Highly elastic scratch-resistant silicone rubber and method for producing the same
By introducing a dynamic self-healing agent containing disulfide bonds and Schiff base imine bonds into silicone rubber, a chemical cross-linking network is formed, which solves the problem of insufficient strength and scratch resistance of silicone rubber and achieves improved high elasticity and self-healing performance.
Patent Information
- Application Number
- CN202611369902.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-04
- Publication Date
- 2026-11-24
AI Technical Summary
Silicone rubber has low strength, hardness, and scratch resistance, which limits its application in high-end decorative items, consumer electronics accessories, and smart wearable devices.
A dynamic self-healing agent containing disulfide bonds and Schiff base imine bonds is mixed with methyl vinyl silicone oil, fillers, silane coupling agents and other components to form a highly elastic scratch-resistant silicone rubber through a chemical crosslinking network and dynamic reversible covalent bonds.
It improves the mechanical properties and scratch resistance of silicone rubber, has good self-healing ability, enhances tensile strength and tear strength, and improves appearance quality.
Smart Images

Figure SMS_5
Abstract
Description
Technical Field
[0001] This invention relates to the field of silicone rubber technology, specifically to a highly elastic, scratch-resistant silicone rubber and its preparation method. Background Technology
[0002] Silicone rubber is a polysiloxane polymer with high elasticity, flexibility, flame retardancy, and aging resistance. It is widely used in electronics, biomedicine, and the automotive industry. However, silicone rubber has low strength and surface hardness, and poor scratch resistance. It is easily scratched and cracked when subjected to external forces, which affects the appearance and performance of silicone rubber materials. This restricts the application and promotion of silicone rubber materials in high-end decorative ornaments, consumer electronics accessories, smart wearable devices, and home furnishings, where appearance quality is a high priority.
[0003] In recent years, the development of self-healing memory polymer materials has been a research hotspot. By introducing metal coordination bonds, reversible ionic hydrogen bonds, and dynamically reversible covalent bonds into polymer materials, self-healing properties can be endowed to the monomers, reducing the formation of scratches and cracks. Patent CN116715694B discloses a class of silane coupling agents containing thiourea bonds, their preparation method, and their application in the preparation of self-healing silicone rubber. The silane coupling agent containing thiourea groups imparts excellent self-healing properties to the silicone rubber. However, this silicone rubber does not possess good mechanical strength, hardness, or scratch resistance. Summary of the Invention
[0004] The technical problem solved by this invention is the low strength, hardness, and scratch resistance of silicone rubber.
[0005] This invention provides a highly elastic, scratch-resistant silicone rubber, comprising, by weight, 100 parts methyl vinyl silicone oil, 5-15 parts dynamic self-healing agent, 28-40 parts filler, 0.8-1 parts silane coupling agent, 1.6-2 parts hydroxyl silicone oil, 1.6-2.1 parts methoxy silicone oil, 3.4-4.7 parts hydrogen-containing silicone oil, 0.07-0.1 parts stearic acid, and 0.3-0.4 parts platinum catalyst; the dynamic self-healing agent is an organosilicon polymer containing disulfide bonds and Schiff base imine bonds.
[0006] Furthermore, the fillers include fumed silica and carbon black.
[0007] Furthermore, the filler silane coupling agent includes vinyltrimethoxysilane and vinyltriethoxysilane.
[0008] Furthermore, the preparation method of highly elastic scratch-resistant silicone rubber is as follows: (1) Add 4,4'-dithiodiphenylamine and 4-vinylbenzaldehyde in a molar ratio of 1:(2-2.2) to ethanol, stir to react, cool and filter, wash the product with ethanol, dry and obtain Schiff base monomer.
[0009] (2) Add Schiff base monomer and tetramethyldisiloxane in a molar ratio of 1:(1.02-1.06) to tetrahydrofuran, add platinum catalyst dropwise, stir the reaction under nitrogen atmosphere, distill under reduced pressure, add ethanol, stir and filter, wash the product with ethanol to obtain dynamic self-healing agent.
