A full-bio-based triboelectric composite film and a preparation method thereof, a device, system and method for hand health monitoring and evaluation
By constructing a bio-based triboelectric composite film, and utilizing electrostatic self-assembly and thermally induced amidation condensation reaction, the problems of difficult degradation and insufficient output performance of the triboelectric layer material were solved, realizing the industrial production of high-performance and degradable triboelectric composite films for application in hand health monitoring and assessment.
Patent Information
- Application Number
- CN202611404876.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-10
- Publication Date
- 2026-11-24
AI Technical Summary
The tribological layer materials of existing high-performance triboelectric nanogenerators are difficult to degrade, leading to environmental pollution. At the same time, they have low surface charge density, resulting in insufficient output performance. Furthermore, the preparation methods are complex, making it difficult to achieve industrial mass production.
By using biomacromolecules such as peanut protein isolate, chitosan, and ε-polylysine, a triboelectric composite film with rigid covalent and flexible non-covalent networks is constructed through electrostatic self-assembly and thermally induced amidation condensation reaction, forming a micro-nano rough morphology and increasing the effective contact area.
A triboelectric composite film with high electrical output performance and full biodegradability has been achieved, simplifying the preparation process, making it suitable for industrial production, and enabling its application in hand health monitoring and assessment.
Smart Images

Figure CN123152302A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of triboelectric nano-power generation technology, specifically to a fully bio-based triboelectric composite thin film and its preparation method, as well as a device, system, and method for hand health monitoring and assessment. Background Technology
[0002] Triboelectric nanogenerators (TENGs), based on the synergistic effect of contact electrification and electrostatic induction, can convert low-frequency mechanical energy in the environment into electrical energy. Due to their simple structure and wide range of material choices, they have become a research hotspot in the fields of distributed energy harvesting and self-driven sensing. However, the triboelectric layer of current high-performance triboelectric nanogenerators is mainly composed of synthetic polymers such as nylon, polyurethane, and polyvinylidene fluoride. Although these materials have excellent output performance, they are extremely difficult to degrade in the natural environment, and large-scale disposal will generate serious electronic waste and microplastic pollution. While replacing synthetic polymers with natural biomolecules can solve the degradation problem, their low surface charge density makes it difficult to meet application requirements in terms of output performance.
[0003] In existing technologies, to improve the triboelectric output of biomass materials, laser etching, freeze drying, or template methods are used to construct micro-nano rough structures on the material surface to increase the effective contact area. However, these methods rely on expensive high-end equipment, have complicated preparation steps, and often involve the use of toxic chemical solvents, which greatly limits industrial mass production. Summary of the Invention
[0004] The purpose of this invention is to provide a fully bio-based triboelectric composite film and its preparation method, a device, system and method for hand health monitoring and assessment, so that the composite film has both high electrical output performance and complete biodegradability, and can be industrialized for mass production.
[0005] To achieve the above objectives, the specific solution adopted by the present invention is as follows: a method for preparing a fully bio-based triboelectric composite thin film, comprising the following steps: Peanut protein isolate was dispersed in deionized water, and the pH of the resulting solution was adjusted to alkaline. The solution was stirred at 30-40℃ for 2-3 hours to obtain a homogeneous solution. Chitosan was dissolved in an aqueous acetic acid solution and stirred at 60°C for 4 hours to obtain a CS solution; ε-polylysine solution was added dropwise to the CS solution at a rate of 15-20 drops per minute to obtain a first mixed solution; a homogeneous solution was added dropwise to the first mixed solution at a rate of 15-20 drops per minute to obtain a second mixed solution; citric acid solution was added to the second mixed solution to obtain a third mixed solution, and the pH was adjusted to acidity; glycerol was added to the third mixed solution, and the solution was dried at 60°C to obtain a composite film.
[0006] As an optimized method for preparing the above-mentioned all-bio-based triboelectric composite film: the peanut protein isolate is obtained by alkaline dissolution and acid precipitation of defatted peanut meal, including: mixing defatted peanut meal with deionized water at a ratio of 1:10 (w / v), adding NaOH solution to adjust the pH to 9.0, stirring at 30-40℃, centrifuging, and taking the supernatant; adding hydrochloric acid solution to the supernatant to adjust the pH to 4.5, stirring, centrifuging, taking the precipitate, washing the precipitate with water until neutral, and freeze-drying to obtain peanut protein isolate.
[0007] As another optimized method for preparing the above-mentioned fully bio-based triboelectric composite film: the concentration of hydrochloric acid solution is 1 mol / L; the concentration of NaOH solution is 1 mol / L.
[0008] As another optimized scheme for the preparation method of the above-mentioned all-bio-based triboelectric composite film: the concentration of peanut protein isolate in the homogeneous solution is 2% (w / v); the ratio of chitosan to aqueous acetic acid is 200 mg: 10 mL; the ratio of ε-polylysine to deionized water in the ε-polylysine solution is 20 mg: 1 mL; the volume ratio of CS solution to ε-polylysine solution is 10:1.3; the volume ratio of homogeneous solution to CS solution is 1:1; the ratio of citric acid to deionized water in the citric acid solution is 100 mg: 1 mL, and the volume ratio of citric acid solution to CS solution is 1:50.
