Low viscosity high thermal conductive silicone gel with oriented arrangement of thermal conductive filler and preparation method thereof
By using three-roll high-shear mixing and dynamic shearing technology, a low-viscosity, high-thermal-conductivity silica gel with an ordered thermally conductive filler structure is formed, which solves the problems of viscosity increase and discontinuous heat conduction path in highly filled silica gels, and achieves high-efficiency thermal conductivity and processability.
Patent Information
- Application Number
- CN202611415499.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-13
- Publication Date
- 2026-11-24
AI Technical Summary
Existing thermally conductive silicone gels suffer from increased viscosity, difficulties in dispersion and degassing, and discontinuous heat conduction paths in random filler networks under high-filling conditions, leading to increased processing difficulty and limited thermal conductivity.
The high-concentration particle system is rearranged in the shear flow field by using three-roll high-shear mixing and dynamic shearing technology before curing, forming an ordered structure of thermally conductive filler. The wetting and dispersion state of the inorganic filler and the organosilicon continuous phase are improved by silane coupling agent treatment, and the microstructure is fixed to reduce flow resistance and improve the effective adjacency and continuity of the pathway between particles.
Without changing the chemical composition and filling amount of the filler, the viscosity is significantly reduced, the thermal conductivity and mechanical properties are improved, and the processability and thermal conductivity of the highly filled silicone gel are ensured.
Abstract
Description
Technical Field
[0001] This invention belongs to the field of materials technology, specifically relating to a low-viscosity, high-thermal-conductivity silica gel with thermally conductive filler oriented, and also to a method for preparing the gel. Background Technology
[0002] As 5G communication equipment, high-performance computing and large-scale integrated circuits, power electronic devices for new energy vehicles, and energy storage systems develop towards higher integration and higher power density, the heat flux density generated per unit volume or unit area continues to increase. Excessive operating temperature of electronic devices accelerates material aging, causes electrical performance drift, and reduces device reliability. Therefore, it is necessary to place thermal interface materials between heat-generating devices and heat sinks to fill the microscopic irregularities and air gaps between the two contact surfaces, reducing interfacial thermal resistance. Thermally conductive silicone gel combines fluidity with post-curing elasticity, allowing it to fully fill the interfacial microscopic gaps under low installation pressure and establish stable heat conduction channels. It is one of the core thermally conductive interface materials for current high-end electronic devices.
[0003] Existing filled thermally conductive silicone gels typically improve overall thermal conductivity by increasing the volume fraction of inorganic thermally conductive fillers such as alumina, boron nitride, and zinc oxide. However, in the high-filling range, the particle spacing is significantly shortened, and particle-particle contact, agglomeration, and hydrodynamic interactions during flow are enhanced. This leads to problems such as rapid increase in apparent viscosity, enhanced yield characteristics, and difficulty in degassing. Excessively high rheological resistance not only increases the difficulty of mixing, metering, and sizing, but may also cause air bubble entrainment, uneven local filler distribution, and insufficient interfacial adhesion, thus offsetting some of the thermal conductivity gains from simply increasing the filler content.
[0004] On the other hand, for filling systems dominated by near-spherical particles, the thermal conduction pathways formed solely by random stacking typically have significant spatial tortuosity. The number and quality of effective contact points between particles are limited, requiring heat to frequently pass through the particle-polymer interface and the tiny gaps between particles, leading to the accumulation of interparticle contact thermal resistance and particle-matrix interface thermal resistance. Traditional blending of fillers with different particle sizes can improve packing efficiency and utilize small particles to fill the gaps between large particles; however, without further control over the flow structure of high-concentration suspension systems, it remains difficult to simultaneously address the processing viscosity and the continuity of the effective thermal conduction network in high-filling systems.
[0005] Therefore, it is necessary to further introduce industrially feasible structural control methods on the basis of particle size distribution and interface modification, so that the filler forms a spatial structure that is more conducive to flow and heat conduction in the pre-processing and curing stages, and fixes the structure as much as possible during the curing process, thereby achieving a synergistic balance between high filler content, processability and high thermal conductivity. Summary of the Invention
[0006] The first objective of this invention is to address the problems of increased viscosity, difficulties in dispersion and degassing caused by increased filler content in highly filled thermally conductive silica gels, as well as the discontinuity of effective heat conduction paths in random filler networks, by providing a low-viscosity, high-thermal-conductivity silica gel with an ordered thermally conductive filler structure and its preparation method.
[0007] The second objective of this invention is to provide a method for preparing low-viscosity, high-thermal-conductivity silicone gel with oriented thermally conductive fillers. Through three-roll high-shear mixing and dynamic shearing before curing, a high-concentration particle system undergoes rearrangement in a shear flow field, resulting in a statistically preferential distribution of particle chains, particle clusters, and their connection paths along the main shear flow lines. This microstructure is then fixed during subsequent addition curing. Without changing the chemical composition and filling amount of the filler, this structural regulation can reduce the flow resistance corresponding to disordered packing and improve the effective adjacency and pathway continuity between thermally conductive fillers.
