355 automotive interior material odor test standard, the level is 1-6, and the lower the level, the less odor. The sample is initially rated by baking at 80℃ in a sealed environment for 2 hours, and then retested after being placed at room temperature for 90 days to verify whether small molecules migrate and return odor, which is suitable for high environmental protection scenarios such as home furnishing and sealed electronics.

[0039] (2) UV yellowing resistance test: According to GB / T 25036-2010, UV aging test for 500 hours is conducted. The color difference ΔE is measured by a colorimeter. The smaller the ΔE, the better the resistance to yellowing and weathering. It is suitable for high-end coating scenarios that require long-term service in outdoor and high-low temperature alternation.

[0040] (3) Transmittance test: According to GB / T 2410-2008, the transmittance of visible light in the range of 400-700nm is tested to verify the high transparency of the material and to make it suitable for transparent lampshades and high-end electronic visualization coating scenarios.

[0041] (4) Cross-cut adhesion test: According to GB / T 9286-1998, the adhesion of the coating to PET flexible substrate and ultra-fine wire harness copper substrate was tested, with grades ranging from 0 to 5, and grade 0 being the best. This test verified the coating adhesion stability under bending conditions on thin-coated and flexible substrates. Quantitative performance test data results for each group of samples: Example 1: Odor rating 1.0, 90d odor return rating 1.0; UV 500h color difference ΔE=0.82; light transmittance 92.6%; cross-cut adhesion rating 0.

[0042] Example 2: Odor rating 1.0, 90d odor return rating 1.0; UV 500h color difference ΔE=0.85; light transmittance 92.3%; cross-cut adhesion rating 0.

[0043] Example 3: Odor rating 1.0, 90d odor return rating 1.0; UV 500h color difference ΔE=0.78; light transmittance 92.8%; cross-cut adhesion rating 0.

[0044] Example 4: Odor rating 1.5, 90d odor return rating 1.5; UV 500h color difference ΔE=0.91; light transmittance 91.8%; cross-cut adhesion rating 1.

[0045] Example 5: Odor rating 1.0, 90d odor return rating 1.0; UV 500h color difference ΔE=0.75; light transmittance 93.0%; cross-cut adhesion rating 0.

[0046] Comparative Example 1 (Conventional unrefined raw materials + general catalytic system): Odor level 3.5, 90d back odor level 4.0; UV 500h color difference ΔE=3.65; light transmittance 88.2%; cross-cut adhesion level 2.

[0047] Comparative Example 2 (Inorganic Filler Flame Retardant System): Odor rating 3.0, 90d odor return rating 3.5; UV 500h color difference ΔE=2.92; light transmittance 78.5%; cross-cut adhesion rating 3.

[0048] The odor levels of all embodiments of this invention are ≤1.5, and there is no odor return after 90 days of long-term storage. In contrast, the two comparative groups showed poor initial odor and severe odor return due to long-term small molecule migration. This proves that the deep purification process of raw materials using vacuum distillation in this invention can remove volatile small molecule impurities from the source, completely solving the defects of existing technologies such as odor residue and poor long-term environmental performance. It can be stably adapted to high environmental protection requirements in scenarios such as sealed electronics and home interiors.

[0049] In the embodiments of this invention, the color difference ΔE after 500 hours of UV aging is less than 1.0, demonstrating excellent resistance to yellowing. In contrast, the comparative example lacks a composite anti-aging system, has a high residual amount of free metal ions, and exhibits a significantly higher color difference, making it prone to yellowing and devitrification during long-term service. This effectively verifies the synergistic effect of a low-residue complexation catalyst + ternary composite anti-aging system, solving the industry pain points of poor weather resistance and insufficient appearance stability of traditional silicone rubber, and making it suitable for the long-term service conditions of high-end products.

[0050] The formulation system of this invention does not contain a large amount of inorganic filler, and the light transmittance of the finished product is higher than 91.5%, with excellent high transparency. At the same time, the thin coating adhesion is excellent, and it can be adapted to the high-precision thin coating process of ultra-fine wire harnesses, flexible substrates and transparent components. It does not have the disadvantages of mutual restriction of existing technologies, and perfectly matches the high-end coating application needs of new energy, high-end electronics and smart home.