[0009] As another optimized method for preparing the above-mentioned fully bio-based triboelectric composite film, the concentration of the acetic acid aqueous solution is 2% (v / v).
[0010] A fully bio-based triboelectric composite thin film was prepared using the above-described preparation method.
[0011] A device for hand health monitoring and assessment includes a spherical base with multiple pressing flaps distributed circumferentially on the base. Each pressing flap is connected to a triboelectric sensing unit between itself and the base. The triboelectric sensing unit includes a first copper electrode layer attached to the inner wall of the pressing flap and a second copper electrode layer attached to the outer wall of the base. A positive friction layer is attached to the first copper electrode layer, and a negative friction layer is attached to the second copper electrode layer. The positive and negative friction layers are separable and contactable. The positive friction layer is made of the aforementioned composite film.
[0012] A hand health monitoring and assessment system includes a data acquisition unit and a data processing unit. The data acquisition unit includes the device described in claim 8. The data processing unit includes a data preprocessing module, a multi-scale feature extraction network, a channel weight adaptive recalibration module, a Transformer encoder, a metric learning module, and a joint training module. The data preprocessing module receives and preprocesses multi-channel data acquired by the device. The multi-scale feature extraction network captures the local instantaneous features of the preprocessed data for each channel. The channel weight adaptive recalibration module adaptively adjusts the feature weights of the corresponding channels. The Transformer encoder extracts the long-range spatiotemporal correlation features of the multi-channel signals. The metric learning module, based on triplet constraints, narrows the feature distance of similar actions or ipsilateral hand shapes in a low-dimensional embedding space, expands the heterogeneous decision boundary, and distinguishes weak asymmetric signals of the left and right hands. The joint training module combines classification loss and metric learning loss to optimize model parameters end-to-end.
[0013] Compared with the prior art, the present invention has the following beneficial effects: This invention provides a fully bio-based triboelectric composite film and its preparation method. ε-polylysine is added dropwise to a CS solution, utilizing the electrostatic adsorption between the high-density positively charged amino groups of ε-polylysine and the chitosan molecular chains to construct a three-dimensional precursor network. Subsequently, a homogeneous solution is added dropwise to trigger in-situ electrostatic self-assembly of the outer anionic sites of peanut protein isolate and the cationic segments of ε-polylysine. Finally, a citric acid solution is added, and the pH is adjusted to 5.0. This pH value falls precisely between the pKa1 (3.13), pKa2 (4.76), and pKa3 (6.40) of the three carboxyl groups in citric acid, allowing some carboxyl groups to remain protonated. During subsequent thermal drying, these carboxyl groups undergo a thermo-induced amidation condensation reaction with the primary amino groups of peanut protein isolate and chitosan, constructing a rigid covalent three-dimensional framework network. The remaining carboxyl groups dissociate into -COO groups. - As an electrostatic anchor point, -NH3 of ε-polylysine + The groups form strong electrostatic ion pairs, participating in the construction of flexible non-covalent networks. During the film formation process at 60℃, the rigid covalent network tends to maintain its original volume, while the flexible non-covalent domains undergo significant volume shrinkage as water evaporates. This results in a strong microscopic internal stress mismatch between the two network domains, driving the spontaneous in-situ evolution of micro-nano rough morphologies with spindle-shaped protrusions on the film surface. Attached Figure Description
[0014] Figure 1 This is a scanning electron microscope (SEM) image of the surface of the all-bio-based triboelectric composite film of the present invention.
[0015] Figure 2This is a comparison of the complete biodegradation process of the fully biobased triboelectric composite film of the present invention under natural soil burial conditions for different times (0 days, 7 days, 22 days).
[0016] Figure 3 This is a real-time short-circuit current response curve of the bio-based triboelectric composite film of the present invention under a 20-minute (1200-second) continuous contact-separation fatigue test.
[0017] Figure 4 This is a comparison chart of the output voltage stability changes of the fully bio-based triboelectric composite film of the present invention during a 21-day long-term storage process (0 days, 4 days, 7 days, 14 days, 21 days).
[0018] Figure 5 This is a graph showing the output voltage response of the all-bio-based triboelectric composite film of the present invention under different relative humidity environments (30% RH, 46% RH, 66% RH, 86% RH).
[0019] Figure 6 This is an exploded view of the structure of the hand health monitoring and assessment device of the present invention.
[0020] Figure 7 This is an isometric schematic diagram of the overall assembly structure of the hand health monitoring and assessment device of the present invention.
[0021] Figure 8 This is a diagram of the gripping test and host computer interaction interface of the hand health monitoring and assessment system of the present invention. Detailed Implementation
[0022] The technical solution of the present invention will be further described in detail below with reference to specific embodiments. Parts not described or disclosed in detail in the following embodiments of the present invention should be understood as prior art known or should be known by those skilled in the art.