[0008] Therefore, the first technical solution provided by this invention is as follows:
[0009] A low-viscosity, high-thermal-conductivity silicone gel with oriented thermally conductive fillers, comprising the following components in parts by weight:
[0010] 100 parts by weight of vinyl-terminated silicone oil;
[0011] 22.35–44.72 parts by weight of hydrogen-containing crosslinking agent;
[0012] 600-1200 parts by weight of spherical alumina surface modified with silane coupling agent;
[0013] Platinum catalyst, 0.1–0.5 parts by weight;
[0014] Acetyl alcohol inhibitors: 0.1–2.0 parts by weight;
[0015] Furthermore, in the aforementioned low-viscosity, high-thermal-conductivity silicone gel with oriented thermally conductive filler, the spherical alumina modified with silane coupling agent is composed of a mixture of large-particle-size spherical alumina and small-particle-size spherical alumina treated with silane coupling agent; the average particle size of the large-particle-size spherical alumina is 20–40 μm, and the average particle size of the small-particle-size spherical alumina is 1–5 μm.
[0016] Furthermore, in the aforementioned low-viscosity, high-thermal-conductivity silicone gel with oriented filler, the mass ratio of large-particle-size spherical alumina treated with a silane coupling agent to small-particle-size spherical alumina treated with a silane coupling agent is 1:1 to 3:1. The synergistic use of different particle sizes facilitates the filling of some gaps between large particles by smaller particles, increasing the probability of particle adjacency and effective filling efficiency.
[0017] Furthermore, in the aforementioned low-viscosity, high-thermal-conductivity silicone gel with oriented thermally conductive fillers, the end-vinyl silicone oil is α,ω-end-vinyl polydimethylsiloxane, with a viscosity of 200–500 mPa·s at 25 °C, and is used as the main vinyl component of the continuous phase and addition-curing network.
[0018] The hydrogen-containing crosslinking agent is hydrogen-terminated polydimethylsiloxane; the active hydrogen mass fraction is 0.05%, which is used to adjust the degree of crosslinking in the addition curing reaction, while taking into account both curing integrity and gel flexibility.
[0019] The platinum catalyst mentioned is a Karstedt platinum catalyst;
[0020] The alkynol inhibitor is 1-ethynyl-1-cyclohexanol; it is used to regulate the reaction rate during room temperature storage and processing, and to improve the workability of mixing, degassing and sizing processes.
[0021] Furthermore, in the aforementioned low-viscosity, high-thermal-conductivity silicone gel with oriented thermally conductive filler, the spherical alumina modified with the silane coupling agent is prepared by the following method: the silane coupling agent is dissolved in anhydrous ethanol, and after thorough stirring and dispersion, large-diameter or small-diameter spherical alumina particles are added; the mixture is stirred at room temperature for 30 min, then heated to 60 °C and reacted for 4 h; after the reaction is completed, the mixture is filtered, and the filter cake is repeatedly washed with anhydrous ethanol; subsequently, it is vacuum dried at 80 °C to obtain spherical alumina with a silanized surface.
[0022] Furthermore, the aforementioned low-viscosity, high-thermal-conductivity silicone gel with oriented thermally conductive fillers is characterized in that the silane coupling agent is γ-mercaptopropyltrimethoxysilane.
[0023] Furthermore, in the aforementioned low-viscosity, high-thermal-conductivity silicone gel with oriented thermally conductive fillers, the mass of the silane coupling agent is 0.5% to 4.0% of the mass of the spherical alumina.
[0024] The second technical solution provided by this invention is a method for preparing a low-viscosity, high-thermal-conductivity silica gel with oriented thermally conductive fillers, which includes the following steps in sequence:
[0025] (1) Add the spherical alumina modified with silane coupling agent to the vinyl-terminated silicone oil in batches. After premixing, use a three-roll mill with a roller speed ratio of 1:2:4 for high shear mixing to disperse and rearrange the filler and obtain the base rubber.
[0026] (2) Add hydrogen-containing crosslinking agent and inhibitor to the base adhesive, disperse, and then add platinum catalyst to continue dispersion and degassing to obtain a curable mixture;
[0027] (3) Before addition curing, a dynamic shear field is applied to the mixture to make the thermally conductive filler form an oriented arrangement in the flow field; after shearing is stopped, pressure is applied to cure under the condition of maintaining the oriented arrangement, so that the polysiloxane crosslinking network is formed and the filler orientation structure is fixed to obtain the low viscosity and high thermal conductivity silicone gel.
[0028] Furthermore, in the above-mentioned method for preparing a low-viscosity, high-thermal-conductivity silica gel with oriented thermally conductive fillers, the premixing temperature in step (1) is 120°C, the front roller speed is 80 rpm, the middle roller speed is 160 rpm, and the rear roller speed is 320 rpm; the roller spacing is gradually reduced to 5-20 μm, the mixing temperature is 80-120°C, and the mixture is repeatedly passed through a three-roll mill 2-4 times.
[0029] In step (2), after high-speed dispersion under vacuum for 20 min, platinum catalyst is added, dispersion continues for 10 min, and then vacuum degassing is performed for 20 min.