[0010] (3) Mix methyl vinyl silicone oil and platinum catalyst to obtain curing agent components; add methyl vinyl silicone oil, dynamic self-healing agent, filler, silane coupling agent, hydroxy silicone oil, methoxy silicone oil, hydrogen-containing silicone oil and stearic acid to the mixer, mix evenly, add curing agent components, stir and mix, degas under vacuum, vulcanize, and obtain high elasticity scratch-resistant silicone rubber.
[0011] Furthermore, in (1), the reaction temperature is 45-55℃ and the reaction time is 7-10h.
[0012] Furthermore, in (2), the reaction temperature is 60-66℃ and the reaction time is 5-7h.
[0013] Furthermore, in (3), the sulfidation is carried out at 90-100℃ for 30-40 minutes.
[0014] The beneficial technical effects of this invention are as follows: By mixing and vulcanizing methyl vinyl silicone oil, dynamic self-healing agent, filler, hydrogen-containing silicone oil, platinum catalyst, etc., a highly elastic scratch-resistant silicone rubber is obtained. The dynamic self-healing agent contains terminal SH bonds, which undergo an addition reaction with methyl vinyl silicone oil to form a chemical cross-linking network, which is beneficial to improving the mechanical properties of silicone rubber. At the same time, the dynamic self-healing agent contains benzene rings, which further enhances the tensile strength, tear strength, hardness, etc. of silicone rubber, resulting in high mechanical strength, good scratch resistance, and excellent elasticity.
[0015] The dynamic self-healing agent of this invention contains disulfide bonds (SS) and Schiff base imine bonds (C=N). When subjected to stress, the low-bond-energy disulfide bonds break to generate sulfur free radicals, which then re-react and bond. The Schiff base imine bonds, as dynamic reversible covalent bonds, break to generate amino and aldehyde groups, which then react to generate Schiff base imine bonds. Under synergistic effect, this imparts excellent scratch resistance and self-healing properties to silicone rubber. Detailed Implementation
[0016] The following describes preferred embodiments of the present invention. It should be noted that those skilled in the art can make various improvements and modifications without departing from the principles of the present invention, and these improvements and modifications are also considered to be within the scope of protection of the present invention.
[0017] The following are product specifications: Methyl vinyl silicone oil (99% purity), Wesley Chemical Technology (Dongguan) Co., Ltd.; Hydroxy silicone oil (model 207-30), Zhejiang Zhenghe Silicon Materials Co., Ltd.; Methoxy silicone oil (model 201-3), Zhejiang Zhenghe Silicon Materials Co., Ltd.; Hydrogen-containing silicone oil (model H-075t-120), Jiangxi Haiduo Organosilicon Materials Co., Ltd.; Platinum catalyst (platinum content 2000ppm), Shenzhen Longdi Chemical Co., Ltd.; Fumed silica (model GCL-40), GCL High-Tech Nanomaterials (Xuzhou) Co., Ltd.
[0018] Example 1 (1) Add ethanol, 4,4'-dithiodiphenylamine and 4-vinylbenzaldehyde in a molar ratio of 1:2 to a flask equipped with a condenser, control the total concentration of the solution to 0.2 mol / L, heat to 45℃, stir the reaction for 10 h, cool and filter, wash the product with ethanol, dry, and obtain the Schiff base monomer. The reaction formula is as follows: .
[0019] (2) Add tetrahydrofuran, Schiff base monomers in a molar ratio of 1:1.04, and tetramethyldisiloxane to a flask equipped with a condenser, controlling the total concentration of the solution to 0.15 mol / L. Add platinum catalyst (0.18% of the mass of tetramethyldisiloxane) dropwise. Heat to 60°C under a nitrogen atmosphere and stir for 7 h. Distill under reduced pressure, add ethanol, stir, filter, and wash the product with ethanol to obtain a dynamic self-healing agent. The reaction formula is as follows: .