[0023] A method for preparing a fully bio-based triboelectric composite thin film includes the following steps: Peanut protein isolate was dispersed in deionized water at a ratio of 200 mg:10 mL. The pH of the resulting solution was adjusted to alkaline using a 1 mol / L NaOH solution. The mixture was stirred at 30-40°C for 3 hours to obtain a 2% (w / v) homogeneous solution. Peanut protein isolate is obtained from defatted peanut meal through alkali dissolution and acid precipitation. Defatted peanut meal serves as the protein source, and its main chain contains abundant amide bonds and polar amino acid residues, providing a high density of electron-donating sites for the membrane and imparting positive triboelectric properties. Specifically, defatted peanut meal was mixed with deionized water at a ratio of 1:10 (w / v), and a 1 mol / L NaOH solution was added to adjust the pH to 9.0. The mixture was stirred at 30-40°C for 2-4 hours to ensure complete protein dissolution. The obtained solution was centrifuged at 3000-4000 r / min for 20-30 min, and the supernatant was collected. A 1 mol / L hydrochloric acid solution was added to the supernatant to adjust the pH to 4.5. After stirring for 25 min, the solution was centrifuged again at 3000-4000 r / min for 20-30 min, and the precipitate was collected. The precipitate was washed with water until neutral and then freeze-dried to obtain peanut protein isolate (PPI). The protein content of peanut protein isolate was 880.9 g / kg, that is, the protein content was ≥88%. As the main film-forming matrix of the composite film, its main chain contains abundant amide bonds and polar amino acid residues, which provide a high density of electron-donating sites for triboelectric charging and endow the film with positive triboelectric properties.
[0024] Chitosan (CS) was dissolved in an aqueous acetic acid solution at a ratio of 200 mg: 10 mL, and stirred at 60 °C for 4 h to obtain a 2% (w / v) CS solution. Chitosan, as a rigid framework of natural polysaccharides, forms an interpenetrating network when blended with peanut protein isolate, improving the mechanical support and film-forming properties of the composite film. The amino and hydroxyl groups on its molecular chain also act as hydrogen bond donors in the construction of the non-covalent network.
[0025] A citric acid solution with a concentration of 100 mg / mL and an ε-polylysine solution with a concentration of 20 mg / mL were prepared using deionized water. ε-polylysine (ε-PL) is rich in high-density primary amino groups (-NH3). + ), plays a triple role in the system: (1) as a polycationic electrolyte, it dissociates from citric acid (CA) -COO -Strong electrostatic complexes are formed, inducing the in-situ precipitation of ion-composite microcrystals, which act as deep charge traps to suppress triboelectric charge dissipation; (2) its large number of -NH sites act as hydrogen bond donors, significantly enhancing the density of non-covalent crosslinking networks; (3) high-density positive charge groups enhance the positive triboelectric output of the film. Citric acid plays a dual crosslinking role as a tricarboxylic acid: (1) some carboxyl groups undergo thermally induced amidation condensation with the primary amino group of PPI / CS to construct a covalent three-dimensional framework network, giving the film excellent hydrolysis resistance; (2) the remaining unreacted carboxyl groups dissociate into -COO under weakly acidic conditions. - As an electrostatically active site, it interacts with the -NH3 group of ε-polylysine. + Ion pairs are formed, participating in the construction of non-covalent networks. ε-polylysine solution is added dropwise to the CS solution at a rate of 15-20 drops per minute, with a volume ratio of CS solution to ε-polylysine solution of 10:1.3, and stirred for 15 min to obtain the first mixed solution. A three-dimensional precursor network is constructed using the electrostatic adsorption of the high-density positively charged amino groups of ε-polylysine with the chitosan molecular chains. A homogeneous solution is added dropwise to the first mixed solution at a rate of 15-20 drops per minute, with a volume ratio of homogeneous solution to CS solution of 1:1, and stirred for 25-30 min to obtain the second mixed solution. This triggers the in-situ electrostatic self-assembly of the outer anionic sites of peanut protein isolate with the cationic segments of ε-polylysine. Citric acid solution was added to the second mixed solution at a volume ratio of 1:50 to obtain the third mixed solution. The pH of the third mixed solution was adjusted to acidic using 1 mol / L NaOH solution. Glycerin was added to the third mixed solution and stirred for 10-20 min at a mass-to-volume ratio of 0.2 g:10 mL. Glycerin acts as a plasticizer to adjust the flexibility of the composite film and prevent it from cracking during drying. The mixture was cast into petri dishes, placed in a drying oven, and dried at 60 °C to obtain the composite film. This process allows some carboxyl groups to remain protonated, undergoing thermally induced amidation condensation with the primary amino groups of peanut protein isolate and chitosan during subsequent thermal drying to construct a rigid covalent three-dimensional framework network; while the remaining carboxyl groups dissociate into -COO groups. - As an electrostatic anchor point, -NH3 of ε-polylysine + The groups form strong electrostatic ion pairs, participating in the construction of flexible non-covalent networks. During the film formation process at 60℃, the rigid covalent network tends to maintain its original volume, while the flexible non-covalent domains undergo significant volume shrinkage as water evaporates. This results in a strong microscopic internal stress mismatch between the two network domains, driving the spontaneous in-situ evolution of micro-nano rough morphologies with spindle-shaped protrusions on the film surface.