[0030] The dynamic shear field mentioned in step (3) is a dynamic rotating shear field with a shear rate of 10–50 s. -1 The processing time is 5 to 15 minutes. After shearing stops, apply a pressure of 20 MPa within 2 minutes and heat to 120 ℃ for 30 minutes to cure.
[0031] The above-mentioned low-viscosity, high-thermal-conductivity silicone gel with oriented filler is used as a thermal interface material.
[0032] Compared with the prior art, the technical solution provided in this application has the following advantages:
[0033] This application improves the rationality of particle packing and space filling by using a compound of spherical alumina with different particle sizes; it treats the alumina surface with a silane coupling agent to improve the wetting and dispersion state between the inorganic filler and the continuous organosilicon phase; through three-roll high-shear mixing and dynamic shearing before curing, the high-concentration particle system is rearranged in the shear flow field, so that the particle chains, particle clusters and their connection paths are statistically preferentially distributed along the main shear flow line, and the microstructure is fixed in the subsequent addition curing process; without changing the chemical composition and filling amount of the filler, the structure regulation can reduce the flow resistance corresponding to disordered packing and improve the effective adjacency and path continuity between thermally conductive fillers. Detailed Implementation
[0034] The present invention will be further described below with reference to the embodiments. The listed embodiments are used to illustrate the technical solutions and effects of the present invention and should not be construed as limiting the scope of protection. Unless otherwise specified, "parts" in each embodiment refers to parts by weight.
[0035] Example 1
[0036] This embodiment provides a low-viscosity, high-thermal-conductivity silicone gel with oriented thermally conductive fillers, which is prepared sequentially through the following steps:
[0037] 1) Weigh 100g of α,ω-terminated vinyl polydimethylsiloxane (model PDMS-Vi200, viscosity at 25℃ 200mPa·s, vinyl content 0.5 wt%), 600g of AO-20 surface-treated with KH590; 0.35g of Karstedt platinum catalyst; 1.18g of 1-ethynyl-1-cyclohexanol; and 29.8g of hydrogen-capped polydimethylsiloxane (CAS:70900-21-9).
[0038] 2) The AO-20 surface-treated with KH590 weighed in step 1) is added in batches to PDMS-Vi200 and premixed in a power mixer at about 120 °C to gradually wet the high-filled powder with the matrix and form a uniform base rubber that can enter the three-roll mill. Then it is fed into the three-roll mill for high-shear mixing. The roller speed ratio of the three-roll mill is controlled at 1:2:4 (front roller speed is 80 rpm, middle roller speed is 160 rpm, and rear roller speed is 320 rpm), the roller spacing is gradually reduced and finally controlled in the range of 10 μm, and the mixing temperature is controlled at 100 °C to obtain the base rubber.
[0039] 3) Add hydrogen-terminated polydimethylsiloxane and 1-ethynyl-1-cyclohexanol to the base gel prepared in step 2), and disperse at high speed under vacuum for 20 min; then add Karstedt platinum catalyst and continue to disperse for 10 min, and then degas under vacuum for 20 min to obtain a curable thermally conductive silicone gel mixture.
[0040] 4) Inject the mixture from step 3) into the mold and apply a shear rate of 20 s before addition curing. -1 A dynamic rotating shear field was applied for 10 min to further rearrange the particle chains, clusters, and their adjacent paths in the flow field, maintaining their oriented and ordered structure. After the shearing treatment, the material was allowed to enter the curing stage as soon as possible to reduce structural relaxation. Subsequently, a pressure of 20 MPa was applied and the temperature was raised to 120 °C for 30 min to cure, allowing the polysiloxane crosslinking network to form and fix the shear-induced filler spatial structure, resulting in a low-viscosity, high-thermal-conductivity silicone gel with an oriented and ordered structure of thermally conductive filler.
[0041] The AO-20 surface-treated with KH590 was prepared by the following method: 20 g of γ-mercaptopropyltrimethoxysilane was dissolved in an appropriate amount of anhydrous ethanol, and after thorough stirring and dispersion, 1000 g of large-particle-size spherical alumina AO-20 with an average particle size of 20 μm was added. The mixture was stirred at room temperature for 30 min, and then heated to 60 ℃ for 4 h. After the reaction was completed, the mixture was filtered, and the filter cake was washed three times with anhydrous ethanol. Then, it was vacuum dried at 80 ℃ to constant weight to obtain large-particle-size spherical alumina with surface silanization treatment.
[0042] Example 2
[0043] This embodiment provides a low-viscosity, high-thermal-conductivity silica gel with thermally conductive fillers arranged in an oriented manner. The preparation steps and process parameters are basically the same as those in Example 1, the only difference being the different mass numbers of each substance in the steps, as detailed below:
[0044] Weigh out 100g of α,ω-terminated vinyl polydimethylsiloxane (model PDMS-Vi200, viscosity at 25 ℃ 200 mPa·s, vinyl content 0.5 wt%), 600g of AO-20 surface-treated with KH590, 300g of AO-05 surface-treated with KH590, 0.35g of Karstedt platinum catalyst, 1.18g of 1-ethynyl-1-cyclohexanol, and 29.8g of hydrogen-capped polydimethylsiloxane (CAS:70900-21-9).