[0020] (3) Mix 50 parts by weight of methyl vinyl silicone oil and 0.34 parts by weight of platinum catalyst to obtain the curing agent component; add 50 parts by weight of methyl vinyl silicone oil, 5 parts by weight of dynamic self-healing agent, 35 parts by weight of fumed silica, 0.8 parts by weight of γ-methacryloyloxypropyltrimethoxysilane, 2 parts by weight of hydroxyl silicone oil, 1.6 parts by weight of methoxy silicone oil, 4.7 parts by weight of hydrogen-containing silicone oil and 0.08 parts by weight of stearic acid to the mixer, mix evenly, add the curing agent component, stir and mix, degas under vacuum, and vulcanize at 90°C for 40 min to obtain high elasticity scratch-resistant silicone rubber.
[0021] Example 2 (1) Add ethanol, 4,4'-dithiodiphenylamine and 4-vinylbenzaldehyde in a molar ratio of 1:2.2 to a flask equipped with a condenser, control the total concentration of the solution to 0.2 mol / L, heat to 55°C, stir for 7 h, cool and filter, wash the product with ethanol, dry and obtain Schiff base monomer.
[0022] (2) Add tetrahydrofuran, Schiff base monomer in a molar ratio of 1:1.02, and tetramethyldisiloxane to a flask equipped with a condenser, control the total concentration of the solution to 0.15 mol / L, add platinum catalyst (0.16% of the mass of tetramethyldisiloxane), heat to 66°C in a nitrogen atmosphere, stir and react for 5 h, distill under reduced pressure, add ethanol, stir and filter, wash the product with ethanol to obtain the dynamic self-healing agent.
[0023] (3) Mix 50 parts by weight of methyl vinyl silicone oil and 0.4 parts by weight of platinum catalyst to obtain curing agent components; add 50 parts by weight of methyl vinyl silicone oil, 8 parts by weight of dynamic self-healing agent, 28 parts by weight of fumed silica, 1 part by weight of vinyltrimethoxysilane, 2 parts by weight of hydroxyl silicone oil, 1.6 parts by weight of methoxy silicone oil, 4.3 parts by weight of hydrogen-containing silicone oil and 0.07 parts by weight of stearic acid to a mixer, mix evenly, add curing agent components, stir and mix, degas under vacuum, and vulcanize at 90°C for 40 min to obtain high elasticity scratch-resistant silicone rubber.
[0024] Example 3 (1) Add tetrahydrofuran, Schiff base monomer (prepared in the same way as in Example 1) in a molar ratio of 1:1.04, and tetramethyldisiloxane to a flask equipped with a condenser. Control the total concentration of the solution to 0.2 mol / L. Add platinum catalyst (0.23% of the mass of tetramethyldisiloxane) dropwise. Heat to 60°C in a nitrogen atmosphere and stir for 7 h. Distill under reduced pressure, add ethanol, stir and filter. Wash the product with ethanol to obtain the dynamic self-healing agent.
[0025] (2) Mix 50 parts by weight of methyl vinyl silicone oil and 0.3 parts by weight of platinum catalyst to obtain the curing agent component; add 50 parts by weight of methyl vinyl silicone oil, 12 parts by weight of dynamic self-healing agent, 40 parts by weight of fumed silica, 0.8 parts by weight of vinyltriethoxysilane, 1.8 parts by weight of hydroxy silicone oil, 1.8 parts by weight of methoxy silicone oil, 3.9 parts by weight of hydrogen-containing silicone oil and 0.07 parts by weight of stearic acid to a mixer, mix evenly, add the curing agent component, stir and mix, degas under vacuum, and vulcanize at 100°C for 30 min to obtain high elasticity scratch-resistant silicone rubber.