[0026] The above method achieves stress-driven self-assembly within a dual-network structure through the synergistic effect of citric acid and ε-polylysine. Citric acid plays a dual cross-linking driving role in this process, simultaneously activating both the thermo-induced amidation covalent cross-linking pathway and the electrostatic ion pair non-covalent cross-linking pathway. Adjusting the pH to 5.0 achieves simultaneous activation of both pathways. ε-polylysine, on the other hand, performs a triple synergistic function: acting as a polycationic electrolyte and reacting with the -COO group dissociated from citric acid. - It forms a high-density electrostatic complex network; its large amount of -NH3 + The sites also act as strong hydrogen bond donors, strengthening the non-covalent hydrogen bond network; the ordered ionic composite microcrystals formed by electrostatic complexation act as deep charge traps during triboelectric charging, effectively capturing and storing the static charge generated by friction, inhibiting the rapid recombination and dissipation of charges, and their charge density is much higher than that provided by the amino groups of chitosan itself.
[0027] Only when citric acid and ε-polylysine coexist in the optimal ratio and the pH is precisely adjusted to 5.0 does the film surface spontaneously evolve an optimized micro / nano rough morphology. This spontaneous formation of the morphology increases the effective contact area by 3 to 5 times compared to a smooth protein film. The optimized film achieves an open-circuit voltage of 418.39 volts, and the in-situ generated ion-complex microcrystals act as deep charge traps, effectively suppressing the dissipation of triboelectric charge. Furthermore, the output performance is optimal when the ε-polylysine concentration is 6.5% by weight. Below this value, there are insufficient electrostatic complexation sites, while above this value, excessive free ε-polylysine segments act as charge recombination centers, accelerating charge neutralization and dissipation.
[0028] Example 1
[0029] A method for preparing a fully bio-based triboelectric composite thin film includes the following steps: S1. Defatted peanut meal and deionized water were mixed at a ratio of 1:10 (w / v), and a 1 mol / L NaOH solution was added to adjust the pH to 9.0. The mixture was stirred at 35°C for 3 hours to ensure complete protein dissolution. The resulting solution was centrifuged at 3500 rpm for 25 minutes, and the supernatant was collected. A 1 mol / L hydrochloric acid solution was added to the supernatant to adjust the pH to 4.5, and the mixture was stirred for 25 minutes. The mixture was then centrifuged again at 3500 rpm for 25 minutes, and the precipitate was collected. The precipitate was washed with water until neutral and then freeze-dried to obtain peanut protein isolate (PPI).
[0030] S2, 200 mg of peanut protein isolate was dispersed in 10 mL of deionized water, and the pH of the resulting solution was adjusted to 9.0 using a 1 mol / L NaOH solution. The solution was stirred at 33 °C for 4 h to obtain a 2% (w / v) homogeneous solution.
[0031] S3, 200 mg of chitosan was dissolved in 10 mL of acetic acid aqueous solution with a concentration of 2% (v / v), and stirred at 60 °C for 4 h to obtain a CS solution with a concentration of 2% (w / v).
[0032] S4. Prepare a citric acid solution with a concentration of 100 mg / mL and an ε-polylysine solution with a concentration of 20 mg / mL using deionized water. Add 1.3 mL of the ε-polylysine solution to 10 mL of CS solution at a rate of 17 drops per minute and stir for 15 min to obtain the first mixed solution. Add 10 mL of homogeneous solution to the first mixed solution at a rate of 17 drops per minute and stir for 30 min to obtain the second mixed solution. Add 0.2 mL of citric acid solution to the second mixed solution to obtain the third mixed solution. Adjust the pH of the third mixed solution to 5.0 using 1 mol / L NaOH solution. Add 200 mg of glycerol to the third mixed solution and stir for 15 min.
[0033] S5. The mixture is poured into a petri dish, placed in a drying oven, and dried at 60°C to obtain a composite film.
[0034] The prepared composite film, such as Figure 1 As shown, the "spindle-shaped protrusions" micro-nano rough morphology spontaneously forms without any external templates or photolithography processes. The entire fabrication process is completed under normal pressure and 60°C conditions, making it simple to operate and easy to scale up for mass production.
[0035] Example 2
[0036] A method for preparing a fully bio-based triboelectric composite thin film includes the following steps: S1. Defatted peanut meal and deionized water were mixed at a ratio of 1:10 (w / v), and a 1 mol / L NaOH solution was added to adjust the pH to 9.0. The mixture was stirred at 30°C for 4 hours to ensure complete protein dissolution. The resulting solution was centrifuged at 3000 rpm for 30 minutes, and the supernatant was collected. A 1 mol / L hydrochloric acid solution was added to the supernatant to adjust the pH to 4.5, and the mixture was stirred for 25 minutes. The mixture was then centrifuged again at 3000 rpm for 30 minutes, and the precipitate was collected. The precipitate was washed with water until neutral and then freeze-dried to obtain peanut protein isolate (PPI).