[0045] The AO-20 surface-treated with KH590 was prepared by the following method: 20 g of γ-mercaptopropyltrimethoxysilane was dissolved in an appropriate amount of anhydrous ethanol, and after thorough stirring and dispersion, 1000 g of large-particle-size spherical alumina AO-20 with an average particle size of 20 μm was added. The mixture was stirred at room temperature for 30 min, and then heated to 60 ℃ for 4 h. After the reaction was completed, the mixture was filtered, and the filter cake was washed three times with anhydrous ethanol. Then, it was vacuum dried at 80 ℃ to constant weight to obtain large-particle-size spherical alumina with surface silanization treatment.
[0046] The AO-05 surface-treated with KH590 was prepared by the following method: 20g of γ-mercaptopropyltrimethoxysilane was dissolved in an appropriate amount of anhydrous ethanol, and after thorough stirring and dispersion, 1000g of small-particle-size spherical alumina AO-05 with an average particle size of 5 μm was added. The mixture was stirred at room temperature for 30 min, and then heated to 60 ℃ for 4 h. After the reaction was completed, the mixture was filtered, and the filter cake was washed three times with anhydrous ethanol. Then, it was vacuum dried at 80 ℃ to constant weight to obtain small-particle-size spherical alumina with surface silanization treatment.
[0047] Example 3
[0048] This embodiment provides a low-viscosity, high-thermal-conductivity silica gel with thermally conductive fillers arranged in an oriented manner. The preparation steps and process parameters are basically the same as those in Example 1, the only difference being the different masses of each substance in the steps, as detailed below:
[0049] Weigh out 100g of α,ω-terminated vinyl polydimethylsiloxane (model PDMS-Vi200, viscosity at 25℃ 200mPa·s, vinyl content 0.5 wt%), 675g of AO-20 surface-treated with KH590, 225g of AO-05 surface-treated with KH590, 0.35g of Karstedt platinum catalyst, 1.18g of 1-ethynyl-1-cyclohexanol, and 29.8g of hydrogen-capped polydimethylsiloxane.
[0050] The preparation methods of AO-20 and AO-05 with KH590 surface treatment are the same as those of AO-20 and AO-05 with KH590 surface treatment in Example 2.
[0051] Example 4
[0052] This embodiment provides a low-viscosity, high-thermal-conductivity silica gel with thermally conductive fillers arranged in an oriented manner. The preparation steps and process parameters are basically the same as those in Example 1, the only difference being the different mass numbers of each substance in the steps, as detailed below:
[0053] Weigh out 100g of α,ω-terminated vinyl polydimethylsiloxane (model PDMS-Vi200, viscosity at 25℃ 200mPa·s, vinyl content 0.5 wt%), 800g of AO-20 surface-treated with KH590, 400g of AO-05 surface-treated with KH590, 0.35g of Karstedt platinum catalyst, 1.18g of 1-ethynyl-1-cyclohexanol, and 29.8g of hydrogen-capped polydimethylsiloxane.
[0054] The preparation methods of AO-20 and AO-05 with KH590 surface treatment are the same as those of AO-20 and AO-05 with KH590 surface treatment in Example 2.
[0055] Example 5
[0056] This embodiment provides a low-viscosity, high-thermal-conductivity silica gel with thermally conductive fillers arranged in an oriented manner. The preparation steps and process parameters are basically the same as those in Example 1, the only difference being the different mass numbers of each substance in the steps, as detailed below:
[0057] Weigh out 100g of α,ω-terminated vinyl polydimethylsiloxane (model PDMS-Vi200, viscosity at 25℃ 200mPa·s, vinyl content 0.5 wt%), 800g of AO-20 surface-treated with KH590, 400g of AO-05 surface-treated with KH590, 0.35g of Karstedt platinum catalyst, 1.18g of 1-ethynyl-1-cyclohexanol, and 44.72g of hydrogen-capped polydimethylsiloxane.
[0058] The preparation methods of AO-20 and AO-05 with KH590 surface treatment are the same as those of AO-20 and AO-05 with KH590 surface treatment in Example 2.
[0059] Example 6
[0060] This embodiment provides a low-viscosity, high-thermal-conductivity silica gel with thermally conductive fillers arranged in an oriented manner. The preparation steps and process parameters are basically the same as those in Example 1, the only difference being the different mass numbers of each substance in the steps, as detailed below:
[0061] 1) Weigh 100g of α,ω-terminated vinyl polydimethylsiloxane (model PDMS-Vi200, viscosity at 25℃ 200mPa·s, vinyl content 0.5 wt%), 800g of AO-20 surface-treated with KH590, 400g of AO-05 surface-treated with KH590, 0.35g of Karstedt platinum catalyst, 1.18g of 1-ethynyl-1-cyclohexanol, and 22.34g of hydrogen-capped polydimethylsiloxane.