[0026] Example 4 (1) Add tetrahydrofuran, Schiff base monomer (prepared in the same way as in Example 1) in a molar ratio of 1:1.06, and tetramethyldisiloxane to a flask equipped with a condenser. Control the total concentration of the solution to 0.15 mol / L. Add platinum catalyst (0.16% of the mass of tetramethyldisiloxane) dropwise. Heat to 66°C in a nitrogen atmosphere and stir for 6 hours. Distill under reduced pressure, add ethanol, stir and filter. Wash the product with ethanol to obtain the dynamic self-healing agent.
[0027] (2) Mix 50 parts by weight of methyl vinyl silicone oil and 0.36 parts by weight of platinum catalyst to obtain curing agent component; add 50 parts by weight of methyl vinyl silicone oil, 15 parts by weight of dynamic self-healing agent, 35 parts by weight of fumed silica, 1 part by weight of vinyltrimethoxysilane, 1.8 parts by weight of hydroxyl silicone oil, 2 parts by weight of methoxy silicone oil, 3.4 parts by weight of hydrogen-containing silicone oil and 0.1 parts by weight of stearic acid to a mixer, mix evenly, add curing agent component, stir and mix, degas under vacuum, vulcanize at 100℃ for 30 min to obtain high elasticity scratch resistant silicone rubber.
[0028] Comparative Example 1 (1) Mix 50 parts by weight of methyl vinyl silicone oil and 0.34 parts by weight of platinum catalyst to obtain the curing agent component; add 50 parts by weight of methyl vinyl silicone oil, 35 parts by weight of fumed silica, 0.8 parts by weight of vinyltriethoxysilane, 2 parts by weight of hydroxyl silicone oil, 1.6 parts by weight of methoxy silicone oil, 4.7 parts by weight of hydrogen-containing silicone oil and 0.08 parts by weight of stearic acid to a mixer, mix evenly, add the curing agent component, stir and mix, degas under vacuum, and vulcanize at 90°C for 40 min to obtain silicone rubber.
[0029] Comparative Example 2 (1) Add tetrahydrofuran, divinyl (CAS No. 1321-74-0) in a molar ratio of 1:1.04, and tetramethyldisiloxane to a flask equipped with a condenser. Control the total concentration of the solution to 0.15 mol / L. Add platinum catalyst (0.18% of the mass of tetramethyldisiloxane) dropwise. Heat to 60°C in a nitrogen atmosphere and stir for 7 h. Distill under reduced pressure, add ethanol, stir and filter. Wash the product with ethanol to obtain the organosilicon polymer.
[0030] (2) Mix 50 parts by weight of methyl vinyl silicone oil and 0.34 parts by weight of platinum catalyst to obtain the curing agent component; add 50 parts by weight of methyl vinyl silicone oil, 5 parts by weight of organosilicon polymer, 35 parts by weight of fumed silica, 0.8 parts by weight of vinyltriethoxysilane, 2 parts by weight of hydroxyl silicone oil, 1.6 parts by weight of methoxy silicone oil, 4.7 parts by weight of hydrogen-containing silicone oil and 0.08 parts by weight of stearic acid to a mixer, mix evenly, add the curing agent component, stir and mix, degas under vacuum, and vulcanize at 90°C for 40 min to obtain silicone rubber.
[0031] Comparative Example 3 (1) Add ethanol, p-phenylenediamine (molar ratio 1:2), and 4-vinylbenzaldehyde to a flask equipped with a condenser, controlling the total concentration of the solution to 0.2 mol / L. Heat to 45°C, stir for 10 h, cool, filter, wash the product with ethanol, and dry to obtain a Schiff base monomer with the following structural formula: .
[0032] (2) Add tetrahydrofuran, Schiff base monomer in a molar ratio of 1:1.04, and tetramethyldisiloxane to a flask equipped with a condenser, control the total concentration of the solution to 0.15 mol / L, add platinum catalyst (0.18% of the mass of tetramethyldisiloxane), heat to 60°C in a nitrogen atmosphere, stir and react for 7 h, distill under reduced pressure, add ethanol, stir and filter, wash the product with ethanol to obtain the dynamic self-healing agent.