[0037] S2, 200 mg of peanut protein isolate was dispersed in 10 mL of deionized water, and the pH of the resulting solution was adjusted to 9.0 using a 1 mol / L NaOH solution. The solution was stirred at 30 °C for 4 h to obtain a 2% (w / v) homogeneous solution.
[0038] S3, 200 mg of chitosan was dissolved in 10 mL of acetic acid aqueous solution with a concentration of 2% (v / v), and stirred at 60 °C for 4 h to obtain a CS solution with a concentration of 2% (w / v).
[0039] S4. Prepare a citric acid solution with a concentration of 100 mg / mL and an ε-polylysine solution with a concentration of 20 mg / mL using deionized water. Add 1.3 mL of the ε-polylysine solution to 10 mL of CS solution at a rate of 15 drops per minute and stir for 15 min to obtain the first mixed solution. Add 10 mL of homogeneous solution to the first mixed solution at a rate of 15 drops per minute and stir for 30 min to obtain the second mixed solution. Add 0.2 mL of citric acid solution to the second mixed solution to obtain the third mixed solution. Adjust the pH of the third mixed solution to 5.0 using 1 mol / L NaOH solution. Add 200 mg of glycerol to the third mixed solution and stir for 15 min.
[0040] S5. The mixture is poured into a petri dish, placed in a drying oven, and dried at 60°C to obtain a composite film.
[0041] Example 3
[0042] A method for preparing a fully bio-based triboelectric composite thin film includes the following steps: S1. Defatted peanut meal and deionized water were mixed at a ratio of 1:10 (w / v), and a 1 mol / L NaOH solution was added to adjust the pH to 9.0. The mixture was stirred at 40°C for 3 hours to ensure complete protein dissolution. The resulting solution was centrifuged at 4000 rpm for 20 minutes, and the supernatant was collected. A 1 mol / L hydrochloric acid solution was added to the supernatant to adjust the pH to 4.5, and the mixture was stirred for 25 minutes. The mixture was then centrifuged again at 4000 rpm for 20 minutes, and the precipitate was collected. The precipitate was washed with water until neutral and then freeze-dried to obtain peanut protein isolate (PPI).
[0043] S2, 200 mg of peanut protein isolate was dispersed in 10 mL of deionized water, and the pH of the resulting solution was adjusted to 9.0 using a 1 mol / L NaOH solution. The solution was stirred at 35 °C for 4 h to obtain a 2% (w / v) homogeneous solution.
[0044] S3, 200 mg of chitosan was dissolved in 10 mL of acetic acid aqueous solution with a concentration of 2% (v / v), and stirred at 60 °C for 4 h to obtain a CS solution with a concentration of 2% (w / v).
[0045] S4. Prepare a citric acid solution with a concentration of 100 mg / mL and an ε-polylysine solution with a concentration of 20 mg / mL using deionized water. Add 1.3 mL of the ε-polylysine solution to 10 mL of CS solution at a rate of 20 drops per minute and stir for 15 min to obtain the first mixed solution. Add 10 mL of homogeneous solution to the first mixed solution at a rate of 20 drops per minute and stir for 30 min to obtain the second mixed solution. Add 0.2 mL of citric acid solution to the second mixed solution to obtain the third mixed solution. Adjust the pH of the third mixed solution to 5.0 using 1 mol / L NaOH solution. Add 200 mg of glycerol to the third mixed solution and stir for 15 min.
[0046] S5. The mixture is poured into a petri dish, placed in a drying oven, and dried at 60°C to obtain a composite film.
[0047] Example 4
[0048] A device for hand health monitoring and assessment is manufactured using polylactic acid (PLA) material through 3D printing. The device includes a spherical base 1 with multiple circumferentially distributed pressing flaps 6. The spherical base 1 is a hollow structure. There are five pressing flaps 6, corresponding one-to-one with the five fingers of the human body. The pressing flaps 6 are arc-shaped, and correspondingly, the outer wall of the spherical base 1 has facets that correspond to the pressing flaps 6. The ergonomic curvature of the pressing flaps 6 corresponds to the contact position of the five fingers when the human body grasps the object. A triboelectric sensing unit is disposed between each pressing flap 6 and the spherical base 1, forming a 5-channel independent decoupled sensing structure, generating 5 channels of signals. The triboelectric sensing unit includes a first copper electrode layer 5 attached to the inner wall of the pressing flap 6 and a second copper electrode layer 2 attached to the outer wall of the spherical base 1. A positive friction layer 4 is attached to the first copper electrode layer 5, and a negative friction layer 3 is attached to the second copper electrode layer 2. The positive friction layer 4 and the negative friction layer 3 can be separated and contacted. The positive friction layer 4 is prepared from a composite film prepared by the method described in Example 1. Specifically, the first copper electrode layer 5 is attached to the inner wall of the pressing flap 6 as an outer conductive electrode; the second copper electrode layer 2 is attached to the outer wall of the spherical base 1 corresponding to the pressing flap 6 as an inner conductive electrode. The positive friction layer 4 and the negative friction layer 3 remain separated in their initial natural state, that is, they are in a separated state when no force is applied.