[0062] 2) The AO-20 surface-treated with KH590 weighed in step 1) is added in batches to PDMS-Vi200 and premixed in a power mixer at about 120 °C to gradually wet the high-filled powder with the matrix and form a homogeneous base rubber that can enter the three-roll mill; then it is fed into the three-roll mill for high-shear mixing; the roller speed ratio of the three-roll mill is controlled at 1:2:4 (front roller speed is 80 rpm, middle roller speed is 160 rpm, and rear roller speed is 320 rpm), and the roller spacing is gradually reduced;
[0063] Repeat step 2) twice, finally controlling the size within the 10 μm range, and control the mixing temperature at 100 ℃ to obtain the base rubber.
[0064] 3) Add hydrogen-terminated polydimethylsiloxane and 1-ethynyl-1-cyclohexanol to the base gel prepared in step 2), and disperse at high speed under vacuum for 20 min; then add Karstedt platinum catalyst and continue to disperse for 10 min, and then degas under vacuum for 20 min to obtain a curable thermally conductive silicone gel mixture.
[0065] 4) Inject the mixture from step 3) into the mold and apply a shear rate of 20 s before addition curing. -1A dynamic rotating shear field was applied for 10 min to further rearrange the particle chains, clusters, and their adjacent paths in the flow field, maintaining their oriented and ordered structure. After the shearing treatment, the material was allowed to enter the curing stage as soon as possible to reduce structural relaxation. Subsequently, a pressure of 20 MPa was applied and the temperature was raised to 120 °C for 30 min to cure, allowing the polysiloxane crosslinking network to form and fix the shear-induced filler spatial structure, resulting in a low-viscosity, high-thermal-conductivity silicone gel with an oriented and ordered structure of thermally conductive filler.
[0066] The AO-20 surface-treated with KH590 was prepared by the following method: 20 g of γ-mercaptopropyltrimethoxysilane was dissolved in an appropriate amount of anhydrous ethanol, and after thorough stirring and dispersion, 1000 g of large-particle-size spherical alumina AO-20 with an average particle size of 20 μm was added. The mixture was stirred at room temperature for 30 min, and then heated to 60 ℃ for 4 h. After the reaction was completed, the mixture was filtered, and the filter cake was washed three times with anhydrous ethanol. Then, it was vacuum dried at 80 ℃ to constant weight to obtain large-particle-size spherical alumina with surface silanization treatment.
[0067] The preparation methods of AO-20 and AO-05 with KH590 surface treatment are the same as those of AO-20 and AO-05 with KH590 surface treatment in Example 2.
[0068] Example 7
[0069] This embodiment provides a low-viscosity, high-thermal-conductivity silica gel with thermally conductive fillers arranged in an oriented manner. The preparation steps and process parameters are basically the same as those in Example 1, the only difference being the different mass numbers of each substance in the steps, as detailed below:
[0070] Weigh out 100g of α,ω-terminated vinyl polydimethylsiloxane (model PDMS-Vi200, viscosity at 25℃ 200mPa·s, vinyl content 0.5 wt%), 450g of AO-20 surface-treated with KH590, 450g of AO-05 surface-treated with KH590, 0.35g of Karstedt platinum catalyst, 1.18g of 1-ethynyl-1-cyclohexanol, and 22.34g of hydrogen-capped polydimethylsiloxane.
[0071] The preparation methods of AO-20 and AO-05 with KH590 surface treatment are the same as those of AO-20 and AO-05 with KH590 surface treatment in Example 2.
[0072] Comparative Example 1
[0073] This comparative example provides a low-viscosity, high-thermal-conductivity silicone gel as a thermally conductive filler, prepared sequentially through the following steps:
[0074] 1) Weigh 100g of α,ω-terminated vinyl polydimethylsiloxane (model PDMS-Vi200, viscosity at 25℃ 200mPa·s, vinyl content 0.5 wt%), 600g of AO-20 surface-treated with KH590, 0.35g of Karstedt platinum catalyst, 1.18g of 1-ethynyl-1-cyclohexanol, and 29.8g of hydrogen-capped polydimethylsiloxane.
[0075] 2) The AO-20 surface-treated with KH590 weighed in step 1) is added in batches to PDMS-Vi200 and premixed in a power mixer at about 120 ℃ to gradually wet the high-filled powder with the matrix and form a uniform base rubber that can enter the three-roll mill. Then, it is fed into the three-roll mill with the roller speed ratio controlled at 1:2:4 (front roller speed is 80 rpm, middle roller speed is 160 rpm, and rear roller speed is 320 rpm) for shearing, controlling the particle size in the range of 10 μm, and the mixing temperature is controlled at 100 ℃ to obtain the base rubber.
[0076] 3) Add hydrogen-terminated polydimethylsiloxane and 1-ethynyl-1-cyclohexanol to the base gel prepared in step 2), and disperse at high speed under vacuum for 20 min; then add Karstedt platinum catalyst and continue to disperse for 10 min, and then degas under vacuum for 20 min to obtain a curable thermally conductive silicone gel mixture.
[0077] 4) Inject the mixture from step 3) into the mold, apply a pressure of 20 MPa and heat to 120 ℃ for 30 min to form a polysiloxane cross-linked network and fix the spatial structure of the filler, thus obtaining a low-viscosity, high-thermal-conductivity silicone gel with disordered thermally conductive filler structure.