[0033] (3) Mix 50 parts by weight of methyl vinyl silicone oil and 0.34 parts by weight of platinum catalyst to obtain the curing agent component; add 50 parts by weight of methyl vinyl silicone oil, 5 parts by weight of dynamic self-healing agent, 35 parts by weight of fumed silica, 0.8 parts by weight of vinyltriethoxysilane, 2 parts by weight of hydroxyl silicone oil, 1.6 parts by weight of methoxy silicone oil, 4.7 parts by weight of hydrogen-containing silicone oil and 0.08 parts by weight of stearic acid to a mixer, mix evenly, add the curing agent component, stir and mix, degas under vacuum, and vulcanize at 90°C for 40 min to obtain silicone rubber.
[0034] Comparative Example 4 (1) Add 150 mL of acetone, 60 mmol of 4,4'-dihydroxydiphenyl disulfide (CAS No. 15015-57-3), and 240 mmol of potassium carbonate to a flask equipped with a condenser. Add 180 mmol of bromopropene dropwise under a nitrogen atmosphere. Heat to 50 °C and stir for 12 h. Filter, evaporate the filtrate by rotary evaporation, and separate by column chromatography to obtain 4,4'-diallyloxydiphenyl disulfide, with the structural formula: .
[0035] (2) Add tetrahydrofuran, 4,4'-diallyloxydiphenyl disulfide in a molar ratio of 1:1.04, and tetramethyldisiloxane to a flask equipped with a condenser, control the total concentration of the solution to 0.15 mol / L, add platinum catalyst (0.18% of the mass of tetramethyldisiloxane), heat to 60°C in a nitrogen atmosphere, stir and react for 7 h, distill under reduced pressure, add ethanol, stir and filter, wash the product with ethanol to obtain the dynamic self-healing agent.
[0036] (3) Mix 50 parts by weight of methyl vinyl silicone oil and 0.34 parts by weight of platinum catalyst to obtain the curing agent component; add 50 parts by weight of methyl vinyl silicone oil, 5 parts by weight of dynamic self-healing agent, 35 parts by weight of fumed silica, 0.8 parts by weight of vinyltriethoxysilane, 2 parts by weight of hydroxyl silicone oil, 1.6 parts by weight of methoxy silicone oil, 4.7 parts by weight of hydrogen-containing silicone oil and 0.08 parts by weight of stearic acid to a mixer, mix evenly, add the curing agent component, stir and mix, degas under vacuum, and vulcanize at 90°C for 40 min to obtain silicone rubber.
[0037] The tensile strength of silicone rubber shall be tested according to GB / T 528-2009. The tear strength shall be tested according to GB / T 529-2008. The hardness shall be tested according to GB / T 39693.4-2025.
[0038] The silicone rubber surface was scratched using a scratch tester with a scratch load of 4N, a scratch speed of 2cm / s, and a scratch length of 10cm. The surface was left at room temperature for 1 hour, and the disappearance of the scratches was observed.
[0039] Table 1
[0040] The silicone rubber in Comparative Example 1 exhibited low tensile strength, tensile strength, and hardness, and the scratches did not disappear after the scratch test. Each Example 1 incorporated a dynamic self-healing agent containing terminal SH bonds, which undergoes an addition reaction with methyl vinyl silicone oil to form a chemical cross-linking network, thus improving the mechanical properties of the silicone rubber. Simultaneously, the dynamic self-healing agent contains benzene rings, further enhancing the mechanical strength of the silicone rubber. Furthermore, the dynamic self-healing agent contains disulfide bonds (SS) and Schiff base imine bonds (C=N). Under stress, the low-bond-energy disulfide bonds break to generate sulfur free radicals, which then re-react and bond. The Schiff base imine bonds, as dynamically reversible covalent bonds, undergo covalent bond cleavage to generate amino and aldehyde groups, which then react to form Schiff base imine bonds. Through this synergistic effect, the silicone rubber acquires excellent scratch resistance and self-healing properties.