[0049] In this embodiment, the positive friction layer 4 and the negative friction layer 3 are kept separated by a return spring 7. Specifically, the spherical base 1 has multiple mounting holes 102, and a return spring 7 for separating the positive friction layer 4 and the negative friction layer 3 is installed in each mounting hole 102. One end of the return spring 7 abuts against the mounting hole 102, and the other end of the return spring 7 abuts against the pressing flap 6. In this embodiment, each pressing flap 6 is kept separated from the positive friction layer 4 and the negative friction layer 3 by two return springs 7, with the two return springs 7 located at opposite ends of the pressing flap 6. Correspondingly, the number of mounting holes 102 on the spherical base 1 corresponds one-to-one with the number of return springs 7. Figure 6 As shown, two opposing bosses 101 are fixedly mounted on the spherical base 1, and mounting holes 102 are formed on the bosses 101. After a finger presses down, the return spring 7 provides a stable radial elastic force, driving the pressing flap 6 to quickly rebound to the initial separation position.
[0050] To limit and guide the movement of the return spring 7, the inner walls of both ends of the pressing flap 6 are integrally provided with radially extending positioning cylinders. The bottom of the mounting hole 102 is provided with a limiting boss, and the center of the limiting boss has a clearance through hole for the positioning cylinder to slide into. The return spring 7 is sleeved on the outer periphery of the positioning cylinder, with one end of the return spring 7 abutting against the inner wall of the pressing flap 6, and the other end of the return spring 7 inserted into the mounting hole 102 and abutting against the limiting boss. When the finger presses the pressing flap 6, the positioning cylinder slides smoothly through the clearance through hole without obstruction, and the return spring 7 is smoothly compressed and reset axially under the support of the positioning cylinder and the constraint of the outer wall of the mounting hole 102.
[0051] Several guide posts 601 are fixedly installed on the pressing flap 6, and multiple guide holes 103 corresponding one-to-one with the guide posts 601 are opened on the spherical base 1. Each pressing flap 6 has four guide posts 601, which are evenly divided into two groups. The two groups of guide posts 601 are located at both ends of the pressing flap 6, and the guide posts are inserted into the guide holes 103 to limit the circumferential tangential displacement and left and right translational sway of the pressing flap 6 during the force process.
[0052] The device works as follows: when the subject presses with one finger or grasps with the whole hand, the finger applies force to push the pressing flap 6 to overcome the elastic force and move it towards the axis of the spherical base 1, causing the positive friction layer 4 and the negative friction layer 3 to make close contact and generate electricity; after releasing the hand, they quickly separate under the action of the return spring 7, thereby generating a transient pulse voltage signal with a high signal-to-noise ratio between the first copper electrode layer 5 and the second copper electrode layer 2, that is, forming a 5-channel signal.
[0053] Example 5
[0054] A hand health monitoring and assessment system includes a data acquisition unit and a data processing unit. The data acquisition unit includes the aforementioned device, and the data processing unit includes a data preprocessing module, a multi-scale feature extraction network, a channel weight adaptive recalibration module, a Transformer encoder, a metric learning module, and a joint training module.
[0055] The data preprocessing module is used to receive and preprocess the multi-channel data collected by the device. It performs digital filtering, instance normalization and adaptive data enhancement on the original 5-channel time-series voltage signal collected by the device. It locks the core power-on segment by centering the peak and incorporates a small amount of random noise and amplitude scaling to expand the sample space boundary, improve the data quality and convert it into a format suitable for model input.
[0056] The multi-scale feature extraction network captures the local transient features of voltage signals in each channel through parallel convolutional kernels with different receptive fields, enabling comprehensive perception of triboelectric waveforms at different time scales.
[0057] The channel weight adaptive recalibration module models the interdependencies between channels and adaptively adjusts the feature weights of the channel corresponding to the currently exerting finger, thereby suppressing signal crosstalk from inactive fingers and environmental background noise.
[0058] The Transformer encoder models the long-range dependencies of multi-channel signals over time and extracts cross-channel spatiotemporal correlation features.
[0059] The metric learning module is based on triple constraints. Using the current signal features as anchors, it reduces the feature distance of similar actions or same-side hand shape samples in the low-dimensional embedding space, expands the decision boundary with dissimilar samples, and significantly improves the ability to distinguish weak asymmetric signals of the left and right hands.
[0060] The joint training module combines metric learning loss with classification loss to optimize the model end-to-end, balancing feature representation capability and classification accuracy. It evaluates classification performance through a confusion matrix and transforms triboelectric waveforms into four clinical indicators—strength, flexibility, endurance, and coordination—through a four-dimensional quantitative dashboard, providing interpretable quantitative assessment data for early screening and rehabilitation training of tendon injuries in rock climbers.
[0061] The system in this embodiment improves electrical output performance while maintaining the complete biodegradability of the composite film. The constructed multi-channel self-powered intelligent hand health monitoring system, combined with the MSI-Transformer fusion deep metric learning algorithm, effectively improves model efficiency and left / right hand recognition accuracy, balances computing resources and real-time requirements, and promotes its widespread application in the field of wearable sports rehabilitation monitoring.