[0078] The AO-20 surface-treated with KH590 described above is prepared using the same method as the AO-20 surface-treated with KH590 described in Example 1.
[0079] Comparative Example 2
[0080] This comparative example provides a low-viscosity, high-thermal-conductivity silicone gel as a thermally conductive filler. The preparation steps and process parameters are basically the same as those of Comparative Example 1, the only difference being the different masses of each substance in the steps, as detailed below:
[0081] Weigh out 100g of α,ω-terminated vinyl polydimethylsiloxane (model PDMS-Vi200, viscosity at 25℃ 200mPa·s, vinyl content 0.5 wt%), 600g of AO-20 surface-treated with KH590, 300g of AO-05 surface-treated with KH590, 0.35g of Karstedt platinum catalyst, 1.18g of 1-ethynyl-1-cyclohexanol, and 29.8g of hydrogen-capped polydimethylsiloxane.
[0082] To verify the test method for low-viscosity, high-thermal-conductivity silicone gel with oriented thermally conductive filler provided in this application, the specific test method used is as follows: The test results are shown in Table 1:
[0083] (1) Base viscosity: The viscosity of liquid samples was determined using an NTV-S1 digital rotational viscometer from Shanghai Nirun Intelligent Technology Co., Ltd., in accordance with GB / T 10247-2008. To ensure the comparability of the comparison results, the same sample pretreatment, test temperature, rotor and rotation speed conditions should be used for the examples and comparative examples in the same group.
[0084] (2) Thermal conductivity: The steady-state heat flow method was used, and the test was conducted in accordance with ASTM D5470-2017. For samples evaluated as thermal interface materials, the sample thickness, clamping pressure and interface treatment conditions of the examples and comparative examples should be consistent to reduce the interference of the difference in contact thermal resistance on the intrinsic comparison of materials.
[0085] (3) Tensile strength: The dumbbell-shaped specimens were tested using an electronic universal testing machine in accordance with the relevant standard GB / T 1040.2-2022, with a tensile rate of 50 mm / min. The examples and comparative examples used the same specimen geometry, curing conditions and testing environment.
[0086] (4) Oil penetration ratio: Place the sample in a 60 ℃ oven for 168 h, measure the size of the oil penetration mark, and calculate the oil penetration ratio according to "oil penetration mark diameter / initial sample diameter". The same sample size, substrate and environmental conditions should be used in the comparative test. The closer the oil penetration ratio is to 1, the less macroscopic oil phase migration there is.
[0087] (5) Thermogravimetric analysis: A Netzsch TG 209 F1 thermogravimetric analyzer was used. 2.00 to 5.00 mg of sample was weighed and placed in a ceramic crucible. Under the condition of nitrogen flow rate of 20 mL / min, the temperature was raised from 30 °C to 700 °C at a heating rate of 10 °C / min. The mass change curve was recorded throughout the process. The temperature at which the mass loss reached 5% of the initial mass was taken as the 5% thermogravimetric temperature, and the residual mass fraction at 700 °C was recorded.
[0088] Table 1
[0089] sample Structural regulation <![CDATA[Base adhesive viscosity / (×10 5 mPa·s)]]> Thermal conductivity / W / (m•K) Tensile strength / MPa Oil penetration ratio <![CDATA[T 5% / ℃]]> Example 1 Orientation Order 3.1 4.12 2.28 1.0612 337 Example 2 Orientation Order 4.9 5.68 2.87 1.0385 345 Example 3 Orientation Order 4.7 5.42 2.75 1.0410 348 Example 4 Orientation Order 8.2 6.35 2.52 1.0352 353 Comparative Example 1 disorder 4.2 3.69 1.95 1.0704 332 Comparative Example 2 disorder 6.8 4.72 2.38 1.0476 339
[0090] As can be seen from Table 1,
[0091] Under the same formulation conditions, the shear-induced filler orientation arrangement has a significant effect on reducing the apparent viscosity of the system. Compared with Comparative Example 1 (same formulation, disordered dispersion), Example 1 (600 parts AO-20, ordered orientation) showed a reduction in base adhesive viscosity from 4.2 × 10⁻⁶. 5 mPa·s decreased to 3.1 × 10 5The viscosity of Example 2 (900 parts compound, ordered orientation) decreased by 26.2% compared to Comparative Example 2 (same formulation, disordered dispersion), which had a viscosity of 6.8 × 10⁻⁶ mPa·s. 5 The mPa·s decreased to 4.9 × 10⁻⁶. 5 The viscosity decreased by 27.9% to mPa·s. These results indicate that, under the same total filler volume fraction, the orientation rearrangement of particle chains / clusters induced by the dynamic shear field can disrupt the randomly overlapping solid-like network, weaken the physical entanglement and friction between particles, and thus macroscopically manifest as a significant decrease in apparent viscosity, effectively improving the processability of the highly filled organosilicon system.