[0041] The organosilicon polymer in Comparative Example 2 does not contain disulfide bonds or Schiff base imine bonds. The silicone rubber prepared from it does not show scratches after a scratch test, and has poor scratch resistance and self-healing properties.
[0042] The dynamic self-healing agent of Comparative Example 3 does not contain disulfide bonds, and the dynamic self-healing agent of Comparative Example 4 does not contain Schiff base imine bonds. The silicone rubber prepared by these two agents has poor scratch resistance and self-healing properties.
Claims
1. A highly elastic, scratch-resistant silicone rubber, characterized in that, The high-elasticity, scratch-resistant silicone rubber comprises, by weight, 100 parts methyl vinyl silicone oil, 5-15 parts dynamic self-healing agent, 28-40 parts filler, 0.8-1 parts silane coupling agent, 1.6-2 parts hydroxyl silicone oil, 1.6-2.1 parts methoxy silicone oil, 3.4-4.7 parts hydrogen-containing silicone oil, 0.07-0.1 parts stearic acid, and 0.3-0.4 parts platinum catalyst; the dynamic self-healing agent is an organosilicon polymer containing disulfide bonds and Schiff base imine bonds.
2. The high-elasticity, scratch-resistant silicone rubber according to claim 1, characterized in that, The filler is fumed silica or carbon black.
3. The high-elasticity, scratch-resistant silicone rubber according to claim 1, characterized in that, The silane coupling agent is γ-methacryloxypropyltrimethoxysilane, γ-methacryloxypropyltriethoxysilane, vinyltrimethoxysilane, or vinyltriethoxysilane.
4. A method for preparing a highly elastic, scratch-resistant silicone rubber as described in any one of claims 1-3, characterized in that, The preparation method is as follows: methyl vinyl silicone oil and platinum catalyst are stirred and mixed to obtain a curing agent component; methyl vinyl silicone oil, dynamic self-healing agent, filler, silane coupling agent, hydroxyl silicone oil, methoxy silicone oil, hydrogen-containing silicone oil, and stearic acid are added to a mixer and mixed evenly; the curing agent component is added, stirred and mixed, vacuum degassing is performed, and vulcanization is carried out to obtain a highly elastic scratch-resistant silicone rubber.
5. The method for preparing highly elastic scratch-resistant silicone rubber according to claim 4, characterized in that, The vulcanization process involves placing the vulcan at 90-100°C for 30-40 minutes.
6. The method for preparing highly elastic scratch-resistant silicone rubber according to claim 4, characterized in that, The preparation method of the dynamic self-healing agent is as follows: (1) Add 4,4'-dithiodiphenylamine and 4-vinylbenzaldehyde in a molar ratio of 1:(2-2.2) to ethanol, stir the reaction, cool and filter, wash the product, dry and obtain Schiff base monomer; (2) Add Schiff base monomer and tetramethyldisiloxane in a molar ratio of 1:(1.02-1.06) to tetrahydrofuran, add platinum catalyst dropwise, stir the reaction under nitrogen atmosphere, distill under reduced pressure, add ethanol, stir and filter, wash the product to obtain dynamic self-healing agent.
7. The method for preparing highly elastic scratch-resistant silicone rubber according to claim 6, characterized in that, The reaction temperature in (1) is 45-55℃ and the reaction time is 7-10h.
8. The method for preparing highly elastic scratch-resistant silicone rubber according to claim 6, characterized in that, The reaction temperature in (2) is 60-66℃ and the reaction time is 5-7h.
9. A highly elastic, scratch-resistant silicone rubber obtained by the preparation method according to any one of claims 1-8.
Citation Information
Patent Citations
A class of silane coupling agents containing thiourea bonds, their preparation methods, and their application in the preparation of self-healing silicone rubber.
CN116715694B