[0062] Example 6
[0063] A method for monitoring and assessing hand health includes the following steps: S1 (Signal Acquisition and Wireless Transmission): The device in Example 4 is attached to the subject's hand to acquire the multi-channel triboelectric response voltage signal emitted by the subject under single-finger pressing or full-hand grasping action. When the subject performs single-finger pressing or full-hand grasping action, the positive and negative friction layers inside each sensing unit periodically contact and separate under the action of the return spring, generating 5 independent transient triboelectric response voltage signals, and sending the 5 channels of raw timing voltage signals to the data processing unit through the Bluetooth wireless transmission module.
[0064] S2 (Signal Preprocessing and Adaptive Data Augmentation): The data preprocessing module of the data processing unit performs digital bandpass filtering on the received 5-channel raw timing voltage signal to remove high-frequency noise, uses instance normalization to eliminate amplitude deviation caused by contact resistance and pressure difference, and locks the core power-on waveform segment through peak centering algorithm. It then incorporates a small amount of random noise and random amplitude scaling into the core power-on waveform segment to complete adaptive data augmentation.
[0065] Step S3 (Multi-scale Local Feature Extraction): The multi-scale feature extraction network uses parallel convolutional kernels with different receptive fields to perform multi-scale feature extraction on the preprocessed 5-channel time-series voltage signal, capturing the local transient features of the waveform of each channel.
[0066] S4 (Channel Weight Adaptive Recalibration): The channel weight adaptive recalibration module models the interdependencies between the five channels, adaptively amplifies the feature weights of the channel corresponding to the currently exerting finger, and suppresses signal crosstalk and environmental background noise in the channel of the inactive finger.
[0067] S5 (Long-range Spatiotemporal Feature Encoding): The Transformer encoder receives the recalibrated feature sequence and extracts the cross-channel long-range spatiotemporal correlation features of the 5-channel signal in the time series through a self-attention mechanism.
[0068] S6 (Deep Metric Learning and Asymmetric Space Mapping): The metric learning module, based on triple constraints, maps long-range spatiotemporal correlation features to a low-dimensional embedding space, narrowing the feature distance between similar actions or same-side hand shape samples, expanding the decision boundary with dissimilar samples, and extracting weak asymmetric features of left and right hand force patterns.
[0069] S7 (Joint Classification and State Recognition): The joint training module combines classification loss and metric learning loss to optimize the model end-to-end. Based on the confidence probability distribution of the network output, it classifies and outputs the subject's force-applying hand (left or right hand) and action category (full hand grasping or specific single-finger pressing) in real time.
[0070] S8 (Four-Dimensional Health Indicator Quantification and Assessment Display): The assessment system converts the decoupled 5-channel triboelectric waveform into quantitative indicators of hand function and displays them on the host computer interface: grip strength is assessed by transient peak voltage, neuromuscular flexibility is assessed by transient signal response time, endurance is assessed by the amplitude decay trend of continuous gripping cycle waveform, and finger coordination is assessed by the consistency of arrival time of characteristic peaks in each channel, thus realizing a quantitative assessment of the subject's hand health and rehabilitation status.
[0071] <Degradability> The composite film from Example 1 was buried in natural soil, and the degradation process of the composite film was as follows: Figure 2 As shown in the figure, the composite film completely degrades within 22 days and integrates with the surrounding soil without any solid residue, thus solving the problem of electronic waste pollution caused by traditional friction materials at its source.
[0072] <Electrical Output Performance> Example 1 prepared a composite thin film, and its electrical output performance was tested. The results showed that at a working frequency of 9 Hz, a separation distance of 8 mm, and a diameter of 4 × 4 cm, the film performed well. 2 Under the given contact area conditions, an open-circuit voltage of 418.7V, a short-circuit current of 15.9μA, and a transferred charge of 32.8nC were achieved. With a 10MΩ matched load, a peak power density of 564.3mW / m² was achieved. 2 It can simultaneously light up 182 commercial LEDs and drive the digital temperature and humidity meter to work normally.
[0073] <Fatigue resistance> The composite film prepared in Example 1 was subjected to a continuous 20-minute contact-separation fatigue test. The results showed that the short-circuit current waveform was sharp and uniform, without distortion, and the baseline was stable. Figure 3 As shown.
[0074] <Stability> The composite film prepared in Example 1 was subjected to stability testing. During a 21-day storage test, the output voltage showed no significant attenuation. Figure 4 As shown.
[0075] <Environmental adaptability> The composite film prepared in Example 1 was subjected to environmental adaptability testing. The results showed that it maintained a clear and discernible electrical output within a relative humidity range of 30%-86%. Figure 5 As shown.
[0076] <Accuracy> The evaluation system achieves high-precision recognition. It can achieve spatial independent decoupling of the five finger channels. When the whole hand is grasping, the five channels burst synchronously. When a single finger is pressed, only the corresponding channel generates a pulse while the other channels maintain the baseline noise level. Combining MSI-Transformer and deep metric learning algorithms, the recognition accuracy of six core hand movements reaches 99.1%, and the accuracy of left and right hand shape discrimination reaches 97.7%.