[0051] The above description is only a preferred embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any equivalent substitutions or modifications made by those skilled in the art within the scope of the technology disclosed in the present invention, based on the technical solution and inventive concept of the present invention, should be covered within the scope of protection of the present invention.

Claims

1. A low-odor, yellowing-resistant liquid silicone rubber for coating, characterized in that, The raw materials include the following parts by weight: 40-60 parts of refined modified vinyl polysiloxane, 10-20 parts of modified hydrogen-containing silicone oil, 0.1-0.5 parts of complex modified platinum catalyst, 1-3 parts of ternary composite anti-yellowing agent, and 2-5 parts of functional modification agent. The refined modified vinyl polysiloxane is a vinyl-terminated polydimethylsiloxane; The modified hydrogen-containing silicone oil is a side-hydrogen type polymethylhydrosiloxane, which is used to undergo a hydrosilylation reaction with vinyl polysiloxane to form a crosslinked network; The complex-modified platinum catalyst is an alkynyl alcohol complex-modified chloroplatinic acid complex, used to reduce the residual free metal ions in the system; The ternary composite anti-yellowing agent is composed of ultraviolet absorber, heat-oxidation stabilizer and metal ion passivator. The functional modification agent is selected from one or more combinations of silane coupling agents and polyether leveling and wetting agents.

2. The low-odor, yellowing-resistant liquid silicone rubber for coating according to claim 1, characterized in that, In the ternary composite anti-yellowing additive, the mass ratio of ultraviolet absorber, thermo-oxidative stabilizer, and metal ion passivator is 1:0.8-1.2:0.5-0.8; the ultraviolet absorber is 2-(2H-benzotriazol-2-yl)-4,6-di-tert-butylphenol; the thermo-oxidative stabilizer is pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate]; and the metal ion passivator is N,N'-bis(3-salicylic acid amino)malonylhydrazide.

3. The low-odor, yellowing-resistant liquid silicone rubber for coating according to claim 1, characterized in that, The side-hydrogen type polymethylhydrosiloxane has a kinematic viscosity of 100–500 mPa·s at 25°C and a hydrogen mass fraction of 0.4%–1.2%.

4. A method for preparing a low-odor, yellowing-resistant liquid silicone rubber for coating as described in any one of claims 1-3, characterized in that, Includes the following steps: S1. Deep refining and pretreatment of raw materials: Vinyl polysiloxane and hydrogen-containing silicone oil are subjected to vacuum distillation to obtain refined modified vinyl polysiloxane and modified hydrogen-containing silicone oil. S2. Uniform compounding of base adhesive: The refined modified vinyl polysiloxane and modified hydrogen-containing silicone oil are mixed and stirred at high speed to obtain a composite base adhesive. S3. Additive Dispersion: Add ternary composite anti-yellowing additive and functional modification additive to the composite base adhesive and stir to disperse; S4. Catalytic curing and molding: Add complexed modified platinum catalyst to the system, stir thoroughly, degas under vacuum, and cure at a constant temperature to obtain low-odor, yellowing-resistant liquid silicone rubber for coating.

5. The method for preparing a low-odor, yellowing-resistant liquid silicone rubber for coating according to claim 4, characterized in that, In step S2, the stirring speed is 300-500 r / min and the stirring time is 20-40 min.

6. A method for preparing a low-odor, yellowing-resistant liquid silicone rubber for coating according to claim 4, characterized in that, In step S3, the stirring temperature is 40-60℃, the stirring speed is 300-500 r / min, and the stirring and dispersion time is 30-50 min.

7. The method for preparing a low-odor, yellowing-resistant liquid silicone rubber for coating according to claim 4, characterized in that, In step S4, the vacuum degassing time is 15-30 min, the curing temperature is 100-150℃, and the curing time is 30-60 min.

8. The method for preparing a low-odor, yellowing-resistant liquid silicone rubber for coating according to claim 4, characterized in that, In step S1, the conditions for vacuum distillation are: temperature 80-120℃, vacuum degree -0.08--0.1MPa for 2-4 hours.

Citation Information

Patent Citations

  • Addition-cured flame-retardant high-temperature resistant silicone rubber, its preparation method and application

    CN114058189B

  • High-flame-retardant insulating liquid silicone rubber as well as preparation method and application thereof

    CN120118522A