[0092] The synergistic effect of filler content and particle size on viscosity was further investigated. When the total filler content was increased from 600 parts (Example 1) to 900 parts (Example 2), the viscosity of the ordered system increased from 3.1 × 10⁻⁶ to 3.1 × 10⁻⁶. 5 The mPa·s increased to 4.9 × 10⁻⁶. 5 The viscosity of the polymer is 4.7 × 10⁻⁶ mPa·s, consistent with the general trend that the viscosity of highly filled polymer systems increases with increasing solid content. However, the presence of the oriented structure effectively suppresses the viscosity increase at the same filling level. It is noteworthy that in Example 3, with a total filler content of 900 parts, using AO-20 and AO-05 in a 3:1 mass ratio (675:225), the viscosity of the base adhesive was 4.7 × 10⁻⁶ mPa·s. 5 The concentration of mPa·s is slightly lower than that of the formulation in Example 2 (which uses AO-20 and AO-05 in a 2:1 mass ratio (600:300)) at 4.9 × 10⁻⁶ mPa·s. 5 This is attributed to the reduced number of high specific surface area small particles in the system of Example 3, which weakens the specific surface area of the filler and the interparticle interface, thus reducing interparticle interface interaction and frictional resistance, and decreasing particle slip resistance during shear flow. When the total filler content was further increased to 1200 parts (Example 4), the viscosity of the ordered system was 8.2 × 10⁻⁶ mPa·s. 5 Based on the viscosity-filler correlation law of highly filled silicone rubber, the viscosity of disordered systems with the same filler content is usually higher than 11.0 × 10⁻⁶ mPa·s. 5 This indicates that even under limiting filling conditions, shear-induced orientation can still reduce the system viscosity by more than 25%, maintaining the necessary process flowability.
[0093] Compared with Comparative Example 1, the thermal conductivity of Example 1 increased from 3.69 W / (m•K) to 4.12 W / (m•K), an increase of 11.7%; compared with Comparative Example 2, the thermal conductivity of Example 2 increased from 4.72 W / (m•K) to 5.68 W / (m•K), an increase of 20.3%. With the increase of the total filler volume fraction, the probability of interparticle adjacency increases, and the shear-induced orientational arrangement causes the particle chains / clusters to be oriented along the heat flow direction, reducing the interfacial thermal resistance and phonon scattering caused by random dispersion, thereby significantly improving the equivalent thermal conductivity of the composite material.
[0094] Comparing Example 2 (900 parts 2:1 blend, 5.68 W / (m•K)) and Example 3 (900 parts 3:1 blend, 5.42 W / (m•K)), it can be seen that, under the premise of the same total filler content, reducing the proportion of small-diameter fillers leads to a weakening of the filling and bridging effect between large particles, a reduction in the number of effective contact points between thermally conductive fillers, and a decrease in the continuity of the thermally conductive network. However, Example 4, with an ultra-high filler content of 1200 parts, achieved a thermal conductivity of 6.35 W / (m•K), indicating that when the filler volume fraction is sufficiently high, the synergistic effect of the dense packing and oriented structure formed by the dual-diameter blend can construct a more complete three-dimensional thermally conductive network, achieving a breakthrough in thermal conductivity.
[0095] The tensile strength of Example 1 was 2.28 MPa, which was 16.9% higher than that of Comparative Example 1 (1.95 MPa); the tensile strength of Example 2 was 2.87 MPa, which was 20.6% higher than that of Comparative Example 2 (2.38 MPa). This phenomenon can be attributed to two factors: firstly, the oriented filler network formed a more uniform stress-bearing skeleton in the polysiloxane matrix; secondly, the alumina surface-treated with γ-mercaptopropyltrimethoxysilane formed a stable chemical / physical interface with the matrix, which reduced the stress concentration effect, thus achieving simultaneous improvement in mechanical properties while improving thermal conductivity.
[0096] The oil penetration ratios in Examples 1 and 2 were 1.0612 and 1.0385, respectively, both lower than the corresponding disordered control group's 1.0704 and 1.0476. In Example 4, the oil penetration ratio further decreased to 1.0352 under high filler content. The closer the oil penetration ratio is to 1, the more restricted the migration of small silicone oil molecules within the cured network. The dense physical network formed by the oriented filler has a stronger binding ability on free silicone oil, thereby inhibiting oil phase precipitation during long-term thermal aging.
[0097] 5% thermogravimetric temperature (T) of Examples 1 and 2 5%The temperatures were 337 ℃ and 345 ℃, respectively. Compared with the comparative examples (332 ℃ and 339 ℃), no thermal stability deterioration was observed, proving that the surface modification of the filler and the high-filler orientation structure improved the processing and thermal conductivity without negatively affecting the intrinsic heat resistance of the material.
[0098] In summary, this invention achieves the oriented arrangement of thermally conductive fillers through shear induction, effectively reducing the apparent viscosity of the system at the same high filler content; by constructing directional heat conduction pathways, it significantly improves the effective thermal conductivity of the composite material, and the higher the filler content, the more significant the thermal conductivity gain; by using silane modification and homogenization of the filler network, it simultaneously improves the mechanical load-bearing performance and oil seepage resistance reliability; and by controlling the spatial organization of the high-concentration particle system through three-roll high shear and dynamic shear before curing, it enables the particle chains, clusters and their connecting pathways to form a statistically directional oriented ordered structure, thereby reducing the viscosity of the base adhesive and increasing its thermal conductivity, while maintaining or improving tensile strength, oil seepage behavior and thermal stability.