[0077] The above description of the disclosed embodiments enables those skilled in the art to make or use the invention. Various modifications to these embodiments will be readily apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the invention. Therefore, the invention is not to be limited to the embodiments shown herein, but is to be accorded the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A method for preparing a fully biobased triboelectric composite film, characterized in that, Includes the following steps: Peanut protein isolate was dispersed in deionized water, and the pH of the resulting solution was adjusted to alkaline. The solution was stirred at 30-40℃ for 2-3 hours to obtain a homogeneous solution. Chitosan was dissolved in an aqueous acetic acid solution and stirred at 60°C for 4 hours to obtain a CS solution; ε-polylysine solution was added dropwise to the CS solution at a rate of 15-20 drops per minute to obtain the first mixed solution; A homogeneous solution is added dropwise to the first mixed solution at a rate of 15-20 drops per minute to obtain a second mixed solution; Add citric acid solution to the second mixed solution to obtain a third mixed solution, and adjust the pH to acidic. After adding glycerol to the third mixed solution, the mixture was dried at 60°C to obtain a composite film.
2. The method for preparing a fully bio-based triboelectric composite thin film as described in claim 1, characterized in that: The peanut protein isolate is obtained by alkaline dissolution and acid precipitation of defatted peanut meal, comprising: mixing defatted peanut meal with deionized water at a ratio of 1:10 (w / v), adding NaOH solution to adjust the pH to 9.0, stirring at 30-40℃, centrifuging, and collecting the supernatant; adding hydrochloric acid solution to the supernatant to adjust the pH to 4.5, stirring, centrifuging, collecting the precipitate, washing the precipitate with water until neutral, and freeze-drying to obtain peanut protein isolate.
3. The method of claim 2, wherein the method further comprises: The concentration of the hydrochloric acid solution is 1 mol / L; the concentration of the NaOH solution is 1 mol / L.
4. The method for preparing a fully bio-based triboelectric composite thin film as described in claim 1, characterized in that: The concentration of peanut protein isolate in the homogeneous solution was 2% (w / v); the ratio of chitosan to aqueous acetic acid was 200 mg: 10 mL; the ratio of ε-polylysine to deionized water in the ε-polylysine solution was 20 mg: 1 mL; the volume ratio of CS solution to ε-polylysine solution was 10:1.3; the volume ratio of homogeneous solution to CS solution was 1:1; the ratio of citric acid to deionized water in the citric acid solution was 100 mg: 1 mL, and the volume ratio of citric acid solution to CS solution was 1:
50.
5. The method for preparing a fully bio-based triboelectric composite thin film as described in claim 1, characterized in that: The concentration of the acetic acid aqueous solution is 2% (v / v).
6. A fully biobased triboelectric composite film, characterized in that: It is prepared by the preparation method described in any one of claims 1-5.
7. A device for monitoring and assessing hand health, characterized in that: The device includes a spherical base (1) on which a plurality of pressing flaps (6) are arranged along its circumference. Each pressing flap (6) is provided with a triboelectric sensing unit between it and the spherical base (1). The triboelectric sensing unit includes a first copper electrode layer (5) attached to the inner wall of the pressing flap (6) and a second copper electrode layer (2) attached to the outer wall of the spherical base (1). A positive friction layer (4) is attached to the first copper electrode layer (5) and a negative friction layer (3) is attached to the second copper electrode layer (2). The positive friction layer (4) and the negative friction layer (3) can be separated and contacted. The positive friction layer (4) is made of the composite film described in claim 6.
8. The hand health monitoring and assessment device as described in claim 7, characterized in that: The spherical base (1) has multiple mounting holes (102). A reset spring (7) for separating the positive friction layer (4) and the negative friction layer (3) is provided in the mounting hole (102). One end of the reset spring (7) abuts against the mounting hole (102), and the other end of the reset spring (7) abuts against the pressing flap (6).
9. The device for hand health monitoring and assessment as described in claim 8, characterized in that: The pressing flap (6) is fixedly provided with several guide posts (601), and the spherical base (1) is provided with multiple guide holes (103) that correspond one-to-one with the guide posts (601).
10. A system for monitoring and assessing hand health, characterized in that: The system includes a data acquisition unit and a data processing unit. The data acquisition unit includes the apparatus described in any one of claims 7 to 9. The data processing unit includes a data preprocessing module, a multi-scale feature extraction network, a channel weight adaptive recalibration module, a Transformer encoder, a metric learning module, and a joint training module. The data preprocessing module receives and preprocesses the multi-channel data acquired by the apparatus. The multi-scale feature extraction network captures the local instantaneous features of the preprocessed data for each channel. The channel weight adaptive recalibration module adaptively adjusts the feature weights of the corresponding channels. The Transformer encoder extracts the long-range spatiotemporal correlation features of the time series of the multi-channel signals. The metric learning module is used to narrow the distance between similar actions or ipsilateral hand features in the low-dimensional embedding space based on triple constraints, expand the decision boundary of dissimilar classes, and distinguish weak asymmetric signals of the left and right hands; the joint training module is used to combine classification loss and metric learning loss to optimize model parameters end-to-end.