Claims
1. A low viscosity high thermal conductivity silicone gel with thermally conductive filler oriented alignment, characterized in that, Made from the following components in parts by weight: 100 parts by weight of vinyl-terminated silicone oil; 22.35–44.72 parts by weight of hydrogen-containing crosslinking agent; 600-1200 parts by weight of spherical alumina surface modified with silane coupling agent; Platinum catalyst, 0.1–0.5 parts by weight; 0.1 to 2.0 parts by weight of alkynol inhibitor.
2. The low viscosity high thermal conductivity silicone gel with thermally conductive filler oriented alignment according to claim 1, characterized in that, The spherical alumina modified by the silane coupling agent is composed of large-particle-size spherical alumina and small-particle-size spherical alumina treated with the silane coupling agent. The average particle size of the large-particle-size spherical alumina is 20-40 μm, and the average particle size of the small-particle-size spherical alumina is 1-5 μm.
3. The low viscosity high thermal conductivity silicone gel with thermally conductive filler oriented alignment according to claim 2, characterized in that, The mass ratio of the large-particle-size spherical alumina surface-treated with silane coupling agent to the small-particle-size spherical alumina surface-treated with silane coupling agent is 1:1 to 3:
1.
4. The low viscosity high thermal conductivity silicone gel with thermally conductive filler oriented alignment according to claim 1, characterized in that, The vinyl-terminated silicone oil is α,ω-vinyl-terminated polydimethylsiloxane; The hydrogen-containing crosslinking agent is hydrogen-terminated polydimethylsiloxane; The platinum catalyst mentioned is a Karstedt platinum catalyst; The alkynol inhibitor is 1-ethynyl-1-cyclohexanol.
5. The low viscosity high thermal conductivity silicone gel of claim 1, wherein the thermal conductive filler is oriented and aligned. The spherical alumina with surface modification of the silane coupling agent was prepared by the following method: the silane coupling agent was dissolved in anhydrous ethanol, and after being fully stirred and dispersed, large-particle-size or small-particle-size spherical alumina was added; the mixture was stirred at room temperature for 30 min, then heated to 60 °C and reacted for 4 h; after the reaction was completed, the mixture was filtered and the filter cake was repeatedly washed with anhydrous ethanol; then it was vacuum dried at 80 °C to obtain spherical alumina with surface silanization treatment.
6. The low viscosity high thermal conductivity silicone gel of claim 5, wherein the thermal conductive filler is oriented and arranged. The silane coupling agent is γ-mercaptopropyltrimethoxysilane.
7. The low viscosity high thermal conductivity silicone gel of claim 5, wherein the thermal conductive filler is oriented and arranged. The mass of the silane coupling agent is 0.5% to 4.0% of the mass of the spherical alumina.
8. The process for preparing a low viscosity high thermal conductivity silicone gel with thermally conductive filler oriented alignment as claimed in claim 1, wherein, The steps are as follows: (1) Add the spherical alumina modified with silane coupling agent to the vinyl-terminated silicone oil in batches. After premixing, use a three-roll mill with a roller speed ratio of 1:2:4 for high shear mixing to disperse and rearrange the filler and obtain the base rubber. (2) After adding a hydrogen-containing crosslinking agent and an alkynol inhibitor to the base adhesive for dispersion, a platinum catalyst is added to continue dispersion and degassing to obtain a curable mixture; (3) Before addition curing, a dynamic shear field is applied to the mixture to cause the thermally conductive filler to form an oriented arrangement in the flow field; After shearing is stopped, pressure is applied and cured while maintaining the orientation arrangement to form a polysiloxane crosslinking network and fix the filler orientation structure, thus obtaining the low viscosity and high thermal conductivity silicone gel.
9. The method for preparing a low-viscosity, high-thermal-conductivity silica gel with oriented thermally conductive fillers according to claim 8, characterized in that, In step (1), the premixing temperature is 120°C, the front roller speed is 80 rpm, the middle roller speed is 160 rpm, and the rear roller speed is 320 rpm; the roller spacing is gradually reduced to 5-20 μm, the mixing temperature is 80-120°C, and the mixture is repeatedly passed through the three-roll mill 2-4 times. In step (2), after high-speed dispersion under vacuum for 20 min, platinum catalyst is added, dispersion continues for 10 min, and then vacuum degassing is performed for 20 min. The dynamic shear field in step (3) is a dynamic rotary shear field, and the shear rate is 10-50 s -1 , the processing time is 5-15 min, and a pressure of 20 MPa is applied within 2 min after the shear is stopped, and the temperature is raised to 120 ℃ for curing for 30 min.
10. The application of the low-viscosity, high-thermal-conductivity silica gel with oriented thermally conductive filler as described in claim 8 as a thermal interface material.